Anti-reflection, liquid-repellent, antifouling and anti-icing coating and preparation method thereof

Through the two-layer coating design, combined with materials such as ethanol, polyacrylic acid and tetraethyl silicate, a hollow silica layer is formed, which solves the problems of insufficient anti-reflection performance and wear resistance of the existing coating, and achieves high transparency Light rate and self-cleaning performance improve the service life and efficiency of the equipment.

CN118994986APending Publication Date: 2024-11-22STATE POWER INVESTMENT GRP GANSU ELECTRIC POWER CO LTD +1
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202411259191.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-09
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

The existing anti-reflection repellent anti-fouling and anti-icing coatings in the field of photovoltaics and wind turbine blades have problems such as insufficient anti-reflection performance or weak mechanical wear resistance, which affects the service life and efficiency of the equipment.

Method used

A two-layer structure coating is adopted, in which the anti-reflective layer A is composed of ethanol, polyacrylic acid and tetraethyl silicate, etc., and the anti-fouling and anti-icing layer B is composed of ethanol, aminopropyltriethoxysilane and polydimethyl The composition of a base silicone or the like is prepared by ultrasonic mixing and pulling method to form a hollow silica layer to improve the light transmittance and hardness of the coating.

Benefits of technology

It significantly improves light transmittance, enhances the hardness and wear resistance of the coating, and gives self-cleaning performance, which can effectively prevent drops of various liquids and improves the service life and efficiency of the equipment.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118994986A_ABST
    Figure CN118994986A_ABST
Patent Text Reader

Abstract

The invention provides an anti-reflection, liquid-repellent, antifouling and anti-icing coating and a preparation method thereof. The coating comprises an antireflection coating A and a liquid-repellent antifouling and anti-icing coating B, the antireflection coating A is prepared by taking ethanol as a solvent, polyacrylic acid as a template agent and tetraethyl silicate as a raw material. And the liquid-repellent, antifouling and anti-icing coating B is prepared by taking ethanol as a solvent, dimethyl dimethoxy silane and aminopropyl triethoxy silane as reactants and polydimethylsiloxane as a molecular brush. The preparation method comprises the following steps: firstly, coating the surface of a transparent substrate with the antireflection coating A, drying, then coating the surface of the antireflection coating A with the liquid-repellent antifouling and anti-icing coating B, and carrying out thermocuring to obtain the antireflection liquid-repellent antifouling and anti-icing coating. The preparation raw materials are simple and easy to obtain, the anti-reflection effect is remarkable, and the liquid repellent, antifouling and anti-icing effects are excellent.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of functional materials, and in particular to an anti-reflection liquid repellent anti-fouling and anti-icing coating and a preparation method thereof. Background Art

[0002] Natural phenomena such as dust, dirt, bird droppings, rain, frost, and rain and snow in winter are common, but in the fields of photovoltaics, wind turbine blades, and glass curtain walls, these natural phenomena will affect normal production efficiency, and even worse, they will seriously reduce the service life of production tools. For example, in solar panels, the role of photovoltaic encapsulation glass cannot be ignored. Photovoltaic encapsulation glass plays a role in protecting solar cells from damage by wind, sand, and rain. However, while protecting solar cells, the transmittance of photovoltaic encapsulation glass itself will affect the solar radiation received by solar cells, and the accumulation of dust for a long time will reduce its transmittance and reduce the efficiency of solar power generation. In addition, the coverage of snow in winter will also seriously affect the transmittance of photovoltaic glass. For another example, on the blades of wind turbines, the covering of ice and snow will destroy the aerodynamic structure of the blades and the balance of the entire turbine, seriously reducing the power generation efficiency of the wind turbine. Therefore, the research and development of coatings with both anti-reflection properties and self-cleaning properties has great research and commercial value.

[0003] At present, there are two main ways to prepare anti-reflective liquid-repellent anti-fouling and anti-icing coatings. The first is to prepare a single-layer or multi-layer anti-reflective film on a substrate, and then perform hydrophilic or hydrophobic modification on its surface. The anti-reflective and anti-fouling coatings obtained in this way usually have weak mechanical wear resistance, such as patents (CN117886518A) and (CN117886518A). The second is to directly prepare a high-molecular polymer coating on the substrate to give it anti-reflective, anti-fouling and anti-icing functions. The anti-reflective and anti-fouling coatings obtained in this way usually have weak anti-reflective performance, such as patent (CN108027451A).

[0004] In view of the above, developing a coating with excellent anti-reflection, liquid-repellent, anti-fouling and anti-icing properties has important application value. Summary of the invention

[0005] In view of the defects in the prior art, the object of the present invention is to provide an anti-reflective liquid-repellent anti-fouling and anti-icing coating and a preparation method thereof.

[0006] To achieve the above object, the present invention provides the following technical solutions:

[0007] In a first aspect, the present invention provides an anti-reflection liquid-repellent anti-fouling and anti-icing coating, comprising an anti-reflection layer A and an anti-fouling and anti-icing layer B, wherein:

[0008] The raw materials of the anti-reflection layer A include, by weight:

[0009] Ethanol 500-1300 parts

[0010] Polyacrylic acid 1-14 parts

[0011] 1-20 parts of tetraethyl silicate

[0012] 20-50 parts of catalyst;

[0013] The raw materials of the liquid-repellent antifouling and anti-icing layer B include, by weight:

[0014] Ethanol 100-500 parts

[0015] 10-30 parts of dimethyldimethoxysilane

[0016] 20-40 parts of aminopropyltriethoxysilane

[0017] Polydimethylsiloxane 1-20 parts

[0018] 1-10 parts of curing agent.

[0019] Preferably, the raw materials of the anti-reflection layer A include, by weight:

[0020] Ethanol 700-1100 parts

[0021] Polyacrylic acid 4-10 parts

[0022] 5-15 parts of tetraethyl silicate

[0023] 30-40 parts of catalyst;

[0024] The raw materials of the liquid-repellent antifouling and anti-icing layer B include, by weight:

[0025] Ethanol 200-400 parts

[0026] 15-25 parts of dimethyldimethoxysilane

[0027] 25-35 parts of aminopropyltriethoxysilane

[0028] Polydimethylsiloxane 5-15 parts

[0029] 3-7 parts of curing agent.

[0030] More preferably, the raw materials of the anti-reflection layer A include, by weight:

[0031] Ethanol 900 parts

[0032] 7 parts of polyacrylic acid

[0033] Tetraethyl silicate 1 0 parts

[0034] 35 parts of catalyst;

[0035] The raw materials of the liquid-repellent antifouling and anti-icing layer B include, by weight:

[0036] 300 parts of ethanol

[0037] 20 parts of dimethyldimethoxysilane

[0038] 30 parts of aminopropyltriethoxysilane

[0039] 10 parts of polydimethylsiloxane

[0040] 5 parts of curing agent.

[0041] Furthermore, the polydimethylsiloxane is selected from polydimethylsiloxane terminated with glycidoxypropyl, tris(glycidoxypropyldimethylsiloxy)phenylsilane, polydimethylsiloxane copolymer terminated with mono(2,3-epoxy)propyl ether or a combination thereof, preferably polydimethylsiloxane terminated with mono(2,3-epoxy)propyl ether.

[0042] Furthermore, the molar mass of the polydimethylsiloxane is 1000-5000 g / mol.

[0043] Furthermore, the catalyst is selected from ammonia water (pH=9), ammonia water (pH=10), ammonia water (pH=11), ammonia water (pH=12) or a combination thereof, preferably ammonia water (pH=10).

[0044] Furthermore, the curing agent is selected from hydrochloric acid solution (pH=1), hydrochloric acid solution (pH=2), sulfuric acid solution (pH=1), sulfuric acid solution (pH=2) or a combination thereof, preferably hydrochloric acid solution (pH=2).

[0045] In a second aspect, the present invention provides a method for preparing an anti-reflective liquid repellent anti-fouling and anti-icing coating, comprising the following steps:

[0046] Step (1), adding polyacrylic acid to ammonia water, ultrasonically mixing, adding to ethanol, and stirring for 10-12 hours to obtain a first component;

[0047] Step (2), at room temperature and pressure, tetraethyl silicate is divided into five equal parts, and each part of tetraethyl silicate is added to the first component in sequence at the same interval while stirring, and stirring is continued for 10-12 hours to obtain a second component;

[0048] Step (3), reflux the second component for 12-24 hours to remove aqueous ammonia to obtain a third component;

[0049] Step (4), coating the third component on the surface of the transparent substrate by a Czochralski method, and standing to dry to obtain an anti-reflection layer A;

[0050] Step (5), dissolving dimethyldimethoxysilane, aminopropyltriethoxysilane and polydimethylsiloxane in ethanol, adding a catalyst, and stirring the mixture to react, thereby obtaining a fourth component.

[0051] Step (6), coating the fourth component on the surface of the anti-reflection layer A by a Czochralski method, and curing the coating to obtain an anti-reflection liquid-repellent anti-fouling and anti-icing coating.

[0052] Furthermore, in step 1, the reaction temperature is 20-35°C, preferably 25°C; the ultrasonic time is 5-15min, preferably 10min.

[0053] Furthermore, in step 2, the interval time is 0.8-1.2h, preferably 1h.

[0054] Furthermore, in step 3, the reflux temperature is 60-100°C, preferably 80°C.

[0055] Furthermore, in step 4, the pulling speed is 4000 μm / min-8000 μm / min, preferably 5000 μm / min; the drying temperature is 60-100°C, preferably 80°C.

[0056] Furthermore, in step 5, the stirring time is 1-2 h, preferably 1.5 h.

[0057] Furthermore, in step 6, the pulling speed is 4000 μm / min-8000 μm / min, preferably 5000 μm / min; the curing temperature is 80-120° C., preferably 100° C., and the curing time is 1-3 h, preferably 2 h.

[0058] The technical solution of the present invention has the following advantages:

[0059] 1. The anti-reflection liquid repellent anti-fouling and anti-icing coating provided by the present invention is coated on the surface of a transparent substrate. Compared with a transparent substrate without a coating, its anti-reflection effect is obvious and the light transmittance can be increased by 3%.

[0060] 2. The anti-reflection layer in the anti-reflection liquid-repellent anti-fouling and anti-icing coating of the present invention is a hollow silica layer, which not only does not affect the liquid-repellent performance of the coating, but can also make the surface tension liquid slide off the coating surface at a smaller sliding angle, and can also increase the light transmittance and hardness of the coating.

[0061] 3. The anti-reflective liquid-repellent anti-fouling and anti-icing coating provided by the present invention is improved on the basis of the super-hydrophobic anti-reflective coating. Compared with the super-hydrophobic anti-reflective coating, the advantage of using an ultra-smooth liquid-like coating is more prominent, which not only improves the hardness and wear resistance of the coating, but also makes the coating have self-cleaning properties for most surface tension liquids. BRIEF DESCRIPTION OF THE DRAWINGS

[0062] In order to more clearly illustrate the specific implementation methods of the present invention or the technical solutions in the prior art, the drawings required for use in the specific implementation methods or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are some implementation methods of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0063] Figure 1 It is an anti-fouling effect diagram of the anti-reflection repellent anti-fouling and anti-icing coating provided by an embodiment of the present invention.

[0064] Figure 2 The diagram is a self-cleaning effect diagram of a glass substrate coated with an anti-reflection liquid anti-fouling and anti-icing coating provided by an embodiment of the present invention and a glass substrate without a coating. DETAILED DESCRIPTION

[0065] The following examples are provided for a better understanding of the present invention, but are not intended to limit the best mode of implementation, nor to limit the content and protection scope of the present invention. Any product identical or similar to the present invention obtained by anyone under the inspiration of the present invention or by combining the features of the present invention with other prior arts shall fall within the protection scope of the present invention.

[0066] If no specific experimental steps or conditions are specified in the examples, the conventional experimental steps or conditions described in the literature in the art can be used. The raw materials or instruments used are all conventional products that can be obtained commercially, including but not limited to the raw materials or instruments used in the examples of this application.

[0067] The following will be combined with the attached Figure 1 and attached Figure 2 , an anti-reflective liquid-repellent anti-fouling and anti-icing coating and a preparation method thereof provided in an embodiment of the present invention are introduced in detail.

[0068] Example 1

[0069] This embodiment provides an anti-reflection liquid-repellent anti-fouling and anti-icing coating, comprising an anti-reflection layer A and an anti-fouling and anti-icing layer B, wherein:

[0070] The raw materials of the anti-reflection layer A include, by weight:

[0071] 700 parts of ethanol

[0072] Polyacrylic acid 5 parts

[0073] 8 parts of tetraethyl silicate

[0074] 30 parts of ammonia water (pH=10);

[0075] The raw materials of the anti-fouling and anti-icing layer B include, by weight:

[0076] Ethanol 100 parts

[0077] 10 parts of dimethyldimethoxysilane

[0078] 20 parts of aminopropyltriethoxysilane

[0079] 8 parts of mono(2,3-epoxy)propyl ether-terminated polydimethylsiloxane

[0080] 3 parts of hydrochloric acid solution (pH=2).

[0081] Specifically, in this embodiment, the method for preparing the anti-reflective liquid repellent anti-fouling and anti-icing coating comprises the following steps:

[0082] Step (1), adding polyacrylic acid to ammonia water (pH=10) at 25° C., ultrasonically mixing for 15 minutes, adding to ethanol, and stirring for 12 hours to obtain a first component;

[0083] Step (2), at 25° C., tetraethyl silicate is divided into five equal parts, and each part of tetraethyl silicate is added to the first component in sequence at intervals of 1 hour while stirring, and stirring is continued for 12 hours to obtain a second component;

[0084] Step (3), reflux the second component at 80° C. for 24 hours to remove aqueous ammonia to obtain a third component;

[0085] Step (4), coating the third component on the surface of the transparent substrate by a pulling method, with a pulling speed of 5000 μm / min and drying at 80° C. to obtain an anti-reflection layer A;

[0086] Step (5), dissolving dimethyldimethoxysilane, aminopropyltriethoxysilane and mono(2,3-epoxy)propyl ether-terminated polydimethylsiloxane in ethanol, adding a catalyst hydrochloric acid solution (pH=2), and stirring the mixture to react for 1.5 hours to obtain a fourth component.

[0087] Step (6), coating the fourth component on the surface of the anti-reflection layer A by a pulling method, with a pulling speed of 5000 μm / min and curing at 100° C. for 2 hours to obtain an anti-reflection liquid-repellent anti-fouling and anti-icing coating.

[0088] Example 2

[0089] This embodiment provides an anti-reflection liquid-repellent anti-fouling and anti-icing coating, comprising an anti-reflection layer A and an anti-fouling and anti-icing layer B, wherein:

[0090] The raw materials of the anti-reflection layer A include, by weight:

[0091] 800 parts of ethanol

[0092] Polyacrylic acid 9 parts

[0093] 9 parts of tetraethyl silicate

[0094] 30 parts of ammonia water (pH=10);

[0095] The raw materials of the anti-fouling and anti-icing layer B include, by weight:

[0096] 200 parts of ethanol

[0097] 15 parts of dimethyldimethoxysilane

[0098] 25 parts of aminopropyltriethoxysilane

[0099] 3 parts of mono(2,3-epoxy)propyl ether terminated polydimethylsiloxane

[0100] 3 parts of hydrochloric acid solution (pH=2).

[0101] Specifically, in this embodiment, the method for preparing the anti-reflective liquid repellent anti-fouling and anti-icing coating comprises the following steps:

[0102] Step (1) adding polyacrylic acid to ammonia water (pH=10) at 25° C., ultrasonically mixing for 20 min, adding to ethanol, and stirring for 12 h to obtain a first component;

[0103] Step (2) at 25° C., tetraethyl silicate was divided into five equal parts, and each part of tetraethyl silicate was added to the first component at intervals of 1 hour while stirring, and stirring was continued for 12 hours to obtain a second component;

[0104] Step (3) reflux the second component at 80° C. for 24 hours to remove aqueous ammonia to obtain a third component;

[0105] Step (4) coating the third component on the surface of the transparent substrate by a Czochralski method at a pulling speed of 5000 μm / min and drying at 80° C. to obtain an anti-reflection layer A;

[0106] Step (5) Dissolve dimethyldimethoxysilane, aminopropyltriethoxysilane and mono(2,3-epoxy)propyl ether-terminated polydimethylsiloxane in ethanol, add a catalyst hydrochloric acid solution (pH=2), and stir the mixture to react for 1.5 hours to obtain a fourth component.

[0107] Step (6) coating the fourth component on the surface of the anti-reflection layer A by a pulling method, with a pulling speed of 5000 μm / min and curing at 100° C. for 2 h to obtain an anti-reflection liquid-repellent anti-fouling and anti-icing coating.

[0108] Example 3

[0109] This embodiment provides an anti-reflection liquid-repellent anti-fouling and anti-icing coating, comprising an anti-reflection layer A and an anti-fouling and anti-icing layer B, wherein:

[0110] The raw materials of the anti-reflection layer A include, by weight:

[0111] Ethanol 900 parts

[0112] 7 parts of polyacrylic acid

[0113] 10 parts of tetraethyl silicate

[0114] 35 parts of ammonia water (pH=10);

[0115] The raw materials of the anti-fouling and anti-icing layer B include, by weight:

[0116] 300 parts of ethanol

[0117] 20 parts of dimethyldimethoxysilane

[0118] 30 parts of aminopropyltriethoxysilane

[0119] 10 parts of mono(2,3-epoxy)propyl ether-terminated polydimethylsiloxane

[0120] 5 parts of hydrochloric acid solution (pH=2).

[0121] Specifically, in this embodiment, the method for preparing the anti-reflective liquid repellent anti-fouling and anti-icing coating comprises the following steps:

[0122] Step (1) adding polyacrylic acid to ammonia water (pH=10) at 25° C., ultrasonically mixing for 20 min, adding to ethanol, and stirring for 12 h to obtain a first component;

[0123] Step (2) at 25° C., tetraethyl silicate was divided into five equal parts, and each part of tetraethyl silicate was added to the first component at intervals of 1 hour while stirring, and stirring was continued for 12 hours to obtain a second component;

[0124] Step (3) reflux the second component at 80° C. for 24 hours to remove aqueous ammonia to obtain a third component;

[0125] Step (4) coating the third component on the surface of the transparent substrate by a Czochralski method at a pulling speed of 5000 μm / min and drying at 80° C. to obtain an anti-reflection layer A;

[0126] Step (5) Dissolve dimethyldimethoxysilane, aminopropyltriethoxysilane and mono(2,3-epoxy)propyl ether-terminated polydimethylsiloxane in ethanol, add a catalyst hydrochloric acid solution (pH=2), and stir the mixture to react for 1.5 hours to obtain a fourth component.

[0127] Step (6) coating the fourth component on the surface of the anti-reflection layer A by a pulling method, with a pulling speed of 5000 μm / min and curing at 100° C. for 2 h to obtain an anti-reflection liquid-repellent anti-fouling and anti-icing coating.

[0128] Example 4

[0129] This embodiment provides an anti-reflection liquid-repellent anti-fouling and anti-icing coating, comprising an anti-reflection layer A and an anti-fouling and anti-icing layer B, wherein:

[0130] The raw materials of the anti-reflection layer A include, by weight:

[0131] Ethanol 1300 parts

[0132] 14 parts of polyacrylic acid

[0133] 20 parts of tetraethyl silicate

[0134] 50 parts of ammonia water (pH=10);

[0135] The raw materials of the anti-fouling and anti-icing layer B include, by weight:

[0136] Ethanol 500 parts

[0137] 30 parts of dimethyldimethoxysilane

[0138] 40 parts of aminopropyltriethoxysilane

[0139] 20 parts of mono(2,3-epoxy)propyl ether-terminated polydimethylsiloxane

[0140] 10 parts of hydrochloric acid solution (pH = 2).

[0141] Specifically, in this embodiment, the method for preparing the anti-reflective liquid repellent anti-fouling and anti-icing coating comprises the following steps:

[0142] Step (1) adding polyacrylic acid to ammonia water (pH=10) at 25° C., ultrasonically mixing for 20 min, adding to ethanol, and stirring for 12 h to obtain a first component;

[0143] Step (2) at 25° C., tetraethyl silicate was divided into five equal parts, and each part of tetraethyl silicate was added to the first component at intervals of 1 hour while stirring, and stirring was continued for 12 hours to obtain a second component;

[0144] Step (3) reflux the second component at 80° C. for 24 hours to remove aqueous ammonia to obtain a third component;

[0145] Step (4) coating the third component on the surface of the transparent substrate by a Czochralski method at a pulling speed of 5000 μm / min and drying at 80° C. to obtain an anti-reflection layer A;

[0146] Step (5) Dissolve dimethyldimethoxysilane, aminopropyltriethoxysilane and mono(2,3-epoxy)propyl ether-terminated polydimethylsiloxane in ethanol, add a catalyst hydrochloric acid solution (pH=2), and stir the mixture to react for 1.5 hours to obtain a fourth component.

[0147] Step (6) coating the fourth component on the surface of the anti-reflection layer A by a pulling method, with a pulling speed of 5000 μm / min and curing at 100° C. for 2 h to obtain an anti-reflection liquid-repellent anti-fouling and anti-icing coating.

[0148] Example 5

[0149] This embodiment provides an anti-reflection liquid-repellent anti-fouling and anti-icing coating, comprising an anti-reflection layer A and an anti-fouling and anti-icing layer B, wherein:

[0150] The raw materials of the anti-reflection layer A include, by weight:

[0151] Ethanol 900 parts

[0152] 7 parts of polyacrylic acid

[0153] Tetraethyl silicate 1 0 parts

[0154] 35 parts of ammonia water (pH=10);

[0155] The raw materials of the anti-fouling and anti-icing layer B include, by weight:

[0156] 300 parts of ethanol

[0157] 20 parts of dimethyldimethoxysilane

[0158] 30 parts of aminopropyltriethoxysilane

[0159] 10 parts of mono(2,3-epoxy)propyl ether-terminated polydimethylsiloxane

[0160] 5 parts of hydrochloric acid solution (pH=2).

[0161] Specifically, in this embodiment, the method for preparing the anti-reflective liquid repellent anti-fouling and anti-icing coating comprises the following steps:

[0162] Step (1) adding polyacrylic acid to ammonia water (pH=10) at 25° C., ultrasonically mixing for 20 min, adding to ethanol, and stirring for 12 h to obtain a first component;

[0163] Step (2) at 25° C., tetraethyl silicate was divided into five equal parts, and each part of tetraethyl silicate was added to the first component at intervals of 1 hour while stirring, and stirring was continued for 12 hours to obtain a second component;

[0164] Step (3) reflux the second component at 80° C. for 24 hours to remove aqueous ammonia to obtain a third component;

[0165] Step (4) coating the third component on the surface of the transparent substrate by a Czochralski method at a pulling speed of 5000 μm / min and drying at 80° C. to obtain an anti-reflection layer A;

[0166] Step (5) Dissolve dimethyldimethoxysilane, aminopropyltriethoxysilane and mono(2,3-epoxy)propyl ether-terminated polydimethylsiloxane in ethanol, add a catalyst hydrochloric acid solution (pH=2), and stir the mixture to react for 1.5 hours to obtain a fourth component.

[0167] Step (6) coating the fourth component on the surface of the anti-reflection layer A by a pulling method, with a pulling speed of 5000 μm / min and curing at 100° C. for 2 h to obtain an anti-reflection liquid-repellent anti-fouling and anti-icing coating.

[0168] Experimental Example 1

[0169] The anti-reflective liquid-repellent anti-fouling and anti-icing coatings prepared in Examples 1 to 5 of the present invention were tested for their liquid-repellent anti-fouling effects.

[0170] Liquid repellency and antifouling test: 10 μl of aqueous ink, muddy water, coffee, long-chain alkane, DMF and DMSO were dropped on the surfaces of the coatings prepared in Examples 1 to 5, respectively, and the sliding angles of various droplets were tested using a sliding angle tester.

[0171] The test results are shown in Table 1.

[0172] Table 1 Test results of liquid repellency and antifouling properties of the anti-reflective liquid repellent antifouling and anti-icing coatings prepared in Examples 1 to 5

[0173]

[0174] like Figure 1 As shown, the anti-reflective liquid repellent antifouling coating provided by the embodiment of the present invention will not change the color of the substrate itself.

[0175] like Figure 1 and Figure 2As shown, 10 microliters of various sample droplets were added to the surface of the anti-reflection repellent anti-fouling and anti-icing coatings prepared in Examples 1 to 5 of the present invention to perform liquid repellency tests. The test results show that the sliding angles of various droplets are all less than 10°. It can be seen that the anti-reflection repellent anti-fouling and anti-icing coatings provided by the present invention have excellent anti-fouling and self-cleaning effects on water-based pollutants such as water-based ink, muddy water, coffee, and non-aqueous pollutants such as long-chain alkanes, DMF, and DMSO.

[0176] Experimental Example 2

[0177] The anti-reflection liquid repellent anti-fouling and anti-icing coatings prepared in Examples 1 to 5 of the present invention were tested for light transmittance and pencil hardness.

[0178] Light transmittance test: A double-beam UV spectrophotometer was used to test the light transmittance of the coating.

[0179] Pencil hardness test: Test the pencil hardness of the coating according to ASTM D3363. First, grind the pencil with 400-grit sandpaper, and then use a test cart equipped with pencils of various hardness to test the hardness of the coating under a load of 750g.

[0180] The test results are shown in Table 2.

[0181] Table 2 Test results of light transmittance and pencil hardness of the anti-reflective liquid repellent antifouling coatings prepared in Examples 1 to 5

[0182]

[0183] As shown in Table 2, compared with uncoated glass, the anti-reflection effect of the glass with the anti-reflection liquid repellent anti-fouling and anti-icing coating of the embodiment of the present invention is significantly improved, the light transmittance is increased by 3% on average, and the hardness can be changed from 3H to 4H. It can be seen that the anti-reflection liquid repellent anti-fouling coating provided by the present invention has high transparency and good hardness.

[0184] Experimental Example 3

[0185] The anti-icing effect of the anti-reflection liquid repellent anti-fouling and anti-icing coatings prepared in Examples 1 to 5 of the present invention was tested.

[0186] Anti-icing test: The laboratory built an anti-icing test device. In the experiment, the polyvinyl chloride tube (test tube) was precooled on the surface of a -15℃ freezer for 10 minutes. This process can prefreeze the moisture in the air in the gap between the test tube and the sample to be tested. This operation is to protect the water column from leaking out of the test tube. Then add a 1.0cm high water column to the test tube and continue freezing for 1h. Then, use a thrust gauge to slowly push the bottom of the test tube horizontally (as close to the bottom as possible) at a speed of 10 mm / min until there is obvious displacement between the test tube and the sample to be tested. In this process, the maximum value of the thrust gauge reading is the thrust value. Since the inner diameter of the test tube is 9.0mm, the adhesion strength of the anti-icing coating can be obtained by the formula P=F / S.

[0187] The test results are shown in Table 3.

[0188] Table 3 Anti-icing performance test results of the anti-reflection repellent anti-fouling and anti-icing coatings prepared in Examples 1 to 5

[0189]

[0190] As shown in Table 3, the adhesion between the anti-reflective liquid repellent anti-fouling and anti-icing coating of the embodiment of the present invention and ice is relatively low, and ice easily falls off the coating surface, thereby reducing adhesion to the substrate surface.

[0191] In summary, the anti-reflection liquid repellent anti-fouling and anti-icing coating provided by the present invention is formed by compounding a self-cleaning anti-reflection coating on the basis of a super-hydrophobic anti-reflection coating. Compared with the super-hydrophobic anti-reflection coating, the advantages of using a super-smooth liquid-like coating are more prominent, which not only improves the hardness and wear resistance of the coating, but also makes the coating have self-cleaning properties for most surface tension liquids. The anti-reflection layer in the anti-reflection liquid repellent anti-fouling and anti-icing coating of the present invention is a hollow silica layer, which not only does not affect the sliding performance of the coating to the droplets, but can make the surface tension liquid slide off the coating surface at a smaller sliding angle, and can increase the light transmittance and hardness of the coating. When applied to a transparent substrate, the anti-reflection liquid repellent anti-fouling and anti-icing coating of the present invention can improve the light transmittance and effectively enhance the anti-reflection effect.

[0192] Obviously, the above embodiments are merely examples for the purpose of clear explanation, and are not intended to limit the implementation methods. For those skilled in the art, other different forms of changes or modifications can be made based on the above description. It is not necessary and impossible to list all the implementation methods here. The obvious changes or modifications derived therefrom are still within the scope of protection of the present invention.

Claims

1. An anti-reflective liquid repellent anti-fouling and anti-icing coating, characterized in that: It includes an anti-reflection layer A and an anti-fouling and anti-icing layer B, wherein: The raw materials of the anti-reflection layer A include, by weight: Ethanol 500-1300 parts Polyacrylic acid 1-14 parts 1-20 parts of tetraethyl silicate 20-50 parts of catalyst; The raw materials of the liquid-repellent antifouling and anti-icing layer B include, by weight: Ethanol 100-500 parts 10-30 parts of dimethyldimethoxysilane 20-40 parts of aminopropyltriethoxysilane Polydimethylsiloxane 1-20 parts 1-10 parts of curing agent.

2. The high performance liquid repellent antifouling coating according to claim 1, characterized in that: Preferably, the raw materials of the anti-reflection layer A include, by weight: Ethanol 700-1100 parts Polyacrylic acid 4-10 parts 5-15 parts of tetraethyl silicate 30-40 parts of catalyst; The raw materials of the liquid-repellent antifouling and anti-icing layer B include, by weight: Ethanol 200-400 parts 15-25 parts of dimethyldimethoxysilane 25-35 parts of aminopropyltriethoxysilane Polydimethylsiloxane 5-15 parts 3-7 parts of curing agent.

3. The high performance liquid repellent antifouling coating according to claim 1, characterized in that: More preferably, the raw materials of the anti-reflection layer A include, by weight: Ethanol 900 parts 7 parts of polyacrylic acid 10 parts of tetraethyl silicate 35 parts of catalyst; The raw materials of the liquid-repellent antifouling and anti-icing layer B include, by weight: 300 parts of ethanol 20 parts of dimethyldimethoxysilane 30 parts of aminopropyltriethoxysilane 10 parts of polydimethylsiloxane 5 parts of curing agent.

4. The anti-reflection liquid repellent anti-fouling and anti-icing coating according to any one of claims 1 to 3, characterized in that: The polydimethylsiloxane is selected from polydimethylsiloxane terminated with glycidoxypropyl, tri(glycidoxypropyldimethylsiloxy)phenylsilane, polydimethylsiloxane copolymer terminated with mono(2,3-epoxy)propyl ether or a combination thereof, preferably polydimethylsiloxane terminated with mono(2,3-epoxy)propyl ether.

5. The anti-reflection liquid repellent anti-fouling and anti-icing coating according to any one of claims 1 to 3, characterized in that: The molar mass of the polydimethylsiloxane is 1000-5000 g / mol.

6. The anti-reflection liquid repellent anti-fouling and anti-icing coating according to any one of claims 1 to 3, characterized in that: The catalyst is selected from ammonia water (pH=9), ammonia water (pH=10), ammonia water (pH=11), ammonia water (pH=12) or a combination thereof, preferably ammonia water (pH=10).

7. The high performance liquid repellent antifouling coating according to claim 1, characterized in that: The curing agent is selected from hydrochloric acid solution (pH=1), hydrochloric acid solution (pH=2), sulfuric acid solution (pH=1), sulfuric acid solution (pH=2) or a combination thereof, preferably hydrochloric acid solution (pH=2).

8. The method for preparing an anti-reflective liquid repellent anti-fouling and anti-icing coating according to any one of claims 1 to 3, characterized in that: The following steps are involved: Step (1), adding polyacrylic acid to ammonia water, ultrasonically mixing, adding to ethanol, and stirring for 10-12 hours to obtain a first component; Step (2), at room temperature and pressure, tetraethyl silicate is divided into five equal parts, and each part of tetraethyl silicate is added to the first component in sequence at the same interval while stirring, and stirring is continued for 10-12 hours to obtain a second component; Step (3), reflux the second component for 12-24 hours to remove aqueous ammonia to obtain a third component; Step (4), coating the third component on the surface of the transparent substrate by a Czochralski method, and standing to dry to obtain an anti-reflection layer A; Step (5), dissolving dimethyldimethoxysilane, aminopropyltriethoxysilane and polydimethylsiloxane in ethanol, adding a catalyst, and stirring the mixture to react, thereby obtaining a fourth component. Step (6), coating the fourth component on the surface of the anti-reflection layer A by a Czochralski method, and curing the coating to obtain an anti-reflection liquid-repellent anti-fouling and anti-icing coating.

9. The method for preparing the anti-reflective liquid repellent anti-fouling and anti-icing coating according to claim 8, characterized in that: In the step (1), the reaction temperature is 20-35°C, and the ultrasonic time is 5-15min; in the step (2), the interval time is 0.8-1.2h; in the step (3), the reflux temperature is 60-100°C; in the step (4), the pulling speed is 4000μm / min-8000μm / min, and the drying temperature is 60-100°C; in the step (5), the stirring time is 1-2h; in the step (6), the pulling speed is 4000μm / min-8000μm / min, the curing temperature is 80-120°C, and the curing time is 1-3h.

Citation Information

Patent Citations

  • Preparation method of damp and heat-resistant anti-reflection coating with high strength

    CN106291779A

  • High-strength anti-reflection super-hydrophobic coating with antibacterial adhesion and sterilization properties and preparation method thereof

    CN108383397A

  • High-performance liquid-repellent antifouling paint and coating and preparation method thereof

    CN117551389A