Rare earth magnesium alloy and preparation method and application thereof
By optimizing the composition and preparation methods of rare earth magnesium alloys, the tensile strength and corrosion resistance are improved, and the problem of insufficient tensile strength and corrosion resistance of existing rare earth magnesium alloys is solved, and the lightweight and high-strength aspects of the aerospace field are met. Material requirements.
Patent Information
- Application Number
- CN202411201260.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-29
- Publication Date
- 2024-11-22
AI Technical Summary
The existing rare earth magnesium alloys have shortcomings in tensile strength and corrosion resistance, which are difficult to meet the demand for lightweight materials of the new generation of spacecraft.
By optimizing the alloy composition, the composition ratios of Zn: 6.0~8.0%, Y: 0.5~2.5%, RE: 0.05~0.33%, Zr: 0.30~0.60%, RE is selected from Nd, Gd, Sm, Y:RE = 10:(1~1.5) to improve the tensile strength and corrosion resistance of the alloy, and to refine the alloy structure through specific preparation methods to improve the mechanical properties.
It significantly improves the tensile strength and ductility of rare earth magnesium alloys, improves corrosion resistance, meets the demand for lightweight and high-strength materials in the aerospace field, and reduces the cost of the alloy.
Smart Images

Figure FT_1 
Figure FT_2 
Figure SMS_1
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of light alloys, and in particular to a rare earth magnesium alloy and a preparation method and application thereof. Background Art
[0002] High-performance lightweight materials control the quality of materials while maintaining excellent performance, and are widely used in the aerospace field. Among them, magnesium alloys are widely used in the aerospace field due to their low density, high specific strength and specific stiffness, good thermal conductivity and electrical conductivity, and good damping and shock absorption performance. In addition to ensuring structural strength, magnesium alloy parts have good thermal conductivity, shock absorption, high modulus and other characteristics, which can greatly simplify functional design and improve the overall level of aerospace components. Large-scale magnesium alloy parts, lightweight large-size components, and structural and functional integration are important development trends for the overall advancement of future aerospace industry technology.
[0003] Among magnesium alloy parts, the traditional magnesium alloy of Mg-Zn system is widely used, but this type of alloy has the disadvantages of poor inherent properties such as strength, plasticity, corrosion resistance and heat resistance. One of the effective measures to improve it is to optimize the alloy composition and process, among which rare earth is the most practical and promising alloy element for optimizing alloy composition. Adding rare earth elements such as La and Ce to magnesium alloys can significantly refine the grain size of the organization and improve the corrosion resistance and mechanical properties of magnesium alloys. Therefore, improving the performance of magnesium alloys by adding rare earth elements has attracted much attention from researchers.
[0004] Patent CN200910064645.0 discloses a rare earth magnesium alloy, which is composed of the following mass percentages: 5-6% Al, 0.6-2.4% Y, 0.3-1.2% Nd, 1.2-4.8% Gd, the total amount of impurity elements Fe, Cu and Ni is less than 0.02%, and the balance is Mg; and the preparation method of the rare earth magnesium alloy is also disclosed. The room temperature tensile strength of the rare earth magnesium alloy is 244 MPa, the elongation is 9.0%, and it has good high temperature resistance. However, the rare earth content in the rare earth magnesium alloy is high, which not only makes the cost high, but also causes its tensile strength to be very limited as the rare earth content increases, making it difficult to meet the demand for lightweight materials for the new generation of spacecraft.
[0005] Patent CN201410250496.8 discloses a method for preparing a Mg-Zn-RE-Zr magnesium alloy, comprising the following steps: 1) melting Mg source, Zn source, Y source, Gd source, La source and Zr source to obtain alloy liquid; 2) casting the alloy liquid to obtain a cast alloy, wherein the casting temperature is 690°C to 720°C; 3) annealing the cast alloy to obtain a Mg-Zn-RE-Zr magnesium alloy, wherein the annealing temperature is 230°C to 320°C. The Mg-Zn-RE-Zr magnesium alloy with good mechanical properties and large diameter, which is mainly composed of Y, Gd and La (the total amount of the three is 1.1% to 2.5%), is prepared, but it also has the problem of poor tensile strength.
[0006] Patent CN202210421841.4 discloses a method for preparing an ultra-high plasticity Mg-RE-Zr magnesium alloy and its deformed material. The magnesium alloy is composed of the following components by weight percentage: rare earth element RE 0.1%~7.0%, Zr 0.1%~1.0%, and the rest is Mg, and the rare earth element is one of Y, Tb, Dy, Ho, Er, Tm, and Yb. It exhibits ultra-high room temperature plasticity, and its alloy mechanical properties are poor, and both tensile strength and yield strength are low, which makes it difficult to meet the strength requirements of aerospace devices.
[0007] Therefore, research and development of a new type of lightweight rare earth magnesium alloy is of great significance for the application of lightweight materials in the aerospace field. Summary of the invention
[0008] In view of this, the technical problem to be solved by the present invention is to provide a rare earth magnesium alloy and a preparation method and application thereof. The rare earth magnesium alloy has significantly improved tensile strength and good ductility.
[0009] In order to achieve the above purpose, the technical solution adopted by the present invention is as follows:
[0010] The present invention provides a rare earth magnesium alloy comprising the following components:
[0011] Zn: 6.0~8.0%, Y: 0.5~2.5%, RE: 0.05~0.33%, Zr: 0.30~0.60%, the rest are magnesium and unavoidable impurities;
[0012] Wherein, RE is selected from one or more of Nd, Gd, and Sm;
[0013] Y:RE = 10: (1~1.5).
[0014] The above rare earth magnesium alloy can be expressed as Mg-Zn-RE-Zr rare earth magnesium alloy.
[0015] The Zn content in the rare earth magnesium alloy is preferably 6.5% to 8.0%; more preferably 6.5% to 7.0%; further preferably 6.5% or 7.0% or 8.0%.
[0016] The Y content in the rare earth magnesium alloy is preferably 1.2% to 2.5%; more preferably 1.2% to 1.5%; further preferably 1.2% or 1.5%.
[0017] The RE content in the rare earth magnesium alloy is preferably 0.12% to 0.33%, more preferably 0.12% to 0.15%, and further preferably 0.12% or 0.15%.
[0018] The Zr content in the rare earth magnesium alloy is preferably 0.40% to 0.60%; more preferably 0.40% to 0.45%; further preferably 0.40% or 0.45%.
[0019] The unavoidable impurities include but are not limited to Fe, Si, Cu, Ni, etc., and the total impurity content does not exceed 0.1%.
[0020] The Zn content in the rare earth magnesium alloy of the present invention affects the mechanical properties, corrosion resistance and processing properties of the alloy. Because Zn forms a solid solution or precipitation phase with magnesium, the Zn content within the above range can better strengthen the alloy and improve the mechanical properties of the alloy such as tensile strength, yield strength and hardness. At the same time, the Zn within the above content range also improves the corrosion resistance of the magnesium alloy in high temperature, humid or chemical corrosion environment, and reduces the corrosion rate of the alloy. In addition, the addition of Zn also improves the heat treatment response of the magnesium alloy, thereby adjusting the structure and properties of the alloy. When the Zn content is less than 6.5%, the strength of the alloy is improved less; when the Zn content is too high and greater than 8%, it will lead to an increase in the tendency of hot cracking of the alloy and a decrease in plasticity. Therefore, the alloy of the present invention preferably uses a zinc element range of 6.5% to 8.0%, and more preferably 6.5% to 7%. When the Zn content is 6.5% to 7%, its strengthening effect on the alloy is the best, making the alloy performance optimal.
[0021] The RE in the rare earth magnesium alloy of the present invention has multiple functions: forming a solid solution with magnesium to improve the mechanical properties of the alloy;
[0022] Refine the grains of rare earth magnesium alloys and improve the uniformity and stability of the microstructure;
[0023] Improve the corrosion resistance of rare earth magnesium alloys;
[0024] Improve the thermal stability of rare earth magnesium alloys;
[0025] Wherein, RE is selected from one or more of Nd, Gd and Sm.
[0026] According to the multi-element microalloying effect, the addition of RE reduces the solubility of the main strengthening element Y in the magnesium alloy and improves the precipitation efficiency of Y, thereby obtaining excellent mechanical properties and maintaining good plasticity. The RE content is 0.05%~0.25%, preferably 0.12%~0.25%; the Y content is 0.5%~2.5%, preferably 1.2%~2.5%. In addition, the RE in the alloy will preferentially dissolve in the magnesium alloy matrix, causing the Y element to preferentially precipitate during the phase change process, so that the nucleation density and precipitation efficiency of the precipitation phase are increased while the total amount remains unchanged, thereby strengthening the effect. At the same time, the multi-element microalloying effect reduces the solid solubility of various rare earth elements Y and RE as a whole, thereby further improving the precipitation efficiency, and the RE and Y have excellent precipitation efficiency under a certain range of matching ratios of 10: (1~1.5).
[0027] In the above-mentioned rare earth magnesium alloy, Y improves the strength and hardness of the rare earth magnesium alloy through the Orwan effect of solid solution strengthening and precipitation strengthening. The Mg-Y phase formed by Y has high temperature stability, which improves the thermal stability of the magnesium alloy and enables it to maintain good performance under high temperature environment. Moreover, Y, as a grain boundary strengthening element, inhibits the growth of magnesium alloy grains, refines and optimizes the alloy structure. In addition, Y also improves the corrosion resistance of the magnesium alloy, making it have better corrosion resistance. When Y is less than 0.5%, the precipitation strengthening effect is not obvious; when Y is too high, the Orwan effect of the alloy is too strong, and the plasticity is significantly reduced. Therefore, the Y content of the present invention is 0.5%~2.5%, and when Y is preferably 1.2%~2.5%, the Mg-Y phase stability is better, the growth inhibition effect on the rare earth magnesium alloy grains is stronger, and a finer and more optimized alloy structure can be obtained.
[0028] The main precipitated phases of the alloy are Mg-Zn and Mg-Zn-Y phases, wherein there is a certain degree of partial substitution of Y by RE in the Mg-Zn-Y phase. The partial substitution of Y by RE makes the Mg-Zn-Y phase evenly broken, reduces the growth rate of the precipitated phase Mg-Zn-Y phase, causes the size of the precipitated phase Mg-Zn-Y phase to be reduced, and obtains a partial Mg-Zn-RE phase, wherein the Mg-Zn-RE phase is more rounded than the broken phase, and the Mg-Zn phase is finer and more dispersed, which brings about the improvement effect of multi-component rare earth alloying, thereby further improving the strength and plasticity of the rare earth magnesium alloy.
[0029] When the RE content is more preferably 0.12% to 0.15%, the Y content is more preferably 1.2% to 1.5%, and the RE to Y content is 10:1, the rare earth magnesium alloy can achieve the highest precipitation efficiency, so that the alloy has optimal mechanical properties and maintains good plasticity.
[0030] The Zr in the rare earth magnesium alloy of the present invention can not only refine the alloy grains, reduce the grain size, improve the plasticity and toughness of the alloy, but also strengthen the solid solution and precipitation, thereby enhancing the mechanical properties of the rare earth magnesium alloy. When the Zr content is preferably 0.40% to 0.60%, and more preferably 0.40% to 0.45%, the grain refinement effect, the strengthening of solid solution and precipitation effect are stronger.
[0031] The microstructure of the rare earth magnesium alloy (Mg-Zn-RE-Zr alloy) includes the coexistence and interaction of multiple phases, which together affect the mechanical properties of the alloy. More preferably, the rare earth magnesium alloy includes the following components:
[0032] Zn: 6.5~7.0%, Y: 1.2~1.5%, RE: 0.12~0.15%, Zr: 0.40~0.45%, the rest is magnesium and unavoidable impurities;
[0033] Wherein, RE is selected from one or more of Nd, Gd, and Sm;
[0034] Y:RE = 10: (1~1.1).
[0035] More preferably in the present invention, the Y:RE = 10:1.
[0036] More preferably in the present invention, the RE is selected from Nd, Gd and Sm.
[0037] The present invention is further preferred that the rare earth magnesium alloy comprises the following components:
[0038] Zn: 6.0%, Y: 0.5%, Nd: 0.02%, Gd: 0.02%, Sm: 0.01%, Zr: 0.30%, the rest is magnesium and unavoidable impurities;
[0039] Alternatively, Zn: 6.0%, Y: 1.0%, Nd: 0.04%, Gd: 0.04%, Sm: 0.02%, Zr: 0.40%, and the remainder being magnesium and unavoidable impurities;
[0040] Alternatively, Zn: 6.5%, Y: 1.2%, Nd: 0.05%, Gd: 0.05%, Sm: 0.02%, Zr: 0.40%, and the remainder is magnesium and unavoidable impurities;
[0041] Alternatively, Zn: 6.5%, Y: 1.5%, Nd: 0.07%, Gd: 0.06%, Sm: 0.02%, Zr: 0.40%, and the remainder being magnesium and unavoidable impurities;
[0042] Alternatively, Zn: 7.0%, Y: 1.5%, Nd: 0.06%, Gd: 0.07%, Sm: 0.02%, Zr: 0.45%, and the remainder being magnesium and unavoidable impurities;
[0043] Alternatively, Zn: 8.0%, Y: 2.5%, Nd: 0.10%, Gd: 0.10%, Sm: 0.05%, Zr: 0.60%, and the remainder being magnesium and inevitable impurities.
[0044] In the above rare earth magnesium alloy, the mass ratio of rare earth element Y to the sum of rare earth elements Nd, Gd, and Sm is 10:1. In addition, the total amount of rare earth elements in the above rare earth alloy (the sum of Y, Nd, Gd, and Sm content) is 0.55% or 1.1% or 1.32% or 1.65% or 2.75%, respectively. Mechanical properties tests show that the tensile strength of the above rare earth magnesium alloy is 365 MPa, 372 MPa, 381 MPa, 385 MPa, 392 MPa or 385 MPa, respectively, and the elongation is 15.5%, 15.7%, 16.0%, 14.9%, 12.2% or 12.0%, respectively. This shows that the composition design of the alloy has a great influence on its performance.
[0045] The rare earth magnesium alloy is subjected to heat treatment to obtain an alloy material having good plasticity and processing properties. The rare earth magnesium alloy is used for the preparation of parts and components of various shapes to meet the requirements of light weight and high strength.
[0046] Through the design of the above alloy components, the nucleation density of the alloy precipitation phase is increased, the precipitation efficiency is increased, the microstructure morphology of the rare earth magnesium alloy is improved, the Mg-Zn-RE phase is more broken and rounded, and the Mg-Zn phase is more fine and dispersed, ultimately achieving the coordination of strengthening and toughness in performance, significantly improving the strength of the rare earth magnesium alloy and reducing plasticity loss.
[0047] The present invention also provides a method for preparing the rare earth magnesium alloy, comprising the following steps:
[0048] 1) Mixing and melting a magnesium ingot, a zinc ingot, a magnesium rare earth master alloy and a flux, heating them, and standing them to obtain a first melt;
[0049] 2) heating the first melt and mixing it with a magnesium-zirconium master alloy to melt the mixture, and allowing the mixture to stand to obtain a second melt;
[0050] 3) refining the second melt, mixing it with a flux, keeping it warm and letting it stand to obtain a third melt;
[0051] 4) casting and cooling the third melt to obtain the rare earth magnesium alloy;
[0052] The magnesium rare earth master alloy is selected from Mg-Y alloy and Mg-RE alloy, wherein RE is selected from one or more of Nd, Gd and Sm;
[0053] The magnesium-zirconium master alloy is selected from Mg-Zr alloy, wherein the Zr content is 20% to 35%. Preferably, the temperature of the heating in step 1) is 700°C to 760°C;
[0054] Preferably, the heating temperature in step 2) is 730°C to 780°C.
[0055] Preferably, the refining temperature in step 3) is 730°C to 780°C.
[0056] The flux includes but is not limited to #6 flux used for magnesium alloy smelting.
[0057] Preferably, the casting temperature in step 4) is 680°C to 720°C;
[0058] Preferably, the cooling temperature in step 4) is below 200°C.
[0059] The preparation method controls the reaction conditions during the preparation of the first melt, the second melt and the third melt, so that the structure of the rare earth magnesium alloy is further refined and optimized, the defects of the alloy structure are reduced, and the alloy performance is improved.
[0060] The present invention also provides applications of the rare earth magnesium alloy in aerospace, rail transportation, and electronic products.
[0061] Compared with the prior art, the rare earth magnesium alloy provided by the present invention includes the following components: Zn: 6.0~8.0%, Y: 0.5~2.5%, RE: 0.05~0.33%, Zr: 0.30~0.60%, and the rest is magnesium and inevitable impurities; wherein RE is selected from one or more of Nd, Gd, and Sm; Y:RE = 10: (1~1.5). The present invention improves the nucleation density and precipitation efficiency of the alloy precipitation phase through the design of alloy components, strengthens the main precipitation phase of the alloy, reduces alloy defects, effectively refines and optimizes the precipitation phase, improves the microstructure morphology of the alloy, and significantly improves the strength and plasticity of the rare earth magnesium alloy. In addition, the preparation method is simple, efficient, and low-cost, suitable for large-scale industrial production, and provides a new idea for the preparation of lightweight materials in related industries such as aerospace. BRIEF DESCRIPTION OF THE DRAWINGS
[0062] Figure 1 The extruded microstructure morphology of the Mg-Zn-RE-Zr rare earth magnesium alloy prepared in Example 1, wherein A is an optical metallographic image of the alloy microstructure, and B is a SEM image of the alloy microstructure;
[0063] Figure 2 The microstructure element distribution analysis diagram of the Mg-Zn-RE-Zr rare earth magnesium alloy prepared in Example 1, wherein Figure 1 The SEM photo of the alloy microstructure is shown in Figure 2. Figure 2 Figure 3 is the distribution of Mg element in the alloy microstructure, Figure 4 is the distribution of Y element in the alloy microstructure, Figure 5 is the distribution of Zr element in the alloy microstructure, and Figure 6 is the distribution of each element in the alloy microstructure. DETAILED DESCRIPTION
[0064] In order to further illustrate the present invention, the rare earth magnesium alloy provided by the present invention and its preparation method and application are described in detail below in conjunction with embodiments.
[0065] Example 1
[0066] The preparation method of Mg-Zn-RE-Zr rare earth magnesium alloy comprises the following steps:
[0067] a) Preheat the melting crucible and sprinkle #6 flux (about 1.5% of the total weight of the melt) for magnesium alloy melting into the bottom;
[0068] b) adding magnesium ingot, zinc ingot and magnesium rare earth master alloy (Mg-Y alloy and Mg-RE alloy) into the crucible in sequence;
[0069] c) Under a protective atmosphere, melt the magnesium ingot, zinc ingot and magnesium rare earth master alloy, heat to 720℃~730℃, stir well and let stand for 10~20 minutes;
[0070] d) The melt is heated to 760°C, magnesium-zirconium master alloy (Mg-Zr alloy, in which the Zr content is 20%~35%) is added, and after melting, it is fully stirred and allowed to stand for 30 minutes;
[0071] e) The melt temperature was maintained at 780°C for refining, and the melt was manually stirred for 30 min under inert gas. At the same time, flux (about 1.5% of the total weight of the melt) was evenly sprinkled in. After stirring, the melt was kept still for 50 min. After the stillness and heat preservation, samples were taken for component analysis, and the specific element contents were shown in Table 1.
[0072] f) After the resting is completed, the melt is cooled and kept at 700°C for casting;
[0073] g) After the casting operation is completed, the ingot is cooled to below 200°C, the mold is opened and the ingot is taken out, and the Mg-Zn-RE-Zr rare earth magnesium alloy is obtained.
[0074] Example 2
[0075] The same as Example 1, except that the melt temperature in step c) is raised to 730° C. to 740° C.; and in step f), the casting temperature is 705° C. In addition, the proportion of each raw material is adjusted accordingly according to the designed Mg-Zn-RE-Zr rare earth magnesium alloy composition.
[0076] Example 3
[0077] The same as Example 1, except that the melt temperature in step c) is raised to 740°C to 750°C; and in step f), the casting temperature is 710°C. In addition, the proportion of each raw material is adjusted accordingly according to the designed Mg-Zn-RE-Zr rare earth magnesium alloy composition.
[0078] Example 4
[0079] The same as Example 1, except that the melt temperature in step c) is raised to 750°C to 760°C; and in step f), the casting temperature is 715°C. In addition, the proportion of each raw material is adjusted accordingly according to the designed Mg-Zn-RE-Zr rare earth magnesium alloy composition.
[0080] Example 5
[0081] The same as Example 1, except that the melt temperature in step c) is raised to 750° C. to 760° C.; and in step f), the casting temperature is 720° C. In addition, the proportion of each raw material is adjusted accordingly according to the designed Mg-Zn-RE-Zr rare earth magnesium alloy composition.
[0082] Example 6
[0083] The same as Example 1, except that the melt temperature in step c) is raised to 760° C. and in step f), the casting temperature is 720° C. In addition, the proportion of each raw material is adjusted accordingly according to the designed Mg-Zn-RE-Zr rare earth magnesium alloy composition.
[0084] In order to evaluate the material performance of the present invention, the alloys of Examples 1-6 were melted and die-cast to prepare single-shoulder cylindrical tensile specimens with a diameter of 6 mm and a gauge length of 60 mm. The tensile strength test (GB / T228.1 Metal Material Room Temperature Tensile Test Method) was performed on the samples of each example. The components and test results of each example are shown in Table 1 and Table 2. Table 1 shows the elemental composition of the Mg-Zn-RE-Zr rare earth magnesium alloy prepared in Examples 1-6. By adjusting the ratio of each raw material and the temperature parameters, the material components obtained in each example are shown in Table 1. Table 2 shows the mechanical property test results of the Mg-Zn-RE-Zr rare earth magnesium alloy prepared in Examples 1-6.
[0085]
[0086] The results in Table 1 and Table 2 show that the Mg-Zn-RE-Zr rare earth magnesium alloy of the present invention has excellent tensile strength, good yield strength and elongation. The excellent performance of the rare earth magnesium alloy is related to the alloy composition, and it first increases and then decreases with the increase of rare earth content (total content of Y+ Nd+Gd+Sm), and the optimization effect of various properties is significantly weakened when the rare earth content is relatively high (2.75%). This is due to the increase in the number of main strengthening phases of the alloy and the change in the morphology of the alloy structure. Since the Orwan effect of the precipitation phase of the rare earth magnesium alloy will be strengthened with the increase of the total amount of rare earth, the dislocation entanglement in the alloy microstructure will be aggravated, thereby reducing the plasticity and comprehensive performance of the material. Therefore, the performance of the alloy of the present invention is closely related to the ratio and content of rare earth elements, and can only have good effects after the composition design and preparation by the above method.
[0087] Figure 1 The extruded microstructure morphology of the Mg-Zn-RE-Zr rare earth magnesium alloy prepared in Example 1. A is an optical metallographic microstructure of the alloy, which reflects the microstructure of the alloy. The results show that the Mg-Zn-RE-Zr rare earth magnesium alloy is composed of a precipitated phase with discontinuous island distribution in an α-Mg matrix. The α-Mg matrix is mainly composed of pure magnesium or a magnesium solid solution, and its size and morphology are affected by the solution treatment and heat treatment process.
[0088] B is the SEM image of the alloy microstructure, which reflects the morphology and distribution of the precipitated phase in the microstructure. The results show that after extrusion deformation, the grain size inside the Mg-Zn-RE-Zr rare earth magnesium alloy becomes smaller and the grains are refined, thereby improving the plasticity and toughness of the alloy. Extrusion deformation changes the clarity of the grain boundaries, the density of the grain boundaries, and the morphology of the grain boundaries of the alloy. In addition, extrusion deformation will introduce a large number of dislocations, especially creep dislocations and dislocations along the extrusion direction, which have a strengthening effect on the mechanical properties and thermal stability of the alloy.
[0089] The morphology and distribution of the precipitated phase in the Mg-Zn-RE-Zr rare earth magnesium alloy affect the mechanical properties and corrosion resistance of the alloy. The precipitated phase is mainly Mg-Zn and Mg-Zn-RE phases. The common Mg-Zn phase or Mg-Zn-RE phase is easy to form a coarse and sharp structure or a continuously distributed LPSO phase. The Mg-Zn-RE phase in the alloy of the present invention is relatively broken and rounded, with a more common size. The Mg-Zn-RE phase is finer and more dispersed, such as Figure 1 and Figure 2 Small Figure 1 As shown, Figure 2 Small Figure 1 and Figure 1There are regional and magnification differences in Figure B. The optimized microstructure reduces the internal defects of the alloy and the stress concentration when subjected to force, so that the alloy structure is refined and optimized, thereby improving the mechanical properties and corrosion resistance of the alloy.
[0090] Figure 2 The microstructure element distribution analysis diagram of the Mg-Zn-RE-Zr rare earth magnesium alloy prepared in Example 1 shows that the main precipitated phase in the Mg-Zn-RE-Zr rare earth magnesium alloy is the Mg-Zn-Y phase. In addition, the Mg-Zn-Y phase is evenly broken and reduced in size, because there is a certain degree of partial substitution of Y by RE in the precipitated phase Mg-Zn-Y phase. The partial substitution of Y by RE makes the Mg-Zn-Y phase evenly broken, thereby reducing its growth rate, resulting in a reduction in the size of the precipitated phase, thereby improving the strength and plasticity of the alloy.
[0091] In summary, the microstructural characteristics of Mg-Zn-RE-Zr alloy are complex, including the coexistence and interaction of multiple phases, which directly affect the mechanical properties, corrosion resistance and thermal stability of the alloy.
[0092] Comparative Example 1
[0093] The specific composition and performance test of commercial MB15 alloy are shown in Tables 3 and 4 respectively.
[0094] Comparative Example 2
[0095] The specific composition and performance tests of commercial AZ31 alloy are shown in Tables 3 and 4 respectively.
[0096] Comparative Example 3
[0097] The preparation method is the same as that of Example 1, except that the alloy composition is different. The specific composition and performance test are shown in Tables 3 and 4 respectively.
[0098] Comparative Example 4
[0099] The preparation method is the same as that of Example 1, except that the alloy composition is different. The specific composition and performance test are shown in Tables 3 and 4 respectively.
[0100]
[0101]
[0102] The tests of the mechanical properties in Table 2 and Table 4 above are all conducted under the reference tensile strength test (GB / T228.1 Metal Material Room Temperature Tensile Test Method).
[0103] The test results in Table 3 and Table 4 show that the commercial magnesium alloys used in Comparative Examples 1 and 2 do not contain rare earth elements, so their overall performance has no advantage over the magnesium alloys prepared in Examples 1-6.
[0104] Comparative Example 3 shows that the main rare earth element in the alloy contains only Y, which will also lead to an overall decrease in the mechanical properties of the magnesium alloy, and the low content of the rare earth element Y will further reduce the mechanical properties of the magnesium alloy. Comparative Example 4 shows that when the main elements in the alloy are the same, but the content is not within the optimized content range described in the present invention, the mechanical properties of the alloy are also poor, and the plasticity of the alloy will decrease rapidly, thereby weakening the comprehensive mechanical properties of the alloy.
[0105] The above embodiments are only used to help understand the method and core idea of the present invention. It should be noted that, for those skilled in the art, several improvements and modifications can be made to the present invention without departing from the principles of the present invention, and these improvements and modifications also fall within the scope of protection of the claims of the present invention.
Claims
1. A rare earth magnesium alloy, characterized in that: Includes the following ingredients: Zn: 6.0~8.0%, Y: 0.5~2.5%, RE: 0.05~0.33%, Zr: 0.30~0.60%, the rest are magnesium and unavoidable impurities; Wherein, RE is selected from one or more of Nd, Gd, and Sm; Y:RE = 10: (1~1.5).
2. The rare earth magnesium alloy according to claim 1, characterized in that: The rare earth magnesium alloy comprises the following components: Zn: 6.5~7.0%, Y: 1.2~1.5%, RE: 0.12~0.15%, Zr: 0.40~0.45%, the rest is magnesium and unavoidable impurities; Wherein, RE is selected from one or more of Nd, Gd, and Sm; Y:RE = 10: (1~1.1).
3. The rare earth magnesium alloy according to claim 2, characterized in that: The Y:RE = 10:
1.
4. The rare earth magnesium alloy according to any one of claims 1 to 3, characterized in that: The RE is selected from the group consisting of Nd, Gd and Sm.
5. The rare earth magnesium alloy according to claim 1, characterized in that: The rare earth magnesium alloy comprises the following components: Zn: 6.0%, Y: 0.5%, Nd: 0.02%, Gd: 0.02%, Sm: 0.01%, Zr: 0.30%, the rest is magnesium and unavoidable impurities; Alternatively, Zn: 6.0%, Y: 1.0%, Nd: 0.04%, Gd: 0.04%, Sm: 0.02%, Zr: 0.40%, and the remainder being magnesium and unavoidable impurities; Or, Zn: 6.5%, Y: 1.2%, Nd: 0.05%, Gd: 0.05%, Sm: 0.02%, Zr: 0.40%, the rest is magnesium and inevitable impurities; Alternatively, Zn: 6.5%, Y: 1.5%, Nd: 0.07%, Gd: 0.06%, Sm: 0.02%, Zr: 0.40%, and the remainder being magnesium and unavoidable impurities; Alternatively, Zn: 7.0%, Y: 1.5%, Nd: 0.06%, Gd: 0.07%, Sm: 0.02%, Zr: 0.45%, and the remainder being magnesium and unavoidable impurities; Alternatively, Zn: 8.0%, Y: 2.5%, Nd: 0.10%, Gd: 0.10%, Sm: 0.05%, Zr: 0.60%, and the remainder being magnesium and inevitable impurities.
6. The method for preparing a rare earth magnesium alloy according to any one of claims 1 to 5, characterized in that: The following steps are involved: 1) Mixing and melting magnesium ingots, zinc ingots, magnesium rare earth master alloy and flux, heating and standing to obtain a first melt; 2) heating the first melt and mixing it with a magnesium-zirconium master alloy to melt the mixture, and allowing the mixture to stand to obtain a second melt; 3) refining the second melt, mixing it with a flux, keeping it warm and letting it stand to obtain a third melt; 4) casting and cooling the third melt to obtain the rare earth magnesium alloy; The magnesium rare earth master alloy is selected from Mg-Y alloy and Mg-RE alloy, wherein RE is selected from one or more of Nd, Gd and Sm; The magnesium-zirconium master alloy is selected from Mg-Zr alloy, wherein the Zr content is 20% to 35%.
7. The preparation method according to claim 6, characterized in that The temperature of the heating in step 1) is 700°C to 760°C; The temperature of the heating in step 2) is 730°C to 780°C.
8. The preparation method according to claim 6, characterized in that The refining temperature in step 3) is 730°C to 780°C.
9. The preparation method according to claim 6, characterized in that The casting temperature in step 4) is 680°C to 720°C; The cooling temperature in step 4) is below 200°C.
10. Application of the rare earth magnesium alloy according to any one of claims 1 to 5 in aerospace, rail transportation, and electronic products.
Citation Information
Cited By
Preparation method of high-alloying rare earth magnesium alloy capable of synchronously regulating and controlling strength and plasticity based on split texture / cylindrical surface composite texture
CN120174284A