Silicone rubber product and preparation method thereof

By adding polyurethane additives and vulcanizing agents to silicone rubber, the problem of insufficient strain rate sensitivity of methyl silicone rubber is solved, and the better fit and instantaneous support of silicone rubber products in the field of biomedical care is achieved, and the complex movement of human body is adapted to state.

CN118994920AInactive Publication Date: 2024-11-22XIAMEN YINING YUANDA TECHNOLOGY CO LTD
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202411231859.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-04
Publication Date
2024-11-22
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Methyl silicone rubber products have insufficient strain rate sensitivity and cannot adapt to the complex and changing movement state of the human body, resulting in the inability to provide sufficient support or fit during rapid movement or sudden stress, affecting the application in the field of biomedical medicine. Effect.

Method used

By adding polyurethane additives and vulcanizing agents to the silicone rubber raw rubber, heating and stirring treatment, ensuring sufficient cross-linking reaction, improving the strain rate sensitivity and mechanical strength of the silicone rubber, thereby enhancing its ability to fit the human body and instantaneous support. sex.

Benefits of technology

It significantly improves the strain rate sensitivity of silicone rubber products, enables them to better adapt to human movement, provide better fit and instant support, and is suitable for the field of biomedical medicine.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005026406160000081
    Figure BDA0005026406160000081
Patent Text Reader

Abstract

The invention relates to the technical field of silicone rubber materials, and provides a silicone rubber product and a preparation method thereof, and the preparation method of the silicone rubber product comprises the following steps: adding a polyurethane auxiliary agent and a vulcanizing agent into raw silicone rubber, uniformly mixing, heating to 160-170 DEG C under the pressure of 10MPa, stirring for 15-20 minutes, and cooling to obtain a finished product. Based on this, the silicone rubber product can have good strain rate sensitivity, can better fit the human body, and also can significantly improve the instantaneous supporting performance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the field of silicone rubber materials, and in particular to a silicone rubber product and a preparation method thereof. Background Art

[0002] Methyl silicone rubber, as a high-performance elastomeric material, has shown a wide range of application potential in the biomedical field. Its excellent biocompatibility, aging resistance and good physical and mechanical properties make methyl silicone rubber a preferred material in the fields of plastic surgery, rehabilitation gear and prosthetic manufacturing.

[0003] However, despite the many advantages of methyl silicone rubber in the biomedical field, it also faces some challenges in its actual application, one of which is the problem of poor strain rate sensitivity. Specifically, when methyl silicone rubber products are used on the human body, they need to be able to adapt to the complex and changeable movement of the human body, including deformations of different rates and amplitudes. However, methyl silicone rubber products have deficiencies in strain rate sensitivity, that is, their mechanical properties (such as hardness, elastic modulus, etc.) cannot be adjusted quickly with changes in strain rate, resulting in insufficient support or fit in some cases (such as rapid movement or sudden force). In plastic surgery, if the implant cannot change flexibly with the patient's physical activities, it may cause discomfort or complications; in the field of rehabilitation gear and prostheses, insufficient strain rate may lead to insufficient support or poor fit, affecting the rehabilitation effect and the patient's daily life.

[0004] Therefore, the present application studies a method for preparing a silicone rubber product, so that the silicone rubber product has good strain rate sensitivity, that is, it can better fit the human body and significantly improve the instantaneous support. Summary of the invention

[0005] In order for silicone rubber products to have better strain rate sensitivity, that is, to better fit the human body, they can also significantly improve instantaneous support.

[0006] On the one hand, the present application provides a method for preparing a silicone rubber product, which adopts the following technical solution:

[0007] A method for preparing a silicone rubber product comprises the following steps: adding a polyurethane auxiliary agent and a vulcanizing agent to a silicone rubber raw rubber, heating the mixture to 160-170°C under a pressure of 10 MPa after uniform mixing, stirring the mixture for 15-20 minutes, and cooling the mixture to obtain a finished product.

[0008] By adopting the above technical scheme, the polyurethane additive helps to improve the strain rate sensitivity of silicone rubber, so that it can better adapt to human body movement, and when stirred at 160-170°C for 15-20 minutes, it can ensure uniform heating and more complete cross-linking reaction of the vulcanizer, so as to obtain silicone rubber products with better mechanical strength. At the same time, due to the effect of the polyurethane additive, the strain rate sensitivity of the silicone rubber product is improved, so that it can better fit the human body and significantly improve the instantaneous support.

[0009] Optionally, the weight of the polyurethane additive is 6-12% of the raw silicone rubber, and the weight of the vulcanizing agent is 0.4-0.6% of the raw silicone rubber.

[0010] Optionally, the silicone rubber raw rubber is methyl vinyl silicone rubber.

[0011] By adopting the above technical solution, methyl vinyl silicone rubber is used as a matrix, which can provide elasticity and aging resistance, and is non-toxic. When used in the medical field, after being prepared with a polyurethane additive, it has better strain rate sensitivity, that is, it can better fit the human body while significantly improving instantaneous support, which has significant advantages.

[0012] Optionally, the polyurethane auxiliary agent includes polyborodimethylsiloxane and polyurethane.

[0013] Optionally, the molecular weight of polyborodimethylsiloxane is 20,000 to 100,000.

[0014] Optionally, polyborodimethylsiloxane accounts for 20% of the polyurethane additive.

[0015] Optionally, the vulcanizing agent includes one or both of 2,4-dichlorobenzoyl peroxide and dipentadienyl vulcanizing agent.

[0016] On the other hand, the present application provides a silicone rubber product, which adopts the following technical solution:

[0017] A silicone rubber product is prepared by the silicone rubber product preparation method.

[0018] In summary, the present application includes at least one of the following beneficial technical effects:

[0019] 1. The polyurethane additive helps to improve the strain rate sensitivity of silicone rubber, so that it can better adapt to human body movement. When stirred at 160-170°C for 15-20 minutes, it can ensure uniform heating and more complete cross-linking reaction of the vulcanizer, so as to obtain silicone rubber products with better mechanical strength. At the same time, due to the effect of the polyurethane additive, the strain rate sensitivity of silicone rubber products is improved, so that they can better fit the human body and significantly improve the instantaneous support.

[0020] 2. Methyl vinyl silicone rubber as a matrix can provide elasticity and aging resistance, and is non-toxic. When used in the medical field, it has better strain rate sensitivity after being prepared with polyurethane additives, which means that it can better fit the human body while significantly improving instantaneous support, which has significant advantages. DETAILED DESCRIPTION

[0021] In the following examples and comparative examples, the raw silicone rubber was cut into blocks with a side length of less than 0.5 cm.

[0022] Embodiment 1:

[0023] A method for preparing a silicone rubber product comprises the following steps: adding 0.06 g of a polyurethane additive and 0.04 g of a vulcanizing agent to 1 g of silicone rubber raw rubber, mixing the mixture evenly, heating the mixture to 160° C. at a pressure of 10 MPa, stirring the mixture for 15 minutes, and cooling the mixture to obtain a finished product.

[0024] The silicone rubber raw rubber is methyl vinyl silicone rubber; the polyurethane additive includes polyborodimethylsiloxane and polyurethane, the polyborodimethylsiloxane and polyurethane are physically mixed, the polyborodimethylsiloxane accounts for 20% of the polyurethane additive content, and the molecular weight of the polyborodimethylsiloxane is 20000; the vulcanizing agent can be one or both of 2,4-dichlorobenzoyl peroxide and dipentadienyl vulcanizing agent.

[0025] Embodiment 2:

[0026] A method for preparing a silicone rubber product comprises the following steps: adding 0.08 g of a polyurethane additive and 0.05 g of a vulcanizing agent to 1 g of silicone rubber raw rubber, mixing the mixture evenly, heating the mixture to 160° C. at a pressure of 10 MPa, stirring the mixture for 15 minutes, and cooling the mixture to obtain a finished product.

[0027] The silicone rubber raw rubber is methyl vinyl silicone rubber; the polyurethane additive includes polyborodimethylsiloxane and polyurethane, the polyborodimethylsiloxane and polyurethane are physically mixed, the polyborodimethylsiloxane accounts for 20% of the polyurethane additive content, and the molecular weight of the polyborodimethylsiloxane is 30,000; the vulcanizing agent can be one or both of 2,4-dichlorobenzoyl peroxide and dipentadienyl vulcanizing agent.

[0028] Embodiment 3:

[0029] A method for preparing a silicone rubber product comprises the following steps: adding 0.1 g of a polyurethane additive and 0.05 g of a vulcanizing agent to 1 g of silicone rubber raw rubber, mixing the mixture evenly, heating the mixture to 160° C. at a pressure of 10 MPa, stirring the mixture for 15 minutes, and cooling the mixture to obtain a finished product.

[0030] Among them, the silicone rubber raw rubber is methyl vinyl silicone rubber; the polyurethane additive includes polyborodimethylsiloxane and polyurethane, and the polyborodimethylsiloxane and polyurethane are physically mixed, the polyborodimethylsiloxane accounts for 20% of the polyurethane additive content, and the molecular weight of the polyborodimethylsiloxane is 40000; the vulcanizing agent can be one or both of 2,4-dichlorobenzoyl peroxide and dipentadienyl vulcanizing agent.

[0031] Embodiment 4:

[0032] A method for preparing a silicone rubber product comprises the following steps: adding 0.12 g of a polyurethane additive and 0.06 g of a vulcanizing agent to 1 g of silicone rubber raw rubber, mixing the mixture evenly, heating the mixture to 160° C. at a pressure of 10 MPa, stirring the mixture for 15 minutes, and cooling the mixture to obtain a finished product.

[0033] The silicone rubber raw rubber is methyl vinyl silicone rubber; the polyurethane additive includes polyborodimethylsiloxane and polyurethane, the polyborodimethylsiloxane and polyurethane are physically mixed, the polyborodimethylsiloxane accounts for 20% of the polyurethane additive content, and the molecular weight of the polyborodimethylsiloxane is 60000; the vulcanizing agent can be one or both of 2,4-dichlorobenzoyl peroxide and dipentadienyl vulcanizing agent.

[0034] Embodiment 5:

[0035] A method for preparing a silicone rubber product comprises the following steps: adding 0.1 g of a polyurethane additive and 0.05 g of a vulcanizing agent to 1 g of silicone rubber raw rubber, mixing the mixture evenly, heating the mixture to 165° C. at a pressure of 10 MPa, stirring the mixture for 15 minutes, and cooling the mixture to obtain a finished product.

[0036] Among them, the silicone rubber raw rubber is methyl vinyl silicone rubber; the polyurethane additive includes polyborodimethylsiloxane and polyurethane, and the polyborodimethylsiloxane and polyurethane are physically mixed, the polyborodimethylsiloxane accounts for 20% of the polyurethane additive content, and the molecular weight of the polyborodimethylsiloxane is 40000; the vulcanizing agent can be one or both of 2,4-dichlorobenzoyl peroxide and dipentadienyl vulcanizing agent.

[0037] Embodiment 6:

[0038] A method for preparing a silicone rubber product comprises the following steps: adding 0.1 g of a polyurethane additive and 0.05 g of a vulcanizing agent to 1 g of silicone rubber raw rubber, mixing the mixture evenly, heating the mixture to 170° C. at a pressure of 10 MPa, stirring the mixture for 15 minutes, and cooling the mixture to obtain a finished product.

[0039] The silicone rubber raw rubber is methyl vinyl silicone rubber; the polyurethane additive includes polyborodimethylsiloxane and polyurethane, the polyborodimethylsiloxane and polyurethane are physically mixed, the polyborodimethylsiloxane accounts for 20% of the polyurethane additive content, and the molecular weight of the polyborodimethylsiloxane is 80,000; the vulcanizing agent can be one or both of 2,4-dichlorobenzoyl peroxide and dipentadienyl vulcanizing agent.

[0040] Embodiment 7:

[0041] A method for preparing a silicone rubber product comprises the following steps: adding 0.1 g of a polyurethane additive and 0.05 g of a vulcanizing agent to 1 g of silicone rubber raw rubber, mixing the mixture evenly, heating the mixture to 170° C. at a pressure of 10 MPa, stirring the mixture for 18 minutes, and cooling the mixture to obtain a finished product.

[0042] The silicone rubber raw rubber is methyl vinyl silicone rubber; the polyurethane additive includes polyborodimethylsiloxane and polyurethane, the polyborodimethylsiloxane and polyurethane are physically mixed, the polyborodimethylsiloxane accounts for 20% of the polyurethane additive content, and the molecular weight of the polyborodimethylsiloxane is 80,000; the vulcanizing agent can be one or both of 2,4-dichlorobenzoyl peroxide and dipentadienyl vulcanizing agent.

[0043] Embodiment 8:

[0044] A method for preparing a silicone rubber product comprises the following steps: adding 0.1 g of a polyurethane additive and 0.05 g of a vulcanizing agent to 1 g of silicone rubber raw rubber, mixing the mixture evenly, heating the mixture to 170° C. at a pressure of 10 MPa, stirring the mixture for 20 minutes, and cooling the mixture to obtain a finished product.

[0045] The silicone rubber raw rubber is methyl vinyl silicone rubber; the polyurethane additive includes polyborodimethylsiloxane and polyurethane, the polyborodimethylsiloxane and polyurethane are physically mixed, the polyborodimethylsiloxane accounts for 20% of the polyurethane additive content, and the molecular weight of the polyborodimethylsiloxane is 100000; the vulcanizing agent can be one or both of 2,4-dichlorobenzoyl peroxide and dipentadienyl vulcanizing agent.

[0046] Comparative Example 1:

[0047] Compared with Example 7, the difference between this comparative example and Example 7 is that: hydrogenated cyanoacrylate thickener is used instead of polyurethane reinforcing agent;

[0048] Except for the differences, the other aspects of this comparative example are the same as those of Example 7.

[0049] Comparative Example 2:

[0050] Compared with Example 7, the difference between this comparative example and Example 7 is that: a silane coupling agent is used instead of a polyurethane reinforcing agent;

[0051] Except for the differences, the other aspects of this comparative example are the same as those of Example 7.

[0052] Comparative Example 3:

[0053] Compared with Example 7, the difference between this comparative example is that the amount of vulcanizing agent used is 0.03g;

[0054] Except for the differences, the other aspects of this comparative example are the same as those of Example 7.

[0055] Comparative Example 4:

[0056] Compared with Example 7, the difference between this comparative example is that the amount of vulcanizing agent used is 0.07g;

[0057] Except for the differences, the other aspects of this comparative example are the same as those of Example 7.

[0058] Comparative Example 5:

[0059] Compared with Example 7, the difference between this comparative example and Example 7 is that the heating temperature is 150°C;

[0060] Except for the differences, the other aspects of this comparative example are the same as those of Example 7.

[0061] Comparative Example 6:

[0062] Compared with Example 7, the difference between this comparative example and Example 7 is that the heating temperature is 180°C;

[0063] Except for the differences, the other aspects of this comparative example are the same as those of Example 7.

[0064] Comparative Example 7:

[0065] Compared with Example 7, the difference between this comparative example is that the stirring time is 10 min;

[0066] Except for the differences, the other aspects of this comparative example are the same as those of Example 7.

[0067] Comparative Example 8:

[0068] Compared with Example 7, the difference between this comparative example is that the stirring time is 25 min;

[0069] Except for the differences, the other aspects of this comparative example are the same as those of Example 7.

[0070] The silicone rubber products obtained in Examples 1-8 and Comparative Examples 1-8 were observed to see whether they have strain rate sensitivity, hardness, and texture. The observation results are shown in Table 1:

[0071] Table 1:

[0072]

[0073] According to Examples 1-8, the silicone rubber products obtained through the examples of the present application are all strain rate sensitive and have moderate hardness. The moderate hardness value of this example is 5, the surface is not sticky, the texture is uniform, and there are no bubbles. When used in the medical field, it can make the human body feel more comfortable and still have supporting force.

[0074] By comparing Example 7 with Comparative Examples 1-2, it can be seen that silicone rubber products with strain rate sensitivity can be obtained by using polyurethane additives, and the use of hydrogenated nitrile acrylate thickeners and silane coupling agents have no strain rate sensitivity and have high hardness. When the hardness is too high, the hardness value is about 20, and there are tiny bubbles.

[0075] By comparing Example 7 with Comparative Examples 3-4, it can be seen that the silicone rubber product obtained by the amount of vulcanizer used in the present application has moderate hardness and a non-sticky surface, while the silicone rubber obtained by the amount of vulcanizer used in Comparative Examples 3-4, that is, the amount outside the embodiments, has no bubbles, but the hardness is too small or too large, and is not strain rate sensitive, and cannot achieve the effect of the present application.

[0076] By comparing Example 7 with Comparative Examples 5-6, it can be seen that the silicone rubber products obtained by the heating temperature of the present application have uniform texture and are free of bubbles, while the silicone rubber products obtained in Comparative Examples 5-6 have a hardness that is too large or too small, and a sticky surface, and are easily unusable due to seepage problems. Moreover, they have no strain rate sensitivity and have a large number of bubbles.

[0077] By comparing Example 7 with Comparative Examples 7-8, it can be seen that the silicone rubber products obtained by the stirring time of the present application are fully vulcanized and have strain rate sensitivity, while the silicone rubber products obtained in Comparative Examples 7-8 have low hardness or too high hardness, and have no strain rate sensitivity, and all produce tiny bubbles with a diameter of 1 mm.

[0078] The above are all preferred embodiments of the present application, and the protection scope of the present application is not limited thereto. Therefore, any equivalent changes made according to the structure, shape, and principle of the present application should be included in the protection scope of the present application.

Claims

1. A method for preparing a silicone rubber product, Features: The following steps are involved: Add polyurethane additive and vulcanizing agent to the silicone rubber raw rubber, mix well, heat to 160-170°C under a pressure of 10MPa, stir for 15-20min, and cool to obtain the finished product.

2. A method for preparing a silicone rubber product according to claim 1, Features: The weight of the polyurethane auxiliary agent is 6-12% of the raw silicone rubber, and the weight of the vulcanizing agent is 0.4-0.6% of the raw silicone rubber.

3. A method for preparing a silicone rubber product according to claim 1, Features: The silicone rubber raw rubber is methyl vinyl silicone rubber.

4. The method for preparing a silicone rubber product according to claim 1, Features: The polyurethane auxiliary agent comprises polyborodimethylsiloxane and polyurethane.

5. A method for preparing a silicone rubber product according to claim 4, Features: The molecular weight of polyborodimethylsiloxane is 20,000 to 100,000.

6. A method for preparing a silicone rubber product according to claim 4, Features: The polyboron dimethylsiloxane accounts for 20% of the polyurethane auxiliary agent.

7. The method for preparing a silicone rubber product according to claim 1, Features: The vulcanizing agent includes one or both of 2,4-dichlorobenzoyl peroxide and dipentadienyl vulcanizing agent.

8. A silicone rubber product, Features: The silicone rubber product is prepared by the method for preparing the silicone rubber product as described in any one of claims 1 to 7.

Citation Information

Patent Citations

  • Silicone rubber / polyurethane thermoplastic vulcanized rubber and preparing method thereof

    CN105924972A

  • Medical silicone rubber with high mechanical property and preparation method thereof

    CN109651822A

  • Waterproof polyborosiloxane impact-resistant damping material and preparation method thereof

    CN110564164A

  • High-resilience and low-pressure-change silicone rubber material and preparation method thereof

    CN113088090A