High-temperature-resistant high-toughness hot work die steel and preparation method thereof

By using specific elements and process processing in hot-working mold steel, high-temperature and high-toughness thermal mold steel is prepared, which solves the problem of poor mechanical properties of traditional mold steel at high temperatures, and achieves excellent performance at high temperatures and Longer service life.

CN118996282AInactive Publication Date: 2024-11-22JINAN GANGNA MATERIAL TECH CO LTD

Patent Information

Application Number
CN202411086048.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-08
Publication Date
2024-11-22
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

The existing thermal working mold steel cannot maintain good mechanical properties at high temperatures, and is prone to failure due to thermal fatigue, and cannot meet the requirements of high temperature and high strength.

Method used

Use specific compositions of high temperature and high toughness heat-working mold steel, including C, Si, Mn, Mo, Ni, Cr, V, Ce, La, Y and other elements, through vacuum smelting, refining, pouring, multi-directional forging, annealing, Through quenching and tempering processes, mold steel with excellent hardness and impact toughness are prepared.

Benefits of technology

It achieves excellent strength and toughness at high temperatures, extends the service life of the mold, and has a wider range of application, solving the problem of poor mechanical properties of traditional hot-working mold steel at high temperatures.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004985209430000111
    Figure BDA0004985209430000111
  • Figure BDA0004985209430000121
    Figure BDA0004985209430000121
Patent Text Reader

Abstract

The invention relates to the technical field of steel smelting, and discloses high-temperature-resistant and high-toughness hot work die steel and a preparation method thereof. The hot work die steel is prepared from the following components in percentage by mass: 0.14 to 0.16 percent of C, 0.40 to 0.90 percent of Si, 0.20 to 0.80 percent of Mn, 1.50 to 3.00 percent of Mo, 4.20 to 4.50 percent of Ni, 0.60 to 1.60 percent of Cr, 0.10 to 0.40 percent of V, 0.20 to 0.90 percent of Ce, 0.021 to 0.075 percent of La, 0.002 to 0.005 percent of Y, less than or equal to 0.012 percent of P, less than or equal to 0.018 percent of S and the balance of Fe and impurities. On the basis of low Cr and high Mo, rare earth elements Ce, La and Y are added, so that the hot work die steel still has excellent strength and toughness at high temperature under the action of multiple aspects.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of steelmaking, and in particular to a high-temperature resistant and high-toughness hot working die steel and a preparation method thereof. Background Art

[0002] Hot working die steel is an important branch of die steel, mainly used to manufacture metal hot processing and forming dies. The precision hot die forging technology based on hot working die steel can produce products close to the final shape. Hot working dies are required in the production of most metal parts in the fields of aviation, rail transportation, automobiles, etc., such as the preparation of key parts such as aircraft engine blades, high-speed rail track fasteners and metal pads, automotive shaft parts, and automotive differential gears.

[0003] Since hot working molds work at relatively high temperatures, thermal fatigue failure is the most common failure form of hot working mold steel. During operation, the high-temperature metal solution and the spray cooling during mold opening produce a large temperature gradient, and the hot and cold cycles produce alternating thermal stress, which causes thermal stress concentration on the mold cavity surface. Under the combined action of thermal stress or thermal stress and external mechanical stress, thermal cracks are easily generated at the stress concentration point. The crack morphology is often radial or mesh-shaped. With continuous hot and cold cycles, the cracks will gradually develop into microcracks, which will further expand and eventually lead to mold failure.

[0004] Traditional hot working die steel is mainly divided into three categories: high alloy hot working die steel, medium alloy hot working die steel and low alloy hot working die steel; among them, high alloy hot working die steel 3Cr2W8V has a high temperature tensile strength of 415MPa at 700℃; medium alloy hot working die steel H13 has a high temperature tensile strength of 292MPa at 700℃; low alloy hot working die steel 5CrMnMoSiV has a high temperature tensile strength of 137MPa at 700℃. Therefore, the existing hot working die steel cannot meet the requirements of high temperature and high strength.

[0005] Therefore, a hot working die steel with high temperature resistance and high toughness is needed to meet greater market demand. Summary of the invention

[0006] In order to solve the problem that the existing hot working die steel cannot maintain good mechanical properties at high temperatures, the present invention provides a high temperature resistant and high toughness hot working die steel and a preparation method thereof.

[0007] In the first aspect, the present invention provides a high temperature resistant and high toughness hot working die steel, which adopts the following technical solution:

[0008] A high-temperature resistant and high-toughness hot working die steel consists of the following components in mass percentage: C: 0.14-0.16%, Si: 0.40-0.90%, Mn: 0.20-0.80%, Mo: 1.50-3.00%, Ni: 4.20-4.50%, Cr: 0.60-1.60%, V: 0.10-0.40%, Ce: 0.20-0.90%, La: 0.021-0.075%, Y: 0.002-0.005%, P: ≤0.012%, S: ≤0.018%, and the balance is Fe and impurities.

[0009] Preferably, the high temperature resistant and high toughness hot working die steel is composed of the following components in mass percentage: C: 0.15-0.16%, Si: 0.55-0.80%, Mn: 0.43-0.75%, Mo: 2.00-2.50%, Ni: 4.25-4.40%, Cr: 1.10-1.55%, V: 0.15-0.30%, Ce: 0.40-0.80%, La: 0.03-0.06%, Y: 0.003-0.004%, P: ≤0.010%, S: ≤0.015%, and the balance is Fe and impurities.

[0010] Preferably, in the hot working die steel, Ce+La+Y is 0.25-0.60%.

[0011] Preferably, in the hot working die steel, Mo / Cr is 2.

[0012] In a second aspect, the present invention provides a method for preparing a high temperature resistant and high toughness hot working die steel, which adopts the following technical solution:

[0013] A method for preparing high-temperature resistant and high-toughness hot working die steel comprises the following steps:

[0014] S1. Take raw materials according to the formula of high temperature resistant and high toughness hot working die steel, melt and refine the raw materials to obtain molten steel, and pour the molten steel to obtain a casting;

[0015] S2, after homogenizing the casting, perform multi-directional forging to obtain a forging module;

[0016] S3. Perform annealing, quenching and tempering treatments on the forging module in sequence to obtain hot working die steel.

[0017] Preferably, the smelting and refining in S1 are as follows: first, industrial pure iron, Mn, Cr, Ni, and Mo are added to a smelting furnace, and a vacuum pump is turned on to evacuate the furnace to a vacuum degree of 6-8 Pa; after the charge begins to melt, argon is introduced until the total pressure in the furnace is 30000-35000 Pa, and after all the charge is melted, graphite is added and the furnace is evacuated again to a vacuum degree of 12-18 Pa, and the temperature is kept for 20 minutes for vacuum refining, and the refining temperature is 1580-1600°C; after the vacuum refining is completed, V, Ce, Si, La, and Y are added in sequence and smelting is continued until the charge is fully melted, and the smelting temperature is 1580-1600°C to obtain molten steel.

[0018] Preferably, the homogenization treatment in step S2 is as follows: heating the casting to 1200-1240°C at a heating rate of 4-6°C / min, keeping warm for 15-25h, then cooling to 700-750°C at a cooling rate of 4-6°C / min, keeping warm for 2-3h, taking out, and air cooling to room temperature.

[0019] Preferably, the multi-directional forging in step S2 is: upsetting and stretching the homogenized casting in three directions of X, Y and Z, and finally stretching it in the Z direction to a finished product, wherein X and Y are two diameter directions perpendicular to each other, Z is the axial direction of the original electroslag ingot, the start forging temperature is 1050-1140°C, and the final forging temperature is 900-1000°C.

[0020] Preferably, the annealing, quenching and tempering in step S3 are as follows: heating the forging module to 850-870°C at a heating rate of 1.5-2.5°C / min, keeping it warm for 6-8h, cooling it to 400-500°C in the furnace, taking it out, and air cooling it to room temperature; then heating the forging module to 920-980°C at a heating rate of 1.5-2.5°C / min, keeping it warm for 1-6h, and cooling the forging module to 50-150°C with water; and then immediately tempering it 1-2 times, with the tempering temperature at 550-580°C and keeping it warm for 4-10h.

[0021] In summary, the present invention has the following beneficial effects:

[0022] 1. Cr is a medium carbide-forming element. Chromium carbide is the smallest carbide among various carbides. It can be evenly distributed in the steel matrix and has high strength, high hardness, high yield point and high wear resistance. Mo has a good grain refining effect, which can increase the strength of steel without reducing plasticity and improve the impact toughness of steel. It can significantly improve the hardenability of steel when combined with Cr. The present invention adopts the design concept of high Mo and low Cr, strictly controls the mass fraction ratio of Mo and Cr, and makes the hot working die steel have excellent hardness and impact toughness.

[0023] 2. The present invention adds rare earth metal elements Ce, La and Y, and controls the sum of the mass fractions of the three. Ce, La and Y work together to form rare earth compounds with elements such as oxygen and sulfur, which have the functions of modifying inclusions, purifying molten steel and refining microstructures; they are also dissolved into the matrix to play a role in solid solution strengthening. The rare earth inclusions formed in the steel have the characteristics of regular morphology, small size, uniform distribution and high melting point, which can improve the microstructure of the material; in addition, they also have the effect of breaking eutectic carbides, improving the isotropy of eutectic carbides, reducing the size of eutectic carbides, and reducing the percentage of eutectic carbides; the comprehensive effect of various aspects makes the mold steel of the present invention have a stable and uniform structure, and still has excellent strength and toughness at high temperatures.

[0024] 3. The preparation method of the hot working die steel of the present invention has simple steps, and is subjected to processes such as melting, refining, pouring, high-temperature homogenization treatment, multi-directional forging, annealing, quenching, and tempering. Among them, the multi-directional forging can greatly refine the grains, improve the strength of the die steel, and reduce the anisotropy, thereby solving the problem that the hot working die steel in the prior art cannot maintain excellent toughness at high temperatures. DETAILED DESCRIPTION

[0025] The present invention is further described in detail below in conjunction with specific embodiments. The examples are only used to explain the present invention and are not used to limit the scope of the present invention.

[0026] To avoid redundancy, the devices used in the following embodiments are all conventional devices in the art unless otherwise specified, and the methods used are all conventional methods in the art unless otherwise specified.

[0027] Example 1

[0028] A high temperature resistant and high toughness hot working die steel, composed of the following components by mass fraction: C: 0.14%, Si: 0.40%, Mn: 0.80%, Mo: 3.00%, Ni: 4.20%, Cr: 1.50%, V: 0.10%, Ce: 0.20%, La: 0.075%, Y: 0.002%, P: 0.012%, S: 0.018%, the balance is Fe and impurities; wherein: Ce+La+Y is 0.277%, Mo / Cr is 2;

[0029] A method for preparing high-temperature resistant and high-toughness hot working die steel comprises the following steps:

[0030] S1. Take raw materials according to the formula of high-temperature resistant and high-toughness hot-working die steel, first add industrial pure iron, Mn, Cr, Ni, and Mo into a smelting furnace, turn on the vacuum pump to evacuate, and the vacuum degree is 6Pa; after the charge begins to melt, introduce argon gas until the total pressure in the furnace is 30000Pa, add graphite after the charge is completely melted, evacuate again to 12Pa, and keep warm for 20 minutes for vacuum refining, and the refining temperature is 1580℃; after the vacuum refining is completed, V, Ce, Si, La, and Y are added in sequence and continue to smelt until the charge is fully melted, and the smelting temperature is 1580℃ to obtain molten steel; the molten steel is poured to obtain a casting;

[0031] S2. First, the casting is homogenized: heated to 1200°C at a heating rate of 4°C / min, kept at this temperature for 15 hours, then cooled to 700°C at a cooling rate of 4°C / min, kept at this temperature for 2 hours, taken out, and air-cooled to room temperature; then multi-directional forging is performed: the casting after homogenization is upset and stretched in three directions of X, Y, and Z, and finally stretched in the Z direction to a finished product, wherein X and Y are two diameter directions perpendicular to each other, and Z is the axial direction of the original electroslag ingot, the start forging temperature is 1050°C, and the final forging temperature is 900°C, to obtain a forging module;

[0032] S3. Heat the forging module to 850°C at a heating rate of 1.5°C / min, keep it warm for 6 hours, cool it to 400°C in the furnace, take it out, and cool it to room temperature with air; then heat the forging module to 920°C at a heating rate of 1.5°C / min, keep it warm for 1 hour, and cool it to 50°C with water; then immediately temper it once, the tempering temperature is 550°C, and keep it warm for 4 hours to obtain hot working die steel.

[0033] Example 2

[0034] A high temperature resistant and high toughness hot working die steel, composed of the following components by mass fraction: C: 0.15%, Si: 0.55%, Mn: 0.75%, Mo: 2.20%, Ni: 4.25%, Cr: 1.10%, V: 0.15%, Ce: 0.40%, La: 0.06%, Y: 0.003%, P: 0.010%, S: 0.015%, the balance is Fe and impurities; wherein: Ce+La+Y is 0.463%, Mo / Cr is 2;

[0035] A method for preparing high-temperature resistant and high-toughness hot working die steel comprises the following steps:

[0036] S1. Take raw materials according to the formula of high-temperature resistant and high-toughness hot-working die steel. First, add industrial pure iron, Mn, Cr, Ni, and Mo into the melting furnace, and start the vacuum pump to evacuate the furnace to a vacuum degree of 6.5Pa; after the charge begins to melt, introduce argon gas until the total pressure in the furnace reaches 32000Pa. After the charge is completely melted, add graphite and evacuate the furnace to 14Pa again. Keep the temperature for 20 minutes for vacuum refining, and the refining temperature is 1585℃; after the vacuum refining is completed, add V, Ce, Si, La, and Y in sequence and continue to smelt until the charge is fully melted, and the smelting temperature is 1595℃ to obtain molten steel; pour the molten steel to obtain a casting;

[0037] S2. The casting is first subjected to homogenization treatment: heated to 1210°C at a heating rate of 4.5°C / min, kept at this temperature for 18 hours, then cooled to 720°C at a cooling rate of 4.5°C / min, kept at this temperature for 2.5 hours, taken out, and air-cooled to room temperature; then multi-directional forging is performed: the casting after homogenization treatment is upset and stretched in three directions of X, Y, and Z, and finally stretched to a finished product along the Z direction, wherein X and Y are two diameter directions perpendicular to each other, and Z is the axial direction of the original electroslag ingot, the start forging temperature is 1080°C, and the final forging temperature is 920°C, to obtain a forging module;

[0038] S3. Heat the forging module to 860°C at a heating rate of 2°C / min, keep it warm for 6.5 hours, cool it to 420°C in the furnace, take it out, and cool it to room temperature with air; then heat the forging module to 940°C at a heating rate of 2°C / min, keep it warm for 3 hours, and cool it to 80°C with water; then immediately temper it twice at a tempering temperature of 560°C and keep it warm for 6 hours to obtain hot working die steel.

[0039] Example 3

[0040] A high temperature resistant and high toughness hot working die steel, composed of the following components by mass fraction: C: 0.15%, Si: 0.70%, Mn: 0.60%, Mo: 2.5%, Ni: 4.30%, Cr: 1.25%, V: 0.30%, Ce: 0.30%, La: 0.055%, Y: 0.004%, P: 0.005%, S: 0.009%, the balance is Fe and impurities; wherein: Ce+La+Y is 0.359%, Mo / Cr is 2;

[0041] A method for preparing high-temperature resistant and high-toughness hot working die steel comprises the following steps:

[0042] S1. Take raw materials according to the formula of high-temperature resistant and high-toughness hot-working die steel. First, add industrial pure iron, Mn, Cr, Ni, and Mo into a smelting furnace, and start a vacuum pump to evacuate the furnace to a vacuum degree of 7Pa; after the charge begins to melt, introduce argon gas until the total pressure in the furnace reaches 32500Pa. After all the charge is melted, add graphite and evacuate the furnace to 15Pa again. Keep the temperature for 20 minutes for vacuum refining, and the refining temperature is 1590℃; after the vacuum refining is completed, add V, Ce, Si, La, and Y in sequence and continue to smelt until the charge is fully melted, and the smelting temperature is 1590℃ to obtain molten steel; pour the molten steel to obtain a casting;

[0043] S2. The casting is first subjected to homogenization treatment: heated to 1220°C at a heating rate of 5°C / min, kept at this temperature for 20 hours, then cooled to 720°C at a cooling rate of 5°C / min, kept at this temperature for 2.5 hours, taken out, and air-cooled to room temperature; then multi-directional forging is performed: the casting after homogenization treatment is upset and stretched in three directions of X, Y, and Z, and finally stretched in the Z direction to a finished product, wherein X and Y are two diameter directions perpendicular to each other, and Z is the axial direction of the original electroslag ingot, the start forging temperature is 1110°C, and the final forging temperature is 950°C, to obtain a forging module;

[0044] S3. Heat the forging module to 870°C at a heating rate of 2°C / min, keep it warm for 7 hours, cool it to 450°C in the furnace, take it out, and cool it to room temperature with air; then heat the forging module to 960°C at a heating rate of 2°C / min, keep it warm for 4 hours, and cool it to 120°C with water; then immediately temper it once, the tempering temperature is 580°C, and keep it warm for 8 hours to obtain hot working die steel.

[0045] Example 4

[0046] A high temperature resistant and high toughness hot working die steel, composed of the following components by mass fraction: C: 0.16%, Si: 0.80%, Mn: 0.43%, Mo: 2.50%, Ni: 4.40%, Cr: 1.25%, V: 0.30%, Ce: 0.50%, La: 0.06%, Y: 0.004%, P: 0.010%, S: 0.015%, the balance is Fe and impurities; wherein: Ce+La+Y is 0.564%, Mo / Cr is 2;

[0047] A method for preparing high-temperature resistant and high-toughness hot working die steel comprises the following steps:

[0048] S1. Take raw materials according to the formula of high-temperature resistant and high-toughness hot-working die steel. First, add industrial pure iron, Mn, Cr, Ni, and Mo into a smelting furnace, and start a vacuum pump to evacuate the furnace to a vacuum degree of 7.5Pa; after the charge begins to melt, introduce argon gas until the total pressure in the furnace reaches 34000Pa. After all the charge is melted, add graphite and evacuate the furnace again to 16Pa. Keep the temperature for 20 minutes for vacuum refining, and the refining temperature is 1590℃; after the vacuum refining is completed, add V, Ce, Si, La, and Y in sequence and continue to smelt until the charge is fully melted, and the smelting temperature is 1590℃ to obtain molten steel; pour the molten steel to obtain a casting;

[0049] S2. First, the casting is homogenized: heated to 1240°C at a heating rate of 6°C / min, kept at this temperature for 22 hours, then cooled to 750°C at a cooling rate of 6°C / min, kept at this temperature for 3 hours, taken out, and air-cooled to room temperature; then multi-directional forging is performed: the casting after homogenization is upset and stretched in three directions of X, Y, and Z, and finally stretched in the Z direction to a finished product, wherein X and Y are two diameter directions perpendicular to each other, and Z is the axial direction of the original electroslag ingot, the start forging temperature is 1140°C, and the final forging temperature is 1000°C, to obtain a forging module;

[0050] S3. Heat the forging module to 870°C at a heating rate of 2.5°C / min, keep it warm for 8 hours, cool it to 500°C in the furnace, take it out, and cool it to room temperature with air; then heat the forging module to 980°C at a heating rate of 2.5°C / min, keep it warm for 6 hours, and cool it to 50-150°C with water; then immediately temper it once, the tempering temperature is 550°C, and keep it warm for 8 hours to obtain hot working die steel.

[0051] Example 5

[0052] A high temperature resistant and high toughness hot working die steel, composed of the following components by mass fraction: C: 0.16%, Si: 0.90%, Mn: 0.20%, Mo: 1.50%, Ni: 4.50%, Cr: 0.75%, V: 0.10%, Ce: 0.48%, La: 0.065%, Y: 0.004%, P: 0.012%, S: 0.018%, the balance is Fe and impurities; wherein: Ce+La+Y is 0.549%, Mo / Cr is 2;

[0053] A method for preparing high-temperature resistant and high-toughness hot working die steel comprises the following steps:

[0054] S1. Take raw materials according to the formula of high-temperature resistant and high-toughness hot-working die steel, first add industrial pure iron, Mn, Cr, Ni, and Mo into the smelting furnace, turn on the vacuum pump to evacuate, and the vacuum degree is 8Pa; after the charge begins to melt, introduce argon gas until the total pressure in the furnace is 35000Pa, add graphite after the charge is completely melted, evacuate again to 18Pa, and keep warm for 20 minutes for vacuum refining, and the refining temperature is 1600℃; after the vacuum refining is completed, add V, Ce, Si, La, and Y in sequence and continue to smelt until the charge is fully melted, and the smelting temperature is 1600℃ to obtain molten steel; pour the molten steel to obtain a casting;

[0055] S2. First, the casting is homogenized: heated to 1240°C at a heating rate of 6°C / min, kept at this temperature for 25 hours, then cooled to 750°C at a cooling rate of 6°C / min, kept at this temperature for 3 hours, taken out, and air-cooled to room temperature; then multi-directional forging is performed: the casting after homogenization is upset and stretched in three directions of X, Y, and Z, and finally stretched in the Z direction to a finished product, wherein X and Y are two diameter directions perpendicular to each other, and Z is the axial direction of the original electroslag ingot, the start forging temperature is 1140°C, and the final forging temperature is 1000°C, to obtain a forging module;

[0056] S3. Heat the forging module to 870°C at a heating rate of 2.5°C / min, keep it warm for 8 hours, cool it to 500°C in the furnace, take it out, and cool it to room temperature with air; then heat the forging module to 980°C at a heating rate of 2.5°C / min, keep it warm for 6 hours, and then cool the forging module to 150°C with water; then immediately temper it twice at a tempering temperature of 580°C and keep it warm for 10 hours to obtain hot working die steel.

[0057] In order to verify the performance of the hot working die steel with high temperature resistance and high toughness provided by the present invention, the inventors set up comparative examples 1-8, wherein:

[0058] Comparative Example 1

[0059] Comparative Example 1 is different from Example 1 only in that Ce is not added.

[0060] Comparative Example 2

[0061] Comparative Example 2 is different from Example 1 only in that La is not added.

[0062] Comparative Example 3

[0063] Comparative Example 3 is different from Example 1 only in that Y is not added.

[0064] Comparative Example 4

[0065] Comparative Example 4 is different from Example 1 only in that Ce: 0.10%, La: 0.01%, Y: 0.01%, and Ce+La+Y is 0.21%.

[0066] Comparative Example 5

[0067] Comparative Example 5 is different from Example 1 only in that Ce: 0.05%, La: 0.30%, Y: 0.45%, and Ce+La+Y is 0.80%.

[0068] Comparative Example 6

[0069] Comparative Example 6 is different from Example 1 only in that Mo: 2.50%, Cr: 0.50%, and Mo / Cr is 5.

[0070] Comparative Example 7

[0071] Comparative Example 7 is different from Example 1 only in that Mo: 1.00%, Cr: 2.50%, and Mo / Cr is 0.4.

[0072] Comparative Example 8

[0073] Comparative Example 8 is different from Example 1 only in that the multi-directional forging in step S2 is changed to unidirectional repeated upsetting and drawing, and the forging temperature is 1000° C., as follows;

[0074] S2. First, the casting is homogenized: heated to 1200°C at a heating rate of 4°C / min, kept warm for 15 hours, then cooled to 700°C at a cooling rate of 4°C / min, kept warm for 2 hours, taken out, and air-cooled to room temperature; then the casting after homogenization is repeatedly upset and drawn in one direction, with a forging temperature of 1000°C, to obtain a forging module.

[0075] The main properties of the hot working die steels in Examples 1-5 and Comparative Examples 1-8 were tested respectively, and the following result parameters were obtained, as shown in Tables 1 and 2:

[0076] Hardness: Refer to "GB / T 230.1-2018 Rockwell hardness test for metallic materials - Part 1: Test method" to test the hardness of hot working die steel; Room temperature performance test: Refer to "GB / T 228.1-2021 Tensile test - Part 1: Room temperature test method" to test the elongation, cross-sectional shrinkage, tensile strength and specified plastic elongation strength of hot working die steel; Impact test: Refer to "GB / T 229-2007 Charpy pendulum impact test method for metallic materials" to test the impact toughness of hot working die steel; High temperature strength test: Refer to "GB / T 4338-2006 High temperature tensile test method for metallic materials" to test the tensile strength and specified plastic elongation strength of hot working die steel at 700°C.

[0077] Table 1 Performance test at room temperature

[0078]

[0079]

[0080] Table 2 High temperature strength test of hot working die steel at 700℃

[0081] Tensile strength / MPa Specified plastic elongation strength / MPa Example 1 684 556 Example 2 678 541 Example 3 717 575 Example 4 705 569 Example 5 695 560 Comparative Example 1 454 378 Comparative Example 2 509 401 Comparative Example 3 510 420 Comparative Example 4 550 452 Comparative Example 5 534 441 Comparative Example 6 425 352 Comparative Example 7 402 380 Comparative Example 8 435 393

[0082] It can be seen from Tables 1 and 2 that the comprehensive performance of the hot working die steels prepared in Examples 1-5 is better than that in Comparative Examples 1-8, which fully demonstrates that the hot working die steels prepared in the present invention have excellent toughness and hardness at room temperature; and still maintain excellent tensile strength and toughness at high temperatures, excellent comprehensive performance, long service life, and a wider range of applications.

[0083] This specific embodiment is merely an explanation of the present invention and is not a limitation of the present invention. After reading this specification, those skilled in the art may make non-creative modifications to the present embodiment as needed. However, as long as they are within the scope of the claims of the present invention, they are protected by the patent law.

Claims

1. A hot working die steel with high temperature resistance and high toughness, characterized in that: The following components are present in percentage by weight Composition: C: 0.14-0.16%, Si: 0.40-0.90%, Mn: 0.20-0.80%, Mo: 1.50-3.00%, Ni: 4.20-4.50%, Cr: 0.60-1.60%, V: 0.10-0.40%, Ce: 0.20-0.90%, La: 0.021-0.075%, Y: 0.002-0.005%, P: ≤0.012%, S: ≤0.018%, the balance is Fe and impurities.

2. The high temperature resistant and high toughness hot working die steel according to claim 1, characterized in that: The following components are present in percentage by weight Composition: C: 0.15-0.16%, Si: 0.55-0.80%, Mn: 0.43-0.75%, Mo: 2.00-2.50%, Ni: 4.25-4.40%, Cr: 1.10-1.55%, V: 0.15-0.30%, Ce: 0.40-0.80%, La: 0.03-0.06%, Y: 0.003-0.004%, P: ≤0.010%, S: ≤0.015%, the balance is Fe and impurities.

3. The high temperature resistant and high toughness hot working die steel according to claim 1, characterized in that: In the hot working die steel, Ce+La+Y is 0.25-0.60%.

4. The high temperature resistant and high toughness hot working die steel according to claim 1, characterized in that: In the hot working die steel, Mo / Cr is 2.

5. A method for preparing high temperature resistant and high toughness hot working die steel according to any one of claims 1 to 4, characterized in that: The following steps are involved: S1. Take raw materials according to the formula of high temperature resistant and high toughness hot working die steel, melt and refine the raw materials to obtain molten steel, and pour the molten steel to obtain a casting; S2, after homogenizing the casting, perform multi-directional forging to obtain a forging module; S3. Perform annealing, quenching and tempering treatments on the forging module in sequence to obtain hot working die steel.

6. The method for preparing high temperature resistant and high toughness hot working die steel according to claim 5, characterized in that: The smelting and refining in S1 are as follows: first, industrial pure iron, Mn, Cr, Ni, and Mo are added into a smelting furnace, and a vacuum pump is turned on to evacuate the furnace to a vacuum degree of 6-8Pa; after the charge begins to melt, argon is introduced until the total pressure in the furnace reaches 30000-35000Pa, and after all the charge is melted, graphite is added and the furnace is evacuated again to a vacuum degree of 12-18Pa, and the temperature is kept for 20 minutes for vacuum refining at a refining temperature of 1580-1600°C; after the vacuum refining is completed, V, Ce, Si, La, and Y are added in sequence and smelting is continued until the charge is fully melted at a smelting temperature of 1580-1600°C to obtain molten steel.

7. The method for preparing high temperature resistant and high toughness hot working die steel according to claim 5, characterized in that: The homogenization treatment in step S2 is as follows: heating the casting to 1200-1240°C at a heating rate of 4-6°C / min, keeping the temperature for 15-25h, then cooling the casting to 700-750°C at a cooling rate of 4-6°C / min, keeping the temperature for 2-3h, taking it out, and air cooling it to room temperature.

8. The method for preparing high temperature resistant and high toughness hot working die steel according to claim 5, characterized in that: The multi-directional forging in step S2 is as follows: the casting after homogenization treatment is upset and stretched in three directions of X, Y and Z, and finally stretched in the Z direction to a finished product, wherein X and Y are two diameter directions perpendicular to each other, Z is the axial direction of the original electroslag ingot, the start forging temperature is 1050-1140°C, and the final forging temperature is 900-1000°C.

9. The method for preparing high temperature resistant and high toughness hot working die steel according to claim 5, characterized in that: The annealing, quenching and tempering in step S3 are as follows: heating the forging module to 850-870°C at a heating rate of 1.5-2.5°C / min, keeping it warm for 6-8h, cooling it to 400-500°C in the furnace, taking it out, and cooling it to room temperature with air; then heating the forging module to 920-980°C at a heating rate of 1.5-2.5°C / min, keeping it warm for 1-6h, and cooling the forging module to 50-150°C with water; and then immediately tempering it 1-2 times, with the tempering temperature of 550-580°C and keeping it warm for 4-10h.

Citation Information

Patent Citations

  • Hot work die steel and production method thereof

    CN109112391A

  • Hot work die steel electroslag remelting ingot and manufacturing method thereof

    CN111101061A

  • Low-temperature high-toughness high-temperature high-intensity high-hardenability hot mould steel and preparation technology thereof

    CN111500928A

  • High-toughness and high-hardenability hot work die steel and preparation method thereof

    CN118127407A

  • Die steel

    KR1020070045921A

Cited By

  • High-thermal-conductivity and high-strength hot work die steel material and preparation method thereof