Ni-Mo-free low-carbon-equivalent 555 MPa strength grade pipeline steel plate and manufacturing method thereof
By designing a chemical composition with low carbon equivalents and no Ni-Mo, and using a specific TMCP process, an economical pipeline steel plate with a strength of 555MPa was prepared. This solved the problem of high cost in existing technologies, achieved a balance between high strength and toughness, and reduced the use of precious metals.
Patent Information
- Application Number
- CN202410910691.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-09
- Publication Date
- 2024-11-22
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
There are few patents in the existing technology involving economical low-carbon equivalent X80 grade pipeline steel plates, and high-strength pipeline steels mostly rely on precious metals Ni and Mo, which are costly.
Using a Ni-Mo-free, low-carbon equivalent chemical composition design, combined with a specific TMCP process, and by adding appropriate amounts of microalloying elements such as C, Mn, Nb, and Ti, and adding Cr to improve strength and hardenability, the microstructure is controlled to be acicular ferrite and quasi-polygonal ferrite. With a strong cooling rate and process design, pipeline steel plates with a strength level of 555MPa are prepared.
Without adding Ni and Mo, pipeline steel plates with a high strength and toughness balance were obtained through reasonable composition and process design, reducing costs while maintaining excellent DWTT drop weight performance.
Smart Images

Figure CN118996271A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of special steel smelting, and specifically relates to a Ni-Mo-free low-carbon equivalent 555MPa strength grade pipeline steel plate and a manufacturing method thereof. Background Art
[0002] At present, fossil energy still occupies the main position in the energy structure of the world's energy demand. The rapid growth of the world economy in recent years has greatly driven the rapid growth of fossil energy demand, which has also greatly promoted the development of long-distance pipelines. In order to improve transportation efficiency and reduce investment, the development trend of steel used in long-distance oil and gas pipelines is to develop towards high-strength or ultra-high steel grades. At present, the highest steel grade of pipeline steel used in countries around the world is X80 steel grade. In order to promote the development of pipeline steel technology and reduce construction costs and improve operational efficiency, reducing operating costs and reducing costs from the perspective of saving element components is one of the effective means to reduce pipeline construction costs.
[0003] There are currently many domestic and foreign patent authorizations or patent applications for X80 pipeline steel, but there are relatively few patents involving economical low-carbon equivalent X80 steel grade pipeline steel plates. Summary of the invention
[0004] The technical problem to be solved by the present invention is to provide a Ni-Mo-free low-carbon equivalent 555MPa strength grade pipeline steel plate and a manufacturing method thereof in view of the above-mentioned prior art.
[0005] The technical solution adopted by the present invention to solve the above problem is: a Ni-Mo-free low carbon equivalent 555MPa strength grade pipeline steel plate, the chemical composition of the steel plate is C: 0.05-0.09%, Mn: 1.65-1.85%, Si: ≤0.35%, S: ≤0.005%, P: ≤0.015%, Nb: 0.033-0.040%, Ti: ≤0.012%, V: ≤0. 008%, Alt: ≤0.06%, N: ≤0.0040%, O: ≤0.004%, Pb≤0.0015%, Zn≤0.003%, Sb≤0.0015%, Sn≤0.0015%, Cr: 0.22-0.30%, Ca: ≤0.015%, Ceq: 0.35-0.40%, the balance is Fe and unavoidable impurity elements; the thickness of the steel plate is not more than 30mm.
[0006] The steel plate has a yield strength of ≥560MPa; a tensile strength of ≥675MPa, a yield strength ratio of ≤0.84, an impact energy of ≥420J at -25°C, an impact energy of ≥310J at -40°C, an impact energy of ≥250J at -60°C, a drop weight shear area of ≥85% at -10°C, and a drop weight shear area of ≥85% at -15°C.
[0007] The reasons for the composition design of the present invention are as follows:
[0008] The composition design principle of the present invention is to use appropriate amounts of C and Mn, add trace amounts of micro-alloying elements such as Nb, V, and Ti, and design without precious metal components such as Ni and Mo. Only an appropriate amount of Cr is added, combined with a specific TMCP process, and still have good DWTT drop weight performance under thicker specifications. The main basic elements have the following functions:
[0009] C: C is the most economical and basic strengthening element in steel. It can significantly improve the strength of steel through solid solution strengthening and precipitation strengthening, but it has an adverse effect on the toughness, ductility and welding performance of steel. Therefore, the development trend of pipeline steel is to continuously reduce the C content. Considering the matching relationship between strength and toughness, the C content is controlled at 0.06-0.09%.
[0010] Mn: It improves the strength of steel through solid solution strengthening. It is the most important element in pipeline steel to make up for the strength loss caused by the reduction of C content. Mn is also an element that expands the γ phase region, which can reduce the γ→α phase transition temperature of steel, help to obtain fine phase transformation products, improve the toughness of steel, and reduce the toughness-brittleness transition temperature. Mn is also an element that improves the hardenability of steel. Considering that Mn segregation has an adverse effect on the drop hammer performance during the inspection process, and taking into account the strength requirements, the Mn content in the present invention is designed to be in the range of 1.65-1.85%. In order to alleviate the central segregation caused by the high Mn content, light pressure is used during continuous casting.
[0011] Nb: It is one of the most important microalloying elements in modern microalloyed steel, especially pipeline steel, and has a very obvious effect on grain refinement. The solid solution drag of Nb and the strain-induced precipitation of Nb (C, N) during hot rolling can hinder the recovery and recrystallization of deformed austenite. The deformed austenite rolled in the non-recrystallized zone is transformed into fine phase transformation products during phase transformation through TMCP, so that the steel has high strength and high toughness. The present invention mainly determines the Nb content range through the relationship between C and Nb content. Considering the solid solution relationship between Nb and C and combining the C content range, Nb is controlled within 0.033-0.040%.
[0012] Ti: is a strong N-fixing element, and the stoichiometric ratio of Ti / N is 3.42. About 0.02% Ti can fix less than 60ppm of N in steel, and TiN precipitation phase can be formed during the slab continuous casting process. This fine precipitation phase can effectively prevent the growth of austenite grains in the slab during heating, help to increase the solid solubility of Nb in austenite, and improve the impact toughness of the welding heat affected zone. It is an indispensable element in pipeline steel, but too high Ti will form large TiN particles, affecting the drop hammer performance. Therefore, this patent application controls Ti to Ti: ≤0.012%.
[0013] S, P: are inevitable impurity elements in pipeline steel. It is hoped that the lower the better. By changing the sulfide form through ultra-low sulfur and Ca treatment, the pipeline steel can have high impact toughness.
[0014] Cr: The addition of Cr can improve the hardenability of steel and is relatively economical.
[0015] The present invention also provides a method for manufacturing a Ni-Mo-free low-carbon equivalent 555MPa strength grade pipeline steel plate, the preparation process of which is as follows: proportioning and preparing materials → smelting in a converter or electric furnace → refining outside the furnace → continuous casting → slab reheating → specific TMCP process + stack cooling after cooling → straightening. The specific process steps are as follows:
[0016] First, the smelting raw materials are sequentially subjected to KR molten iron pretreatment, converter smelting, LF refining, RH vacuum refining and continuous casting to produce continuous casting billets that meet the chemical composition requirements and have a thickness of no less than 350 mm;
[0017] During continuous casting, light reduction is used to improve the core segregation caused by high Mn content, and the light reduction is not less than 14 mm. The process of using a larger reduction in the front 4 rollers and a smaller reduction in the back 4 rollers is used to improve the liquid phase hole in the ingot.
[0018] The continuous casting ingot is reheated to no higher than 1150-1180℃. At the same time, in order to further improve segregation, the high temperature event of the heating furnace is not less than 3 hours, followed by a specific TMCP process + water cooling + pile cooling + straightening.
[0019] The specific TMCP process includes two-stage rolling and intermediate billet cooling: the first stage is recrystallization zone rolling, the start rolling temperature is not higher than 1160°C and the final rolling temperature is controlled at no higher than 1100°C, and the single pass reduction rate of two to three consecutive passes is controlled to be no less than 20% during recrystallization zone rolling, and the cumulative reduction rate is no less than 45%;
[0020] The second stage is non-recrystallization zone rolling (finish rolling), the starting rolling temperature is not higher than 850°C, preferably the finishing rolling starting temperature range is 860-880°C, and the cumulative reduction rate is not less than 60%.
[0021] In the 3rd to 4th pass before finishing rolling, the steel plate is rolled with a delay of 5 to 15 seconds. The purpose is to compensate for the plate shape problem caused by the use of lower temperature rolling after the cancellation of Ni-Mo.
[0022] The final rolling temperature is between Ar3 and Ar3-20℃;
[0023] After rolling, the steel plate is cooled by water cooling, the starting cooling temperature is controlled to be no higher than 790°C, the ending cooling temperature is controlled to be no higher than 400°C, and the cooling rate is 10-35°C / s; after cooling, it is straightened and finally directly cooled to room temperature to obtain the finished steel plate.
[0024] Compared with the prior art, the advantages of the present invention are:
[0025] 1) When designing the composition, only Cr is used to improve the strength and hardenability of the steel plate, which is economical in composition and makes full use of the action mechanism of Cr in steel. In addition to weakly affecting the phase diagram of steel, Ni mainly improves the toughness of steel. Mo, like Cr, has a strong influence on the phase diagram, but Mo has a greater effect. Therefore, in addition to adding Cr, a stronger cooling rate is used to achieve the same effect as Mo.
[0026] 2) In order to coordinate the composition design and process design, the 3rd to 4th pass before finishing rolling is delayed by 5 to 15 seconds, and the final rolling temperature is between Ar3 and Ar3-20°C, so as to ensure toughness while improving the strength.
[0027] 3) To obtain the same strength and other properties, the cooling speed needs to be increased, so the cooling capacity of the ACC cooling equipment is increased;
[0028] 4) The present patent application utilizes the relatively cheap element Cr, reasonably designs the composition and process, and utilizes the strong cooling capacity without adding precious metals such as Ni and Mo, and also obtains a structure mainly composed of acicular ferrite, containing a small amount of quasi-polygonal ferrite and bainite, and also obtains relatively excellent strength and toughness. BRIEF DESCRIPTION OF THE DRAWINGS
[0029] Figure 1 This is a schematic diagram of the metallographic structure of Example 1 of the present invention.
[0030] Figure 2 This is a schematic diagram of the metallographic structure of Example 2 of the present invention. DETAILED DESCRIPTION
[0031] The technical solution of the present invention is described in more detail in conjunction with the preferred embodiments of the present invention. However, these embodiments are only descriptions of the preferred implementation methods of the present invention and cannot impose any limitation on the scope of the present invention.
[0032] The embodiment of the present invention relates to a Ni-Mo-free low-carbon equivalent 555MPa strength grade pipeline steel plate and a manufacturing method thereof, and the specific process is as follows:
[0033] Proportioning and preparing materials → smelting in converter or electric furnace → refining outside the furnace → continuous casting → slab reheating → specific TMCP process + stack cooling after cooling → straightening.
[0034] The specific process steps are as follows: the smelting raw materials are sequentially subjected to KR hot metal pretreatment, converter smelting, LF refining, RH vacuum refining and continuous casting. The light reduction process is used during continuous casting to improve the core segregation caused by the high Mn content. A continuous casting billet with a thickness of 350mm that meets the chemical composition requirements is manufactured; the continuous casting billet is reheated to no more than 1180℃ and subjected to a specific TMCP process + water cooling + stack cooling + straightening.
[0035] The specific TMCP process includes two-stage rolling: the first stage is recrystallization zone rolling, the final rolling temperature is controlled to be no higher than 1150°C, and the single pass reduction rate of two to three consecutive passes is controlled to be no less than 20% during recrystallization zone rolling;
[0036] The second stage is rolling in the non-recrystallization zone, the starting rolling temperature is not higher than 900°C, and the final rolling temperature is controlled at the phase transformation critical temperature Ar3.
[0037] After rolling, the steel plate is cooled by water cooling, the starting cooling temperature is controlled to be no higher than 790°C, the ending cooling temperature is controlled to be no higher than 400°C, and the cooling rate is 10-35°C / s; after the water cooling is completed, it is straightened and finally directly cooled to room temperature to obtain the finished steel plate.
[0038] The specific chemical composition of the steel plates involved in each embodiment is shown in Table 1, the specific TMCP process parameters are shown in Table 2, and the main mechanical properties are shown in Table 3.
[0039] Table 1
[0040]
[0041] Table 2
[0042]
[0043] Table 3
[0044]
[0045] Although the preferred embodiments of the present invention are described in detail above, it should be clearly understood that various modifications and variations are possible for those skilled in the art. Any modification, equivalent substitution, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.
Claims
1. A Ni-Mo-free low carbon equivalent 555MPa strength grade pipeline steel plate, Features: The chemical composition of the steel plate is, by mass percentage, C: 0.05-0.09%, Mn: 1.65-1.85%, Si: ≤0.35%, S: ≤0.005%, P: ≤0.015%, Nb: 0.033-0.040%, Ti: ≤0.012%, V: ≤0.008%, Alt: ≤0.06%, N: ≤0.0040%, O: ≤0.004%, Pb≤0.0015%, Zn≤0.003%, Sb≤0.0015%, Sn≤0.0015%, Cr: 0.22-0.30%, Ca: ≤0.015%, Ceq: 0.35-0.40%, and the balance is Fe and unavoidable impurity elements.
2. The Ni-Mo-free low carbon equivalent 555 MPa strength grade pipeline steel plate according to claim 1, Features: The thickness of the steel plate is not more than 30 mm.
3. The Ni-Mo-free low carbon equivalent 555 MPa strength grade pipeline steel plate according to claim 1, Features: The metallographic structure of the steel plate is mainly composed of acicular ferrite, and contains a small amount of quasi-polygonal ferrite and bainite.
4. The Ni-Mo-free low carbon equivalent 555 MPa strength grade pipeline steel plate according to claim 1, Features: The steel plate has a yield strength of ≥560Mpa; a tensile strength of ≥675Mpa, a yield strength ratio of ≤0.84, a round bar elongation of ≥25%, an impact energy of ≥350J at -25°C, an impact energy of ≥280J at -40°C, an impact energy of ≥250J at -60°C, a drop weight shear area of ≥85% at -10°C, and a drop weight shear area of ≥85% at -15°C.
5. A method for manufacturing a Ni-Mo-free low carbon equivalent 555 MPa strength grade pipeline steel plate as claimed in claim 1, Features: The method specifically comprises the following steps: Step 1: First, the smelting raw materials are sequentially subjected to KR molten iron pretreatment, converter smelting, LF refining, RH vacuum refining and continuous casting to produce a continuous casting billet that meets the chemical composition requirements and has a thickness of not less than 350 mm; Step 2: Heat the continuous casting billet to a temperature not higher than 1150-1180°C. To further improve segregation, the heating furnace is kept at high temperature for not less than 3 hours. Step 3: The heated continuous casting billet is subjected to TMCP process, including two-stage rolling and intermediate billet cooling: The first stage is recrystallization zone rolling, the starting rolling temperature is not higher than 1160℃ and the final rolling temperature is controlled at no higher than 1100℃. During recrystallization zone rolling, the single pass reduction rate of two to three consecutive passes is controlled to be no less than 20%, and the cumulative reduction rate is no less than 45%; The second stage is non-recrystallization zone rolling, the start rolling temperature is not higher than 850°C, the preferred finish rolling start rolling temperature range is 860-880°C, the cumulative reduction rate is not less than 60%, and the final rolling temperature is between Ar3 and Ar3-20°C; Step 4: Cool the steel plate by water cooling after rolling, control the starting cooling temperature to be no higher than 790°C, control the ending cooling temperature to be no higher than 400°C, and the cooling rate to be 10-35°C / s; straighten after cooling, and finally cool directly to room temperature to obtain the finished steel plate.
6. The method for manufacturing a Ni-Mo-free low carbon equivalent 555 MPa strength grade pipeline steel plate according to claim 5, Features: During continuous casting, light reduction is used to improve the core segregation caused by high Mn. The light reduction is not less than 14 mm, and a process is adopted in which the front 4 rollers have a larger reduction and the rear 4 rollers have a smaller reduction to improve the liquid phase holes in the ingot.
7. The method for manufacturing a Ni-Mo-free low carbon equivalent 555 MPa strength grade pipeline steel plate according to claim 5, Features In the second stage of finishing rolling, the 3rd to 4th pass from the end, the steel plate is rolled with a delay of 5 to 15 seconds. The purpose is to compensate for the plate shape problem caused by the use of lower temperature rolling after the cancellation of Ni-Mo.
Citation Information
Cited By
Low-cost X80 pipeline steel thick plate and efficient preparation method thereof
CN121951399A