Flame-retardant silicone rubber foam material and preparation method thereof

Through the synergistic action of molecular sieve and aluminum hydroxide and the use of modified flame retardants, the flame retardant and mechanical properties of silicone rubber foamed materials are improved, and the combustion problem under high-temperature fire conditions is solved, and low density is achieved. High strength and non-toxic and pollution-free effect.

CN118994919APending Publication Date: 2024-11-22HUBEI XINGRUI SILICON MATERIAL CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411130375.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-16
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

Silicone rubber foaming materials are prone to continuous combustion under high temperature or fire conditions, and the high foaming ratio is difficult to flame retardant, which limits its safety and practicality in aerospace, new energy and other fields.

Method used

Through the synergistic action of molecular sieve and aluminum hydroxide, a modified flame retardant is prepared, combined with vinyl silicone oil, α,ω-dihydroxypolydimethylsiloxane and other materials, the flame retardant performance of silicone rubber foamed materials is improved, and The pore structure of molecular sieve is used to absorb smoke and reduce smoke density.

Benefits of technology

It significantly improves the flame retardant and mechanical properties of silicone rubber foaming materials, reduces smoke density, achieves the characteristics of non-toxic and pollution-free, and has the advantages of low density and high strength.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention provides a flame-retardant silicone rubber foam material and a preparation method thereof, the flame-retardant silicone rubber foam material is prepared from the following raw materials in parts by mass: a component A consisting of 5-50 parts of vinyl silicone oil and 10-80 parts of alpha, beta-propylene glycol, and a component B consisting of 5-50 parts of vinyl silicone oil and 10-80 parts of alpha, beta-propylene glycol; the composition is prepared from the following components in parts by weight: 1-20 parts of alpha, omega-dihydroxyl polydimethylsiloxane, 1-20 parts of low-viscosity hydroxyl silicone oil, 20-40 parts of a flame retardant, 1-35 parts of fumed silica and 0.01-5 parts of a platinum catalyst. The component B is prepared from the following components in parts by weight: 5 to 50 parts of vinyl silicone oil, 10 to 80 parts of alpha, omega-dihydroxy polydimethylsiloxane, 1 to 25 parts of hydrogen-containing silicone oil, 20 to 40 parts of flame retardant, 1 to 35 parts of fumed silica and 0.1 to 1 part of inhibitor. The preparation method is simple and low in cost, the flame retardant is coated with the rubber material in the mixing process, and finally the component A and the component B are evenly mixed according to the proportion of 1: 1 to prepare the foaming material. The silicone rubber foaming material prepared by the method not only has better flame retardant property and lower smoke density, but also has the advantages of no toxicity, no pollution, low density and high strength.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of organic silicon foam materials, and in particular relates to a flame retardant silicone rubber foam material and a preparation method thereof. Background Art

[0002] As a kind of high molecular elastic material with porous structure, silicone rubber foam material is widely used in aerospace, construction, energy chemical industry, national defense and other fields. This material not only has the excellent properties of silicone rubber products such as non-toxic and environmentally friendly, heat-resistant, flame-resistant, and good electrical insulation, but also has the properties of foam materials such as damping, vibration reduction, sound insulation, heat insulation, sealing, and light weight.

[0003] However, due to the large number of hydrocarbon groups on the side chains of silicone rubber foam materials, they will continue to burn under high temperature or fire conditions. In addition, the pore structure of silicone rubber foam materials increases the contact area between the substrate and the air, which is more conducive to combustion. The higher the foaming ratio, the greater the difficulty of flame retardancy, which greatly limits its safety and practicality during use.

[0004] With the continuous development of my country's and the world's economy, and the rise of emerging industries such as aerospace and new energy vehicles, the demand for silicone rubber foam materials is increasing, and the requirements for various performance indicators of silicone rubber foam materials are constantly increasing. Functionalized, high-performance silicone rubber foam materials have become one of the most popular materials in the field of foam materials. How to manufacture silicone rubber foam materials with excellent flame retardancy, mechanical properties and low cost is a difficult problem that needs to be solved.

[0005] Based on the above analysis, a method for preparing a silicone rubber foam material with a simple preparation process and excellent flame retardant properties is provided, which is of great significance for its application in the new energy industry. Summary of the invention

[0006] In view of the defects of the above-mentioned prior art, the purpose of the present invention is to provide a flame retardant silicone rubber foam material and a preparation method, thereby improving the flame retardant effect of the silicone rubber foam material through the synergy between molecular sieve and aluminum hydroxide. At the same time, the pore structure of the molecular sieve can absorb smoke and reduce the smoke density, so that the silicone rubber foam material has the characteristics of non-toxic and non-polluting.

[0007] A flame retardant silicone rubber foam material, prepared from two components A and B, wherein the A component comprises: vinyl silicone oil, α, ω-dihydroxy polydimethylsiloxane, low-viscosity hydroxy silicone oil, flame retardant, fumed silica, and platinum catalyst, and the B component comprises: vinyl silicone oil, α, ω-dihydroxy polydimethylsiloxane, hydrogen-containing silicone oil, flame retardant, fumed silica, and inhibitor; The flame retardant is obtained by compounding molecular sieve and aluminum hydroxide and then adding a modifier for modification.

[0008] Furthermore, in parts by mass, the component A comprises: 5-50 parts of vinyl silicone oil, 10-80 parts of α, ω-dihydroxy polydimethylsiloxane, 1-20 parts of low-viscosity hydroxy silicone oil, 20-40 parts of flame retardant, 1-35 parts of fumed silica, and 0.01-5 parts of platinum catalyst; the component B comprises: 5-50 parts of vinyl silicone oil, 10-80 parts of α, ω-dihydroxy polydimethylsiloxane, 1-25 parts of hydrogen-containing silicone oil, 20-40 parts of flame retardant, 1-35 parts of fumed silica, and 0.1-1 parts of inhibitor.

[0009] Furthermore, the preparation method of the flame retardant is as follows: S1: Mix the dried molecular sieve and aluminum hydroxide in a mass ratio of 1:(1-5), add water and stir evenly at a constant temperature, filter and dry to obtain a composite powder; S2: Add 10%-40% of the mass of the modifier to the compound powder obtained in S1 and stir evenly; S3: Add water to the product obtained in S2, stir to form a slurry, filter and dry to obtain a flame retardant.

[0010] Furthermore, the vinyl content of the vinyl silicone oil is 0.1-1.2%; the hydroxyl content of the α,ω-dihydroxy polydimethylsiloxane is 0.01-0.1%; the hydroxyl content of the low-viscosity hydroxy silicone oil is 1-4%, and the viscosity is 20-200cps; the hydrogen content of the hydrogen-containing silicone oil is 0.1-3%; the platinum catalyst is one or more of 3000ppm or 5000ppm; the inhibitor is one or more of 2-methyl-3-butyn-2-ol or ethynyl cyclohexanol.

[0011] Furthermore, the modifier is a cationic surfactant, and its structural formula is Si(OR1) (OR2)(OR3) (CH2) x N + (CH3)2(CH2) y CH3Cl - , wherein R1, R2, and R3 are each independently a C1-C4 alkyl group, x is an integer of 2 to 6, and y is an integer of 9 to 20; preferably, R1, R2, and R3 are all methyl groups, x=3, and y=15.

[0012] Furthermore, the molecular sieve is one or more of Y-type molecular sieve, ZSM-5 molecular sieve, 4A molecular sieve or MCM-41.

[0013] Furthermore, the aluminum hydroxide powder has a particle size of 1-5 μm.

[0014] A method for preparing a flame retardant silicone rubber foam material comprises the following steps: Preparation of component A: vinyl silicone oil, fumed silica, α,ω-dihydroxy polydimethylsiloxane, low-viscosity hydroxy silicone oil, and platinum catalyst are mixed, and then flame retardant is added and mixed thoroughly. After mixing, three-roll grinding is performed to obtain material A; Preparation of component B: vinyl silicone oil, fumed silica, α,ω-dihydroxy polydimethylsiloxane, low-viscosity hydrogenated silicone oil and inhibitor are mixed, and then flame retardant is added and mixed thoroughly. After mixing, three-roll grinding is performed to obtain material B; Preparation of foaming material: Weigh equal masses of A and B materials and mix them quickly, roll the sample through a roller, put it into an oven for one-stage vulcanization and two-stage vulcanization to obtain the final sample.

[0015] Furthermore, the first stage vulcanization temperature is 50-110° C., and the vulcanization time is 5-20 min.

[0016] Furthermore, the second stage vulcanization temperature is 150-200° C., and the vulcanization time is 20-80 min.

[0017] The beneficial effects of the technical solution provided by this application are: The present invention utilizes the composite modification of molecular sieve and aluminum powder to obtain flame retardant powder, so that the silicone rubber foam material has good flame retardant properties. Due to the presence of Si-OH and Al-OH in the molecular sieve and the molecular sieve pores, aluminum powder is easier to combine with it, and the combined powder can be better coated with silicone oil after modification, so that the silicone rubber foam material has a better flame retardant effect; at the same time, the catalytic performance of the molecular sieve can promote the carbonization of organic polymers during combustion, thereby improving the flame retardant effect, and the pore structure of the molecular sieve also has a certain adsorption function, which can be adsorbed to reduce smoke density, thereby reducing pollution. In addition, the flame retardant foamed silicone rubber prepared by the present invention also has the advantages of low density and high strength. DETAILED DESCRIPTION

[0018] The embodiments of the present invention will be described in detail below with reference to examples. The following examples are only used to illustrate the present invention and should not be construed as limiting the scope of the present invention.

[0019] In this application, vinyl silicone oil, hydrogenated silicone oil, hydroxy silicone oil, etc. are sourced from Ningbo Runhe High-tech Materials Technology Co., Ltd. and Shandong Dayi Chemical Co., Ltd.; fumed silica is sourced from Hubei Huifu Nanomaterials Co., Ltd.; α, ω-dihydroxypolydimethylsiloxane and modifier are sourced from Hubei Xingrui Silicon Materials Co., Ltd.; inhibitor is sourced from Wuhan Chengtian Fine Chemical Co., Ltd.; catalyst is sourced from Shanghai Bozhijie New Materials Co., Ltd.; aluminum hydroxide is sourced from Xinxiang Shengda Aluminum Hydroxide Co., Ltd.; molecular sieve is sourced from Hebi Bowen Kefeng Catalysis Technology Co., Ltd.

[0020] The preparation method of the flame retardant is as follows: S1: Mix the dried molecular sieve and aluminum hydroxide in a mass ratio of 1:(1-5), add 30% water of the total mass of the molecular sieve and aluminum hydroxide, stir at a constant temperature of 90-100°C for 20-30 minutes, filter and dry to obtain a composite powder; S2: Add 10%-40% of the mass of the modifier to the compound powder obtained in S1 and stir for 5 minutes; S3: Add 300% water of the compound powder mass and stir to form a slurry, stir at 60-90°C for 20-30 minutes, filter and dry to obtain a flame retardant.

[0021] The modifier used in the present invention is a cationic surfactant, and its structural formula is Si(OR1) (OR2) (OR3)(CH2) x N + (CH3)2(CH2) y CH3Cl - , wherein R1, R2, and R3 are each independently a C1-C4 alkyl group, x is an integer of 2 to 6, and y is an integer of 9 to 20.

[0022] Example 1 Preparation of flame retardant: Add dried ZSM-5 molecular sieve and 1μm aluminum hydroxide in a constant temperature stirrer at a mass ratio of 1:1, and add pure water of 30% of the powder mass, stir at a constant temperature of 90°C for 20 minutes, filter and dry to obtain a composite powder after mixing; then transfer the composite powder to a constant temperature stirrer, add 10% of the composite powder mass of surfactant 3-trimethylsilylpropyl hexadecyldimethylammonium chloride (TPHAC) and stir for 5 minutes, then add 300% of the composite powder mass of water and stir to a slurry, then stir at 60°C for 20 minutes, filter and dry to obtain a modified flame retardant. Among them, 3-trimethylsilylpropyl hexadecyldimethylammonium chloride: R1, R2, and R3 are all methyl, x=3, y=15.

[0023] Preparation of component A: Mix 50 parts of 0.1wt% vinyl silicone oil, 10 parts of 0.01wt% α,ω-dihydroxypolydimethylsiloxane, 20 parts of 1% low-viscosity hydroxy silicone oil, 35 parts of fumed silica, and 5 parts of 3000ppm platinum catalyst, then add 40 parts of flame retardant and mix thoroughly; after mixing, perform three-roll grinding to obtain material A.

[0024] Preparation of component B: 50 parts of 0.1wt% vinyl silicone oil, 10 parts of 0.01wt% α,ω-dihydroxy polydimethylsiloxane, 25 parts of 0.1wt% hydrogenated silicone oil, 35 parts of fumed silica, and 1 part of 2-methyl-3-butyn-2-ol were mixed according to the formula, and 40 parts of flame retardant were added and mixed thoroughly. After mixing, three-roll grinding was performed to obtain material B.

[0025] Preparation of foaming material: Weigh equal masses of A and B rubber materials and mix them quickly, roll the sample through a roller, put it into a 50°C oven for 5 min first-stage vulcanization and a 150°C oven for 20 min second-stage vulcanization to obtain the final sample.

[0026] Example 2 Preparation of flame retardant: Dry ZSM-5 molecular sieve and 5μm aluminum hydroxide are added into a constant temperature stirrer in a mass ratio of 1:1, and pure water accounting for 30% of the mass of the powder is added, and stirred at a constant temperature of 100°C for 30 minutes. After mixing, filter and dry to obtain a composite powder; then transfer the composite powder into a constant temperature stirrer, add TPHAC accounting for 40% of the mass of the composite powder and stir for 5 minutes, then add water accounting for 300% of the mass of the composite powder and stir to form a slurry, then stir at 90°C for 30 minutes, filter and dry to obtain a flame retardant.

[0027] Preparation of component A: 5 parts of 1.2wt% vinyl silicone oil, 80 parts of 0.1wt% α,ω-dihydroxy polydimethylsiloxane, 1 part of 4wt% low-viscosity hydroxy silicone oil, 1 part of fumed silica, and 0.01 part of 5000ppm platinum catalyst were mixed according to the formula, and then 20 parts of flame retardant were added and mixed thoroughly. After mixing, three-roll grinding was performed to obtain material A.

[0028] Preparation of component B: 5 parts of 1.2wt% vinyl silicone oil, 80 parts of 0.1wt% α,ω-dihydroxy polydimethylsiloxane, 1 part of 3wt% hydrogenated silicone oil, 1 part of fumed silica, and 0.1 part of 2-methyl-3-butyn-2-ol were mixed according to the formula, and then 20 parts of flame retardant were added and mixed thoroughly. After mixing, three-roll grinding was performed to obtain material B.

[0029] Preparation of foaming material: Weigh equal masses of A and B rubber materials and mix them quickly, roll the sample through a roller, put it into a 110°C oven for 20 min of first-stage vulcanization and a 200°C oven for 80 min of second-stage vulcanization to obtain the final sample.

[0030] Example 3 Preparation of flame retardant: Dry ZSM-5 molecular sieve and 1μm aluminum hydroxide are added into a constant temperature stirrer in a mass ratio of 1:4, and pure water accounting for 30% of the mass of the powder is added, and stirred at a constant temperature of 100°C for 30 minutes. After mixing, filter and dry to obtain a composite powder; then transfer the composite powder into a constant temperature stirrer, add 40% of the mass of the powder modifier TPHAC and stir for 5 minutes, then add 300% of the mass of the powder into water and stir to form a slurry, then stir at 90°C for 30 minutes, filter and dry to obtain a flame retardant.

[0031] Preparation of component A: 45 parts of 0.2wt% vinyl silicone oil, 60 parts of 0.04wt% α,ω-dihydroxy polydimethylsiloxane, 5 parts of 3wt% low-viscosity hydroxy silicone oil, 20 parts of fumed silica, and 1 part of 5000ppm platinum catalyst were mixed according to the formula, and then 40 parts of flame retardant were added and mixed thoroughly. After mixing, three-roll grinding was performed to obtain material A.

[0032] In the second step, component B is prepared by mixing 45 parts of 0.2wt% vinyl silicone oil, 60 parts of 0.04wt% α,ω-dihydroxy polydimethylsiloxane, 9 parts of 2wt% hydrogenated silicone oil, 20 parts of fumed silica, and 0.5 parts of ethynyl cyclohexanol according to the formula, and then adding 40 parts of flame retardant and mixing them thoroughly. After mixing, three-roll grinding is performed to obtain material B.

[0033] The third step is the preparation of the foaming material. The A and B rubber materials of equal mass are weighed and mixed quickly. The sample is rolled by a roller and placed in a 75°C oven for 10 min of first-stage vulcanization and a 150°C oven for 60 min of second-stage vulcanization to obtain the final sample.

[0034] Example 4 The flame retardant compounding and modification method is consistent with that in Example 1, except that: 4A molecular sieve and aluminum hydroxide with a particle size of 1 μm are compounded in a mass ratio of 1:5.

[0035] Preparation of component A: 30 parts of 1wt% vinyl silicone oil, 70 parts of 0.5wt% α,ω-dihydroxy polydimethylsiloxane, 10 parts of 4wt% low-viscosity hydroxy silicone oil, 35 parts of fumed silica, and 0.5 parts of platinum catalyst were mixed according to the formula, and then 35 parts of flame retardant were added and mixed thoroughly. After mixing, three-roll grinding was performed to obtain material A.

[0036] Preparation of component B: 30 parts of 1wt% vinyl silicone oil, 70 parts of 0.5wt% α,ω-dihydroxy polydimethylsiloxane, 15 parts of hydrogenated silicone oil, 35 parts of fumed silica, and 0.9 parts of 2-methyl-3-butyn-2-ol were mixed according to the formula, and 35 parts of flame retardant were added and mixed thoroughly. After mixing, three-roll grinding was performed to obtain material B.

[0037] Preparation of foaming material: Weigh equal mass of A / B rubber materials and mix them quickly, roll the sample through a roller, put it into a 60°C oven for 7 min of first-stage vulcanization and a 160°C oven for 60 min of second-stage vulcanization to obtain the final sample.

[0038] Example 5 The flame retardant compounding and modification method is consistent with that in Example 2, and is different from that in Example 1 in that the Y-type molecular sieve and aluminum hydroxide with a particle size of 5 μm are compounded in a ratio of 1:5.

[0039] Preparation of component A: 20 parts of 0.5wt% vinyl silicone oil, 80 parts of 0.05wt% α,ω-dihydroxy polydimethylsiloxane, 20 parts of 2wt% low-viscosity hydroxy silicone oil, 35 parts of fumed silica, and 0.2 parts of 3000ppm platinum catalyst were mixed according to the formula, and then 20 parts of flame retardant were added and mixed thoroughly. After mixing, three-roll grinding was performed to obtain material A.

[0040] Preparation of component B: 20 ​​parts of 0.5wt% vinyl silicone oil, 80 parts of 0.05wt% α,ω-dihydroxy polydimethylsiloxane, 25 parts of 2wt% hydrogenated silicone oil, 35 parts of fumed silica, and 0.1 parts of 2-methyl-3-butyn-2-ol were mixed according to the formula, and then 20 parts of flame retardant were added and mixed thoroughly. After mixing, three-roll grinding was performed to obtain material B.

[0041] The third step is the preparation of the foaming material. A / B rubber materials of equal mass are weighed and mixed quickly. The sample is rolled by a roller and placed in an oven at 80°C for 15 min of first-stage vulcanization and in an oven at 180°C for 80 min of second-stage vulcanization to obtain the final sample.

[0042] Example 6 The only difference from Example 3 is that the flame retardant is a mixture of MCM-41 molecular sieve and 1 μm aluminum hydroxide in a ratio of 1:1.

[0043] Example 7 The only difference from Example 3 is that the flame retardant is a mixture of MCM-41 molecular sieve and 1 μm aluminum hydroxide in a ratio of 1:5.

[0044] Example 8 The only difference from Example 3 is that the flame retardant is a mixture of MCM-41 molecular sieve and 5 μm aluminum hydroxide in a ratio of 1:1.

[0045] Example 9 The only difference from Example 3 is that the flame retardant is a mixture of MCM-41 molecular sieve and 5 μm aluminum hydroxide in a ratio of 1:4.

[0046] Example 10 The only difference from Example 3 is that the flame retardant is a mixture of MCM-41 molecular sieve and 5 μm aluminum hydroxide in a ratio of 1:5.

[0047] Embodiment 11 The only difference from Example 3 is that the modifiers R1 and R2 are both methyl, R3 is ethyl, x=2, y=9.

[0048] Example 12 The only difference from Example 3 is that the modifiers R1 and R2 are both methyl, R3 is ethyl, x=6, y=20.

[0049] Comparative Example 1 The only difference from Example 3 is that the flame retardant is 1 μm aluminum hydroxide and has not been compounded and modified.

[0050] Comparative Example 2 The only difference from Example 3 is that the flame retardant is 5 μm aluminum hydroxide and has not been compounded and modified.

[0051] Comparative Example 3 The only difference from Example 3 is that the flame retardant is MCM-41 molecular sieve, which has not been subjected to compounding and modification treatment.

[0052] Comparative Example 4 The only difference from Example 3 is that there is no flame retardant.

[0053] Comparative Example 5 The only difference from Example 3 is that the flame retardant preparation method is to modify the molecular sieve and aluminum hydroxide separately and then compound them.

[0054] Flame retardant preparation: (1) Molecular sieve modification: The modification method is the same as in Example 3, except that no aluminum hydroxide is added; (2) Aluminum hydroxide modification: The modification method is the same as in Example 3, except that no molecular sieve is added; (3) Flame retardant compounding: The modified molecular sieve obtained in steps (1) and (2) is compounded with aluminum hydroxide in a mass ratio of 1:4.

[0055] The preparation method of component A, component B and foaming material is the same as that of Example 3.

[0056] Comparative Example 6 The only difference from Example 3 is that the modifier is γ-aminopropyltriethoxysilane.

[0057] Comparative Example 7 The only difference from Example 3 is that the modifier is bis((3,4-epoxycyclohexyl)methyl)adipate.

[0058] The samples obtained from the above embodiments and comparative examples were tested according to the following test standards: ASTM D412-16 (tensile strength test), UL94-2013 (flame retardant test), GB / T 6343 (apparent density test), and ASTM E662 (smoke density test).

[0059] Table 1 Performance test results of examples and comparative examples sample Limiting oxygen index LOI / % UL-94 Smoke density level SDR / % Maximum smoke density MSD / % <![CDATA[Density after foaming g / cm 3 > Tensile strength MPa Example 1 29.6 V-0 39.6 49.9 0.42 0.47 Example 2 28.3 V-0 41.7 48.4 0.41 0.45 Example 3 33.6 V-0 35.4 45.5 0.35 0.50 Example 4 30.2 V-0 38.3 49.2 0.37 0.47 Example 5 29.1 V-0 40.1 49.1 0.39 0.45 Example 6 29.6 V-0 36.4 46.3 0.39 0.48 Example 7 31.7 V-0 36.9 47.4 0.41 0.48 Example 8 30 V-0 36.5 47.8 0.40 0.47 Example 9 31.4 V-0 38.7 50.6 0.39 0.46 Example 10 32 V-0 49.1 52.1 0.38 0.46 Embodiment 11 31.5 V-0 38.6 49.1 0.36 0.49 Example 12 32.8 V-0 37.2 46.7 0.35 0.49 Comparative Example 1 28.6 V-0 51.3 60.2 0.44 0.39 Comparative Example 2 29.0 V-0 52.7 65.3 0.4 0.38 Comparative Example 3 26.3 V-1 34.9 43.2 0.41 0.35 Comparative Example 4 18.4 V-3 70.6 80.5 0.42 0.36 Comparative Example 5 29.3 V-0 48.7 55.4 0.40 0.40 Comparative Example 6 30.1 V-0 49.5 57.4 0.42 0.37 Comparative Example 7 29.8 V-0 49.2 55.3 0.43 0.39 From the comparison between comparative examples 1-7 and embodiments 3, 6-10 in Table 1, it is found that the flame retardant properties of the silicone rubber foam material prepared by the flame retardant obtained by compounding and modification are better. It can be seen from Examples 1-10 that the more the molecular sieve particle size matches the aluminum hydroxide particle size, the better the flame retardant properties of the silicone rubber foam material. The presence of Si-OH and Al-OH in the molecular sieve and the molecular sieve pores make it easier for aluminum powder to be combined with it; the powder after compounding and modification can be better coated with silicone oil, so that the silicone rubber foam material has a better flame retardant effect. The catalytic performance of the molecular sieve can promote carbonization of organic polymers during combustion, thereby improving the flame retardant effect; and the pore structure of the molecular sieve also has a certain adsorption function, which can be adsorbed to reduce smoke density, thereby reducing pollution. It can be seen from Examples 3, 11, 12 and Comparative Examples 6 and 7 that the use of organosilicon cationic surfactants such as TPHAC to modify aluminum hydroxide and molecular sieves is conducive to a better compounding and combination of the two, thereby achieving a better flame retardant effect.

[0060] In addition, the flame retardant foamed silicone rubber prepared by the present invention also has the advantages of low density and high strength. It can be seen from Example 3 and Comparative Examples 4 and 5 that the flame retardant treated by the compounding and modification method of the present application is added to the silicone rubber system to reduce the silicone rubber foaming density and improve the mechanical strength.

[0061] The above description is only a specific implementation of the present application, so that those skilled in the art can understand or implement the present application. Various modifications to these embodiments will be apparent to those skilled in the art, and the general principles defined herein can be implemented in other embodiments without departing from the spirit or scope of the present application. Therefore, the present application will not be limited to the embodiments shown herein, but will conform to the widest range consistent with the principles and novel features applied for herein.

Claims

1. A flame retardant silicone rubber foam material, characterized in that: It is prepared from two components A and B, wherein the A component includes: vinyl silicone oil, α,ω-dihydroxy polydimethylsiloxane, low-viscosity hydroxy silicone oil, flame retardant, fumed silica, and platinum catalyst, and the B component includes: vinyl silicone oil, α,ω-dihydroxy polydimethylsiloxane, hydrogen-containing silicone oil, flame retardant, fumed silica, and inhibitor; The flame retardant is obtained by compounding molecular sieve and aluminum hydroxide and then adding a modifier for modification.

2. The flame retardant silicone rubber foam material according to claim 1, characterized in that: In terms of mass, the component A includes: 5-50 parts of vinyl silicone oil, 10-80 parts of α, ω-dihydroxy polydimethylsiloxane, 1-20 parts of low-viscosity hydroxy silicone oil, 20-40 parts of flame retardant, 1-35 parts of fumed silica, and 0.01-5 parts of platinum catalyst; the component B includes: 5-50 parts of vinyl silicone oil, 10-80 parts of α, ω-dihydroxy polydimethylsiloxane, 1-25 parts of hydrogen-containing silicone oil, 20-40 parts of flame retardant, 1-35 parts of fumed silica, and 0.1-1 parts of inhibitor.

3. The flame retardant silicone rubber foam material according to claim 1, characterized in that: The preparation method of the flame retardant is as follows: S1: Mix the dried molecular sieve and aluminum hydroxide in a mass ratio of 1:(1-5), add water and stir evenly at a constant temperature, filter and dry to obtain a composite powder; S2: Add 10%-40% of the mass of the modifier to the compound powder obtained in S1 and stir evenly; S3: Add water to the product obtained in S2, stir to form a slurry, filter and dry to obtain a flame retardant.

4. The flame retardant silicone rubber foam material according to claim 1, characterized in that: The vinyl content of the vinyl silicone oil is 0.1-1.2%; the hydroxyl content of the α,ω-dihydroxy polydimethylsiloxane is 0.01-0.1%; the hydroxyl content of the low-viscosity hydroxy silicone oil is 1-4%, and the viscosity is 20-200cps; the hydrogen content of the hydrogen-containing silicone oil is 0.1-3%; the platinum catalyst is one or more of 3000ppm or 5000ppm; the inhibitor is one or more of 2-methyl-3-butyn-2-ol or ethynyl cyclohexanol.

5. The flame retardant silicone rubber foam material according to claim 3, characterized in that: The modifier is a cationic surfactant with the structural formula of Si(OR1) (OR2) (OR3) (CH2) x N + (CH3)2(CH2) y CH3Cl - , wherein R1, R2, and R3 are each independently a C1-C4 alkyl group, x is an integer of 2 to 6, and y is an integer of 9 to 20; preferably, R1, R2, and R3 are all methyl groups, x=3, and y=15.

6. The flame retardant silicone rubber foam material according to claim 1, characterized in that: The molecular sieve is one or more of Y-type molecular sieve, ZSM-5 molecular sieve, 4A molecular sieve or MCM-41.

7. The flame retardant silicone rubber foam material according to claim 1, characterized in that: The aluminum hydroxide powder has a particle size of 1-5 μm.

8. The method for preparing the flame retardant silicone rubber foam material according to any one of claims 1 to 7, characterized in that: The following steps are involved: Preparation of component A: vinyl silicone oil, fumed silica, α,ω-dihydroxy polydimethylsiloxane, low-viscosity hydroxy silicone oil, and platinum catalyst are mixed, and then flame retardant is added and mixed thoroughly. After mixing, three-roll grinding is performed to obtain material A; Preparation of component B: vinyl silicone oil, fumed silica, α,ω-dihydroxy polydimethylsiloxane, low-viscosity hydrogenated silicone oil and inhibitor are mixed, and then flame retardant is added and mixed thoroughly. After mixing, three-roll grinding is performed to obtain material B; Preparation of foaming material: Weigh equal masses of A and B materials and mix them quickly, roll the sample through a roller, put it into an oven for one-stage vulcanization and two-stage vulcanization to obtain the final sample.

9. The method for preparing the flame retardant silicone rubber foam material according to claim 8, characterized in that: The first stage vulcanization temperature is 50-110° C., and the vulcanization time is 5-20 minutes.

10. The method for preparing the flame retardant silicone rubber foam material according to claim 8, characterized in that: The second stage vulcanization temperature is 150-200° C., and the vulcanization time is 20-80 minutes.