Phenolphthalein polyarylene ether nitrile modified bismaleimide-triazine resin and preparation method of glass fiber reinforced composite material of phenolphthalein polyarylene ether nitrile modified bismaleimide-triazine resin
By introducing phenolphthalein-type polyarylethernitrile and grading temperature control treatment in bismaleimide-triazine resin, the problem of insufficient mechanical properties of bismaleimide-triazine resin is solved, and the integration of materials is significantly improved Performance, suitable for high-frequency printed circuit boards and other fields.
Patent Information
- Application Number
- CN202411206583.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-30
- Publication Date
- 2024-11-22
AI Technical Summary
The mechanical properties of bismaleimide-triazine resin and its composite materials are poor, including poor bending performance, interlayer performance and impact performance, which limits its application in high-frequency printed circuit boards and other fields.
Phenolphthalein polyarylethernitrile as toughening agent blended with bismaleimide-triazine resin, and prepared phenolphthalethalethalethalethalethalethalethalethalethalethalethalethalethalethalethalethalethalethalethalethalethalethalethalethalethalethalethalethalethalethalethalethalethalethalethalethalethalethalethalethalethalethalethalethalethalethalethalethalethalethalethalethalethalethalethalethalethalethalethalethalethalethalethalethalethalethalethalethalethalethalethalethalethalethalethalethalethalethalethalethalethalethalethalethalethalethalethalethalethalethalethalethalethalethalethalethalethalethalethalethalethalethalethalethalethalethalethalethalethalethalethalethalethalethalethalethalethalethalethalethalethalethalethalethalethalethalethalethalethalethalethalethalethalethalethalethalethalethalethalethalethalethalethalethalethalethalethalethalethalethalethalethalethalethalethalethale Amines-triazine resin and its glass fiber reinforced composite materials improve their mechanical properties and heat resistance.
It significantly improves the comprehensive performance of the material, including bending, interlayer shear and impact performance, expanding its application prospects in the field of electronic materials.
Smart Images

Figure CN118994905A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of polymer materials, and relates to a preparation method of a phenolphthalein type polyarylethernitrile modified bismaleimide-triazine resin having the characteristics of low temperature curing, high heat resistance, high moisture resistance, low expansion coefficient, and the like, and a glass fiber reinforced composite material having excellent mechanical properties. Technical Background
[0002] With the development of high-frequency and high-speed communications, the comprehensive performance requirements of printed circuit board substrates are getting higher and higher. Bismaleimide-triazine (BT) resin is a thermosetting resin formed by bismaleimide and cyanate ester as the main resin components. BT resin combines the advantages of the two components. It not only has a low dielectric constant and extremely small dielectric loss, but also has good heat resistance and moisture resistance. Glass fiber reinforced BT resin composites meet the needs of high frequency, high functionality, high signal transmission and harsh environment, and have been successfully used in high-frequency printed circuit boards (PCBs), high-performance wave-transmitting structural materials, strong electric field electrical product materials, aerospace structural composite materials and other fields. However, due to its poor mechanical properties, including bending performance, interlayer performance and impact performance, which need to be improved urgently, its practical application is limited, so it needs to be modified in processing technology and performance.
[0003] Although patent CN116425977A discloses a method for preparing phthalonitrile-type bismaleimide-triazine resin with the characteristics of low-temperature curing, high glass transition temperature, high initial decomposition temperature, etc., BT resin, as a thermosetting resin, has the inherent brittleness of the group cross-linked network, resulting in poor impact toughness and interlaminar shear performance of BT resin and its composite materials, limiting the further expansion of its application field. Summary of the invention
[0004] The purpose of the present invention is to provide a method for preparing a phenolphthalein type polyarylether nitrile modified bismaleimide-triazine resin and a glass fiber reinforced composite material thereof in view of the above problems. The present invention uses phthalonitrile as a curing agent, adopts phenolphthalein type polyarylether nitrile to blend and modify bismaleimide-triazine resin, and after the formed copolymer is stirred evenly, a graded temperature control treatment is adopted to prepare the phenolphthalein type polyarylether nitrile modified bismaleimide-triazine resin; finally, the bismaleimide-triazine resin is evenly coated on glass fiber, hot-pressed and formed to prepare the glass fiber reinforced composite material thereof.
[0005] The preparation method of the phenolphthalein type polyarylethernitrile modified bismaleimide-triazine resin and the glass fiber reinforced composite material system provided by the present invention is simple, and while improving the mechanical properties of the bismaleimide-triazine resin, the heat resistance, dielectric properties and moisture resistance thereof can also be improved, and the resin has a broader application prospect in the field of electronic materials.
[0006] In order to achieve the above object, the technical solution provided by the present invention is as follows:
[0007] Provided is a method for preparing a phenolphthalein type polyarylethernitrile modified bismaleimide-triazine resin and a glass fiber reinforced composite material thereof, which specifically comprises the following steps:
[0008] (1) Preparation of phenolphthalein type poly(arylene ether nitrile) modified bismaleimide-triazine resin prepolymer. Composite resins with various ratios were prepared by adding different amounts of poly(arylene ether nitrile).
[0009] Specifically, the content of phenolphthalein polyarylethernitrile affects the curing temperature of the resin. At the same curing temperature, resins with different curing degrees are prepared, resulting in differences in various properties. At the same time, the phase structures of the blends with different contents are different, and the single phase, dual continuous phase, and phase separation structures formed have different effects on the thermal properties, dielectric properties, and moisture resistance of the material. Therefore, by adjusting different proportions, the resin and its composite with the best comprehensive performance are selected.
[0010] (2) Preparation of phenolphthalein type poly(arylene ether nitrile) modified bismaleimide-triazine resin, and obtaining a resin system with excellent performance through graded temperature control.
[0011] Specifically, by controlling the curing process, extending the curing time, and improving the curing degree of the resin, the mechanical properties are more excellent. However, if the curing time is too long, the dielectric properties of the resin will increase. By adjusting the graded curing process and curing time, the cross-linking density can be regulated to prepare the resin with the best comprehensive performance.
[0012] (3) Preparation of phenolphthalein type poly(arylene ether nitrile) modified bismaleimide-triazine resin glass fiber reinforced composite materials. By adjusting the coating resin content, hot pressing pressure, temperature and time, a composite material with excellent performance was obtained.
[0013] Specifically, the different coating resin content will affect the content and uniformity of the resin on the glass fiber after coating. The hot pressing pressure affects the composite molding effect. If the pressure is too low, the resin and glass fiber are not firmly bonded, and the delamination phenomenon is serious; if the pressure is too high, the glue flow phenomenon is serious. The hot pressing temperature and time affect the curing degree of the resin, resulting in differences in various properties.
[0014] It should be noted that BT resin usually has a high cross-linking density and rigid structure to ensure excellent heat resistance and moisture resistance. However, the interpenetrating polymer network formed after cross-linking of CE resin and BMI resin increases the inherent brittleness of the cross-linking network, resulting in poor impact toughness and interlaminar shear performance of BT resin and its composite materials, which seriously limits the further expansion of its application field. Polyarylethernitrile is a thermoplastic polymer with aromatic rings and ether bonds as the main chain and cyanide side groups. It has the characteristics of high toughness, high strength, high modulus, high temperature resistance, good dimensional stability, and excellent electrical properties. The single cyanide group of polyarylethernitrile can be catalyzed in the preparation of the resin system, and phthalonitrile is more likely to generate triazine rings, so an appropriate amount of polyarylethernitrile can effectively improve the dielectric properties of the material.
[0015] Furthermore, phenolphthalein type polyarylethernitrile (PP-PEN) has a high glass transition temperature and better solubility and processing performance. This thermoplastic polymer is blended with BT resin to form a co-soluble homogeneous toughened structure, which can improve its thermal stability, mechanical properties, etc. to varying degrees.
[0016] Furthermore, the phenolphthalein type polyarylether nitrile modified bismaleimide-triazine resin prepolymer is composed of bismaleimide, cyanate, phenolphthalein type polyarylether nitrile, curing agent and solvent system; wherein bismaleimide and cyanate are blended at 80-140°C for 10-40 minutes in a mass ratio of (50-100): (20-50), then blended at 80-140°C for 10-40 minutes, and a curing agent is added and blended for 10-20 minutes to complete the control index of 200°C gelation time, thereby obtaining a bismaleimide-triazine resin prepolymer; 5-30 parts of phenolphthalein type polyarylether nitrile are added to 50-80 parts of N,N-dimethylformamide, and after stirring and dispersing evenly, the solution is added to the bismaleimide-triazine resin prepolymer, and copolymerization is performed to obtain a phenolphthalein type polyarylether nitrile modified bismaleimide-triazine resin prepolymer;
[0017] Furthermore, the types of bismaleimide are mainly diphenylmethane bismaleimide, N,N'-m-phenylene bismaleimide, N,N'-(1,4-phenylene) bismaleimide, 1,2-bis(maleimide)ethane and N,N'-tetramethylene bismaleimide, and their structures are as follows:
[0018]
[0019] The types of cyanate esters are mainly bisphenol A cyanate ester, phenol AF cyanate ester, bisphenol F cyanate ester, bisphenol E cyanate ester and bisphenol M cyanate ester, and their structures are as follows:
[0020]
[0021] The types of curing agents are mainly 3-APN, 4-APN and 4-aminophthalonitrile, and their structures are as follows:
[0022]
[0023] The phenolphthalein type polyarylethernitrile has the following structure:
[0024]
[0025] Furthermore, the solvent for dissolving the phenolphthalein type poly(arylene ether nitrile) is mainly N,N-dimethylformamide.
[0026] Furthermore, the preparation of the phenolphthalein type polyarylether nitrile modified bismaleimide-triazine resin is as follows: the copolymer is cast into a preheated mold, vacuum-debubbled at 120°C, and subjected to graded temperature control treatment at 140-240°C. After the heat treatment, the copolymer is naturally cooled to room temperature, and demolded to obtain the phenolphthalein type polyarylether nitrile modified bismaleimide-triazine resin. Adjusting the holding time at different temperatures for 1-4 hours can change the performance indicators of the final product, such as the thermal expansion coefficient, initial decomposition temperature, dielectric constant and dielectric loss, and moisture resistance.
[0027] Furthermore, a prepolymer of phenolphthalein type polyarylethernitrile modified bismaleimide-triazine resin with a glue content of 30-70 is uniformly coated on electronic grade glass fiber with a surface density of 150-240, a length of 15-20 cm, and a width of 12-18 cm according to a mass ratio of 30-80 of prepolymer resin solution and 30-60 of glass fiber, and is placed in a blast oven. After drying, 10-15 sheets of the composite material are heat treated for 2 hours at 220-240° C. and 20-30 MPa in a hot press, and finally the heat resistance, dielectric properties and comprehensive mechanical properties (bending, interlaminar shear, and impact properties) of the glass fiber reinforced material are improved.
[0028] Compared with the prior art, the beneficial effects of the present invention are as follows:
[0029] (1) The present invention uses phenolphthalein type polyarylether nitrile as a toughening agent to modify bismaleimide-triazine resin, which effectively improves the reaction activity, improves its thermal expansion coefficient, dielectric properties, moisture resistance, etc. without affecting the thermal properties of the resin, and has better comprehensive performance.
[0030] (2) The present invention uses glass fiber reinforced phenolphthalein type polyarylether nitrile as a toughening agent to modify the composite material of bismaleimide-triazine resin. The interpenetrating network structure formed by the composite material improves its heat resistance, dielectric properties and comprehensive mechanical properties (bending, interlaminar shear, impact performance), and has a broader application prospect. BRIEF DESCRIPTION OF THE DRAWINGS
[0031] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on the provided drawings without paying creative work.
[0032] Figure 1 It is the gelation time at 200°C of the prepolymer of phenolphthalein type poly(arylene ether nitrile) modified bismaleimide-triazine resin.
[0033] Figure 2 This is the TMA curve of phenolphthalein type poly(arylene ether nitrile) modified bismaleimide-triazine resin glass fiber reinforced composite material.
[0034] Figure 3 The flexural strength and flexural modulus of phenolphthalein type poly(arylene ether nitrile) modified bismaleimide-triazine resin glass fiber reinforced composite materials.
[0035] Figure 4 The interlaminar shear strength of phenolphthalein type poly(arylene ether nitrile) modified bismaleimide-triazine resin glass fiber reinforced composite material.
[0036] Figure 5 The impact strength of phenolphthalein type polyarylethernitrile modified bismaleimide-triazine resin glass fiber reinforced composite materials. DETAILED DESCRIPTION
[0037] The following will be combined with the embodiments of the present invention and the drawings of the specification to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0038] The embodiment of the invention discloses a preparation method of a phenolphthalein type polyarylethernitrile modified bismaleimide-triazine resin and a glass fiber reinforced composite material thereof.
[0039] Embodiment 1:
[0040] A method for preparing a phenolphthalein type polyarylethernitrile modified bismaleimide-triazine resin and a glass fiber reinforced composite material thereof, specifically comprising the following steps:
[0041] (1) 80 parts of bismaleimide and 20 parts of cyanate solution were stirred at 120° C. for half an hour to obtain a bismaleimide-triazine resin prepolymer;
[0042] (2) Add 10 parts of phthalonitrile as a curing agent to the bismaleimide-triazine resin prepolymer and stir at 120°C for 3 hours;
[0043] (3) adding 5 parts of phenolphthalein type polyarylether nitrile to 50 parts of N,N-dimethylformamide, stirring and dispersing the mixture evenly, and then adding the mixture to a bismaleimide-triazine resin prepolymer, and copolymerizing the mixture to obtain a bismaleimide-triazine resin prepolymer modified with phenolphthalein type polyarylether nitrile;
[0044] (4) The prepolymer is cast into a preheated mold, and the solvent is removed in a vacuum oven at 120°C for 1 hour, and then a graded temperature control treatment is performed in a programmed temperature rising device, with the heat treatment temperatures being 140°C and 160°C for 1 hour each, and the treatment times at 200°C, 220°C and 240°C are all 2 hours. After the heat treatment, the prepolymer is naturally cooled to room temperature, and demolded to obtain a phenolphthalein type poly(arylene ether nitrile) modified bismaleimide-triazine resin.
[0045] (5) A prepolymer of phenolphthalein type polyarylether nitrile modified bismaleimide-triazine resin with a glue content of 40% is uniformly coated on the glass fiber in a ratio of 60% prepolymer resin solution to 60% glass fiber, placed in a blast oven, and after drying, 12 sheets of the composite material are heat treated in a hot press at 240°C and 20MPa for 2h. After cooling, a phenolphthalein type polyarylether nitrile modified bismaleimide-triazine resin glass fiber reinforced composite material is obtained.
[0046] Embodiment 2:
[0047] A method for preparing a phenolphthalein type polyarylethernitrile modified bismaleimide-triazine resin and a glass fiber reinforced composite material thereof, specifically comprising the following steps:
[0048] (1) 80 parts of bismaleimide and 20 parts of cyanate solution were stirred at 120° C. for half an hour to obtain a bismaleimide-triazine resin prepolymer;
[0049] (2) Add 10 parts of phthalonitrile as a curing agent to the bismaleimide-triazine resin prepolymer and stir at 120°C for 3 hours;
[0050] (3) adding 10 parts of phenolphthalein type polyarylether nitrile to 50 parts of N,N-dimethylformamide, stirring and dispersing the mixture evenly, and then adding the mixture to a bismaleimide-triazine resin prepolymer, and copolymerizing the mixture to obtain a bismaleimide-triazine resin prepolymer modified with the phenolphthalein type polyarylether nitrile;
[0051] (4) The prepolymer is cast into a preheated mold, and the solvent is removed in a vacuum oven at 120°C for 1 hour, and then a graded temperature control treatment is performed in a programmed temperature rising device, with the heat treatment temperatures being 140°C and 160°C for 1 hour each, and the treatment times at 200°C, 220°C and 240°C are all 2 hours. After the heat treatment, the prepolymer is naturally cooled to room temperature, and demolded to obtain a phenolphthalein type poly(arylene ether nitrile) modified bismaleimide-triazine resin.
[0052] (5) A prepolymer of phenolphthalein type polyarylether nitrile modified bismaleimide-triazine resin with a glue content of 40% is uniformly coated on the glass fiber in a ratio of 60% prepolymer resin solution to 60% glass fiber, placed in a blast oven, and after drying, 12 sheets of the composite material are heat treated in a hot press at 240°C and 20MPa for 2h. After cooling, a phenolphthalein type polyarylether nitrile modified bismaleimide-triazine resin glass fiber reinforced composite material is obtained.
[0053] Embodiment 3:
[0054] A method for preparing a phenolphthalein type polyarylethernitrile modified bismaleimide-triazine resin and a glass fiber reinforced composite material thereof, specifically comprising the following steps:
[0055] (1) 80 parts of bismaleimide and 20 parts of cyanate solution were stirred at 120° C. for half an hour to obtain a bismaleimide-triazine resin prepolymer;
[0056] (2) Add 10 parts of phthalonitrile as a curing agent to the bismaleimide-triazine resin prepolymer and stir at 120°C for 3 hours;
[0057] (3) adding 20 parts of phenolphthalein type polyarylether nitrile to 50 parts of N,N-dimethylformamide, stirring and dispersing the mixture evenly, and then adding the mixture to a bismaleimide-triazine resin prepolymer, and copolymerizing the mixture to obtain a bismaleimide-triazine resin prepolymer modified with the phenolphthalein type polyarylether nitrile;
[0058] (4) The prepolymer is cast into a preheated mold, and the solvent is removed in a vacuum oven at 120°C for 1 hour, and then a graded temperature control treatment is performed in a programmed temperature rising device, with the heat treatment temperatures being 140°C and 160°C for 1 hour each, and the treatment times at 200°C, 220°C and 240°C are all 2 hours. After the heat treatment, the prepolymer is naturally cooled to room temperature, and demolded to obtain a phenolphthalein type poly(arylene ether nitrile) modified bismaleimide-triazine resin.
[0059] (5) A prepolymer of phenolphthalein type polyarylether nitrile modified bismaleimide-triazine resin with a glue content of 40% is uniformly coated on the glass fiber in a ratio of 60% prepolymer resin solution to 60% glass fiber, placed in a blast oven, and after drying, 12 sheets of the composite material are heat treated in a hot press at 240°C and 20MPa for 2h. After cooling, a phenolphthalein type polyarylether nitrile modified bismaleimide-triazine resin glass fiber reinforced composite material is obtained.
[0060] Embodiment 4:
[0061] A method for preparing a phenolphthalein type polyarylethernitrile modified bismaleimide-triazine resin and a glass fiber reinforced composite material thereof, specifically comprising the following steps:
[0062] (1) 80 parts of bismaleimide and 20 parts of cyanate solution were stirred at 120° C. for half an hour to obtain a bismaleimide-triazine resin prepolymer;
[0063] (2) Add 10 parts of phthalonitrile as a curing agent to the bismaleimide-triazine resin prepolymer and stir at 120°C for 3 hours;
[0064] (3) adding 20 parts of phenolphthalein type polyarylether nitrile to 50 parts of N,N-dimethylformamide, stirring and dispersing the mixture evenly, and then adding the mixture to a bismaleimide-triazine resin prepolymer, and copolymerizing the mixture to obtain a bismaleimide-triazine resin prepolymer modified with the phenolphthalein type polyarylether nitrile;
[0065] (4) The prepolymer is cast into a preheated mold, and the solvent is removed in a vacuum oven at 120°C for 1 hour, and then a graded temperature control treatment is performed in a programmed temperature rising device, with the heat treatment temperatures being 140°C and 160°C for 1 hour each, and the treatment times at 200°C, 220°C and 240°C are all 2 hours. After the heat treatment, the prepolymer is naturally cooled to room temperature, and demolded to obtain a phenolphthalein type poly(arylene ether nitrile) modified bismaleimide-triazine resin.
[0066] (5) A prepolymer of phenolphthalein type polyarylether nitrile modified bismaleimide-triazine resin with a glue content of 40% is uniformly coated on the glass fiber in a ratio of 60% prepolymer resin solution to 60% glass fiber, placed in a blast oven, and after drying, 12 sheets of the composite material are heat treated in a hot press at 240°C and 20MPa for 2h. After cooling, a phenolphthalein type polyarylether nitrile modified bismaleimide-triazine resin glass fiber reinforced composite material is obtained.
[0067] Comparative Example 1
[0068] (1) 80 parts of bismaleimide and 20 parts of cyanate solution were stirred at 120° C. for half an hour to obtain a bismaleimide-triazine resin prepolymer;
[0069] (2) Add 10 parts of phthalonitrile as a curing agent to the bismaleimide-triazine resin prepolymer and stir at 120°C for 3 hours;
[0070] (3) The prepolymer is cast into a preheated mold, and the solvent is removed in a vacuum oven at 120°C for 1 hour, followed by a stepwise temperature control treatment in a programmed temperature rising device, with the heat treatment temperatures being 140°C and 160°C for 1 hour each, and the treatment times at 200°C, 220°C and 240°C being 2 hours each. After the heat treatment, the prepolymer is naturally cooled to room temperature, and demolded to obtain a bismaleimide-triazine resin.
[0071] (4) The bismaleimide-triazine resin prepolymer is uniformly coated on the glass fiber and placed in a forced air oven. After drying, 12 sheets of the composite material are heat treated in a hot press at 240°C and 20 MPa for 2 h. After cooling, a bismaleimide-triazine resin glass fiber reinforced composite material is obtained.
[0072] The performance test was conducted on the above-mentioned Examples 1 to 4 and Comparative Example 1 to verify and illustrate the superior effect of the present technology compared with the prior art. The specific experimental contents and experimental analysis are as follows:
[0073] like Figure 1 As shown in the figure, after adding phenolphthalein poly(arylether nitrile), the gel time of PEN / BT prepolymer at 200°C is significantly reduced compared with pure BT resin. Phenolphthalein poly(arylether nitrile) as a plasticizer increases the reactivity of the mixture system. Specifically, the gel time of pure BT resin mixture is 615s, and the gel time of catalyst-containing mixed glue is 481s, 436s, 302s and 266s as the proportion of xylene methane bismaleimide increases from 50 parts to 80 parts.
[0074] like Figure 2 As shown in the figure, as the addition amount of phenolphthalein poly(arylether nitrile) increases from 0 to 20 parts, the glass transition temperature and thermal expansion coefficient of the glass fiber composite material are improved to varying degrees. The glass transition temperature increases from 262.1℃ of pure BT resin to 284.6℃, 281.1℃, 270.2℃, and 286.4℃ respectively; the thermal expansion coefficient increases from 24.87×10 -6 / K, respectively, increased to 26.77×10 -6 / K,19.00×10 -6 / K,26.97×10 -6 / K, 20.89×10 -6 / K.
[0075] like Figure 3 , 4As shown in Figure 5, different proportions of phenolphthalein type polyarylether nitrile modified BT resin have different degrees of improvement in comprehensive mechanical properties. Due to the different crosslinking degrees of the materials, the macromolecules and small molecules complement each other to improve the interface strength and the phase transition of single phase, bicontinuous phase and phase separation, so that the flexural strength of the composite material is increased from 355.02 to 502.21MPa, 581.63MPa, 525.98MPa, 465.75MPa respectively; the flexural modulus is changed from 22.77GPa to 30.45GPa, 40.38GPa, 22.53GPa, 20.35GPa; the interlaminar shear strength is improved from 34.66 to 38.57MPa, 45.54MPa, 42.54MPa, 35.09MPa; the impact strength is improved from 83.67KJ / m 3 , improved to 113.83 KJ / m 3 , 131.99 KJ / m 3 , 105.83 KJ / m 3 , 80.37 KJ / m 3 .
[0076] The above description of the disclosed embodiments enables one skilled in the art to implement or use the present invention. Various modifications to these embodiments will be apparent to one skilled in the art, and the general principles defined herein may be implemented in other embodiments without departing from the spirit or scope of the present invention. Therefore, the present invention will not be limited to the embodiments shown herein, but rather to the widest scope consistent with the principles and novel features disclosed herein.
Claims
1. A method for preparing a phenolphthalein type polyarylether nitrile modified bismaleimide-triazine resin, characterized in that: The method specifically comprises the following steps: (1) prepolymerizing 50-100 parts of bismaleimide and 20-50 parts of cyanate solution to obtain a bismaleimide-triazine resin prepolymer; (2) adding 5 to 30 parts of phthalonitrile as a curing agent to the bismaleimide-triazine resin prepolymer; (3) adding 5 to 30 parts of phenolphthalein type polyarylether nitrile to 50 to 80 parts of N,N-dimethylformamide, stirring and dispersing the mixture evenly, and then adding the mixture to a bismaleimide-triazine resin prepolymer to copolymerize the mixture to obtain a bismaleimide-triazine resin prepolymer modified with the phenolphthalein type polyarylether nitrile; (4) Casting the prepolymer into a preheated mold, removing the solvent in a vacuum oven, and then performing a graded temperature control treatment in a programmed temperature rising device. After the heat treatment, the prepolymer is naturally cooled to room temperature, and demolding is performed to obtain the phenolphthalein type polyarylether nitrile modified bismaleimide-triazine resin.
2. The method for preparing the phenolphthalein type polyarylether nitrile modified bismaleimide-triazine resin according to claim 1, characterized in that: In the step (3), the amount of phenolphthalein polyarylether nitrile added is 5 to 30 parts, and the structural formula of the phenolphthalein polyarylether nitrile is as follows, wherein M is 5W to 10W: 。 3. The method for preparing the phenolphthalein type polyarylether nitrile modified bismaleimide-triazine resin according to claim 1, characterized in that: In the step (3), phenolphthalein type polyarylethernitrile is added to 50-80 parts of N,N-dimethylformamide, stirred at 100-140°C for uniform dispersion, and then continued to be added and stirred for 0.5-2h.
4. The method for preparing the phenolphthalein type polyarylether nitrile modified bismaleimide-triazine resin according to claim 1, characterized in that: In the step (4), the temperature of the vacuum oven is 120°C, and the temperature is controlled in stages from 140°C to 240°C; and the specific operation of the temperature control is as follows: 140℃ 1h, 160℃ 1h, 180℃ 2h, 220℃ 2h, 240℃ 2h.
5. A preparation of a glass fiber reinforced composite material, characterized in that: The method specifically comprises the following steps: (1) Evenly coating the bismaleimide-triazine resin modified with phenolphthalein poly(arylether nitrile) with a glue content of 30-70% on both sides of the glass fiber; (2) The obtained composite material is desolventized in a blast oven, and 10 to 15 sheets of the composite material are cut neatly and heat treated in a hot press.
6. The preparation of a glass fiber reinforced composite material according to claim 9, characterized in that: The prepolymer of phenolphthalein type polyarylethernitrile modified bismaleimide-triazine resin has a rubber content of 30-70.
7. The preparation of a glass fiber reinforced composite material according to claim 9, characterized in that: The glass fiber is electronic grade glass fiber with a surface density of 150-240, a length of 15-20 cm, and a width of 12-18 cm.
8. The preparation of a glass fiber reinforced composite material according to claim 9, characterized in that: It is composed of the following formula, which is calculated by weight: Prepolymer resin solution 30-80, glass fiber 30-60.
9. The preparation of a glass fiber reinforced composite material according to claim 9, characterized in that: 10-15 sheets of the composite material were heat treated in a hot press at 220-240°C and 20-30 MPa for 2 h.
Citation Information
Cited By
High-temperature-resistant copper-clad plate based on modified bismaleimide resin and preparation method of high-temperature-resistant copper-clad plate