Coating as well as preparation method and application thereof

Through the combination of water-based systems and specific resins, the problem of insufficient scratch resistance and wear resistance of ultra-matte coatings is solved, and the improvement of high blackness and optical properties is achieved, while reducing VOC emissions, which is suitable for a variety of substrates. Improves the imaging quality and service life of optical devices.

CN118995019AActive Publication Date: 2024-11-22HUNAN SOKAN NEW MATERIALS CO LTD
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202411222252.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-02
Publication Date
2024-11-22
Estimated Expiration
2044-09-02

AI Technical Summary

Technical Problem

While pursuing high blackness and optical properties, existing ultra-matte coatings have insufficient scratch resistance and wear resistance, and solvent-based systems lead to emissions of volatile organic compounds, affecting the environment and human health.

Method used

The coating is formulated using an aqueous system, and the combination of epoxy modified acrylic resin and polyurethane resin is used to improve scratch resistance and wear resistance through the encapsulation and structural stabilization of inorganic matting powder and resin, and achieve near super dumbness through precise ratios. The light effect is maintained at a high blackness, reducing the amount of matting powder to reduce VOC emissions.

Benefits of technology

It realizes a coating with low L value and good scratch resistance, has excellent adhesion and chemical resistance, reduces VOC emissions, meets environmental protection requirements, is suitable for a variety of substrates, and improves the imaging quality and service life of optical equipment. .

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005023370260000161
    Figure BDA0005023370260000161
  • Figure BDA0005023370260000181
    Figure BDA0005023370260000181
  • Figure BDA0005023370260000191
    Figure BDA0005023370260000191
Patent Text Reader

Abstract

The invention provides a coating as well as a preparation method and application thereof. The coating is prepared from a component A, a component B and a component C. The component A comprises epoxy modified acrylic resin, polyurethane resin, black paste, a defoaming agent, a base material wetting agent, a solvent A, a solvent B, an organic tin drier, a dispersing agent, a wear-resistant auxiliary, matting powder, a tackifier, water and a pH regulator, the component B comprises isocyanate, and the component C comprises water. The coating provided by the invention realizes an extremely low L value, provides higher blackness and optical properties, and has good scratch resistance and wear resistance. The invention also provides a preparation method and application of the coating.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of matte coatings, and in particular relates to a coating and a preparation method and application thereof. Background Art

[0002] In the relevant technical field, the L value of traditional matte paint is usually about 24, which represents the intensity of reflected light of the paint. The lower the L value, the higher the blackness of the paint and the less light it reflects, making the paint surface look deeper. However, although some super matte paints can achieve lower L values, even below 21, to achieve a deeper blackness effect, these paints show obvious deficiencies in other aspects.

[0003] Achieving an ultra-matte effect typically requires a large amount of matting powder, which is used to reduce the gloss of the coating and enhance its matte effect. However, too much matting powder can cause these particles to accumulate on the surface of the paint film, which can have a negative impact on the physical properties of the coating. Specifically, excessive accumulation of these matting powders can significantly reduce the coating's scratch resistance. Scratch resistance is an important measure of coating durability, especially in applications where the coating surface needs to remain intact for a long time. In addition, the coating's wear resistance can also be affected. Ultra-matte coating surfaces are prone to scratches or wear, which makes the coating more susceptible to damage during use, especially in environments that require high durability. This damage not only affects the aesthetics of the coating, but can also result in exposure of the substrate, which can affect the overall protective effect of the coating.

[0004] At present, there are almost no coatings on the market that can simultaneously meet high blackness and excellent scratch resistance. Especially in the field of optical equipment, the blackness of coatings is required to be higher. In optical equipment, coatings with high L values ​​may cause stray scattering of light, thereby affecting the imaging quality of the equipment. Coatings with high blackness can effectively suppress stray scattering of light, improve the imaging performance of optical components, and make the equipment perform better in high-precision applications. Therefore, in these application areas, the requirements for coatings are not only the matte effect on their appearance, but more importantly, the blackness of the coating can achieve optimal optical performance. In addition, most of the existing ultra-matte coatings use solvent systems, which means that they contain high volatile organic compounds (VOCs). These volatile substances are released into the air during the production and use of coatings, which have adverse effects on the environment. Volatile organic compounds are not only potentially harmful to human health, but also cause air pollution and aggravate environmental problems. Therefore, there is an urgent need for an environmentally friendly and high-performance coating on the market to meet the dual requirements of modern industry and environmental protection. In order to overcome these problems, it is necessary to develop a new type of coating that can not only achieve an extremely low L value, thereby providing higher blackness and optical performance, but also has good scratch and abrasion resistance. At the same time, the coating formula should minimize the content of volatile organic compounds to reduce the negative impact on the environment. Such a coating will be able to meet demanding optical applications, provide long-lasting durability, and meet environmental standards. This will not only enhance the market competitiveness of coatings, but also bring more efficient and environmentally friendly solutions to related industries in the context of continuous progress in science and technology. Summary of the invention

[0005] The present invention aims to solve at least one of the above technical problems existing in the prior art. To this end, the present invention provides a coating that achieves an extremely low L value, provides higher blackness and optical properties, and has good scratch resistance and abrasion resistance.

[0006] The invention also provides a method for preparing the coating.

[0007] The invention also provides application of the coating in optical components.

[0008] The first aspect of the present invention provides a coating, wherein the raw materials for preparing the coating include component A, component B and component C, and the component A includes, in parts by mass:

[0009] Epoxy modified acrylic resin: 30-40 parts,

[0010] Polyurethane resin: 10-20 parts,

[0011] Black paste: 10-15 parts,

[0012] Defoaming agent: 0.2-0.3 parts,

[0013] Substrate wetting agent: 0.5-1.0 parts,

[0014] Solvent A: 3.0-5.0 parts,

[0015] Solvent B: 3.0-5.0 parts,

[0016] Organic tin drier: 0.1-0.2 parts,

[0017] Dispersant: 3.0-4.0 parts,

[0018] Wear-resistant additive: 3-5 parts,

[0019] Matting powder: 4-6 parts,

[0020] Thickener: 0.2-0.3 parts,

[0021] Water: 10-30 parts,

[0022] pH regulator: 0.1-0.2 parts;

[0023] The component B comprises isocyanate;

[0024] The component C includes water.

[0025] One of the technical solutions of the present invention regarding the coating has at least the following beneficial effects:

[0026] The present invention adopts a water-based system, which can achieve good scratch resistance (almost no mark remains after skin contact) when the L value is about 17, while satisfying good adhesion and chemical resistance.

[0027] The present invention adopts a water-based PU system, which has stricter VOC requirements than solvent-based products, and a smaller range of raw materials can be selected. In the coating of the present invention, the matting efficiency of inorganic matting powder is better than that of organic matting powder, because the oil absorption and specific surface area of ​​inorganic matting powder are larger, but the strength and wear resistance of inorganic matting powder are worse than those of organic ones, but it is difficult to achieve a super matte effect by matting with organic matting powder, so the blackness is not low enough. How to ensure scratch resistance and wear resistance while achieving a super matte effect with inorganic matting powder becomes a key issue. The resin B used in the present invention has strong powder encapsulation, and the matte effect resin itself can further reduce the amount of matting powder in the formula, so that the amount of matting powder floating to the surface of the paint film during the drying process of the coating can be reduced to improve the scratch resistance; in addition, the resin of the present invention contains benzene rings or carbonate bonds, both of which are structurally stable groups, which can improve the rigidity of the paint film to improve the wear resistance, solving the above problems. Through the precise proportion of matting powder and tackifier, the present invention can achieve a nearly super-matte effect while maintaining a high blackness, effectively suppress stray scattering of light, and improve optical performance.

[0028] The coating of the present invention has excellent adhesion on a variety of complex substrates, good chemical and weather resistance, and can be adapted to optical devices made of different types of materials.

[0029] The water-based system and optimized formula make the coating preparation process simpler, reduce the complexity and cost of the production process, and make the coating easier to operate and control during application. The excellent adhesion on a variety of substrates makes the coating suitable for a wide range of applications, including different types of optical equipment, ensuring the reliability and durability of the coating. The improvement of chemical and weather resistance allows the coating to maintain stability under different environmental conditions, extending the service life of the coating.

[0030] According to some embodiments of the present invention, the epoxy-modified acrylic resin includes WLW-270 of DIC.

[0031] The epoxy-modified acrylic resin used in the present invention has excellent chemical resistance, hardness and adhesion on many substrates, and the hydroxyl groups inside the epoxy-modified acrylic resin react with isocyanate to form crosslinks. According to some embodiments of the present invention, the polyurethane resin includes Covestro's U-2757.

[0032] The polyurethane resin used in the present invention has good elasticity, self-repairing ability, good chemical resistance and scratch resistance, and is a self-matting resin.

[0033] According to some embodiments of the present invention, the black slurry uses carbon black produced by a high pigment furnace method as a raw material, and the raw materials include: 30 parts of carbon black, 30 parts of dispersant, 35 parts of deionized water, 0.2 parts of defoamer, 0.6 parts of pH regulator, 0.2 parts of thickener and 4 parts of solvent. Specifically, the carbon black is Orion FW200, the dispersant is BYK2013, the defoamer is BYK011, the pH regulator is DMEA, the thickener is Tego3060, and the solvent is propylene glycol. Preparation steps:

[0034] 1. Prepare materials and clean equipment;

[0035] 2. Add deionized water, add defoamer, dispersant and carbon black in order while stirring at 300-500rpm, stir for 2-3 minutes, disperse at high speed at 600-800rpm for 10-15 minutes (the temperature is controlled at 5-40℃ throughout the process), grind to a fineness of ≤15um, then add pH adjuster and solvent in order, stir for 3-5 minutes, and adjust the pH to 7.5-8.5 with DMEA.

[0036] According to some embodiments of the present invention, the defoaming agent is at least one of a polyether siloxane copolymer and polydimethylsiloxane.

[0037] According to some embodiments of the present invention, the defoaming agent is at least one of Tego810 and Tego902W of Tego and BYK024 of BYK Chemical.

[0038] According to some embodiments of the present invention, the substrate wetting agent is a polyether siloxane copolymer. The wetting agent is used to improve the wetting of the coating on the substrate, reduce the surface energy of the material, improve the fluidity of the coating on the substrate, and prevent shrinkage.

[0039] According to some embodiments of the present invention, the coating is at least one of Tego 270 and BYK 347 produced by Digo.

[0040] According to some embodiments of the present invention, both the solvent A and the solvent B are alcohol ether solvents.

[0041] The solvent is mainly used to lower the Tg point of the coating so that it can be cured into a film at a lower temperature. The solvent used in the present invention can lower the Tg point by 30-40°C.

[0042] According to some embodiments of the present invention, the solvent A comprises diethylene glycol butyl ether (DB).

[0043] According to some embodiments of the invention, the solvent B comprises dipropylene glycol methyl ether (DPM).

[0044] According to some embodiments of the present invention, the solvent A dries relatively quickly, while the solvent B dries relatively slowly. The different evaporation rates of the solvents in the wet film are used to adjust the evaporation gradient, improve the leveling of the paint film, solve the problem of gun clogging during paint spraying, and improve the construction performance.

[0045] According to some embodiments of the present invention, the organotin drier improves the drying performance of the water-based two-component polyurethane coating, reduces the drying time, and simultaneously improves the scratch resistance, hardness and mechanical resistance of the coating film.

[0046] According to some embodiments of the present invention, the organotin drier is Borchers' LH 10.

[0047] According to some embodiments of the present invention, the dispersant is at least one of a high molecular weight block copolymer solution, a copolymer containing pigment affinity groups, and an organic modified polyacrylate solution containing pigment affinity groups. The dispersant is used to disperse the matting powder so that the prepared coating has strong uniformity, is delicate and does not bloom.

[0048] According to some embodiments of the present invention, the dispersant is at least one of BYK2012, BYK2013 of BYK and Tego Dispers 735W and Tego Dispers 750W of Tego.

[0049] According to some embodiments of the present invention, the wear-resistant additive contains active hydroxyl groups at both ends, which can participate in a cross-linking reaction with isocyanate, thereby improving the cross-linking degree and hardness of the paint film, improving the scratch resistance and resistance to matte powder scratches, having a certain matting effect, and slightly reducing the amount of matte powder used.

[0050] According to some embodiments of the present invention, the wear-resistant additive is M-3062B from Guangzhou Chuying New Materials.

[0051] According to some embodiments of the present invention, the matting powder is a precipitated silica matting powder treated with a surfactant, which is easy to disperse, has an average particle size of 1.5 μm, and has a high matting efficiency. By adding a small amount of it, the gloss of the coating can reach below 0.2°. It has excellent transparency and can be used for matting without damaging the base color of the coating. The special surface treatment makes it highly stable in the system and does not produce hard precipitation.

[0052] According to some embodiments of the present invention, the matting powder is TS-100 produced by Evonik.

[0053] According to some embodiments of the present invention, the tackifier is a low-shear polyurethane thickener, which is used to provide thixotropy to the coating and prevent the wet film of the coating from sagging.

[0054] According to some embodiments of the present invention, the tackifier is Evonik's Tego 3060.

[0055] According to some embodiments of the present invention, the pH adjuster is an amine neutralizer, which mainly adjusts the pH of the coating to a weakly alkaline range, which is beneficial to the storage of water-based coatings, improves activation and prevents sedimentation, etc.

[0056] According to some embodiments of the invention, the pH adjuster is DMEA.

[0057] According to some embodiments of the present invention, the mass ratio of component A, component B and component C is 10:3:1-3.

[0058] According to some embodiments of the present invention, the component B includes an isocyanate, including hexamethylene diisocyanate, specifically Covestro's XP 2487 / 1.

[0059] According to some embodiments of the present invention, the method for preparing component A comprises the following steps:

[0060] (1) adding the epoxy-modified acrylic resin and the polyurethane resin into a dispersion container at a first stirring speed, adding the premixed solvent A and solvent B for stirring, then adding the substrate wetting agent, black slurry, wear-resistant additive and organic tin drier, stirring for 5-8 minutes, increasing the speed to a second stirring speed, adding the defoamer and dispersant, and stirring for 5-10 minutes;

[0061] (2) adding deionized water while reducing the speed, gradually increasing the speed to the third stirring speed, adding the matting powder, and stirring for 20-30 minutes;

[0062] (3) Add the pre-mixed water and pH adjuster, add the viscosity enhancer, and filter with a 250-350 mesh filter to obtain component A.

[0063] According to some embodiments of the present invention, the first stirring speed is 300 rpm-500 rpm.

[0064] According to some embodiments of the present invention, the second stirring speed is 500 rpm-800 rpm.

[0065] According to some embodiments of the present invention, the third stirring speed is 800 rpm-1500 rpm.

[0066] According to some embodiments of the present invention, the preparation method of component A may be:

[0067] S1. Add resin A and resin B into a dispersion container at a slow speed of 300-500 rpm;

[0068] S2. Add the premixed solvent 1 and solvent 2 at a slow speed of 300-500 rpm, stir for 3-5 minutes, and pay attention to scraping the edges;

[0069] S3, then add wetting agent, black slurry, wear-resistant additive and drying agent at 300-500 rpm, stir for 5-8 minutes, increase the speed to 500-800 rpm, add defoamer and dispersant, and stir for 5-10 minutes;

[0070] S4. Add deionized water while reducing the speed, gradually increase the speed to 800-1500 rpm, add matting powder, and stir at high speed for 20-30 minutes. Please pay attention to cooling during the process.

[0071] S5. Add deionized water, pH regulator and thickener. Please mix the deionized water and pH regulator in advance and let them stand for more than 5 minutes at room temperature before adding; adjust the pH with pH regulator and adjust the viscosity with deionized water; (the temperature is controlled at 5-35℃ throughout the process);

[0072] S6. Filter the package with a 250-350 mesh filter to obtain component A.

[0073] The second aspect of the present invention provides a method for preparing the coating of the first aspect of the present invention, the preparation method comprising the step of mixing the component A, component B and component C.

[0074] A technical solution in the method for preparing the coating of the present invention has at least the following beneficial effects:

[0075] The coating preparation method of the present invention does not require expensive equipment and complex process control, has undemanding reaction conditions, has readily available raw materials, has low production costs, and is easy to industrialize.

[0076] The third aspect of the present invention provides use of the coating according to the first aspect of the present invention in an optical component.

[0077] A technical solution of the present invention regarding the application of coating in optical components has at least the following beneficial effects:

[0078] Improved imaging quality. The high blackness of the coating effectively suppresses the stray scattering of light and reduces the reflection and scattering of light on the surface of components, thereby improving imaging clarity and image contrast and optimizing the imaging performance of optical equipment.

[0079] Enhanced optical performance. Low L value coatings on optical components can reduce the reflection and absorption of light, making the equipment perform better in high-precision applications and improving the overall performance and effect of optical equipment.

[0080] Improved durability. The coating's good scratch resistance and abrasion resistance ensure the durability of the coating during long-term use, avoid the degradation of optical performance due to surface damage, and maintain the long-term stability and reliability of components.

[0081] Multi-substrate adaptability. The coating can achieve excellent adhesion on a variety of complex substrates, ensuring stable performance and effects in optical components with different materials and surface types.

[0082] Environmental performance. Using a water-based system instead of a solvent-based system reduces the emission of volatile organic compounds (VOCs), meets environmental protection requirements, helps protect the environment and improves operational safety.

[0083] Improve production efficiency. The optimized coating formula and process simplify the coating and drying process, improve production efficiency, reduce manufacturing costs, and make the production of optical components more economical and efficient.

[0084] During construction, add component B and component C to component A, spray it on the surface of various substrates such as PC / PC+ABS, with a film thickness of 15-30μm, flash dry at room temperature for 3-5 minutes, and then bake at 80℃ for 2h to obtain a coating that meets the performance requirements. DETAILED DESCRIPTION

[0085] The following are specific embodiments of the present invention, and the technical solutions of the present invention are further described in conjunction with the embodiments, but the present invention is not limited to these embodiments.

[0086] In the first aspect, in some embodiments of the present invention, a coating is provided, wherein the raw materials for preparing the coating include component A, component B and component C, and in parts by mass, component A includes:

[0087] Epoxy modified acrylic resin: 30-40 parts,

[0088] Polyurethane resin: 10-20 parts,

[0089] Black paste: 10-15 parts,

[0090] Defoaming agent: 0.2-0.3 parts,

[0091] Substrate wetting agent: 0.5-1.0 parts,

[0092] Solvent A: 3.0-5.0 parts,

[0093] Solvent B: 3.0-5.0 parts,

[0094] Organic tin drier: 0.1-0.2 parts,

[0095] Dispersant: 3.0-4.0 parts,

[0096] Wear-resistant additive: 3-5 parts,

[0097] Matting powder: 4-6 parts,

[0098] Thickener: 0.2-0.3 parts,

[0099] Water: 10-30 parts,

[0100] pH regulator: 0.1-0.2 parts;

[0101] Component B includes isocyanate;

[0102] Component C includes water.

[0103] It can be understood that the present invention adopts a water-based system, which can achieve good scratch resistance (almost no mark remains after skin contact) when the L value is about 17, while satisfying good adhesion and chemical resistance.

[0104] The present invention adopts a water-based PU system, which has stricter VOC requirements than solvent-based products, and a smaller range of raw materials can be selected. In the coating of the present invention, the matting efficiency of inorganic matting powder is better than that of organic matting powder, because the oil absorption and specific surface area of ​​inorganic matting powder are larger, but the strength and wear resistance of inorganic matting powder are worse than those of organic ones, but it is difficult to achieve a super matte effect by matting with organic matting powder, so the blackness is not low enough. How to ensure scratch resistance and wear resistance while achieving a super matte effect with inorganic matting powder becomes a key issue. The resin B used in the present invention has strong powder encapsulation, and the matte effect resin itself can further reduce the amount of matting powder in the formula, so that the amount of matting powder floating to the surface of the paint film during the drying process of the coating film can be reduced to improve the scratch resistance; in addition, the resin of the present invention contains benzene rings or carbonate bonds, both of which are structurally stable groups, which can improve the rigidity of the paint film to improve the wear resistance, solving the above problems. Through the precise proportion of matting powder and tackifier, the present invention can achieve a nearly super-matte effect while maintaining a high blackness, effectively suppress stray scattering of light, and improve optical performance.

[0105] The coating of the present invention has excellent adhesion on a variety of complex substrates, good chemical and weather resistance, and can be adapted to optical devices made of different types of materials.

[0106] The water-based system and optimized formula make the coating preparation process simpler, reduce the complexity and cost of the production process, and make the coating easier to operate and control during application. The excellent adhesion on a variety of substrates makes the coating suitable for a wide range of applications, including different types of optical equipment, ensuring the reliability and durability of the coating. The improvement of chemical and weather resistance allows the coating to maintain stability under different environmental conditions, extending the service life of the coating.

[0107] In combination with the first aspect, in some embodiments of the present invention, the epoxy-modified acrylic resin includes WLW-270 from DIC.

[0108] The epoxy-modified acrylic resin used in the present invention has excellent chemical resistance, hardness and adhesion on many substrates, and the hydroxyl groups inside the epoxy-modified acrylic resin react with isocyanate to form crosslinks. According to some embodiments of the present invention, the polyurethane resin includes Covestro's U-2757.

[0109] The polyurethane resin used in the present invention has good elasticity, self-repairing ability, good chemical resistance and scratch resistance, and is a self-matting resin.

[0110] Combined with the first aspect, in some embodiments of the present invention, the black slurry uses carbon black produced by a high pigment furnace method as a raw material, and the raw materials are: 30 parts of carbon black, 30 parts of dispersant, 35 parts of deionized water, 0.2 parts of defoamer, 0.6 parts of pH regulator, 0.2 parts of thickener and 4 parts of solvent. Specifically, the carbon black is Orion FW200, the dispersant is BYK2013, the defoamer is BYK011, the pH regulator is DMEA, the thickener is Tego3060, and the solvent is propylene glycol. Preparation steps:

[0111] 1. Prepare materials and clean equipment;

[0112] 2. Add deionized water, add defoamer, dispersant and carbon black in order while stirring at 300-500rpm, stir for 2-3 minutes, disperse at high speed at 600-800rpm for 10-15 minutes (the temperature is controlled at 5-40℃ throughout the process), grind to a fineness of ≤15um, then add pH adjuster and solvent in order, stir for 3-5 minutes, and adjust the pH to 7.5-8.5 with DMEA.

[0113] In combination with the first aspect, in some embodiments of the present invention, the defoaming agent is at least one of a polyether siloxane copolymer and polydimethylsiloxane.

[0114] In combination with the first aspect, in some embodiments of the present invention, the defoaming agent is at least one of Tego810 and Tego902W of Tego and BYK024 of BYK Chemical.

[0115] In combination with the first aspect, in some embodiments of the present invention, the substrate wetting agent is a polyether siloxane copolymer. The wetting agent is used to improve the wetting of the coating on the substrate, reduce the surface energy of the material, improve the fluidity of the coating on the substrate, and prevent shrinkage.

[0116] In combination with the first aspect, in some embodiments of the present invention, at least one of Tego 270 and BYK 347 from Tego Corporation.

[0117] In combination with the first aspect, in some embodiments of the present invention, solvent A and solvent B are both alcohol ether solvents.

[0118] The solvent is mainly used to lower the Tg point of the coating so that it can be cured into a film at a lower temperature. The solvent used in the present invention can lower the Tg point by 30-40°C.

[0119] In combination with the first aspect, in some embodiments of the present invention, solvent A includes diethylene glycol butyl ether (DB).

[0120] In combination with the first aspect, in some embodiments of the present invention, solvent B includes dipropylene glycol methyl ether (DPM).

[0121] In combination with the first aspect, in some embodiments of the present invention, solvent A dries relatively quickly and solvent B dries relatively slowly. The different evaporation rates of the solvents in the wet film are used to adjust the evaporation gradient, improve the leveling of the paint film, solve the problem of gun clogging during paint spraying, and improve the construction performance.

[0122] In combination with the first aspect, in some embodiments of the present invention, the organotin drier improves the drying performance of the waterborne two-component polyurethane coating, reduces the drying time, and simultaneously improves the scratch resistance, hardness and mechanical resistance of the coating film.

[0123] In combination with the first aspect, in some embodiments of the present invention, the organotin drier is Borchers' LH 10.

[0124] In combination with the first aspect, in some embodiments of the present invention, the dispersant is at least one of a high molecular weight block copolymer solution, a copolymer containing pigment affinity groups, and an organic modified polyacrylate solution containing pigment affinity groups. The dispersant is used to disperse the matting powder so that the prepared coating has strong uniformity, is delicate and does not bloom.

[0125] In combination with the first aspect, in some embodiments of the present invention, the dispersant is at least one of BYK2012, BYK2013 produced by BYK and Tego Dispers 735W and Tego Dispers 750W produced by Tego.

[0126] In combination with the first aspect, in some embodiments of the present invention, the wear-resistant additive contains active hydroxyl groups at both ends, which can participate in the cross-linking reaction with isocyanate, thereby improving the cross-linking degree and hardness of the paint film, improving the scratch resistance and resistance to matte powder scratches, having a certain matting effect, and slightly reducing the amount of matte powder used.

[0127] In combination with the first aspect, in some embodiments of the present invention, the wear-resistant additive is M-3062B from Guangzhou Chuying New Materials.

[0128] Combined with the first aspect, in some embodiments of the present invention, the matting powder is a precipitated silica matting powder treated with a surfactant, which is easy to disperse, has an average particle size of 1.5 μm, and has a high matting efficiency. A small amount of addition can make the coating gloss reach below 0.2°. It has excellent transparency and can be used as a matting agent without damaging the base color of the coating. The special surface treatment makes it highly stable in the system and does not produce hard precipitation.

[0129] In combination with the first aspect, in some embodiments of the present invention, the matting agent is TS-100 produced by Evonik.

[0130] In combination with the first aspect, in some embodiments of the present invention, the tackifier is a low shear polyurethane thickener, which is used to provide thixotropy to the coating and prevent the wet film of the coating from sagging.

[0131] In combination with the first aspect, in some embodiments of the present invention, the tackifier is Evonik's Tego 3060.

[0132] In combination with the first aspect, in some embodiments of the present invention, the pH adjuster is an amine neutralizer, which mainly plays the role of adjusting the pH of the coating to a weakly alkaline range, which is beneficial to the storage of water-based coatings, improving activation and preventing sedimentation, etc.

[0133] In combination with the first aspect, in some embodiments of the present invention, the pH adjuster is DMEA.

[0134] In combination with the first aspect, in some embodiments of the present invention, the mass ratio of component A, component B and component C is 1:3:1-3.

[0135] In combination with the first aspect, in some embodiments of the present invention, component B includes isocyanate, specifically hexamethylene diisocyanate, specifically Covestro's XP 2487 / 1.

[0136] In combination with the first aspect, in some embodiments of the present invention, the preparation method of component A comprises the following steps:

[0137] (1) adding epoxy-modified acrylic resin and polyurethane resin into a dispersion container at a first stirring speed, adding premixed solvent A and solvent B for stirring, then adding substrate wetting agent, black slurry, wear-resistant additive and organic tin drier, stirring for 5-8 minutes, increasing the speed to a second stirring speed, adding defoamer and dispersant, and stirring for 5-10 minutes;

[0138] (2) Add deionized water while reducing the speed, gradually increase the speed to the third stirring speed, add matting powder, and stir for 20-30 minutes;

[0139] (3) Add the pre-mixed water and pH adjuster, add the viscosity enhancer, and filter with a 250-350 mesh filter to obtain component A.

[0140] In combination with the first aspect, in some embodiments of the present invention, the first stirring speed is 300 rpm-500 rpm.

[0141] In combination with the first aspect, in some embodiments of the present invention, the second stirring speed is 500 rpm-800 rpm.

[0142] In combination with the first aspect, in some embodiments of the present invention, the third stirring speed is 800 rpm-1500 rpm.

[0143] In combination with the first aspect, in some embodiments of the present invention, the preparation method of component A can be:

[0144] S1. Add resin A and resin B into a dispersion container at a slow speed of 300-500 rpm;

[0145] S2. Add the premixed solvent 1 and solvent 2 at a slow speed of 300-500 rpm, stir for 3-5 minutes, and pay attention to scraping the edges;

[0146] S3, then add wetting agent, black slurry, wear-resistant additive and drying agent at 300-500 rpm, stir for 5-8 minutes, increase the speed to 500-800 rpm, add defoamer and dispersant, and stir for 5-10 minutes;

[0147] S4. Add deionized water while reducing the speed, gradually increase the speed to 800-1500 rpm, add matting powder, and stir at high speed for 20-30 minutes. Please pay attention to cooling during the process.

[0148] S5. Add deionized water, pH regulator and thickener. Please mix the deionized water and pH regulator in advance and let them stand for more than 5 minutes at room temperature before adding; adjust the pH with pH regulator and adjust the viscosity with deionized water; (the temperature is controlled at 5-35℃ throughout the process);

[0149] S6. Filter the package with a 250-350 mesh filter to obtain component A.

[0150] In a second aspect, in some embodiments of the present invention, a method for preparing the coating of the first aspect of the present invention is provided, the preparation method comprising the step of mixing component A, component B and component C.

[0151] A technical solution in the method for preparing the coating of the present invention has at least the following beneficial effects:

[0152] The coating preparation method of the present invention does not require expensive equipment and complex process control, has undemanding reaction conditions, has readily available raw materials, has low production costs, and is easy to industrialize.

[0153] In a third aspect, some embodiments of the present invention provide use of the coating according to the first aspect of the present invention in an optical component.

[0154] The invention relates to the application of coating in optical components, which improves the imaging quality. The high blackness of the coating effectively suppresses the stray scattering of light, reduces the reflection and scattering of light on the surface of the component, thereby improving the imaging clarity and image contrast, and optimizing the imaging performance of the optical device.

[0155] Enhanced optical performance. Low L value coatings on optical components can reduce the reflection and absorption of light, making the equipment perform better in high-precision applications and improving the overall performance and effect of optical equipment.

[0156] Improved durability. The coating's good scratch resistance and abrasion resistance ensure the durability of the coating during long-term use, avoid the degradation of optical performance due to surface damage, and maintain the long-term stability and reliability of components.

[0157] Multi-substrate adaptability. The coating can achieve excellent adhesion on a variety of complex substrates, ensuring stable performance and effects in optical components with different materials and surface types.

[0158] Environmental performance. Using a water-based system instead of a solvent-based system reduces the emission of volatile organic compounds (VOCs), meets environmental protection requirements, helps protect the environment and improves operational safety.

[0159] Improve production efficiency. The optimized coating formula and process simplify the coating and drying process, improve production efficiency, reduce manufacturing costs, and make the production of optical components more economical and efficient.

[0160] During construction, add component B and component C to component A, spray it on the surface of various substrates such as PC / PC+ABS, with a film thickness of 15-30μm, flash dry at room temperature for 3-5 minutes, and then bake at 80℃ for 2h to obtain a coating that meets the performance requirements.

[0161] The following will be combined with the embodiments to clearly and completely describe the concept of the present invention and the technical effects produced, so as to fully understand the purpose, characteristics and effects of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, other embodiments obtained by those skilled in the art without creative work are all within the scope of protection of the present invention.

[0162] In the description of the present invention, the description with reference to the terms "one embodiment", "some embodiments", "illustrative embodiments", "examples", "specific examples", or "some examples" means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representation of the above terms does not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described may be combined in any one or more embodiments or examples in a suitable manner.

[0163] Unless otherwise specified, "room temperature" in the present invention means 25°C±5°C.

[0164] Unless otherwise specified, "about" in the present invention means that the allowable error is within ±2%.

[0165] If the specific conditions are not specified in the examples, the experiments were carried out under conventional conditions or conditions recommended by the manufacturer. If the manufacturers of the reagents or instruments are not specified, they are all conventional products that can be purchased commercially.

[0166] Example 1

[0167] A coating was prepared, and the raw materials for the preparation were component A, component B and component C. Among them, based on 100 parts by mass, the raw materials of component A were: epoxy modified acrylic resin: 30 parts, polyurethane resin: 20 parts, black paste: 10 parts, defoamer: 0.2 parts, substrate wetting agent: 0.5 parts, solvent A: 5.0 parts, solvent B: 4.0 parts, organic tin drier: 0.1 parts, dispersant: 3.0 parts, wear-resistant additive: 4.0 parts, matting powder: 5 parts, tackifier: 0.2 parts, pH adjuster: 0.2 parts, and the balance was water, which was filled to 100 parts.

[0168] Component B is an isocyanate, specifically hexamethylene diisocyanate, Covestro's XP 2487 / 1.

[0169] Component C is water.

[0170] The mass ratio of component A, component B and component C is 10:3:3.

[0171] In component A, the epoxy-modified acrylic resin is WLW-270 from DIC, and the polyurethane resin is U 2757. Solvent A is diethylene glycol butyl ether. Solvent B is dipropylene glycol methyl ether.

[0172] The black paste uses carbon black produced by the high pigment furnace method as raw material. The raw materials are: 30 parts of carbon black, 30 parts of dispersant, 35 parts of deionized water, 0.2 parts of defoamer, 0.6 parts of pH regulator, 0.2 parts of thickener and 4 parts of solvent. Specifically, the carbon black is Orion FW200, the dispersant is BYK2013, the defoamer is BYK011, the pH regulator is DMEA, the thickener is Tego3060, and the solvent is propylene glycol. Preparation steps:

[0173] 1. Prepare materials and clean equipment;

[0174] 2. Add deionized water, add defoamer, dispersant and carbon black in order while stirring at 300-500rpm, stir for 2-3 minutes, disperse at high speed at 600-800rpm for 10-15 minutes (the temperature is controlled at 5-40℃ throughout the process), grind to a fineness of ≤15um, then add pH adjuster and solvent in order, stir for 3-5 minutes, and adjust the pH to 7.5-8.5 with DMEA.

[0175] The defoaming agent is Tego 810, the substrate wetting agent is Tego 270, the organic tin drier is Borchers' LH 10, the dispersant is Tego Dispers 735W, the wear-resistant additive is Guangzhou Chuying New Materials' M-3062B, the matting powder is Evonik's TS-100, the tackifier is Evonik's Tego3060, and the pH adjuster is DMEA.

[0176] The preparation method of component A is:

[0177] S1. Add resin A and resin B into a dispersion container at a slow speed of 400 rpm;

[0178] S2, add pre-mixed solvent 1 and solvent 2 at a slow speed of 400 rpm, stir for 4 minutes, and pay attention to scraping the edges;

[0179] S3, then add wetting agent, black slurry, wear-resistant additive and drying agent at 400 rpm, stir for 6 minutes, increase the speed to 700 rpm, add defoamer and dispersant, and stir for 7 minutes;

[0180] S4. Add deionized water while reducing the speed, gradually increase the speed to 1200 rpm, add matting powder, and stir at high speed for 25 minutes. Please pay attention to cooling during the process.

[0181] S5. Add deionized water, pH regulator and thickener. Please mix the deionized water and pH regulator in advance and let them stand for more than 5 minutes at room temperature before adding; adjust the pH with pH regulator and adjust the viscosity with deionized water; (the temperature is controlled at 5-35℃ throughout the process);

[0182] S6. Filter the package with a 300-mesh filter to obtain component A.

[0183] The coating is prepared by mixing component A, component B and component C in proportion.

[0184] Examples 2 to 4

[0185] A coating was prepared respectively, and the difference from Example 1 was that the addition amount of each component was different. The details are shown in Table 1.

[0186] Table 1

[0187]

[0188]

[0189] Comparative Examples 1 to 4

[0190] A coating was prepared respectively, and the difference from Example 1 was that the addition amount of each component was different. The details are shown in Table 1.

[0191] Table 2

[0192] Comparative Example No. 1 2 3 4 Epoxy modified acrylic resin 40 60 0 0 Polyurethane resin 0 0 40 60 Black pulp 10 10 10 10 Defoaming agent 0.2 0.2 0.2 0.2 Wetting Agents 0.5 0.5 0.5 0.5 Solvent A 5.0 5.0 5.0 5.0 Solvent B 4.0 4.0 4.0 4.0 Dispersants 3.0 3.0 3.0 3.0 Drier 0.1 0.1 0.1 0.1 Matting powder 5.0 5.0 5.0 5.0 Wear-resistant additives 5.0 5.0 5.0 5.0 Thickener 0.2 0.2 0.2 0.2 pH Adjusters 0.2 0.2 0.2 0.2 Deionized water margin margin margin margin total 100.00 100.00 100.00 100.00

[0193] The coatings prepared in Examples 1 to 4 and Comparative Examples 1 to 4 were sprayed on the surface of the PC substrate to form a coating film with a thickness of 20 μm, flash-dried at room temperature for 3 minutes, and then baked at 80° C. for 2 hours to test the coating film properties. The results are shown in Table 3.

[0194] Table 3

[0195]

[0196]

[0197]

[0198] It should be noted that the coating of the present invention is not only suitable for PC substrates, but also suitable for the surfaces of various substrates such as PC+ABS.

[0199] The product of the present invention adopts a water-based PU system. Compared with traditional oil-based products, it has low VOC characteristics, meets environmental protection requirements, solves the problem that ultra-matte coatings are not scratch-resistant, has low blackness and scratch resistance, and has excellent wear resistance. In addition, the coating of the present invention has good adhesion on a variety of complex substrates and excellent chemical and weather resistance.

[0200] It should also be noted that the purpose of the present invention is to solve the problem of poor scratch resistance and wear resistance of conventional coatings under the premise of achieving super matte. Based on this as a guiding direction, the resin raw materials used in the present invention are determined by screening, because many resins cannot achieve a super matte effect with a gloss lower than 1° even if an excess of matting powder is added; the resins used in the present invention can achieve a super matte effect, but the wear resistance and scratch resistance are not ideal when used alone. The present invention is compounded according to a certain ratio to obtain a solution that can meet various performance requirements.

[0201] In the coating of the present invention, the epoxy modified acrylic resin has poor scratch resistance and abrasion resistance when used alone, and the L value is relatively high, because the resin itself has high gloss, and the gloss is higher than that of the polyurethane resin when the same amount of matting powder is added; the polyurethane resin is a self-matting resin and the paint film has a self-repairing function. It can achieve a lower L value when used alone, and the surface scratch resistance is relatively good, but it still cannot meet the requirements. The adhesion of the paint film is general, and the hardness is biased. Because the resin is a polycarbonate type polyurethane, the hardness is general, and the molecular weight is large, resulting in a lower film density than the epoxy modified acrylic resin, but also due to the large molecular weight, the encapsulation of the matting powder is stronger, so compared with the epoxy modified acrylic resin, the scratch resistance is better.

[0202] Increasing the amount of wear-resistant additive in the present invention will further improve the Taber test. Comprehensive evaluation of various properties shows that the range disclosed in the present invention is close to the optimal addition amount.

[0203] When the coating of the present invention is used in optical components, the high blackness of the coating effectively suppresses the stray scattering of light, reduces the reflection and scattering of light on the surface of the component, thereby improving the imaging clarity and image contrast, and optimizing the imaging performance of the optical device. The low L value coating can reduce the reflection and absorption of light on the optical components, so that the equipment performs better in high-precision applications, and improves the overall performance and effect of the optical equipment. The good scratch resistance and wear resistance of the coating ensure the durability of the coating in long-term use, avoid the degradation of optical performance caused by surface damage, and maintain the long-term stability and reliability of the components. The coating can achieve excellent adhesion on various complex substrates, ensuring that stable performance and effects can be obtained in optical components of different materials and surface types. The use of a water-based system rather than a solvent-based system reduces the emission of volatile organic compounds (VOCs), meets environmental protection requirements, helps to protect the environment and improve operational safety. The optimized coating formula and process simplify the coating and drying process, improve production efficiency, reduce manufacturing costs, and make the production of optical components more economical and efficient.

[0204] The present invention has been described in detail above in conjunction with the embodiments, but the present invention is not limited to the above embodiments, and various changes can be made within the knowledge scope of ordinary technicians in the relevant technical field without departing from the purpose of the present invention.

Claims

1. A coating, characterized in that: The raw materials for preparation include component A, component B and component C. In parts by mass, component A includes: Epoxy modified acrylic resin: 30-40 parts, Polyurethane resin: 10-20 parts, Black paste: 10-15 parts, Defoaming agent: 0.2-0.3 parts, Substrate wetting agent: 0.5-1.0 parts, Solvent A: 3.0-5.0 parts, Solvent B: 3.0-5.0 parts, Organic tin drier: 0.1-0.2 parts, Dispersant: 3.0-4.0 parts, Wear-resistant additive: 3-5 parts, Matting powder: 4-6 parts, Thickener: 0.2-0.3 parts, Water: 10-30 parts, pH regulator: 0.1-0.2 parts; The component B comprises isocyanate; The component C includes water.

2. The coating according to claim 1, characterized in that The epoxy-modified acrylic resin includes WLW-270 from DIC.

3. The coating according to claim 1, characterized in that The polyurethane resin includes Covestro's U-2757.

4. The coating according to claim 1, characterized in that The solvent A includes diethylene glycol butyl ether.

5. The coating according to claim 1, characterized in that The solvent B includes dipropylene glycol methyl ether.

6. The coating according to claim 1, characterized in that The mass ratio of component A, component B and component C is 10:3:1-3.

7. The coating according to any one of claims 1 to 6, characterized in that The preparation method of component A comprises the following steps: S1, adding the epoxy-modified acrylic resin and the polyurethane resin into a dispersion container at a first stirring speed, adding the premixed solvent A and solvent B for stirring, then adding the substrate wetting agent, black slurry, wear-resistant additive and organic tin drier, stirring for 5-8 minutes, increasing the speed to a second stirring speed, adding the defoamer and dispersant, and stirring for 5-10 minutes; S2, add deionized water while reducing the speed, gradually increase the speed to the third stirring speed, add the matting powder, and stir for 20-30 minutes; S3, adding the pre-mixed water and pH regulator, adding the viscosity enhancer, and filtering with a 250-350 mesh filter to obtain the component A.

8. The coating according to claim 7, characterized in that The first stirring speed is 300rpm-500rpm; and / or, the second stirring speed is 500rpm-800rpm; and / or, the third stirring speed is 800rpm-1500rpm.

9. A method for preparing a coating as claimed in any one of claims 1 to 8, characterized in that: The method comprises the step of mixing the component A, component B and component C.

10. Use of the coating according to any one of claims 1 to 8 in optical components.

Citation Information

Patent Citations

  • Preparation device and preparation method of modified silicon dioxide and application of modified silicon dioxide

    CN107841186A

  • Ultra-black coating, LED display screen and preparation method of LED display screen

    CN114133841A

  • Coating as well as preparation method and application thereof

    CN115197597A

  • Ultra-matte water-based amino stoving varnish capable of being attached to multiple base materials and preparation method of ultra-matte water-based amino stoving varnish

    CN117777798A