Self-lubricating hard alloy coating and preparation process thereof

By using cheap Cr3C2 and TiC instead of WC, Ni instead of Co, and combined with supersonic flame spraying technology, self-lubricated carbide coating is prepared, which solves the problem of high cost of HVOF spraying method, and achieves performance optimization and cost reduction. It is suitable for use in the process of suitable use. Large-scale application.

CN118996312AActive Publication Date: 2024-11-22TIANJIN DETIANZHU AMORPHOUS NANOTECHNOLOGY CO LTD
View PDF 14 Cites 0 Cited by

Patent Information

Application Number
CN202411476894.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-10-22
Publication Date
2024-11-22
Estimated Expiration
2044-10-22

AI Technical Summary

Technical Problem

The preparation of WC cemented carbide coating by HVOF spraying method has problems such as high gas consumption, high powder price, low deposition rate during spraying and high post-processing costs, which leads to high costs and limits its wide range of applications.

Method used

Inexpensive carbides Cr3C2 and TiC are used to partially replace WC, and inexpensive bonding phase Ni is used to partially replace Co., combined with supersonic flame spraying technology, self-lubricated carbide coating is prepared to reduce raw material costs and improve spraying efficiency.

Benefits of technology

While ensuring performance, production costs are reduced, large-scale application of the coating is achieved, and the friction coefficient is reduced by adding a self-lubricating phase, the wear resistance and wear reduction performance are improved, and the spraying efficiency and performance of the coating are improved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118996312A_ABST
    Figure CN118996312A_ABST
Patent Text Reader

Abstract

The invention relates to the field of metal materials, in particular to a self-lubricating hard alloy coating and a preparation process thereof. The invention discloses a self-lubricating hard alloy coating which comprises an alloy coating arranged on the surface of steel and comprises the following elements in percentage by mass (Wt / %): 20-30% of WC, 0-10% of TiC, 1-5% of Co, 10-14% of Ni, 1-5% of Cr and the balance of Cr3C2. According to the self-lubricating hard alloy coating, WC is partially replaced with cheap carbides Cr3C2 and TiC, Co is partially replaced with a cheap binding phase Ni, the cost price of raw materials is reduced under the condition that the performance is guaranteed, and therefore the production cost of the self-lubricating hard alloy coating is reduced on the whole, and large-scale application becomes possible; and the self-lubricating phase is added, the friction coefficient is reduced by improving the proportion, and the wear-resisting and anti-attrition performance of the hard alloy coating is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of metal materials, and in particular to a self-lubricating hard alloy coating and a preparation process thereof. Background Art

[0002] Cemented carbide is a metal-ceramic material prepared by powder metallurgy using micron-level high-hardness refractory carbides such as tungsten carbide (WC), titanium carbide (TiC) and chromium carbide (Cr3C2) and transition metals cobalt (Co), nickel (Ni) and other trace element powders. It is also often used as a coating in surface engineering. With its good performance, it has been widely used in many fields. The application of cemented carbide coatings in the field of material surfaces has doubled the wear resistance, corrosion resistance and other properties of the base material, greatly reducing production costs and improving production efficiency. In the process of preparing WC cemented carbide coatings, HVOF spraying has greater advantages than other spraying methods in terms of work efficiency and coating quality. It is currently the most important method for preparing WC-based coatings.

[0003] The WC cemented carbide coating prepared by HVOF spraying has the characteristics of good wear resistance and corrosion resistance. It has successfully replaced the electroplating hard chrome process in many fields such as aviation and machinery. However, it also has defects such as high gas consumption, high powder price, and low deposition rate during spraying. In addition, the high post-processing costs caused by the high hardness of the coating lead to the high price of HVOF sprayed WC coating. This makes it difficult to apply HVOF sprayed WC coating on a large scale. Current research on WC coatings mainly focuses on improving coating performance, and rarely considers how to reduce the preparation cost of alternative coatings while meeting the use requirements.

[0004] Based on the characteristics of WC cemented carbide coating, its wear is a very common problem, involving almost all the movement processes of mechanical parts. Failure and replacement caused by wear greatly reduce the service life and production efficiency of parts. WC coating has a large number of applications in the industrial field due to its excellent wear resistance. The hard phase WC particles increase the average hardness, and the bonding phases such as Co, Ni, and Cr connect the carbide particles to improve the toughness of the material. The friction and wear properties of wear-resistant coatings such as WC-Co and WC-Co-Cr obtained by the composite of hard phase and bonding phase are affected by powder type, mechanical properties of coating, microstructure, spraying process and wear conditions. On the other hand, it is also because of different working conditions in actual applications and different types of wear. Usually, the wear types in the mechanical wear process of coatings are divided into corrosive wear, abrasive wear, erosion wear, fatigue wear and adhesive wear. Wear in real situations is often the result of the idealized effect of two or more wear types. Summary of the invention

[0005] In view of this, the present invention hopes to provide a self-lubricating cemented carbide coating and its preparation process, using cheap carbides Cr3C2 and TiC to partially replace WC, and cheap bonding phase Ni to partially replace Co, so as to achieve a reduction in raw material cost while ensuring performance, thereby reducing its production cost as a whole and making large-scale application possible.

[0006] The technical solution of the embodiment of the present invention is achieved as follows: A self-lubricating cemented carbide coating is special in that its composition includes an alloy coating arranged on the surface of a steel material, including the following elements in weight percent (Wt / %): WC: 20-30%, TiC: 0-10%, Co: 1-5%, Ni: 10-14%, Cr: 1-5%, and the remainder is Cr3C2.

[0007] The alloy coating comprises a cemented carbide phase and a cobalt-chromium-nickel bonding phase, and the cobalt-chromium-nickel bonding phase surrounds the cemented carbide phase in a network shape.

[0008] The alloy coating comprises the following elements in weight percent (Wt / %): WC: 20%, Co: 1%, Ni: 10%, Cr: 5%, and the balance is Cr3C2.

[0009] The alloy coating comprises the following elements in weight percent (Wt / %): WC: 25%, Co: 3%, Ni: 14%, Cr: 5%, and the remainder is Cr3C2.

[0010] The alloy coating comprises the following elements in weight percent (Wt / %): WC: 25%, TiC: 10%, Co: 1%, Ni: 12%, Cr: 5%, and the remainder is Cr3C2.

[0011] The alloy coating comprises the following elements in weight percent (Wt / %): WC: 30%, TiC: 5%, Co: 1%, Ni: 14%, Cr: 5%, and the remainder is Cr3C2.

[0012] The alloy coating comprises the following elements in weight percent (Wt / %): WC: 20%, Co: 1%, Ni: 14%, and the balance being Cr3C2.

[0013] The alloy coating comprises the following elements in weight percent (Wt / %): WC: 20%, h-BN: 1-3%, Co: 1%, Ni: 14%, Cr: 5%, and the balance is Cr3C2.

[0014] On the other hand, a preparation process of a self-lubricating cemented carbide coating includes the following steps: preparing materials according to the elemental composition of the self-lubricating cemented carbide coating, mixing the various raw materials, and obtaining spray powder by spray granulation; spraying the spray powder by supersonic flame to obtain a coating.

[0015] Supersonic flame spraying was used, and the process parameters were: air flow rate 104psi, propane flow rate 97psi, spraying distance 180mm-220mm, and powder delivery efficiency 7.4.

[0016] In the above-mentioned preparation process, the supersonic flame is used for spraying, and the process parameters are: air flow rate 107 psi, propane flow rate 91 psi, spraying distance 220 mm, and powder delivery efficiency 7.4.

[0017] Compared with the prior art, the present invention has the following beneficial effects: The present invention provides a self-lubricating cemented carbide coating, which partially replaces WC with cheap carbides Cr3C2 and TiC, and partially replaces Co with cheap bonding phase Ni, thereby reducing the cost of raw materials while ensuring performance, thereby reducing its production cost as a whole, making large-scale application possible; and by adding a self-lubricating phase and exploring its optimal addition ratio, the friction coefficient is reduced and the wear resistance and friction reduction performance of the cemented carbide coating is improved. At the same time, the present invention provides an optimal preparation process for the self-lubricating cemented carbide coating, and obtains a coating with the highest spraying efficiency and the best performance. BRIEF DESCRIPTION OF THE DRAWINGS

[0018] The present invention is further described below in conjunction with the accompanying drawings and embodiments.

[0019] Figure 1 This is a cross-sectional image of the cemented carbide coating described in Example 1 of the present invention under a 5KX scanning electron microscope (scale is 2 μm); Figure 2 This is a cross-sectional image of the cemented carbide coating described in Example 2 of the present invention under a 5KX scanning electron microscope (scale is 2 μm); Figure 3 This is a cross-sectional image of the cemented carbide coating described in Example 3 of the present invention under a 5KX scanning electron microscope (scale is 2 μm); Figure 4 This is a cross-sectional image of the cemented carbide coating described in Example 4 of the present invention under a 5KX scanning electron microscope (scale is 2 μm); Figure 5 This is a cross-sectional image of the cemented carbide coating described in Example 5 of the present invention under a 5KX scanning electron microscope (scale is 1 μm); Figure 6 This is a cross-sectional image of the cemented carbide coating described in Example 6 of the present invention under a 5KX scanning electron microscope (scale is 3 μm); Figure 7 This is a cross-sectional image of the cemented carbide coating described in Example 7 of the present invention under a 5KX scanning electron microscope (scale is 2 μm); Figure 8 This is a cross-sectional image of the cemented carbide coating described in Example 8 of the present invention under a 5KX scanning electron microscope (scale is 2 μm); Fig. 9 This is a cross-sectional image of the cemented carbide coating described in Example 9 of the present invention under a 5KX scanning electron microscope (scale is 2 μm); Fig.10 for Figure 5 Energy spectrum analysis of coating points at positions 1, 2, 3 and 4 (scale is 1μm); Fig.11A This is a morphology image of the cemented carbide coating described in Example 1 of the present invention after a friction and wear test under a 500X electron microscope (scale is 20 μm); Fig. 11B This is a morphology image of the cemented carbide coating described in Example 1 of the present invention after a friction and wear test under a 5KX electron microscope (scale is 2 μm); Fig. 12A This is a morphology image of the cemented carbide coating described in Example 2 of the present invention after a friction and wear test under a 500X electron microscope (scale is 100 μm); Fig. 12B This is a morphology image of the cemented carbide coating described in Example 2 of the present invention after a friction and wear test under a 5KX electron microscope (scale is 2 μm); Fig.13A This is a morphology image of the cemented carbide coating described in Example 3 of the present invention after a friction and wear test under a 500X electron microscope (scale is 20 μm); Fig. 13B This is a morphology image of the cemented carbide coating described in Example 3 of the present invention after a friction and wear test under a 5KX electron microscope (scale is 2 μm); Fig.14A This is a morphology image of the cemented carbide coating described in Example 4 of the present invention after a friction and wear test under a 500X electron microscope (scale is 20 μm); Fig. 14B This is a morphology image of the cemented carbide coating described in Example 4 of the present invention after a friction and wear test under a 5KX electron microscope (scale is 2 μm); Fig.15A This is a morphology image of the cemented carbide coating described in Example 5 of the present invention after a friction and wear test under a 500X electron microscope (scale is 100 μm); Fig. 15BThis is a morphology image of the cemented carbide coating described in Example 5 of the present invention after a friction and wear test under a 5KX electron microscope (scale is 2 μm); Fig.16A This is a morphology image of the cemented carbide coating described in Example 6 of the present invention after a friction and wear test under a 500X electron microscope (scale is 20 μm); Fig. 16B This is a morphology image of the cemented carbide coating described in Example 6 of the present invention after a friction and wear test under a 5KX electron microscope (scale is 2 μm); Fig.17A This is a morphology image of the cemented carbide coating described in Example 7 of the present invention after a friction and wear test under a 500X electron microscope (scale is 20 μm); Fig. 17B This is a morphology image of the cemented carbide coating described in Example 7 of the present invention after a friction and wear test under a 5KX electron microscope (scale is 2 μm); Fig.18A This is a morphology image of the cemented carbide coating described in Example 8 of the present invention after a friction and wear test under a 500X electron microscope (scale is 20 μm); Fig.18B This is a morphology image of the cemented carbide coating described in Example 8 of the present invention after a friction and wear test under a 5KX electron microscope (scale is 2 μm); Fig.19A This is a morphology image of the cemented carbide coating described in Example 9 of the present invention after a friction and wear test under a 500X electron microscope (scale is 20 μm); Fig.19B This is a morphology image of the cemented carbide coating described in Example 9 of the present invention after a friction and wear test under a 5KX electron microscope (scale is 2 μm); Fig. 20 The morphology and local magnification of the s-1 coating, s-2 coating and s-3 coating under a 500X electron microscope (the scale of the morphology diagram is 10μm); Figure 21-23 These are the porosity images of s-1 coating, s-2 coating and s-3 coating after being processed by ImageJ software; Fig.24 It is the real-time curve of friction coefficient of self-lubricating coating; Fig.25 Polarization curve of self-lubricating coating. DETAILED DESCRIPTION

[0020] The technical solutions in the embodiments of the present invention will be described clearly and completely below in conjunction with the accompanying drawings in the embodiments of the present invention.

[0021] The selection of powder raw materials is mainly to reduce costs while meeting performance requirements. The principle of the present invention is to partially replace Co with Ni and partially replace WC with TiC and Cr3C2 in the selection of hard phases, and design a new coating system of WC-Cr3C2-TiC-Co-Ni-Cr system. Based on the above-mentioned principles, the present invention provides a self-lubricating cemented carbide coating. Different from the prior art, the self-lubricating cemented carbide coating provided by the present invention comprises an alloy coating arranged on the surface of a steel material, including the following elements in a mass percentage content (Wt / %): WC: 20-30%, TiC: 0-10%, Co: 1-5%, Ni: 10-14%, Cr: 1-5%, and the remainder is Cr3C2.

[0022] Preferably, the self-lubricating cemented carbide coating comprises the following elements in weight percent (Wt / %): WC: 20%, h-BN: 1-3%, Co: 1%, Ni: 14%, Cr: 5%, and the remainder is Cr3C2.

[0023] Among them, h-BN is hexagonal boron nitride, which has lubricity in a wide temperature range.

[0024] Specifically, the self-lubricating cemented carbide coating proposed by the present invention comprises an alloy coating disposed on the surface of a steel material, comprising the following elements in a weight percent content (wt / %), and the specific compositions of each embodiment and each comparative example are as described in Table 1 below: On the other hand, a preparation process of a self-lubricating cemented carbide coating includes the following steps: preparing materials according to the elemental composition of the self-lubricating cemented carbide coating, mixing the raw materials, and then ball milling, spray granulation, high-temperature sintering, and supersonic flame spraying; obtaining spray powder by spray granulation; and spraying the spray powder by supersonic flame to obtain a coating.

[0025] The process parameters for spray granulation are shown in Table 2 below: The process parameters for high temperature sintering are: sintering at 1120°C using a molybdenum wire furnace.

[0026] Supersonic flame spraying was carried out, and the process parameters were: air flow rate 104psi, propane flow rate 97psi, spraying distance 180mm-220mm, and powder delivery efficiency 7.4.

[0027] Preferably, the supersonic flame is used for spraying, and the process parameters are: air flow rate 107psi, propane flow rate 91psi, spraying distance 220mm, and powder delivery efficiency 7.4.

[0028] Embodiment 1: The self-lubricating cemented carbide coating includes the following elements in weight percent (Wt / %): WC: 20%, TiC: 0%, Co: 1%, Ni: 10%, Cr: 5%, and the balance is Cr3C2.

[0029] The specific preparation process of the self-lubricating cemented carbide coating is as follows: prepare the materials according to the elemental composition of the self-lubricating cemented carbide coating, mix the various raw materials, and then perform ball milling, spray granulation, high-temperature sintering, and supersonic flame spraying; obtain the spray powder by spray granulation; spray the spray powder by supersonic flame to obtain the coating.

[0030] Among them, the process parameters for spray granulation are shown in Table 2 above: The process parameters for high temperature sintering are: sintering at 1120°C using a molybdenum wire furnace.

[0031] Supersonic flame spraying was carried out, and the process parameters were: air flow rate 107psi, propane flow rate 91psi, spraying distance 220mm, and powder delivery efficiency 7.4.

[0032] The prepared self-lubricating cemented carbide coating was subjected to performance testing, and the results are shown in Table 3 below: Embodiment 2: The self-lubricating cemented carbide coating includes the following elements in weight percent (Wt / %): WC: 20%, TiC: 5%, Co: 3%, Ni: 12%, Cr: 5%, and the balance is Cr3C2.

[0033] The preparation process is the same as that of Example 1. The prepared self-lubricating cemented carbide coating was tested for performance, and the results are shown in Table 4 below: Embodiment 3: The self-lubricating cemented carbide coating includes the following elements in weight percent (Wt / %): WC: 20%, TiC: 10%, Co: 5%, Ni: 14%, Cr: 5%, and the balance is Cr3C2.

[0034] The preparation process is the same as that of Example 1. The prepared self-lubricating cemented carbide coating was tested for performance, and the results are shown in Table 5 below: Embodiment 4: The self-lubricating cemented carbide coating includes the following elements in weight percent (Wt / %): WC: 25%, TiC: 0%, Co: 3%, Ni: 14%, Cr: 5%, and the balance is Cr3C2.

[0035] The preparation process is the same as that of Example 1. The prepared self-lubricating cemented carbide coating was tested for performance, and the results are shown in Table 6 below: Embodiment 5: The self-lubricating cemented carbide coating includes the following elements in weight percent (Wt / %): WC: 25%, TiC: 5%, Co: 5%, Ni: 10%, Cr: 5%, and the balance is Cr3C2.

[0036] The preparation process is the same as that of Example 1. The prepared self-lubricating cemented carbide coating was tested for performance, and the results are shown in Table 7 below: Embodiment 6: The self-lubricating cemented carbide coating includes the following elements in weight percent (Wt / %): WC: 25%, TiC: 10%, Co: 1%, Ni: 12%, Cr: 5%, and the balance is Cr3C2. The preparation process is the same as that of Example 1. The prepared self-lubricating cemented carbide coating was tested for performance, and the results are shown in Table 8 below: Embodiment 7: The self-lubricating cemented carbide coating includes the following elements in weight percent (Wt / %): WC: 30%, TiC: 0%, Co: 5%, Ni: 12%, Cr: 5%, and the balance is Cr3C2. The preparation process is the same as that of Example 1. The prepared self-lubricating cemented carbide coating was tested for performance, and the results are shown in Table 9 below: Embodiment 8: The self-lubricating cemented carbide coating includes the following elements in weight percent (wt / %): WC: 30%, TiC: 5%, Co: 1%, Ni: 14%, Cr: 5%, and the balance is Cr3C2. The preparation process is the same as that of Example 1. The prepared self-lubricating cemented carbide coating was tested for performance, and the results are shown in Table 10 below: Embodiment 9: The self-lubricating cemented carbide coating includes the following elements in weight percent (Wt / %): WC: 30%, TiC: 10%, Co: 3%, Ni: 10%, Cr: 5%, and the balance is Cr3C2. The preparation process is the same as that of Example 1. The prepared self-lubricating cemented carbide coating was tested for performance, and the results are shown in Table 11 below: Figure 1-Figure 9The cross-sectional images of the coatings of Examples 1-9 under a 5KX scanning electron microscope show that there are four main regions: light gray, dark gray, white, and black. Figure 5 , a cross-sectional image of the coating of Example 5 under a 5KX scanning electron microscope, and Fig.10 The energy spectrum analysis of Example 5 shown in the figure shows that the light gray position (position 1) has a high distribution of Co, Cr, Ni and other binder phases, and surrounds other phases in a network shape, and is distributed in the interphases of other colors, indicating that this position is mainly the area where the binder phase is distributed. The dark gray position (position 2) with a large block distribution has a very high content of Cr and W elements, indicating that this position is mainly composed of Cr carbides Cr3C2, Cr7C3 and Cr 23 C6. The white position (position 3) has more W elements, indicating that this position is a hard phase WC with a polygonal distribution. The black position (position 4) energy spectrum shows that there is a large distribution of Ti elements, which can be determined to be a hard phase TiC.

[0037] Specifically in Fig.10 In the spectrum analysis, the horizontal axis is the energy axis, the unit is kiloelectron volts (KeV); the vertical axis is the intensity axis, which represents the intensity of X-ray photons, the unit is pulse counts (counts); At room temperature, the wear resistance of each group of coatings is tested by sliding friction method. By studying the wear mechanism and wear conditions, the coating component with the best wear resistance is determined. The friction coefficient can reflect the friction performance of the coating to a certain extent. The smaller the friction coefficient, the better the wear resistance, and vice versa.

[0038] After the friction and wear experiment, the wear scar morphology was observed using a scanning electron microscope. Figures 11A-19BThe wear scar morphology of the coating of Example 1-Example 9 under a 500X electron microscope (magnification 500 times) and a 5KX electron microscope (magnification 5000 times) can be seen from the morphology. It can be seen that there is flaking and curling at the wear scar. The flaking phenomenon is mainly caused by fatigue wear. During the wear process, the coating is subjected to the shear force, and the shear deformation accumulates a large amount of dislocation accumulation on the coating surface to form cracks. When the cracks accumulate to a certain extent and reach the critical point, the coating surface will flak off. Under a 5KX electron microscope, a large number of lumpy coatings that have fallen off and coatings that are about to fall off, as well as a large number of cracks can be seen in the morphology of the wear scar magnified 5000 times. And the cracks occur at the junction of the dark gray hard phase and the light gray bonding phase around it, and first occur on the bonding phase. A large amount of bonding phase is pulled out to form wear debris, which is also reflected in the electron microscope photos. When the bonding phase is severely damaged, the large hard phase particles will lose support and eventually be pulled out, causing coating damage. This shows that the staggered distribution state of the hard phase and the bonding phase and the combination of the two are particularly important for the friction resistance of the coating, and the porosity in the hard phase and the bonding phase in the coating has an important influence on its wear resistance.

[0039] In the coating morphology pictures of Examples 2, 3, 5, 6, 7 and 8, it can be seen that the surface coating is rolled up. This is mainly because the hard phase in the coating and the interaction with the grinding ball produce a cutting effect on the coating during the friction process, resulting in plastic deformation. The scratching effect of the grinding debris forms scratches on the coating surface and causes the coating surface to fall off. The main mechanism of this coating wear is abrasive wear.

[0040] In addition, abrasives accumulate at the edges of the wear marks of each coating, and the heights on both sides of the scratch edges are higher than the middle of the wear marks. This is mainly because during the friction process, the friction pair will continuously push the wear debris, which eventually accumulates at the edges of the wear marks, forming wear debris accumulation.

[0041] Among them, in this application, the hardness test of the coating uses a microhardness tester to measure the substrate and the coating cross section in turn. In all samples, 15 points are selected at equal intervals on the surface and cross section, and records are made. The data are summarized and the average value is taken as the measurement result.

[0042] The coating porosity was tested by using image analysis method to measure the porosity, and ImagePro-Plus software was used to identify and statistically calculate the porosity of the coating cross section.

[0043] Friction and wear test, using a high temperature friction and wear tester to examine the wear resistance of the coating. After the friction and wear test, the wear and friction of the coating was observed using SEM, and the possible wear mechanism was inferred through the secondary electron scanning image taken. Then, the LEXTOLS4000 laser confocal microscope produced by Olympus was used to measure the friction track to obtain a two-dimensional scratch profile and a three-dimensional wear scar map.

[0044] The corrosion resistance test of the coating was carried out using the tensile test method of the bonded specimen in accordance with the ASTM C633-01 standard.

[0045] Comparative Example 1 The self-lubricating cemented carbide coating includes the following elements in weight percent (Wt / %): WC: 25%, TiC: 0%, Co: 20%, Ni: 0%, Cr: 0%, and the balance is Cr3C2.

[0046] The preparation process is the same as that of Example 1. The average wear rate and average friction coefficient of the prepared self-lubricating cemented carbide coating were tested. The results are as follows: average wear rate 12.5*10 -9 mm 3 ·N -1 ·m -1 , the average friction coefficient is 0.54.

[0047] Comparative Example 2 The self-lubricating cemented carbide coating includes the following elements in weight percent (Wt / %): WC: 25%, TiC: 0%, Co: 0%, Ni: 20%, Cr: 0%, and the balance is Cr3C2.

[0048] The preparation process is the same as that of Example 1. The average wear rate and average friction coefficient of the prepared self-lubricating cemented carbide coating were tested. The results are as follows: the average wear rate is 13.8*10 -9 mm 3 ·N -1 ·m -1 , the average friction coefficient is 0.53.

[0049] Comparative Example 3 The self-lubricating cemented carbide coating includes the following elements in weight percent (Wt / %): WC: 25%, TiC: 0%, Co: 0%, Ni: 0%, Cr: 20%, and the balance is Cr3C2.

[0050] The preparation process is the same as that of Example 1. The average wear rate and average friction coefficient of the prepared self-lubricating cemented carbide coating were tested. The results are as follows: the average wear rate is 14.7*10 -9 mm 3 ·N -1 ·m-1 , the average friction coefficient is 0.56.

[0051] After the friction and wear experiment, the optimal formula was found by experimental analysis based on the wear volume. As shown in Table 13, the optimal coating composition formula was explored based on the experimental results of the orthogonal experiment with 4 factors and 3 levels. In Table 12, A, B, C, and D represent WC, TiC, Co, and Ni, and 1, 2, and 3 represent the corresponding composition levels of WC, TiC, Co, and Ni, respectively.

[0052] First, we calculated the sum of the average wear rates of each factor (A, B, C, D) at three different levels, and recorded them as K1, K2, and K3. By comparative calculation, considering only the average wear rate, the minimum arithmetic mean of A corresponds to level 1, the minimum arithmetic mean of B corresponds to level 1, the minimum arithmetic mean of C corresponds to level 1, and the minimum arithmetic mean of D corresponds to level 3. Therefore, the best wear-resistant component is A1B1C1D3, and the ratio of the best components is shown in Table 14. Since there is no formula with this ratio in the experimental group, a verification test is needed to verify the results.

[0053] According to Table 14, the composition of the best coating with average wear rate after orthogonal analysis is 20WC-59Cr3C2-Co-5Cr-14Ni. According to this coating formula, the coating (verification group) was prepared, and its various properties were tested as shown in Table 15 below; It can be seen that the average friction coefficient of the verification group is 0.42. The average wear area of ​​the cross section of the verification group is 1113.38 μm 2 , which is smaller than 1160.08 μm of the coating in Example 1 with the smallest average cross-sectional wear area in the experimental group. 2 The wear rate of the verification group is 1.84*10 -9 mm 3 ·N -1 ·m -1 , which is less than 1.92*10 of the coating in Example 1 with the lowest wear rate in the experimental group. -9 mm 3 ·N -1 ·m -1 The wear rate decreased by 4.20% compared with the coating in Example 1.

[0054] Example 10 Self-lubricating cemented carbide coating, h-BN phase is selected as the self-lubricating phase, and they are listed as s-1 coating, s-2 coating, and s-3 coating; wherein, s-1 coating, s-2 coating, and s-3 coating are doped into the cemented carbide coating by 1%, 2%, and 3%, respectively, to improve the wear resistance of the coating, and the preparation process of s-1 coating, s-2 coating, and s-3 coating is consistent with that in Example 1; The raw material ratios of the s-1 coating, s-2 coating, and s-3 coating are shown in Table 16 below: Fig. 20 The morphology and partial magnification of the S-1 coating, S-2 coating and S-3 coating under 1000 times scanning electron microscope. It can be found that obvious defects such as holes and cracks can be seen in the 1000 times magnified morphology and partial magnification, especially in the morphology of the S-3 coating. It can also be found that holes and cracks are generally located at the junction of the hard phase and the bonding phase, which will have an adverse effect on the hardness, toughness, wear resistance and corrosion resistance of the coating.

[0055] Figure 21-23 These are the porosity images of the s-1 coating, s-2 coating, and s-3 coating after being processed by ImageJ software. From the distribution of the porosity of the self-lubricating coating, the porosity of the s-1 coating is the lowest, at 0.25%, which is at a lower level than the coating without the addition of the self-lubricating phase. The porosity of the s-2 coating increased to 0.55%, while the porosity of the s-3 coating increased significantly to 1.55%, which is at a higher level than the coating without the addition of the self-lubricating phase. It is verified that the doping of h-BN has an important influence on the density of the coating, and the porosity of the coating will increase with the increase of the lubricating phase content.

[0056] As for the microhardness of the coating, the microhardness of the s-1 coating is 1163.12 HV, which is greater than the 1110.67 HV of the non-lubricating phase verification coating. However, the microhardness of the s-2 coating has decreased to varying degrees compared with the s-1 coating and the s-3 coating. This is mainly because the s-2 coating and the s-3 coating have more porosity, which affects the microhardness of the coating.

[0057] Fig.24The real-time curve of the friction coefficient of the self-lubricating coating, the horizontal axis is time, the unit is min, and the vertical axis is the friction coefficient. From the real-time curve of the friction coefficient of the self-lubricating coating, it can be seen that its fluctuation trend is consistent with the law of the friction coefficient in the previous experiment. When friction occurs, the friction coefficient increases rapidly to a certain order of magnitude, followed by a small drop, and continues to fluctuate for about 5 minutes, and then fluctuates slightly within a certain range. From the real-time curve, it can be seen that the friction coefficient of the s-1 coating is the largest, followed by the s-3 coating, and the s-2 coating is the smallest. In terms of the average friction coefficient, the s-1 coating is 0.32, the s-2 coating is 0.27, and the s-3 coating is 0.29. Compared with the average friction coefficient of the coating without a lubricating phase ranging from 0.30-0.61, the lubricating phase will reduce the friction coefficient to some extent. The average wear area of ​​the cross section of the s-3 coating is 1299.21μm 2 The wear rate is 2.03 * 10 -9 mm 3 ·N -1 ·m -1 The average wear area of ​​the cross section of the s-2 coating is 890.29 μm 2 The wear rate is 1.47*10 - 9 mm 3 ·N -1 ·m -1 The average wear area of ​​the cross section of the s-1 coating is 1025.69 μm 2 The wear rate is 1.69*10 -9 mm 3 ·N -1 ·m -1 The wear rate of the s-2 coating decreased by 20.10% compared with the non-lubricating phase verification coating, and the wear rate of the s-2 coating decreased by 8.15% compared with the non-lubricating phase verification coating. The wear rate of the s-3 coating increased slightly compared with the non-lubricating phase verification coating.

[0058] Fig.25 This is the polarization curve of the self-lubricating coating. The horizontal axis is the current in A, and the vertical axis is the voltage in V. The self-corrosion potential of the coating is -0.54 V, and the corrosion current density is 1.73 μA·cm -2 The self-corrosion potential of the s-2 coating is -0.48 V, and the corrosion current density is 1.86 μA·cm -2 The self-corrosion potential of the s-3 coating is -0.71 V, and the corrosion current density is 5.25 μA·cm -2 The corrosion current density of the s-3 coating is the largest, mainly because it has more holes and cracks.

[0059] (1) The doping of h-BN will have an adverse effect on the compactness of the coating. As the doping ratio increases, the porosity and cracks in the coating will increase.

[0060] (2) The reason why the self-lubricating phase can reduce the friction coefficient and wear rate is that it can form a lubricating film between the friction pair and the coating surface, so that the wear process can only exist in the form of abrasion wear, greatly reducing the friction coefficient and wear rate.

[0061] (3) Due to the high melting point of h-BN, h-BN can still partially exist in the sprayed coating after high-temperature burning during supersonic flame spraying.

[0062] (4) h-BN doped with 2% has the lowest wear rate, and the average wear area of ​​the cross section is 890.29 μm 2 The wear rate is 1.47*10 -9 mm 3 ·N -1 ·m -1 The wear rate of the coating decreased by 20.10% compared with the coating without lubrication phase verification.

[0063] The present invention optimizes the process parameters through orthogonal experiments, selects the best process parameters under different standards, and conducts verification tests on the process parameters with the best comprehensive scores. The verification experiments prove that the coating has better performance under the process parameters of the present application. The relevant summary is as follows: (1) The order of the influence of process parameters on the score is: air flow > propane pressure > spray distance > powder delivery efficiency. The order of the influence of process parameters on particle temperature is: propane > air > spray distance > powder delivery efficiency. The order of the influence of process parameters on particle velocity is: spray distance > air > powder delivery efficiency > propane.

[0064] (2) Taking the comprehensive score as the main evaluation criterion, the best process parameters are: air flow rate 104psi, propane flow rate 97psi, spray distance 220mm, and powder delivery efficiency 7.4. Taking the particle temperature score as the main evaluation criterion, the best process parameters are: air flow rate 104psi, propane flow rate 97psi, spray distance 180mm, and powder delivery efficiency 7.4. Taking the particle velocity score as the main evaluation criterion, the best process parameters are: air flow rate 107psi, propane flow rate 91psi, spray distance 220mm, and powder delivery efficiency 7.4.

[0065] (3) Under the preparation process of the present application, with the score as the main evaluation criterion, the score calculated by particle temperature and velocity is 832.70, which is greater than the maximum 824.57 in the orthogonal experiment. With the particle temperature as the main evaluation criterion, the particle temperature is tested to be 1500°C, which is greater than the maximum 1470°C in the orthogonal experiment. When the particle velocity is the main evaluation criterion, the particle velocity is tested to be 1021m / s, which is also greater than the maximum particle velocity of 1000m / s in the orthogonal experiment.

[0066] (4) In the process parameter verification test with the best score, the coating had very good density and the porosity was only 0.11%, a decrease of 47.61%.

[0067] (5) The hardness of the coating verified by process parameters was also slightly improved, reaching 1192.63 HV, an increase of 2.54% compared to the highest hardness without parameter optimization.

[0068] (6) The average friction coefficient of the process verification coating is 0.25, which is a decrease of 7.40%. The average wear area of ​​the cross section is 792.56 μm 2 The wear rate is 1.31*10 -9 mm 3 ·N -1 ·m -1 Compared with the wear rate of s-2 coating without parameter optimization, the wear rate is 1.47*10 -9 mm 3 ·N -1 ·m -1 , the wear rate decreased by 10.75%.

[0069] (7) Process parameter verification: the self-corrosion potential of the coating is -0.46 V and the corrosion current density is 0.72 μA·cm -2 Compared with the minimum 0.90μA·cm in the non-process optimized coating -2 , down 20.00%.

[0070] The above is only a specific embodiment of the present invention, but the protection scope of the present invention is not limited thereto. Any person skilled in the art can easily think of changes or substitutions within the technical scope disclosed by the present invention, which should be included in the protection scope of the present invention. Therefore, the protection scope of the present invention should be based on the protection scope of the claims.

Claims

1. A self-lubricating cemented carbide coating, characterized in that: Its composition includes an alloy coating arranged on the surface of the steel material, including the following elements in percent by mass: WC: 20-30%, TiC: 0-10%, Co: 1-5%, Ni: 10-14%, Cr: 1-5%, and the balance is Cr3C2.

2. The self-lubricating cemented carbide coating according to claim 1, characterized in that: The alloy coating comprises a cemented carbide phase and a cobalt-chromium-nickel bonding phase, and the cobalt-chromium-nickel bonding phase surrounds the cemented carbide phase in a network shape.

3. The self-lubricating cemented carbide coating according to claim 1, characterized in that: The alloy coating comprises the following elements in percentage by mass: WC: 20%, Co: 1%, Ni: 10%, Cr: 5%, and the remainder is Cr3C2.

4. The self-lubricating cemented carbide coating according to claim 1, characterized in that: The alloy coating includes the following elements in percentage by mass: WC: 25%, Co: 3%, Ni: 14%, Cr: 5%, and the remainder is Cr3C2.

5. The self-lubricating cemented carbide coating according to claim 1, characterized in that: The alloy coating comprises the following elements in percentage by mass: WC: 25%, TiC: 10%, Co: 1%, Ni: 12%, Cr: 5%, and the remainder is Cr3C2.

6. The self-lubricating cemented carbide coating according to claim 1, characterized in that: The alloy coating includes the following elements in percentage by mass: WC: 30%, TiC: 5%, Co: 1%, Ni: 14%, Cr: 5%, and the remainder is Cr3C2.

7. The self-lubricating cemented carbide coating according to claim 1, characterized in that: The alloy coating includes the following elements in percentage by mass: WC: 20%, Co: 1%, Ni: 14%, and the remainder is Cr3C2.

8. The self-lubricating cemented carbide coating according to claim 1, characterized in that: The alloy coating comprises the following elements in percentage by mass: WC: 20%, h-BN: 1-3%, Co: 1%, Ni: 14%, Cr: 5%, and the remainder is Cr3C2.

9. A process for preparing a self-lubricating cemented carbide coating, characterized in that: The following steps are involved: The materials are prepared according to the element composition of the self-lubricating cemented carbide coating, and after mixing the raw materials, spray granulation is performed to obtain the spray powder; The spray powder is sprayed by supersonic flame to produce the coating; Supersonic flame spraying was used, and the process parameters were: air flow rate 104psi, propane flow rate 97psi, spraying distance 180mm-220mm, and powder delivery efficiency 7.

4.

10. The preparation process according to claim 9, characterized in that: The supersonic flame was used for spraying, and the process parameters were: air flow rate 107 psi, propane flow rate 91 psi, spraying distance 220 mm, and powder delivery efficiency 7.4.

Citation Information

Patent Citations

  • Fe / Ni-based carbide alloy coating cutter material for cutting rolled steel and preparation thereof

    CN101301686A

  • Hypersonic flame spraying process for self-lubricating wear-resistant coating

    CN101736279A

  • Solid lubricating high-temperature anti-wearing powder composition and preparation method of compound coating of composition

    CN102836996A

  • Heat-resistant steel structure hard alloy and preparation method thereof

    CN104328322A

  • Surface layer cobalt-rich cubic-phase-free gradient cemented carbide

    CN109680196A