High-performance selective etching solution for silicon in silicon germanium / silicon lamination
By using an etching solution composed of quaternary ammonium hydroxide and alkanolamine, combined with a SiGe inhibitor, highly selective etching of silicon in SiGe multilayer structures was achieved, solving the problems of high surface roughness and limited etching rate in existing technologies, and meeting the material processing precision requirements of GAA MOSFET technology.
Patent Information
- Application Number
- CN202410967984.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-18
- Publication Date
- 2024-11-22
- Estimated Expiration
- 2044-07-18
AI Technical Summary
Existing technologies struggle to achieve highly selective removal of the Si sacrificial layer while protecting the SiGe nanowires during the etching of SiGe multilayer structures. This results in high surface roughness and limited etching rate, failing to meet the material processing precision requirements of GAA MOSFET technology.
An etching solution composition comprising quaternary ammonium hydroxide, alkanolamine, SiGe inhibitor, and water is used to achieve highly selective etching of silicon by controlling the etching conditions, while protecting the silicon-germanium layer from etching. The etching solution composition may also contain SiGe inhibitors such as quinoline compounds and polyamine compounds to improve the selectivity.
Highly efficient etching of silicon was achieved, with a silicon/silicon-germanium selectivity ratio of over 20 and an etching rate controlled within 2 Å/min, ensuring the integrity of the SiGe nanowires and meeting the processing precision requirements of GAA MOSFET technology.
Smart Images

Figure SMS_1 
Figure SMS_2 
Figure SMS_3
Abstract
Description
Technical Field
[0001] The invention belongs to the field of electronic chemicals, and in particular relates to an etching solution suitable for selectively removing silicon relative to silicon germanium from a silicon germanium / silicon stack in a microelectronic device. Background Art
[0002] For the future evolution of CMOS technology, we are committed to exploring GAA MOSFET (Gate All Around Metal Oxide Semiconductor Field Effect Transistor) as a successor to FINFET (Fin Field Effect Transistor) technology. The core of this transformation is to explore how to cleverly integrate SiGe or Ge materials, supplemented by precise material removal technology, to optimize the comprehensive solution of short channel effect. Specifically, the construction process of GAA MOSFET involves the removal of Si or SiGe layers with high selectivity in a multi-layer structure to achieve FINFET structure and patterning. The steps in these processes include depositing alternating nanoscale Si sacrificial layers and SiGe channel layers through epitaxial growth, and then using a high-selectivity etching process to remove the Si sacrificial layer and properly control the erosion of the main substrate, leaving a SiGe nanowire channel on the suspended trench. Finally, a thin gate dielectric layer is deposited around the SiGe nanowires and trenches, and covered with metal to form the gate electrode of the GAA MOSFET.
[0003] In the realization of this complex process, the wet etching technology based on alkaline solution is favored because of its low cost, convenient operation and low corrosion to silicon oxide. Among them, KOH and TMAH (tetramethylammonium hydroxide) are the two mainstream etchants, each with its own advantages and disadvantages. Although KOH is widely used, its reaction process may introduce potassium ions that affect device performance, and the etched surface roughness is relatively high. In comparison, TMAH exhibits better integrated circuit process compatibility, but the etching rate is limited at high concentrations, and the etching selectivity for the Si sacrificial layer in the Si / SiGe multilayer structure is not ideal, which can easily cause damage to the SiGe nanowires.
[0004] In view of this, the current field urgently needs an etching composition to improve the etching process accuracy of the sacrificial layer Si, while achieving highly selective protection of SiGe nanowires, so as to meet the stringent requirements of GAA MOSFET technology advancement on material processing accuracy. Summary of the invention
[0005] In order to solve the above problems, the present invention provides a high-performance selective etching solution for silicon in a silicon germanium / silicon stack, which etches the silicon-containing layer in the presence of a silicon germanium layer. The etching solution comprises quaternary ammonium hydroxide, alkanolamine, SiGe inhibitor and water.
[0006] Further, the quaternary ammonium hydroxide is R4NOH, where R is four identical or different aliphatic hydrocarbon groups or aromatic hydrocarbon groups, preferably one or more of tetramethylammonium hydroxide, tetraethylammonium hydroxide, tetrapropylammonium hydroxide, tetrabutylammonium hydroxide, methyltriethylammonium hydroxide, ethyltrimethylammonium hydroxide, benzyltrimethylammonium hydroxide, benzyltriethylammonium hydroxide, 2-hydroxyethyltrimethylammonium hydroxide, and most preferably tetramethylammonium hydroxide.
[0007] Further, the dosage of the quaternary ammonium hydroxide is 0.3-50 wt%, preferably 1-40 wt%, more preferably 5-30 wt%, and most preferably 10-20 wt%.
[0008] Further, the alkanolamine is selected from one or more of monoethanolamine, diethanolamine, 2-(ethylamino)ethanol, 2-dibutylaminoethanol, N,N-diethylethanolamine, triethanolamine, monoisopropanolamine, diisopropanolamine, triisopropanolamine, cyclohexylamine diethanol, and preferably triethanolamine.
[0009] Further, the dosage of the alkanolamine is 0.01-50 wt%, preferably 0.1-40 wt%, more preferably 0.5-30 wt%, and most preferably 1-20 wt%.
[0010] Further, the SiGe inhibitor is selected from one or more of quinoline compounds, polyamine compounds, furan ring compounds, and aromatic ether compounds.
[0011] Further, the dosage of the SiGe inhibitor is 0.001-10 wt%, preferably 0.002-5 wt%, more preferably 0.005-2 wt%, and most preferably 0.01-0.5 wt%.
[0012] Further, the quinoline compounds are selected from one or more of 8-hydroxyquinoline, 2-amino-8-hydroxyquinoline, and 4-amino-2-methylquinoline.
[0013] Further, the polyamine compounds are selected from one or more of NH2(CH2) n NH2, polyvinylpyrrolidone, benzotriazole, hexamethylenetetramine, and preferably 1,6-hexanediamine, polyvinylpyrrolidone, benzotriazole, hexamethylenetetramine.
[0014] Further, in the NH2(CH2) n NH2, the value of n is 3 < n < 10; the viscosity K value of the polyvinylpyrrolidone is 8-100, preferably 10-40, and most preferably 12-20.
[0015] Furthermore, the furan ring compound is selected from one or more of furan, dihydrofuran, tetrahydrofuran, 2-methylfuran, 3-methylfuran, 2,5-dimethylfuran, 2-ethylfuran, 2,2-dimethyltetrahydrofuran, 2-phenylfuran, 2-acetylfuran, and 5-methyl-2-acetylfuran; preferably one or more of furan, 2-ethylfuran, 2-phenylfuran, and 2-acetylfuran.
[0016] Furthermore, the aromatic ether compound is selected from one or more of anisole, phenethyl ether, o-methoxyphenol, p-methoxyphenol, 2-methoxynaphthalene, phenoxybenzene, phenyl benzyl ether, 1,2-dimethoxybenzene, and 2,4-dimethoxybenzaldehyde; preferably one or more of anisole, p-methoxyphenol, and 2,4-dimethoxybenzaldehyde.
[0017] Furthermore, the etching solution may also contain one or more water-soluble organic solvents, which are one or more of propanol, isopropanol, propylene glycol, butanol, butyl diglycol, cyclohexane, dimethylformamide, cyclopentane sulfone, and dimethyl sulfoxide; preferably one or more of isopropanol, dimethylformamide, cyclopentane sulfone and dimethyl sulfoxide, and more preferably isopropanol.
[0018] Furthermore, the water-soluble organic solvent is used in an amount of 0.1-60 wt %, preferably 1-40 wt %, more preferably 2-30 wt %, and most preferably 5-20 wt %.
[0019] The present invention also provides a method for selectively etching silicon in a silicon germanium / silicon stack using the above etching solution, the steps of which are as follows: The etching solution contacts the microelectronic device including the silicon germanium / silicon stack at a temperature of 10° C. to 100° C. to complete the etching of the silicon layer.
[0020] Furthermore, the contact time is less than 24 hours, preferably 1-60 minutes.
[0021] Furthermore, the contact temperature is preferably 20-80°C, more preferably 25-60°C.
[0022] Further, the Si / SiGe etching selectivity ratio is >20, preferably >50, and more preferably >340.
[0023] Furthermore, the etching rate of SiGe is less than 10Å / min, preferably less than 5Å / min, and more preferably less than 2Å / min.
[0024] Further, the thermal oxide etch rate is <2Å / min, preferably <0.2Å / min.
[0025] Furthermore, the rate at which silicon is removed can be adjusted by increasing or decreasing etching conditions, such as temperature.
[0026] Furthermore, SiGe inhibitors can be used in combination to further improve the Si / SiGe selectivity.
[0027] Further, the water-miscible organic solvent is preferably miscible with water at least in a 1:1 (wt) ratio at 20° C. and ambient pressure.
[0028] Furthermore, the etching solution may further include one or more surfactants, including but not limited to: Anionic surfactants, zwitterionic surfactants, nonionic surfactants.
[0029] The anionic surfactant is preferably ammonium lauryl sulfate, dodecylbenzene sulfonate, fatty alcohol polyoxyethylene ether sulfate, fatty alcohol polyoxyethylene ether carboxylate, alkyl ether phosphate, and fluorine-containing surfactant; the fluorine-containing surfactant is preferably perfluorodecyltrimethoxysilane, tridecafluorooctylethyltrimethoxysilane, perfluoroalkylsulfonamide salt, perfluorooctanesulfonate, perfluorobutanesulfonate, perfluorononanoate and perfluorooctanoate.
[0030] Zwitterionic surfactants, preferably dodecyl dimethyl betaine, cocamidopropyl hydroxysulfonate, cocamidopropyl-2-hydroxy-3-sulfonate, lauroamidopropyl betaine, lauroamidopropyl hydroxysulfonate, palmitamidopropyl betaine, stearamidopropyl betaine, stearamidopropyl hydroxysulfonate, phosphatidylserine, phosphatidylethanolamine, phosphatidylcholine.
[0031] The nonionic surfactant is preferably a fatty alcohol polyoxyethylene ether, an alkylphenol polyoxyethylene ether, a fatty acid methyl ester ethoxylate, a fatty acid glyceride, a polyoxyethylene fatty acid ester, a polyethylene glycol fatty acid ester, a polyoxyethylene alkylamine, a polyoxyethylene alkylamide, or a polyether surfactant.
[0032] Furthermore, the surfactant is more preferably or comprises perfluoro N-substituted alkylsulfonamide ammonium salt.
[0033] Further, preferred surfactants do not contain metals or metal ions.
[0034] Further, the total amount of the surfactant is 0.0001-10 wt %, preferably 0.0005-5 wt %, more preferably 0.001-1 wt %, and most preferably 0.002-0.2 wt %.
[0035] Furthermore, the etching solution is most preferably an aqueous solution without a surfactant.
[0036] Furthermore, the etching solution may also contain one or more chelating agents, including but not limited to ethylenediaminetetraacetic acid, butanediaminetetraacetic acid, propylenediaminetetraacetic acid, diethylenetriaminepentaacetic acid, triethylenetetraaminehexaacetic acid, diethylenetriaminepentaacetic acid, cystine, and gallic acid.
[0037] Further, the total amount of the chelating agent is 0.0001-10 wt %, preferably 0.0005-5 wt %, more preferably 0.001-1 wt %, and most preferably 0.002-0.2 wt %.
[0038] Furthermore, the etching solution is most preferably an aqueous solution without a chelating agent.
[0039] Furthermore, after etching is completed, the etching solution can be easily removed from the microelectronic device by rinsing, washing or other removal steps. For example, the etching solution can be removed by rinsing with a rinsing solution such as deionized water or an organic solvent, and / or drying (such as spin drying, N2, steam drying, etc.); or the entire device structure can be cleaned with an aqueous solution containing 0.5wt% HF at room temperature for about 30s-240s, preferably 60s, and more preferably 30s to remove the etching solution.
[0040] The beneficial effects of this application are as follows: The high-performance, high-selectivity etching composition provided in the present application can have an anti-corrosion effect on silicon germanium while maintaining efficient etching of silicon, with a silicon / silicon germanium selectivity ratio of >20; when furan ring compounds and polyamine compounds are used in combination in a certain proportion, the silicon / silicon germanium selectivity ratio is as high as 345. DETAILED DESCRIPTION
[0041] The embodiments of the present invention will be described in detail below with reference to examples. The following examples are only used to illustrate the present invention and should not be construed as limiting the scope of the present invention.
[0042] The etching composition of the present invention is suitable for microelectronic devices including silicon and silicon germanium, preferably SiGe25, and in particular layers containing or consisting of SiGe alloys (such as high-K materials, low-K materials).
[0043] It should be understood that the term "silicon" as a material deposited on a microelectronic device includes, but is not limited to, amorphous silicon, crystalline silicon, polycrystalline silicon, p-type doped silicon, n-type doped silicon, and the like.
[0044] As used herein, a "silicon germanium containing layer" or "SiGe layer" corresponds to a layer comprising or consisting of a silicon germanium alloy known in the art and represented by the formula SixGey, where x+y=1.00. SiGe25 herein means that y is 0.25.
[0045] As defined herein, "high-k materials" (materials with high dielectric constants) are often used to replace traditional silicon dioxide (SiO2) as the dielectric layer of capacitors. High-k materials can be hafnium dioxide (HfO2), hafnium oxynitride (HfON), zirconium dioxide (ZrO2), zirconium oxynitride (ZrON), aluminum oxide (Al2O3), aluminum oxynitride (AlON), hafnium silicon oxide (HfSiO2), hafnium aluminum oxide (HfAlO), zirconium silicon oxide (ZrSiO2), tantalum dioxide (Ta2O5), aluminum oxide, titanium oxide (TiO2), aluminum-doped hafnium dioxide, bismuth strontium titanium (BST), or platinum zirconium titanium (PZT).
[0046] As defined herein, "low-K dielectric materials" (materials with a dielectric constant <3.5) correspond to any material used as a dielectric material in a layered microelectronic device. Examples include silicon-containing organic polymers, silicon-containing hybrid organic / inorganic materials, organosilicate glass (OSG), TEOS, fluorinated silicate glass (FSG), silicon dioxide, and carbon-doped oxide (CDO) glass. It should be understood that low-K dielectric materials can have different densities and different porosities.
[0047] The abbreviations involved in the examples and comparative examples of the present application are as follows: TMAH (tetramethylammonium hydroxide), DIW, TEA (triethanolamine), IPA (isopropyl alcohol), PVP (polyvinyl pyrrolidone), BTA (benzotriazole), HMTA (hexamethylenetetramine), HDM (1,6-hexanediamine).
[0048] Preparation and etching method: (1) Preparation: According to the components and contents in the table below, weigh the corresponding raw materials by percentage calculation to prepare different selective etching solutions, with water as the balance.
[0049] (2) Etching conditions: 50°C, 300 r / min stirring and soaking for 1-10 min.
[0050] (3) Etching test piece: Si / SiGe stack, including Si (110) and SiGe 25.
[0051] The formulations and test data of the embodiments and comparative examples are shown in Tables 1-5. Table 1 Etching solution formula ratio and test data of different quinoline compounds
[0052] Table 2 Etching solution formula ratio and test data of different polyamine compounds
[0053] Table 3 Etching solution formula ratio and test data of different furan ring compounds
[0054] Table 4 Etching solution formula ratio and test data of different aromatic ether compounds
[0055] Table 5 Preferred embodiment ratio and test data
[0056] From the above experimental data, it can be seen that by adding quinoline, polyamine, furan ring, aromatic ether and other compounds, the etching of silicon can be promoted and the etching of silicon germanium can be inhibited. From Examples 4, 9 and 15, it can be seen that the etching selectivity of the polyamine compound 1,6-hexanediamine and the furan ring compound 2-ethylfuran is as high as 345.
[0057] The foregoing description is primarily for illustrative purposes. Although the present invention has been shown and described with respect to exemplary embodiments thereof, it will be appreciated by those skilled in the art that the foregoing and various other changes, omissions and additions may be made in its form and details without departing from the spirit and scope of the present invention.
Claims
1. A high performance selective etching solution for silicon in a silicon germanium / silicon stack, characterized in that: Contains quaternary ammonium hydroxide, alkanolamine, SiGe inhibitor and water.
2. The high performance selective etching solution for silicon in a silicon germanium / silicon stack according to claim 1, characterized in that: The quaternary ammonium hydroxide is R4NOH, wherein R is four identical or different aliphatic or aromatic groups; the amount of the quaternary ammonium hydroxide is 0.3-50 wt%, preferably 1-40 wt%, more preferably 5-30 wt%, and most preferably 10-20 wt%.
3. The high performance selective etching solution for silicon in a silicon germanium / silicon stack according to claim 1, characterized in that: The etching solution comprises a water-soluble organic solvent, and the water-soluble organic solvent is one or more of propanol, isopropanol, propylene glycol, butanol, butyl diglycol, cyclohexane, dimethylformamide, cyclopentane, and dimethyl sulfoxide; the amount of the water-soluble organic solvent is 0.1-60wt%, preferably 1-40wt%, more preferably 2-30wt%, and most preferably 5-20wt%.
4. The high performance selective etching solution for silicon in a silicon germanium / silicon stack according to claim 1, characterized in that: The alkanolamine is selected from one or more of monoethanolamine, diethanolamine, 2-(ethylamino)ethanol, 2-dibutylaminoethanol, N,N-diethylethanolamine, triethanolamine, monoisopropanolamine, diisopropanolamine, triisopropanolamine, and cyclohexylaminediethanol; the amount of the alkanolamine is 0.01-50 wt%, preferably 0.1-40 wt%, more preferably 0.5-30 wt%, and most preferably 1-20 wt%.
5. The high performance selective etching solution for silicon in a silicon germanium / silicon stack according to claim 1, characterized in that: The SiGe inhibitor is selected from one or more of quinoline compounds, polyamine compounds, furan ring compounds, and aromatic ether compounds; the amount of the SiGe inhibitor is 0.001-10 wt%, preferably 0.002-5 wt%, more preferably 0.005-2 wt%, and most preferably 0.01-0.5 wt%.
6. The high performance selective etching solution for silicon in a silicon germanium / silicon stack according to claim 5, characterized in that: The quinoline compound is selected from one or more of 8-hydroxyquinoline, 2-amino-8-hydroxyquinoline, and 4-amino-2-methylquinoline.
7. The high performance selective etching solution for silicon in a silicon germanium / silicon stack according to claim 5, characterized in that: The polyamine compound is selected from one or more of NH2(CH2) n NH2, polyvinylpyrrolidone, benzotriazole, hexamethylenetetramine; in the NH2(CH2) n NH2, the value of n is 3 < n < 10; the viscosity K value of the polyvinylpyrrolidone is 8-100, preferably 10-40, and most preferably 12-20.
8. The high performance selective etching solution for silicon in a silicon germanium / silicon stack according to claim 5, characterized in that: The furan ring compound is selected from one or more of furan, dihydrofuran, tetrahydrofuran, 2-methylfuran, 3-methylfuran, 2,5-dimethylfuran, 2-ethylfuran, 2,2-dimethyltetrahydrofuran, 2-phenylfuran, 2-acetylfuran and 5-methyl-2-acetylfuran.
9. The high performance selective etching solution for silicon in a silicon germanium / silicon stack according to claim 5, characterized in that: The aromatic ether compound is selected from one or more of anisole, phenethyl ether, o-methoxyphenol, p-methoxyphenol, 2-methoxynaphthalene, phenoxybenzene, phenyl benzyl ether, 1,2-dimethoxybenzene, and 2,4-dimethoxybenzaldehyde.
10. Use of the etching solution according to any one of claims 1 to 9 for high performance selective etching of silicon in a silicon germanium / silicon stack, characterized in that: Here are the steps: The etching solution contacts a microelectronic device comprising a silicon germanium / silicon stack at a temperature of 10°C-100°C to complete silicon layer etching; the Si / SiGe etching selectivity ratio is greater than 20, preferably greater than 50, and more preferably greater than 340; and the thermal oxide etching is less than 2Å / min, preferably less than 0.2Å / min.
Citation Information
Patent Citations
Etching solution for selectively removing silicon over silicon-germanium alloy from a silicon-germanium / silicon stack during manufacture of a semiconductor device
CN109423288A
Etching solution having silicon oxide corrosion inhibitor and method of using the same
CN111197182A
Silicon selective etching liquid relative to silicon germanium
CN117417747A
Use of composition for selectively etching silicon and method for selectively etching silicon
CN117616544A
Silicon etching solution, substrate processing method, and silicon device manufacturing method
JP2024075502A