Double-oriented high-silicon steel based on rolling method combined with surface energy annealing and preparation method of double-oriented high-silicon steel

By combining the rolling method with surface energy annealing, the problems of difficult forming and insufficient magnetic properties of high-silicon steel were solved, and a double-oriented high-silicon steel with sharp cubic texture was prepared, achieving softness with low iron loss and high magnetic induction Magnetic performance, suitable for cores of power electronic equipment.

CN118996086AActive Publication Date: 2024-11-22LIAONING UNIVERSITY OF TECHNOLOGY
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
CN202410811570.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-21
Publication Date
2024-11-22
Estimated Expiration
2044-06-21

AI Technical Summary

Technical Problem

The prior art is difficult to effectively prepare Fe-6.5 wt% Si thin strips, and the magnetic properties of high silicon steels are sensitive to texture, and high hardness and brittleness lead to difficulty in processing and forming, making it difficult to prepare oriented high silicon steels with strong Gaussian texture.

Method used

Using the rolling method combined with surface energy annealing method, through hot rolling, pickling, multiple warm rolling and intermediate annealing, the surface energy effect of cubic orientation is used to prepare bi-oriented high-silicon steel with sharp cubic texture, and reinforced silicon steel. Forming and magnetic properties.

Benefits of technology

It realizes soft magnetic properties with low iron loss and high magnetic induction, and is suitable for the core of power electronic equipment, meeting the requirements of high efficiency, energy saving, miniaturization and high frequency.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118996086A_ABST
    Figure CN118996086A_ABST
Patent Text Reader

Abstract

The invention provides double-oriented high-silicon steel based on combination of a rolling method and surface energy annealing and a preparation method of the double-oriented high-silicon steel. According to the preparation method, a silicon-containing square ingot is sequentially subjected to hot rolling, acid pickling, three times of warm rolling, two times of intermediate annealing and final annealing, and then a double-oriented high-silicon steel thin strip is prepared; wherein three times of warm rolling are combined with two times of intermediate annealing to improve the percentage content of the cubic texture; and finally annealing is conducted, the {100} low surface energy is used for inducing abnormal growth of cubic orientation grains, the finished product of the double-orientation high silicon steel with the sharp cubic texture is prepared, and the low-iron-loss and high-magnetic-induction non-oriented electrical steel is prepared by conducting hot rolling, three-time warm rolling and annealing on the high-silicon steel and utilizing the cubic orientation surface energy effect. According to the method, the plasticizing and toughening rolling technology of the high-silicon steel is fully utilized, the forming property is ensured, meanwhile, the recrystallization texture of the high-silicon steel is optimized through surface energy annealing, and the finished product of the double-oriented high-silicon steel with the sharp cube texture is prepared.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to the technical field of metal material preparation, and in particular to a double-oriented high silicon steel based on a rolling method combined with surface energy annealing and a preparation method thereof. [Background technology]

[0002] Although Fe-6.5wt%Si alloy has excellent soft magnetic properties and is an ideal material for making low iron loss and vibration-free iron cores, it is difficult to prepare Fe-6.5wt%Si thin strips by conventional forming methods due to its poor room temperature plasticity. At present, only Japan's JFE Company has successfully achieved industrial production of Fe-6.5wt%Si thin strips using chemical vapor deposition, but this high-temperature siliconization treatment process requires the use of highly toxic SiCl4 gas, which seriously pollutes the environment and is contrary to my country's sustainable development strategy. Compared with ordinary silicon steel, the magnetic properties of high silicon steel are more sensitive to recrystallization texture, but due to its high hardness and brittleness, research on high silicon steel has long focused on how to improve its processing and forming. Although there have been many studies on the texture of high silicon steel, there has been little progress, and there is still a lot of room for improvement in the magnetic properties of high silicon steel. Research on texture control of high silicon steel mainly focuses on two directions: one is to use the low temperature nitriding technology of Fe-3.0%Si oriented silicon steel to overcome the brittleness and surface oxide layer structure of high silicon steel, so that the Gossian oriented grains grow abnormally and prepare oriented high silicon steel with strong Gossian texture characteristics; the other is to use ND columnar crystals to retain the {100} texture and prepare λ( <001> / / ND) non-oriented high silicon steel with recrystallization texture characteristics. The preparation process of oriented silicon steel is complex, the alloy composition is strictly controlled, the size, distribution and quantity of inhibitor particles are accurately controlled, and especially the texture control has reached the ultimate level. The intrinsic brittleness of high silicon steel forces the use of warm rolling system in the forming process of high silicon steel. This rolling system weakens the formation of shear bands and is not conducive to the retention of Gaussian oriented grains. Therefore, for high silicon steel, there are inherent disadvantages in the preparation of oriented high silicon steel with Gaussian texture as the main feature. The production of non-oriented silicon steel requires strict control of the γ( <111> / / ND) fiber texture components, but the current production technology of non-oriented electrical steel is difficult to achieve γ( <111> / / ND) effective control of recrystallization texture to obtain strong λ( <001> / / ND) textured silicon steel sheets are even more difficult.

[0003] Double-oriented high silicon steel refers to the finished product with cubic ({100} <001> Compared with the single easy magnetization direction along the rolling direction of general oriented silicon steel, the cubic texture in the bi-oriented high silicon steel can provide two most easily magnetized directions on the surface of the steel plate at the same time. <001> Crystal orientation, so for non-oriented silicon steel used in rotating magnetic fields and oriented silicon steel in directional magnetic fields, cubic texture is the most ideal recrystallization texture. Patents CN 201710402819.4 and CN201980078053.6 respectively use twin-roller thin strip continuous casting technology and add alloy elements to increase the cubic component after annealing. The {100} texture formed by these methods has a limited cubic proportion and is difficult to be used as a dual orientation. Surface energy-induced secondary recrystallization of cubic oriented grains is a relatively effective method to obtain strong cubic texture.

[0004] Therefore, in view of the unparalleled magnetic properties of the dual-oriented high silicon steel, the inherent brittleness of the high silicon steel material and the use of multiple-pass recovery rolling with small deformation, the silicon steel strip product after rolling is thinner and has obvious surface effect, and the "gradual toughening rolling technology" of high silicon steel is fully utilized to weaken the γ( <111> / / ND) texture component, improve the cubic component, and later combine surface energy annealing to induce secondary recrystallization of cubic oriented grains to prepare a finished product of dual-oriented high silicon steel with a sharp cubic texture to address the shortcomings of the prior art and to solve or alleviate one or more of the above problems. [Summary of the invention]

[0005] In view of this, the present invention provides a dual-oriented high silicon steel based on rolling combined with surface energy annealing and a preparation method thereof, and prepares the dual-oriented high silicon steel based on plasticization and toughening rolling combined with surface energy annealing, and prepares low iron loss and high magnetic induction non-oriented electrical steel by hot rolling, three warm rollings and annealing of high silicon steel, and utilizing the surface energy effect of cubic orientation. The method makes full use of the "plasticization and toughening rolling technology" of high silicon steel, and while ensuring the formability, optimizes the recrystallization texture of high silicon steel by surface energy annealing, and prepares the finished product of dual-oriented high silicon steel with sharp cubic texture.

[0006] On the one hand, the present invention provides a method for preparing a dual-oriented high silicon steel based on a rolling method combined with surface energy annealing, wherein the preparation method sequentially performs hot rolling, pickling, three warm rollings, two intermediate annealings and final annealing on a silicon-containing square ingot, thereby preparing a dual-oriented high silicon steel thin strip;

[0007] Among them, three warm rolling combined with two intermediate annealings are used to increase the percentage of cubic texture;

[0008] The final annealing utilizes the low surface energy of {100} to induce the abnormal growth of cubic oriented grains, and the finished product is a dual-oriented high-silicon steel with a sharp cubic texture.

[0009] According to the above aspects and any possible implementation, there is further provided an implementation, wherein the silicon content in the silicon-containing ingot is 6.0% to 6.5%.

[0010] As described above and any possible implementation method, an implementation method is further provided, wherein the hot rolling adopts lubrication rolling, the hot rolling temperature is controlled at 1050℃~1150℃, multiple rolling with small deformation is carried out within this temperature range, the reduction amount of each pass is controlled at 10%~25%, and the total reduction rate of hot rolling is controlled at 50%~90%.

[0011] According to the above aspects and any possible implementation, there is further provided an implementation, wherein in the three warm rollings, the temperature of the first warm rolling is 700°C to 600°C.

[0012] According to the above aspects and any possible implementation, there is further provided an implementation, wherein in the three warm rollings, the temperature of the second warm rolling is 600°C to 500°C.

[0013] According to the above aspects and any possible implementation, there is further provided an implementation, wherein in the three warm rollings, the temperature of the first warm rolling is 500°C to 400°C.

[0014] According to the above aspects and any possible implementation, there is further provided an implementation, wherein the reduction rate of each warm rolling in the three warm rolling passes is controlled within a range of 40% to 70%.

[0015] According to the above aspects and any possible implementation, there is further provided an implementation, wherein the intermediate annealing temperature is 800° C. to 850° C., and the texture of the finished plate is mainly cubic texture.

[0016] According to the aspects and any possible implementation methods described above, a dual-oriented high-silicon steel based on a rolling method combined with surface energy annealing is further provided, which is prepared by the preparation method. The chemical composition of the dual-oriented high-silicon steel is as follows: Si: 6.3-6.5wt%, Mn: 0.05-0.8wt%, P: 0.005-0.009wt%, C: <0.01wt%, S: <0.01wt%, and the rest is Fe and unavoidable impurities.

[0017] According to the above aspects and any possible implementation, a further implementation is provided, wherein the dual-oriented high silicon steel P 2 / 1000 Between 0.56W / kg~0.92W / kg, P 10 / 400 Between 3.18W / kg and 4.27W / kg.

[0018] Compared with the prior art, the present invention can achieve the following technical effects:

[0019] The high silicon steel prepared by the present invention has the soft magnetic properties of low iron loss, high magnetic permeability and low noise; as a soft magnetic alloy widely used in the power electronics industry, it is suitable for making the iron cores of generators, motors, transformers and other instruments, and can meet the requirements of high efficiency, energy saving, miniaturization and high frequency of power electronic equipment.

[0020] Of course, any product implementing the present invention does not necessarily need to achieve all of the above-mentioned technical effects at the same time.

Brief Description of the Drawings

[0021] In order to more clearly illustrate the technical solutions of the embodiments of the present invention, the drawings required for use in the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0022] Figure 1 It is a flow chart of a method for preparing dual-oriented high silicon steel based on a rolling method combined with surface energy annealing according to the present invention;

[0023] Figure 2 This is the microstructure of the dual-oriented high silicon steel after high temperature annealing in Example 5 of the present invention;

[0024] Figure 3 This is a 45° ODF diagram of the dual-oriented high silicon steel after high temperature annealing in Example 5 of the present invention;

[0025] Figure 4 This is a grain orientation imaging diagram of the dual-oriented high silicon steel after high temperature annealing in Example 5 of the present invention. [Specific implementation method]

[0026] In order to better understand the technical solution of the present invention, the embodiments of the present invention are described in detail below with reference to the accompanying drawings.

[0027] It should be clear that the described embodiments are only some embodiments of the present invention, not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0028] The terms used in the embodiments of the present invention are only for the purpose of describing specific embodiments, and are not intended to limit the present invention. The singular forms "a", "said" and "the" used in the embodiments of the present invention and the appended claims are also intended to include plural forms, unless the context clearly indicates other meanings.

[0029] like Figure 1As shown, the present invention provides a method for preparing a dual-oriented high silicon steel based on a rolling method combined with surface energy annealing, wherein the preparation method sequentially performs hot rolling, pickling, three warm rollings, two intermediate annealings and final annealing on a silicon-containing square ingot, thereby preparing a dual-oriented high silicon steel thin strip;

[0030] Among them, three warm rolling combined with two intermediate annealings are used to increase the percentage of cubic texture;

[0031] The final annealing utilizes the low surface energy of {100} to induce the abnormal growth of cubic oriented grains, and the finished product is a dual-oriented high-silicon steel with a sharp cubic texture.

[0032] The silicon content in the silicon-containing square ingot is 6.0% to 6.5%.

[0033] The hot rolling adopts lubrication rolling, the hot rolling temperature is controlled at 1050℃~1150℃, multiple passes of small deformation rolling are carried out within this temperature range, the reduction of each pass is controlled at 10%~25%, and the total reduction rate of hot rolling is controlled at 50%~90%.

[0034] In the three warm rollings, the temperature of the first warm rolling is 700°C to 600°C. In the three warm rollings, the temperature of the second warm rolling is 600°C to 500°C. In the three warm rollings, the temperature of the first warm rolling is 500°C to 400°C. The reduction rate of each warm rolling in the three warm rollings is controlled at 40% to 70%.

[0035] The intermediate annealing temperature is 800° C. to 850° C., and the texture of the finished plate is mainly cubic texture.

[0036] The present invention also provides a dual-oriented high silicon steel based on rolling combined with surface energy annealing, which is prepared by the preparation method, and the chemical composition of the dual-oriented high silicon steel is as follows: Si: 6.3-6.5wt%, Mn: 0.05-0.8wt%, P: 0.005-0.009wt%, C: <0.01wt%, S: <0.01wt%, and the rest is Fe and unavoidable impurities. The dual-oriented high silicon steel P 2 / 1000 Between 0.47W / kg and 0.84W / kg, P 10 / 400 Between 3.16W / kg and 4.21W / kg.

[0037] The basic principles of the present invention are as follows:

[0038] (1) Hot rolling: Based on the academic idea that {100} oriented grains are stable under plane strain compression and not easy to recrystallize, the hot rolling shear deformation is avoided to retain the {100} texture. Low temperature lubrication rolling can be used. Low temperature lubrication rolling weakens the shear texture of the surface and subsurface of the hot rolled plate, increases the deformed near cubic texture component, weakens the Goss component, and prevents the abnormal growth of Goss during the subsequent high temperature annealing process.

[0039] (2) Warm rolling: Three small deformation warm rolling combined with two intermediate annealings are used to weaken the {111} <112> Texture, increase the proportion of cubic components, on the other hand to achieve "gradual plasticization", promote the transformation of high silicon steel from order to disorder, and prevent high silicon steel from cracking during deformation. The texture control concept is related to the deformation and recrystallization characteristics of cubic oriented grains. Cubic oriented grains are typical axisymmetric grains. After rolling with a small deformation, the cubic orientation does not rotate too far to other places. The subsequent intermediate recovery annealing causes the cubic grains to recover dynamically, thereby increasing the cubic texture component.

[0040] (3) Intermediate annealing: The intermediate annealing temperature cannot be too high and should be matched with the holding time. This is to inhibit the dynamic recrystallization of the warm-rolled plate, to uniformly organize the warm-rolled plate and its morphological characteristics, and to optimize the recrystallization texture of the finished product after annealing. The intermediate annealing process improves the plastic deformation capacity of the high-silicon steel plate on the one hand, and regulates the texture on the other hand. Generally, γ-ray grains have higher deformation storage energy, and are more likely to recrystallize at the grain boundaries during the subsequent annealing process to form new γ-oriented grains. The γ-ray texture is weakened by intermediate annealing, and the lower γ grain boundary density cannot provide more nucleation sites for the formation of new γ grains, thereby increasing the cubic texture component.

[0041] (4) High temperature annealing: High temperature annealing uses pure hydrogen atmosphere annealing. The combination of annealing temperature and time, on the one hand, improves the favorable orientation environment and thermodynamic conditions for the secondary recrystallization of cubic oriented grains, and on the other hand, regulates the grain size and organizational uniformity, thereby preparing high-performance dual-oriented high-silicon steel. The annealing heating rate needs to be increased rapidly, i.e. 50℃~100℃ / min, to control the size of the primary recrystallized grains and avoid the abnormal phenomenon of secondary recrystallization of cubic oriented grains.

[0042] The chemical composition of the high silicon steel applicable to the manufacturing method of the present invention is as follows by mass percentage: Si: 6.3-6.5wt%, Mn: 0.05-0.8wt%, P: 0.005-0.009wt%, C: <0.01wt%, S: <0.01wt%, and the rest is Fe and unavoidable impurities.

[0043] The reasons for the ingredient restrictions are as follows:

[0044] Si: The mass percentage of Si is in the range of 6.3-6.5 wt%. Si increases the resistivity and reduces the eddy current.

[0045] On the other hand, if the silicon content exceeds 6.5wt%, the coercive force increases, the saturation magnetic induction intensity and the maximum magnetic permeability decrease, and the processability deteriorates significantly.

[0046] Mn: The mass percentage of Mn ranges from 0.05 to 0.8 wt%. Mn is an essential element for improving hot rolling performance, and the improvement effect is insufficient when the content is less than 0.05 wt%.

[0047] P: The mass percentage of P ranges from 0.005 to 0.009 wt%. P is an essential element for improving the workability of punching sheets. If it is less than 0.005 wt%, no effect can be achieved, and if it exceeds 0.1 wt%, the cold workability will deteriorate.

[0048] C: The range of C mass percentage is <0.01wt%. C is an element harmful to magnetic properties. If it exceeds 0.01wt%, decarburization annealing is required and the decarburization time is too long, which reduces production efficiency.

[0049] S: The mass percentage of S is within the range of <0.01wt%. S is a formation element of non-metallic phases such as MnS that are harmful to magnetic properties, and its content should be less than 0.01wt%.

[0050] Example 1

[0051] (1) Raw material preparation: The square steel ingot has a silicon content of 6.5% and a thickness of 20 mm. The steel ingot is placed in a heating furnace and heated to 1150°C.

[0052] (2) Hot rolling: the hot rolling start temperature is 1150°C, the final rolling temperature is 900°C, lubrication rolling is used, the final slab is rolled to 2 mm, and the total hot rolling reduction rate is 80%;

[0053] (3) Warm rolling: the first warm rolling temperature is 700℃, the final rolling temperature is 600℃, and the rolling thickness is 2mm to 0.8mm;

[0054] The secondary warm rolling starts at 600°C, the final rolling temperature is 500°C, and the thickness is 0.8mm to 0.4mm.

[0055] The three-stage warm rolling process starts at 500°C, ends at 400°C, and is 0.4mm to 0.2mm.

[0056] (4) Intermediate annealing: 850°C for 30 min, air cooling;

[0057] (5) Final annealing: The warm rolled sheet was annealed at 1150°C in a pure hydrogen atmosphere at a heating rate of 100°C / min.

[0058] Example 2

[0059] (1) Raw material preparation: The square steel ingot has a silicon content of 6.5% and a thickness of 20 mm. The steel ingot is placed in a heating furnace and heated to 1100°C.

[0060] (2) Hot rolling: the hot rolling start temperature is 1100°C, the final rolling temperature is 870°C, lubrication rolling is used, the final slab is rolled to 2 mm, and the total hot rolling reduction rate is 80%;

[0061] (3) Warm rolling: the first warm rolling temperature is 700℃, the final rolling temperature is 600℃, and the rolling thickness is 2mm to 0.8mm;

[0062] The secondary warm rolling starts at 600°C, the final rolling temperature is 500°C, and the thickness is 0.8mm to 0.4mm.

[0063] The secondary warm rolling starts at 500°C, the final rolling temperature is 400°C, and the thickness is 0.4mm to 0.2mm.

[0064] (4) Intermediate annealing: 850°C for 30 min, air cooling;

[0065] (5) Final annealing: anneal the warm rolled sheet at 1150°C in a pure hydrogen atmosphere at a heating rate of 100°C / min.

[0066] Example 3

[0067] (1) Raw material preparation: The square steel ingot has a silicon content of 6.5% and a thickness of 20 mm. The steel ingot is placed in a heating furnace and heated to 1050°C.

[0068] (2) Hot rolling: the hot rolling start temperature is 1050°C, the final rolling temperature is 800°C, lubrication rolling is used, the final slab is rolled to 2 mm, and the total hot rolling reduction rate is 60%;

[0069] (3) Warm rolling: the first warm rolling temperature is 700℃, the final rolling temperature is 600℃, and the rolling thickness is 2mm to 0.8mm;

[0070] The secondary warm rolling starts at 600°C, the final rolling temperature is 500°C, and the thickness is 0.8mm to 0.4mm.

[0071] The secondary warm rolling starts at 500°C, the final rolling temperature is 400°C, and the thickness is 0.4mm to 0.2mm.

[0072] (4) Intermediate annealing: 850°C for 30 min, air cooling;

[0073] (5) Final annealing: The warm rolled sheet was annealed at 1150°C in a pure hydrogen atmosphere at a heating rate of 100°C / min.

[0074] Among them, the above examples 1, 2, and 3 mainly study the effect of hot rolling temperature on weakening shear texture and improving {100} texture under the same hot rolling reduction rate. As the hot rolling temperature decreases, the degree of dynamic recrystallization of the surface layer and subsurface layer is significantly reduced, the Goss shear texture is significantly weakened, and the proportion of λ texture (001∥ND) is significantly increased. When the hot rolling temperature is 1050℃, the texture of the center layer of the hot rolled plate is mainly {100} <031> , {100} <021> The main structure is {114}, and there is a small amount of Goss shear texture in the subsurface. When the hot rolling temperature is 1100℃, <481> The steel is significantly enhanced, and there are more brass textures in the subsurface. As the hot rolling temperature is further reduced, the texture is mainly {100} <011> , {112} <110> The grain rotation law is as follows: In the center layer, under plane strain compression, for the initial rotated cubic oriented grains: {100} <011> Around <110> Axis steering {112} <110> ; For initial cubic oriented grains: {100} <001> Turn to {100} first <021> , and then turned to {114} <481> , and the lower α* line is close. The degree of orientation rotation is mainly affected by the hot rolling temperature.

[0075] Comparative Example 1

[0076] (1) Raw material preparation: The square steel ingot has a silicon content of 6.5% and a thickness of 5 mm. The steel ingot is placed in a heating furnace and heated to 1050°C.

[0077] (2) Hot rolling: The hot rolling start temperature is 1050°C, the final rolling temperature is 800°C, the final slab is rolled to 2 mm, and the total hot rolling reduction is 60%;

[0078] (3) Warm rolling: the first warm rolling temperature is 700℃, the final rolling temperature is 600℃, and the rolling thickness is 2mm to 0.8mm;

[0079] The secondary warm rolling starts at 600°C, the final rolling temperature is 500°C, and the thickness is 0.8mm to 0.4mm.

[0080] The secondary warm rolling starts at 500°C, the final rolling temperature is 400°C, and the thickness is 0.4mm to 0.2mm.

[0081] (4) Intermediate annealing: 850°C for 30 min, air cooling;

[0082] (5) Final annealing: The warm rolled sheet was annealed at 1150°C in a pure hydrogen atmosphere at a heating rate of 100°C / min.

[0083] Comparative Example 1 is compared with Example 3 to study the effect of hot rolling reduction on hot rolling texture. From the perspective of microscopic orientation, when the hot rolling reduction is small, the proportion of {100}<20° oriented grains inside the hot rolled plate is greater than that of hot rolling with a large reduction rate, the former is 23.5%, and the latter is 18.2%, while the proportion of the shear texture orientation area represented by Goss, brass and copper type is much smaller than that of the case of large reduction rate, the former is 3.2%, and the latter is 8.6%, and exists in large quantities in the sub-surface layer, indicating that small reduction can inhibit the formation of sub-surface shear texture and is conducive to the retention of {100} texture.

[0084] Example 4

[0085] (1) Raw material preparation: The square steel ingot has a silicon content of 6.5% and a thickness of 20 mm. The steel ingot is placed in a heating furnace and heated to 1050°C.

[0086] (2) Hot rolling: the hot rolling start temperature is 1050°C, the final rolling temperature is 800°C, lubrication rolling is used, the final slab is rolled to 2 mm, and the total hot rolling reduction rate is 60%;

[0087] (3) Warm rolling: the first warm rolling temperature is 700℃, the final rolling temperature is 600℃, and the rolling thickness is 2mm to 0.8mm;

[0088] The secondary warm rolling starts at 700°C, the final rolling temperature is 700°C, and the thickness is 0.8mm to 0.4mm.

[0089] The three-stage warm rolling process starts at 700°C, ends at 700°C, and is 0.4mm to 0.2mm thick.

[0090] Intermediate annealing: 950℃ for 40min, oil cooling;

[0091] (4) Intermediate annealing: 850°C for 30 min, air cooling;

[0092] (5) Final annealing: The warm rolled sheet was annealed at 1150°C in a pure hydrogen atmosphere at a heating rate of 100°C / min.

[0093] The comparison between Example 4 and Example 3 is mainly to study the effect of warm rolling temperature on the texture and plasticity of warm rolled plate. The higher the warm rolling temperature, the better the plasticity of the warm rolled plate, the lower the deformation energy storage, the lower the nucleation rate in the shear band, the larger the size of the primary recrystallized grains, and the unsatisfactory secondary recrystallization kinetic conditions of the cubic oriented grains, resulting in abnormal secondary recrystallization structure, which in turn affects the texture and magnetic properties of the finished plate.

[0094] Example 5

[0095] (1) Raw material preparation: The square steel ingot has a silicon content of 6.5% and a thickness of 5 mm. The steel ingot is placed in a heating furnace and heated to 1050°C.

[0096] (2) Hot rolling: the hot rolling start temperature is 1050°C, the final rolling temperature is 800°C, lubrication rolling is used, the final slab is rolled to 2 mm, and the total hot rolling reduction rate is 60%;

[0097] (3) Warm rolling: the first warm rolling temperature is 700℃, the final rolling temperature is 600℃, and the rolling thickness is 2mm to 0.8mm;

[0098] The secondary warm rolling starts at 600°C, the final rolling temperature is 500°C, and the thickness is 0.8mm to 0.4mm.

[0099] The secondary warm rolling starts at 500°C, the final rolling temperature is 400°C, and the thickness is 0.4mm to 0.2mm.

[0100] (4) Intermediate annealing: 850°C for 30 min, air cooling;

[0101] (5) Final annealing: The warm rolled sheet was annealed at 1150°C in a pure hydrogen atmosphere at a heating rate of 50°C / min.

[0102] The magnetic properties of the finished plate of Example 5 are shown in Table 1. The microstructure of the dual-oriented high silicon steel after high temperature annealing is as follows: Figure 2 As shown, the 45°ODF diagram after high temperature annealing is as follows Figure 3 As shown, the grain orientation imaging after high temperature annealing is shown in Figure 4 As shown, the above examples 1-5 and comparative example 1 show that by using a small reduction rate hot rolling (60%) combined with low temperature lubrication rolling (1050°C), three warm rollings combined with two intermediate annealings are used to weaken the γ texture and increase the {100} texture component. During the high temperature (1150°C) annealing process, rapid heating is used to suppress the size of the primary recrystallization grains, providing a favorable thermodynamic environment and orientation environment for the secondary recrystallization of the cubic orientation. The cubic orientation grains are secondary recrystallized by taking advantage of the low surface energy of {100}, and finally a finished product with excellent magnetic properties and mainly cubic texture of high silicon steel thin strip is prepared.

[0103] Table 1

[0104]

[0105] The present invention uses silicon steel ingots containing 6.0% to 6.5% Si and the balance being Fe and inevitable impurities as raw materials, and improves cubic texture components through hot rolling, three warm rollings combined with two intermediate annealings, and induces secondary recrystallization of cubic oriented grains by utilizing the advantage of {100} low surface energy after high temperature annealing to prepare dual-oriented high silicon steel with excellent magnetic properties in both rolling and transverse directions. This dual-oriented high silicon steel sheet is widely used and can be used as the iron core of electrical equipment such as motors, generators, small transformers, voltage stabilizers, inductors, etc.

[0106] The above is a detailed introduction to a dual-oriented high silicon steel based on rolling combined with surface energy annealing and a preparation method thereof provided in the embodiment of the present application. The description of the above embodiment is only used to help understand the method and its core idea of ​​the present application; at the same time, for a person skilled in the art, according to the idea of ​​the present application, there will be changes in the specific implementation method and application scope. In summary, the content of this specification should not be understood as a limitation on the present application.

[0107] For example, certain words are used in the specification and claims to refer to specific components. Those skilled in the art should understand that hardware manufacturers may use different nouns to refer to the same component. This specification and claims do not use differences in names as a way to distinguish components, but use differences in the functions of components as the criteria for distinction. As mentioned throughout the specification and claims, "including" and "comprising" are open-ended terms, so they should be interpreted as "including / including but not limited to". "Approximately" means that within an acceptable error range, those skilled in the art can solve the technical problem within a certain error range and basically achieve the technical effect. The subsequent description of the specification is a preferred embodiment of the present application, but the description is for the purpose of illustrating the general principles of the present application, and is not used to limit the scope of the present application. The scope of protection of the present application shall be determined by the definition of the attached claims.

[0108] It should also be noted that the terms "include", "comprises" or any other variations thereof are intended to cover non-exclusive inclusion, so that a product or system including a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such a product or system. In the absence of more restrictions, the elements defined by the sentence "comprises a ..." do not exclude the existence of other identical elements in the product or system including the elements.

[0109] It should be understood that the term "and / or" used in this article is only a description of the association relationship of associated objects, indicating that there can be three relationships. For example, A and / or B can represent: A exists alone, A and B exist at the same time, and B exists alone. In addition, the character " / " in this article generally indicates that the associated objects before and after are in an "or" relationship.

[0110] The above description shows and describes several preferred embodiments of the present application, but as mentioned above, it should be understood that the present application is not limited to the form disclosed herein, and should not be regarded as excluding other embodiments, but can be used in various other combinations, modifications and environments, and can be modified within the scope of the application concept described herein through the above teachings or the technology or knowledge of the relevant field. The changes and modifications made by those skilled in the art do not deviate from the spirit and scope of the present application, and should be within the scope of protection of the claims attached to the present application.

Claims

1. A method for preparing dual-oriented high silicon steel based on rolling method combined with surface energy annealing, characterized in that: The preparation method prepares a bi-oriented high silicon steel thin strip by sequentially hot rolling, pickling, three warm rollings, two intermediate annealings and final annealing on a silicon-containing square ingot; Among them, three warm rolling combined with two intermediate annealings are used to increase the percentage of cubic texture; The final annealing utilizes the low surface energy of {100} to induce the abnormal growth of cubic oriented grains, and the finished product is a dual-oriented high-silicon steel with a sharp cubic texture.

2. The preparation method according to claim 1, characterized in that: The silicon content in the silicon-containing square ingot is 6.0% to 6.5%.

3. The preparation method according to claim 1, characterized in that: The hot rolling adopts lubrication rolling, the hot rolling temperature is controlled at 1050℃~1150℃, multiple passes of small deformation rolling are carried out within this temperature range, the reduction of each pass is controlled at 10%~25%, and the total reduction rate of hot rolling is controlled at 50%~90%.

4. The preparation method according to claim 1, characterized in that: In the three warm rolling processes, the temperature of the first warm rolling process is 700°C to 600°C.

5. The preparation method according to claim 4, characterized in that: In the three warm rolling processes, the temperature of the second warm rolling process is 600°C to 500°C.

6. The preparation method according to claim 5, characterized in that: In the three warm rolling processes, the temperature of the first warm rolling is 500°C to 400°C.

7. The preparation method according to claim 6, characterized in that: The reduction rate of each warm rolling in the three warm rolling processes is controlled at 40% to 70%.

8. The preparation method according to claim 1, characterized in that: The intermediate annealing temperature is 800° C. to 850° C., and the texture of the finished plate is mainly cubic texture.

9. A dual-oriented high silicon steel based on rolling combined with surface energy annealing, prepared by the preparation method according to any one of claims 1 to 8, characterized in that: The chemical composition of the dual-oriented high silicon steel is as follows: Si: 6.3-6.5wt%, Mn: 0.05-0.8wt%, P: 0.005-0.009wt%, C: <0.01wt%, S: <0.01wt%, and the rest is Fe and unavoidable impurities.

10. The dual-oriented high silicon steel according to claim 9, characterized in that: The core loss of the dual-oriented high silicon steel P 2 / 1000 Between 0.47W / kg and 0.84W / kg, P 10 / 400 Between 3.16W / kg and 4.21W / kg.

Citation Information

Patent Citations

  • Method for preparing cubic double-oriented silicon steel based on thin-strip continuous casting

    CN107164691A

  • Doubly oriented electrical steel sheet and manufacturing method therefor

    CN113166872A

  • Method for preparing high-magnetic-strength non-oriented electrical steel by using columnar crystals

    CN104294023A

  • Dual-oriented electrical steel sheet and method for producing same

    CN115053005A