Heterogeneous aluminum alloy friction stir welding part and heat treatment method thereof

Through the combination of solid solution treatment, cold deformation and aging treatment, the problem of low yield ratio of 2195 aluminum-lithium alloy and 2219 aluminum-copper alloy in friction stir welding is solved, which significantly improves the mechanical properties of the welded parts and meets the aerospace field. high strength and lightweight requirements.

CN118996294APending Publication Date: 2024-11-22YANSHAN UNIV
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202411097948.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-12
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

During friction stir welding, the joints of 2195 aluminum lithium alloy and 2219 aluminum copper alloy softener, with low yield and strength ratio, which is prone to brittle fracture, and the welding plate has weak resistance to deformation, which cannot meet the high strength and lightweight requirements in the aerospace field. .

Method used

The combined method of solid solution treatment, cold deformation and aging treatment is adopted. The specific steps include solid solution treatment at 500-520°C, cold deformation 2-10%, and aging treatment at 160-170°C for 12-18 hours to regulate the grain structure. , inhibit abnormal growth of grains and improve the strength and yield ratio of welding joints.

Benefits of technology

The yield strength, ultimate tensile strength and yield strength ratio of heterogeneous aluminum alloy friction stir welded parts are significantly improved, and the deformation resistance of the welded parts is enhanced, and the high strength and lightweight needs in the aerospace field are met.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure HDA0004988529070000011
    Figure HDA0004988529070000011
  • Figure HDA0004988529070000021
    Figure HDA0004988529070000021
  • Figure HDA0004988529070000022
    Figure HDA0004988529070000022
Patent Text Reader

Abstract

The invention provides a heterogeneous aluminum alloy friction stir welding part and a heat treatment method thereof, and belongs to the field of metal material welding. The invention provides a heat treatment method for a heterogeneous aluminum alloy friction stir welding part. The heat treatment method comprises the steps of solid solution treatment, cold deformation treatment and aging treatment on the heterogeneous aluminum alloy friction stir welding part. Solution treatment is conducted on the heterogeneous aluminum alloy friction stir welding part, the solid solution temperature is controlled, a large number of fine grains in a nugget zone can be reserved, and the uniformity and stability of a weld joint structure are improved; and meanwhile, the solid solution is subjected to cold deformation, a large number of dislocations can be generated, precipitation of a precipitation phase in subsequent aging treatment of the aluminum alloy is promoted, and the strength and the yield ratio of heterogeneous welding parts are effectively improved. The result of the embodiment shows that the yield strength of the heterogeneous aluminum alloy friction stir welding part provided by the invention is 358.57 to 366.80 MPa, the ultimate tensile strength of the heterogeneous aluminum alloy friction stir welding part is 448.52 to 453.09 MPa, and the yield ratio of the heterogeneous aluminum alloy friction stir welding part is 0.79 to 0.82.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of metal material welding, and in particular to a heterogeneous aluminum alloy friction stir welded part and a heat treatment method thereof. Background Art

[0002] With the continuous development of the aerospace field, the demand for comprehensive performance and lightweight materials is getting higher and higher. Aluminum alloys are widely used in this field due to their low density, high strength, and strong corrosion resistance. Among them, 2219 aluminum-copper alloy and 2195 aluminum-lithium alloy are both widely used materials in this field.

[0003] Compared with 2219 aluminum-copper alloy, 2195 aluminum-lithium alloy has stronger load-bearing capacity and lower density, and has great advantages in the application of rocket fuel tanks; however, it cannot be widely used in this field due to factors such as complex preparation process, high cost, and low output. In the 1980s, 2195 and 2219 plates were creatively stir-friction welded and used to manufacture space shuttle tanks, which effectively increased the load and greatly reduced the cost while achieving lightweight. However, for 2195 and 2219 precipitation-strengthened aluminum alloys, the stir-friction welding process causes softening at the joint, which is mainly manifested in that the mechanical properties of the heterogeneous alloy welded joint are between the two parent materials, the yield strength ratio is not high, brittle fracture is prone to occur, and the welded plate has weak deformation resistance. Therefore, the welded plate must be strengthened to improve the weld's deformation resistance and the overall load-bearing capacity of the welded part.

[0004] The yield strength ratio refers to the ratio of the material's yield strength to its tensile strength. The larger the yield strength ratio (saturation value is 1), the stronger the material's ability to resist deformation and the better the material's stability. For heterogeneous friction stir welded plates, the higher the yield strength ratio, the higher the reliability of the welded joint, the stronger the overall deformation resistance of the welded part, the less likely it is to deform, and the better the stability.

[0005] Friction stir welding (FSW) refers to the use of heat generated by friction between a high-speed rotating welding tool and a workpiece to locally soften the welded material. When the welding tool moves forward along the welding interface, the softened material flows from the retreating side (RS) to the advancing side (AS) under the friction of the welding tool, and forms a dense weld under the extrusion of the welding tool. The friction stir welding joint can be roughly divided into the following areas: the shoulder affected zone (SAZ) only affected by the shoulder extrusion, the heat affected zone (HAZ) only affected by the welding heat input, the weld nugget zone (NZ) directly affected by the rotation of the stirring needle, and the thermo-mechanical affected zone (TMAZ) affected by the welding heat input and the rotation of the stirring needle. During the welding process, the metal in the weld nugget zone is subjected to strong mechanical stirring. The metal rotates and rises along the thread of the stirring needle, and the grains are completely broken. With the heat generated by friction, the weld nugget zone undergoes dynamic recrystallization, generating a large number of fine equiaxed crystals. The friction heat will also increase the temperature of this area to between the dissolution temperature of the precipitate phase and the melting temperature of the matrix. The precipitate phase dissolves back and re-precipitates evenly during the subsequent cooling process. The two work together to strengthen the weld nugget zone. However, due to the effect of heat conduction, the grains in the other areas on both sides of the weld are coarsened to a certain extent. In particular, the HAZ is only affected by heat input and is not affected by other factors. The strength loss is the greatest, and material failure is prone to occur in this area.

[0006] The 2195 aluminum-lithium alloy and 2219 aluminum-copper alloy used in the present invention are both precipitation-strengthened alloys. Generally, for precipitation-strengthened materials, in order to reduce the HAZ strength loss after friction stir welding, the welded parts are usually subjected to solid solution-aging heat treatment. However, in the post-weld heat treatment process of several FSW aluminum alloys, it was observed that fine equiaxed crystals in the joint area all grew up due to secondary recrystallization, and even millimeter-level grains appeared. The fracture was brittle ductile fracture, which could not effectively improve the strength of the friction stir welding welded parts, and the yield strength ratio was relatively low; for example, the prior art "The Effect of Post-weld Heat Treatment on the Microstructure and Mechanical Properties of 6063-T6 Aluminum Alloy Friction Stir Welding Joint" disclosed that after the aluminum alloy friction stir welding joint was subjected to solid solution and aging treatment, the yield strength of the welded joint was only 130.7MPa, the tensile strength was only 182.1MPa, and the yield strength ratio was only 0.71. The strength and yield strength ratio of the welded joint cannot meet the needs of practical applications. Summary of the invention

[0007] The purpose of the present invention is to provide a heterogeneous aluminum alloy friction stir welded part and a heat treatment method thereof. The heat treatment method provided by the present invention can effectively improve the strength and yield strength ratio of the heterogeneous aluminum alloy friction stir welded part.

[0008] In order to achieve the above-mentioned object of the invention, the present invention provides the following technical solutions:

[0009] The present invention provides a heat treatment method for improving the yield strength ratio of heterogeneous aluminum alloy friction stir welded parts, comprising the following steps:

[0010] (1) subjecting the heterogeneous aluminum alloy friction stir welded parts to a solid solution treatment to obtain a solid solution; the temperature of the solid solution treatment is 500 to 520° C.;

[0011] (2) cold deforming the solid solution obtained in step (1) to obtain a deformed body;

[0012] (3) subjecting the deformed body obtained in step (2) to aging treatment to obtain a heat-treated heterogeneous aluminum alloy friction stir welded part.

[0013] Preferably, the heterogeneous aluminum alloy friction stir welded part in step (1) is a friction stir welded part of 2195 aluminum alloy and 2219 aluminum alloy.

[0014] Preferably, the 2195 aluminum alloy is a T8 rolled plate, and the 2219 aluminum alloy is a T6 rolled plate.

[0015] Preferably, the heterogeneous aluminum alloy friction stir welded parts are prepared by friction stir welding of 2195 aluminum alloy and 2219 aluminum alloy, and the parameters of friction stir welding include: the rotation speed of the stirring head is 700-900rpm, the travel speed of the stirring head is 150-250mm / min, the inclination angle of the stirring head is 1-2°, and the downward pressure of the stirring head is 0.1-0.2mm.

[0016] Preferably, the solution treatment time in step (1) is 0.5 to 1.5 hours.

[0017] Preferably, the cooling method of the solution treatment in step (1) is water quenching.

[0018] Preferably, the water quenching time is 5 to 10 seconds.

[0019] Preferably, the amount of cold deformation in step (2) is 2 to 10%.

[0020] Preferably, the temperature of the aging treatment in step (3) is 160-170° C., and the time of the aging treatment is 12-18 hours.

[0021] The present invention also provides a heat-treated heterogeneous aluminum alloy friction stir welded part obtained by the heat treatment method described in the above technical solution.

[0022] The present invention provides a heat treatment method for a heterogeneous aluminum alloy friction stir welded part, comprising the following steps: (1) subjecting the heterogeneous aluminum alloy friction stir welded part to a solid solution treatment, wherein the temperature of the solid solution treatment is 500-520°C; (2) subjecting the solid solution obtained in the step (1) to cold deformation, thereby obtaining a deformed body; (3) subjecting the deformed body obtained in the step (2) to an aging treatment, thereby obtaining a heat-treated heterogeneous aluminum alloy friction stir welded part. The present invention uses a solid solution treatment to treat the heterogeneous aluminum alloy friction stir welded part and controls the solid solution temperature, thereby effectively regulating the grain structure, inhibiting the abnormal growth of grains, allowing a large number of fine grains to remain in the weld nugget zone, improving the uniformity and stability of the weld structure, and thus improving the strength of the weld joint; at the same time, the solid solution is cold deformed, causing the aluminum matrix lattice to be distorted, inhibiting the further growth of grains in the aging process to a certain extent, promoting the precipitation of the precipitated phase of the aluminum alloy in the subsequent aging treatment, further improving the re-deformation strength of the weld joint, and correspondingly improving the overall yield strength of the welded part, and increasing the yield strength ratio. The results of the embodiments show that the yield strength of the heterogeneous aluminum alloy friction stir welded parts provided by the present invention is 358.57-366.80 MPa, the ultimate tensile strength is 448.52-453.09 MPa, and the yield strength ratio is 0.79-0.82. BRIEF DESCRIPTION OF THE DRAWINGS

[0023] Figure 1 Flow chart of the heat treatment method of heterogeneous aluminum alloy friction stir welded parts in the embodiment;

[0024] Figure 2 The metallographic image of the weld nugget area of ​​the weld joint of the heterogeneous aluminum alloy friction stir welded piece after heat treatment in Example 2;

[0025] Figure 3 The metallographic image of the weld nugget area of ​​the weld joint of the heterogeneous aluminum alloy friction stir welded part after heat treatment in Example 3;

[0026] Figure 4 The metallographic image of the welded joint of the heterogeneous aluminum alloy friction stir welded piece after heat treatment in Comparative Example 1;

[0027] Figure 5 The metallographic image of the weld nugget area of ​​the weld joint of the heterogeneous aluminum alloy friction stir welded piece after heat treatment in Comparative Example 2;

[0028] Figure 6 This is a metallographic image of the forward side of the heterogeneous aluminum alloy friction stir welded piece after heat treatment in Comparative Example 3;

[0029] Figure 7 This is a comparison chart of the mechanical properties of the heterogeneous aluminum alloy friction stir welded parts after heat treatment in Examples 1 to 3 and Comparative Examples 1 to 3. DETAILED DESCRIPTION

[0030] The present invention provides a heat treatment method for a heterogeneous aluminum alloy friction stir welded part, comprising the following steps:

[0031] (1) subjecting the heterogeneous aluminum alloy friction stir welded parts to a solid solution treatment to obtain a solid solution; the temperature of the solid solution treatment is 500 to 520° C.;

[0032] (2) cold deforming the solid solution obtained in step (1) to obtain a deformed body;

[0033] (3) subjecting the deformed body obtained in step (2) to aging treatment to obtain a heat-treated heterogeneous aluminum alloy friction stir welded part.

[0034] The invention performs solid solution treatment on heterogeneous aluminum alloy friction stir welding parts to obtain a solid solution.

[0035] In the present invention, the heterogeneous aluminum alloy friction stir welded parts are preferably friction stir welded parts of 2195 aluminum alloy and 2219 aluminum alloy; the 2195 aluminum alloy is preferably a T8 state rolled plate, and the 2219 aluminum alloy is preferably a T6 state rolled plate.

[0036] In the present invention, the heterogeneous aluminum alloy friction stir welded parts are preferably prepared by friction stir welding of 2195 aluminum alloy and 2219 aluminum alloy, and the parameters of the friction stir welding preferably include: the rotation speed of the stirring head is preferably 700-900rpm, more preferably 750-850rpm, and most preferably 780-800rpm; the travel speed of the stirring head is preferably 150-250mm / min, more preferably 180-230mm / min, and most preferably 200-210mm / min; the inclination angle of the stirring head is preferably 1-2°, and most preferably 2°; the downward pressure of the stirring head is preferably 0.1-0.2mm, and most preferably 0.1mm; the 2195 aluminum alloy is preferably on the advancing side, and the 2219 aluminum alloy is preferably on the retreating side. In the present invention, by limiting the parameters of stir friction, the combination of the 2195-T8 rolled plate on the forward side and the 2219-T6 rolled plate on the backward side is further promoted, weld defects are eliminated, and the strength of the welded part is further improved; by limiting the types of alloy plates on the forward side and the backward side, it is beneficial to drive the 2219-T6 rolled plate with lower strength and better plasticity to the forward side during stir friction welding, which is beneficial to the full combination of the 2195-T8 rolled plate and the 2219-T6 rolled plate, thereby obtaining a defect-free weld, realizing the reinforcement effect of the 2195-T8 rolled plate on the 2219-T6 rolled plate, and is beneficial to improving the strength and yield strength ratio of heterogeneous aluminum alloy stir friction welded parts.

[0037] The present invention has no special limitation on the sources of the 2195 aluminum alloy and the 2219 aluminum alloy, and commercially available products may be used.

[0038] In the present invention, the temperature of the solution treatment is 500-520°C, preferably 505-515°C, more preferably 508-512°C, and most preferably 509-510°C; the time of the solution treatment is preferably 0.5-1.5h, more preferably 0.8-1.2h, and most preferably 0.9-1h. In the present invention, the first inducement for the abnormal grain growth phenomenon is the temperature of the solution treatment. For precipitation-strengthened aluminum alloys, the solution temperature during treatment is generally higher than the recrystallization temperature of the aluminum matrix. Therefore, solution treatment of the joint will cause abnormal growth of the joint grains. The growth of the grains is inevitable, but the scale of the grain growth can be controlled. The present invention limits the temperature of the solution treatment to ensure that the scale of abnormal grain growth can be controlled in each area of ​​the stir friction welding joint, promote the uniformity of element distribution at the welding joint, and improve the plasticity of the welding joint. At the same time, the time of the solution treatment is limited to avoid excessive time that leads to an increase in the scale of grain growth, further improve the plasticity of the welded part, reduce the tendency of brittle fracture in the weld core zone, and further improve the strength and yield strength ratio of the welded part.

[0039] In the present invention, the cooling method of the solution treatment is preferably water quenching; the time of the water quenching is preferably 5 to 10 seconds, more preferably 6 to 9 seconds, and most preferably 7 to 8 seconds. In the present invention, by limiting the time of the water quenching treatment, the supersaturated solid solution in the matrix is ​​retained to the greatest extent, providing a basis for the precipitation of more strengthening phases during the subsequent aging treatment.

[0040] After obtaining the solid solution, the present invention performs cold deformation on the obtained solid solution to obtain a deformed body.

[0041] In the present invention, the deformation amount of the cold deformation is preferably 2-10%, more preferably 2-8%, and most preferably 3-7%. In the present invention, by cold deformation of the solid solution, combined with the subsequent aging treatment, the problem of joint strength reduction caused by incomplete and insufficient dissolution of the second phase during the solution treatment can be effectively compensated. Cold deformation can make the second phase precipitate more and more dispersed in the subsequent aging treatment, promote the uniform dispersion of various elements at the weld joint, and improve the strength and stability of the weld joint; at the same time, the lattice distortion caused by cold deformation can inhibit the growth of grain boundaries during subsequent aging treatment, so that the fine grain part in the weld core area of ​​the weld joint is retained to the maximum extent, reducing the proportion of coarse grains, and greatly reducing the crystallization of the rest of the joint. The grain size can be effectively controlled to effectively control the abnormal growth scale of grains in the weld nugget zone; the cold deformation process can also promote grain slip, make the grains elongated, broken and fibrous, and at the same time generate residual stress inside the metal, hindering the deformation again after the joint is unloaded, and improving the yield strength of the welded joint; the deformation amount is limited to ensure the effect of cold deformation on the welded joint, increase the dislocation density in the joint area, and a large number of dislocations can provide more nucleation sites for the precipitation of the second phase in the subsequent aging treatment, which is beneficial to the precipitation of the main strengthening phase θ' phase and other alloy phases, and at the same time promote the dispersed distribution of the precipitated phase, further improving the strength and yield strength ratio of the welded joint.

[0042] After the deformed body is obtained, the present invention performs aging treatment on the deformed body to obtain a heat-treated heterogeneous aluminum alloy friction stir welded part.

[0043] In the present invention, the temperature of the aging treatment is preferably 160-170°C, more preferably 163-167°C, and most preferably 164-165°C; the time of the aging treatment is preferably 12-18h, more preferably 13-16h, and most preferably 14-15h. In the present invention, the internal stress in the deformed body is effectively eliminated by aging treatment to avoid excessive deformation of the deformed body; at the same time, the solute atoms precipitate nano-scale second phase particles at the grain boundary or in the crystal, effectively improving the strength of the welded joint; the process parameters of the aging treatment are controlled to further improve the effect of the aging treatment, and further improve the yield strength and plasticity of the welded joint.

[0044] The present invention adopts solution treatment-cold deformation-artificial aging to treat heterogeneous aluminum alloy stir friction welded parts. By controlling the solution temperature, the grain structure of the joint area can be effectively regulated, the abnormal growth scale of the grains can be suppressed, a large number of fine grains can be retained in the weld core area, and the uniformity and stability of the weld structure can be improved; at the same time, the solid solution is cold deformed to increase the lattice distortion and dislocation density, which can suppress the growth of grains in the aging process and promote the precipitation of the precipitate phase of the aluminum alloy in the subsequent aging treatment; finally, the deformed body is artificially aged to eliminate the internal stress of part of the deformed body, so that the precipitate phase is uniformly precipitated in the deformed body, the strength, yield strength ratio and plasticity of the joint are further improved, and the brittle fracture tendency of the weld core area is reduced.

[0045] The present invention also provides a heat-treated heterogeneous aluminum alloy friction stir welded part obtained by the heat treatment method described in the above technical solution.

[0046] The heat-treated heterogeneous aluminum alloy friction stir welded part obtained by the heat treatment method provided by the present invention has excellent mechanical properties and can meet the needs of practical applications.

[0047] The technical solutions in the present invention will be described clearly and completely below in conjunction with the embodiments of the present invention. Obviously, the described embodiments are only a part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0048] Example 1

[0049] A heat treatment method for a heterogeneous aluminum alloy friction stir welded part comprises the following steps:

[0050] (1) A heterogeneous aluminum alloy friction stir welded part obtained by friction stir welding a 2195-T8 aluminum-lithium alloy plate and a 2219-T6 aluminum-copper alloy plate was solution treated at 515°C for 1 h and water quenched at 20°C for 5 s to obtain a solid solution; wherein the rotation speed of the friction stir welding stirring head is 800 rpm, the travel speed of the stirring head is 200 mm / min, the inclination angle of the stirring head is 2°, and the downward pressure of the stirring head is 0.1 mm.

[0051] (2) cold deforming the solid solution obtained in step (1) to obtain a deformed body; wherein the deformation amount of the cold deformation is 3%;

[0052] (3) The deformed body obtained in step (2) is subjected to aging treatment at 165° C. for 12 hours to obtain a heat-treated heterogeneous aluminum alloy friction stir welded part.

[0053] Example 2

[0054] The difference between Example 2 and Example 1 is that the deformation amount of cold deformation in step (2) is 5%, and the rest is the same as Example 1.

[0055] The weld nugget area of ​​the heat-treated heterogeneous aluminum alloy friction stir welded joint obtained in Example 2 was observed using a Zeiss optical metallographic microscope. The obtained metallographic image is as follows: Figure 2 As shown. Figure 2It can be seen that a large number of fine grains remain in the weld core area of ​​the weld joint of the welded part treated by the heat treatment method provided in Example 2, which achieves effective control of the grain growth scale and can effectively improve the comprehensive performance of the welded part.

[0056] Example 3

[0057] The only difference between Example 3 and Example 1 is that the deformation amount of the cold deformation in step (2) is 7%, and the rest is the same as Example 1.

[0058] The weld nugget area of ​​the heat-treated heterogeneous aluminum alloy friction stir welded joint obtained in Example 3 was observed using a Zeiss optical metallographic microscope, and the obtained metallographic image is as follows: Figure 3 As shown. Figure 3 It can be seen that a large number of fine grains remain in the weld core area of ​​the welded joint of the welded part treated by the heat treatment method provided in Example 3, which achieves effective control of the grain growth scale and can effectively improve the comprehensive performance of the welded part.

[0059] Comparative Example 1

[0060] The difference between Comparative Example 1 and Example 1 is that the temperature of the solution treatment in step (1) is 535° C., step (2) is omitted, and the rest is the same as Example 1.

[0061] The heat-treated heterogeneous aluminum alloy friction stir welded joint area obtained in Comparative Example 1 was observed using a Zeiss optical metallographic microscope, and the obtained metallographic image is as follows: Figure 4 As shown. Figure 4 It can be seen that for the weld joint treated by the heat treatment method provided in Comparative Example 1, all the grains in the weld core area of ​​the joint undergo secondary recrystallization and then grow into large millimeter-sized grains, which cannot effectively improve the overall performance of the joint.

[0062] Comparative Example 2

[0063] The difference between Comparative Example 2 and Example 1 is that step (2) is omitted, and the rest is the same as Example 1.

[0064] The weld nugget area of ​​the heat-treated heterogeneous aluminum alloy friction stir welded joint obtained in Comparative Example 2 was observed using a Zeiss optical metallographic microscope, and the metallographic image obtained is as follows: Figure 5 As shown. Figure 5 It can be seen that for the welded parts treated by the heat treatment method provided in Comparative Example 2, the small equiaxed crystals in the lower left and lower right corners of the weld core area of ​​the weld joint grew and merged into several large grains of different colors due to different corrosion resistance, and a small amount of precipitates were present in the grains; most of the fine equiaxed crystals were still retained in the center of the weld core area, and the comprehensive performance of the welded parts could not be effectively improved.

[0065] Comparative Example 3

[0066] The difference between Comparative Example 3 and Example 1 is that the temperature of the solution treatment in step (1) is 525° C., step (2) is omitted, and the rest is the same as Example 1.

[0067] The weld nugget zone on the forward side of the weld joint of the heat-treated heterogeneous aluminum alloy friction stir welded part obtained in Comparative Example 3 was observed using a Zeiss optical metallographic microscope. The metallographic image obtained is as follows: Figure 6 As shown. Figure 6 It can be seen that in the joint area of ​​the welded parts treated by the heat treatment method provided in Comparative Example 3, the grains in the lower left corner of the weld core area have grown, no fine grains remain, and the large grain boundaries are more distorted and easily cause impurity phase segregation. The presence of these large grains will greatly reduce the plasticity and corrosion resistance of the joint, increase the tendency of brittle fracture of large grain boundaries, and cannot effectively improve the overall performance of the joint.

[0068] The yield strength, tensile strength, elongation and yield strength ratio of the heat-treated heterogeneous aluminum alloy friction stir welded parts of Examples 1 to 3 and Comparative Examples 1 to 3 were tested using an INSTRON-8801 electro-hydraulic servo universal testing machine. The results are shown in Table 1.

[0069] Table 1 Mechanical properties of heterogeneous aluminum alloy friction stir welded parts after heat treatment of Examples 1 to 3 and Comparative Examples 1 to 3

[0070] Example Yield strength (MPa) Ultimate tensile strength (MPa) Elongation(%) Yield-to-strength ratio Example 1 358.57 453.09 6.63 0.79 Example 2 359.14 451.61 7.84 0.8 Example 3 366.80 448.52 7.06 0.82 Comparative Example 1 312.50 450.67 5.82 0.69 Comparative Example 2 296.77 436.16 7.86 068 Comparative Example 3 307.54 443.68 5.68 0.69

[0071] As can be seen from Table 1, the heat treatment method provided by the present invention reduces the solution temperature and increases the cold deformation treatment, thereby greatly improving the yield strength of the welded part while ensuring the plasticity of the heterogeneous aluminum alloy stir friction welded part. The average yield strength ratio is increased by about 17% compared with the average yield strength ratio of the control ratio, the deformation resistance is enhanced, the risk of brittle fracture in the weld core zone is reduced, the reliability of the heterogeneous stir friction welding joint is enhanced, and the comprehensive mechanical properties of the welded joint are effectively improved.

[0072] The mechanical properties of the heterogeneous aluminum alloy friction stir welded parts after heat treatment in Examples 1 to 3 and Comparative Examples 1 to 3 are as follows: Figure 7 As shown. Figure 7 It can be seen that the heat treatment method provided by the present invention can ensure the mechanical properties of the welded parts under the condition of lowering the solid solution temperature.

[0073] In summary, the heat treatment method provided by the present invention can effectively regulate the grain structure, inhibit the abnormal growth of grains, greatly improve the yield strength, yield strength ratio and elongation of the welded parts, and effectively improve the comprehensive mechanical properties of the welded parts.

[0074] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.

Claims

1. A heat treatment method for a heterogeneous aluminum alloy friction stir welded part, comprising the following steps: (1) subjecting the heterogeneous aluminum alloy friction stir welded parts to a solid solution treatment to obtain a solid solution; the temperature of the solid solution treatment is 500 to 520° C.; (2) cold deforming the solid solution obtained in step (1) to obtain a deformed body; (3) subjecting the deformed body obtained in step (2) to aging treatment to obtain a heat-treated heterogeneous aluminum alloy friction stir welded part.

2. The heat treatment method according to claim 1, characterized in that The heterogeneous aluminum alloy friction stir welded parts in step (1) are friction stir welded parts of 2195 aluminum alloy and 2219 aluminum alloy.

3. The heat treatment method according to claim 2, characterized in that: The 2195 aluminum alloy is a T8 rolled plate, and the 2219 aluminum alloy is a T6 rolled plate.

4. The heat treatment method according to claim 2 or 3, characterized in that: The heterogeneous aluminum alloy friction stir welded parts are prepared by friction stir welding of 2195 aluminum alloy and 2219 aluminum alloy, and the parameters of friction stir welding include: the rotation speed of the stirring head is 700-900rpm, the travel speed of the stirring head is 150-250mm / min, the inclination angle of the stirring head is 1-2°, and the downward pressure of the stirring head is 0.1-0.2mm.

5. The heat treatment method according to claim 1, characterized in that: The time of the solution treatment in step (1) is 0.5 to 1.5 hours.

6. The heat treatment method according to claim 1 or 5, characterized in that: The cooling method of the solution treatment in step (1) is water quenching.

7. The heat treatment method according to claim 6, characterized in that: The water quenching time is 5 to 10 seconds.

8. The heat treatment method according to claim 1, characterized in that: The amount of cold deformation in step (2) is 2 to 10%.

9. The heat treatment method according to claim 1, characterized in that: The temperature of the aging treatment in step (3) is 160-170° C., and the time of the aging treatment is 12-18 hours.

10. A heat-treated heterogeneous aluminum alloy friction stir welded part obtained by the heat treatment method according to any one of claims 1 to 9.

Citation Information

Cited By

  • Composite board with multi-layer heterogeneous interface and preparation method thereof

    CN119566502A