Large-area sulfide electrode for catalyzing water electrolysis and preparation method of large-area sulfide electrode
By spraying and calcining the sulfide electrode on the metal substrate, the problems of harsh sulfide electrode synthesis conditions and low raw material utilization in the prior art are solved, efficient catalytic water electrolysis and the preparation of large-area electrodes are achieved, and catalysis is improved Activity and binding power.
Patent Information
- Application Number
- CN202411182960.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-27
- Publication Date
- 2024-11-22
- Estimated Expiration
- 2044-08-27
AI Technical Summary
In the catalytic water electrolysis, the synthesis conditions of sulfide electrodes are harsh, especially hydrothermal method and vapor deposition method, which require high temperature and high pressure or inert atmosphere, resulting in low raw material utilization and limited electrode base area, making it difficult to prepare large-area electrodes. .
Using ethanol as solvent, the sulfur source, reducing agent and metal salt are prepared into a mixed solution, sprayed onto the metal substrate in the heating environment, and calcined under vacuum, control the temperature and spray speed, and form a tight sulfide electrode to improve Raw material utilization and electrode area.
It achieves efficient catalytic water electrolysis, has better catalytic activity than traditional methods, and has strong binding force with metal substrates. It is suitable for large-area electrode preparation, reducing the preparation cost and environmental impact.
Smart Images

Figure CN118996484A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a large-area sulfide electrode for catalyzing water electrolysis and a preparation method thereof, belonging to the technical field of hydrogen energy material preparation. Background Art
[0002] With the rapid development of society, the rate of energy consumption is increasing. Compared with traditional energy, which produces a large amount of carbon dioxide and harmful substances during use, hydrogen only produces water after use, which is clean, environmentally friendly and pollution-free. In addition, hydrogen can be obtained in large quantities by coupling photovoltaic power generation with water electrolysis to produce hydrogen. Therefore, vigorously developing water electrolysis hydrogen production technology is an important strategy to achieve carbon emission reduction.
[0003] In the process of water electrolysis, the oxidation process at the anode end involves four-electron transfer, and the reaction rate is lower than that at the cathode end, so it becomes a key part that restricts the reaction rate of water electrolysis. In recent years, many sulfides have shown good catalytic water electrolysis oxygen decomposition activity, but the synthesis conditions of sulfides are relatively harsh. When using the hydrothermal method for preparation, high temperature and high pressure conditions above 150 degrees Celsius are usually required. In addition, the treatment of waste liquid after the hydrothermal method is also a major problem, which is not suitable for large-scale production and preparation. Many researchers use high-temperature vapor deposition to prepare sulfides, but this method needs to be carried out in an inert atmosphere, and the sulfur source needs to be driven by the gas to purge the sample all the time, resulting in a waste of raw materials. In addition, the area of the electrode substrate that can be accommodated by the tubular furnace is limited, and it is not suitable for the preparation of large-area electrode materials. Summary of the invention
[0004] In order to overcome the deficiencies of the prior art, the present invention provides a large-area sulfide electrode for catalytic water electrolysis and a preparation method thereof, which has high raw material utilization and a large electrode base area.
[0005] The technical solution adopted by the present invention to solve its technical problem is: In a first aspect, the present application provides a method for preparing a large-area sulfide electrode for catalytic water electrolysis, comprising the following steps: Using ethanol as solvent, a sulfur source, a reducing agent and a metal salt are prepared into a mixed solution; the metal salt is at least one of a nickel salt and an iron salt; Placing the metal substrate in a heating environment, spraying the mixed solution onto the metal substrate while volatilizing the mixed solution until the mixed solution is completely volatilized; The metal substrate is calcined under a vacuum environment, and after natural cooling, the large-area sulfide electrode for catalyzing water electrolysis is obtained.
[0006] The large-area sulfide electrode preparation method for catalytic water electrolysis provided in the present application has a high raw material utilization rate, can accurately control the ratio and content of the metal salt and sulfur source attached to the metal substrate, and can form a compact sulfide electrode on the metal substrate simply by calcining in a vacuum environment.
[0007] Furthermore, the temperature of the heating environment is 50°C to 100°C. Too high a temperature or too low a temperature is not conducive to uniformly loading the metal salt and the sulfur source on the metal substrate. When the temperature is too high, the sprayed mixed solution evaporates quickly before reaching the metal substrate, and the metal salt and the sulfur source have insufficient adhesion on the metal substrate; when the temperature is too low, the mixed solution evaporates slowly on the metal substrate, and the substances are prone to agglomeration and growth.
[0008] Furthermore, in the step of spraying the mixed solution onto the metal substrate while volatilizing, an intermittent operation is adopted to divide the mixed solution into multiple spray liquids, and after each spray liquid is sprayed, the spray liquid is evaporated before the next spray liquid is sprayed.
[0009] During spraying, the temperature of the metal substrate surface will drop sharply. If the heating temperature of the metal substrate is increased to keep the metal substrate at a high temperature, the ambient temperature will also rise, causing most of the sprayed mixed solution to evaporate in advance. Moreover, continuous volatilization will cause the ethanol vapor pressure above the metal substrate to be large, which is not conducive to the rapid evaporation of the mixed solution. Intermittent operation allows the last sprayed liquid to completely evaporate and fix before the next spraying, which can make the metal substrate have a higher evaporation efficiency of the spray after each spraying, and can also avoid the need to spray at a higher ambient temperature.
[0010] Furthermore, when spraying the liquid, the spraying speed per square centimeter of the metal substrate is 18.5 μL / s~37.2 μL / s, which is conducive to the rapid evaporation of the mixed solution on the metal substrate, reduces the flow of the mixed solution on the metal substrate, and reduces the agglomeration of the mixed solution droplets on the metal substrate due to surface tension.
[0011] Furthermore, the nozzle outlet is 100 mm to 300 mm away from the metal substrate. If the distance is too large, the volatilization time of the mixed solution from the nozzle to the surface of the metal substrate will be increased, and if the distance is too small, it will not be conducive to uniform spraying.
[0012] Furthermore, the step of calcining the metal substrate under a vacuum environment includes: heating to 200° C. to 400° C. at a rate of 2° C. / min to 10° C. / min, and calcining for 0.5 h to 5 h.
[0013] Furthermore, in the step of calcining the metal substrate under a vacuum environment, the vacuum degree of the environment in which the metal substrate is located is below 0.1 bar, which is beneficial to reducing the air in the sulfurization process, avoiding the conversion of sulfides into oxides, and ensuring the electrode performance.
[0014] Furthermore, in the step of preparing a mixed solution of the sulfur source, the reducing agent and the metal salt using ethanol as a solvent, the solution is dissolved by ultrasound for 1 min to 10 min, and the molar ratio of the metal salt: the reducing agent: the sulfur source: the ethanol is 1:0.1~10:0.2~20:500~5000.
[0015] Furthermore, the sulfur source is sulfur powder, thiourea or sodium thiosulfate, the reducing agent is citric acid, sodium citrate or ascorbic acid, the nickel salt is nickel chloride hexahydrate, and the iron salt is ferric chloride hexahydrate.
[0016] In a second aspect, the present application provides a large-area sulfide electrode for catalyzing water electrolysis, which is made by the large-area sulfide electrode preparation method for catalyzing water electrolysis described in the first aspect, has good catalytic activity, and has a strong bonding force with a metal substrate.
[0017] The beneficial effects of the present invention are as follows: the present invention has a high raw material utilization rate, can accurately control the ratio and content of the metal salt and sulfur source attached to the metal substrate, and can form a compact sulfide electrode on the metal substrate after calcination under a vacuum environment. The catalytic water electrolysis oxygen activity of the catalytic electrode is better than that of the sulfide electrode obtained by the traditional hydrothermal method and the vapor deposition method, and has a strong bonding force with the metal substrate, and can be used stably for a long time under standard working conditions.
[0018] Other features and advantages of the present application will be described in the following description, and partly become apparent from the description, or understood by practicing the present application. The purpose and other advantages of the present application can be realized and obtained by the structures particularly pointed out in the written description and the drawings. BRIEF DESCRIPTION OF THE DRAWINGS
[0019] Figure 1 This is a physical picture of the large-area sulfide electrode for catalytic water electrolysis made in Example 1 of the present application.
[0020] Figure 2 , Figure 3 and Figure 4 It is a scanning electron microscope image of the large-area sulfide electrode for catalytic water electrolysis prepared in Example 1 of the present application at different magnifications.
[0021] Figure 5 This is an elemental surface scan of the large-area sulfide electrode for catalytic water electrolysis made in Example 1 of the present application.
[0022] Figure 6 , Figure 7 and Figure 8 These are scanning electron microscope images of the large-area sulfide electrode for catalytic water electrolysis prepared in Example 2 of the present application at different magnifications.
[0023] Fig. 9 This is an elemental surface scan of the large-area sulfide electrode for catalytic water electrolysis made in Example 2 of the present application.
[0024] Fig.10 This is a comparison chart of the electrochemical performance of the large-area sulfide electrode and the Ni mesh electrode for catalytic water electrolysis made in Examples 1 and 2 of the present application.
[0025] Fig.11 It is a comparison chart of the electrochemical performance of the electrodes prepared in Example 1, Control Sample 1 and Control Sample 2.
[0026] Fig.12 This is a comparison chart of the constant current test results of the large-area sulfide electrodes for catalytic water electrolysis made in Examples 1 and 2 of the present application. DETAILED DESCRIPTION
[0027] In order to make the purpose, technical solution and advantages of the embodiments of the present disclosure clearer, the technical solution of the embodiments of the present disclosure is clearly and completely described below. Obviously, the described embodiments are part of the embodiments of the present disclosure, not all of the embodiments. Based on the described embodiments of the present disclosure, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0028] It should be understood that, under the premise of no conflict, any and all embodiments of the present invention can be combined with the technical features in any other embodiment or multiple other embodiments to obtain another embodiment. The present invention includes such a combination to obtain another embodiment.
[0029] Unless otherwise specified, all technical and scientific terms used herein have the standard meaning in the field to which the claimed subject matter belongs. If there are multiple definitions for a term, the definition herein shall prevail.
[0030] Before the date of this application, some researchers used a hydrothermal method to grow a sulfide catalyst layer in situ on a metal substrate, but the hydrothermal method requires a high temperature and high pressure environment, which is not conducive to subsequent scale-up production. At the same time, some researchers also used a tubular furnace to perform chemical vapor deposition on a metal substrate to achieve a sulfurization effect, but the electrode area was limited by the diameter of the tubular furnace, and it was also difficult to scale up production. Moreover, before the date of this application, the preparation of sulfide electrodes had low requirements for raw material utilization. Most of the metal salts in the hydrothermal method remained in the solution, causing a lot of waste. The vapor deposition method requires a large amount of sulfur source and inert gas to continuously contact the metal substrate, increasing the preparation cost. It has been reported in the literature that sulfides have a significant effect on catalyzing the electrolysis of oxygen by water, but there are few reports on the precise regulation and synthesis of large-area sulfides.
[0031] In view of the above problems, the present invention provides a method for preparing a large-area sulfide electrode for catalytic water electrolysis, comprising the following steps: S1: Using ethanol as solvent, a sulfur source, a reducing agent and a metal salt are prepared into a mixed solution. The metal salt is at least one of a nickel salt and an iron salt.
[0032] S2: placing the metal substrate in a heating environment, spraying the mixed solution onto the metal substrate while evaporating the mixed solution until the mixed solution is completely evaporated.
[0033] S3: The metal substrate is calcined in a vacuum environment, and after natural cooling, a large-area sulfide electrode for catalytic water electrolysis is obtained. Specifically, it is a catalytic electrode for the anode end of water electrolysis.
[0034] This method can form a dense sulfide catalyst in situ. The metal elements in the sulfide are in a higher valence state, which can reduce the energy barrier of oxidizing hydroxide and reduce the energy required for electrolysis of water. At the same time, the sulfur ions can be oxidized to high-valence sulfate groups, resisting the corrosion of some negative ions in the alkali solution on the active sites and stabilizing the catalytic activity of the sulfide. The catalyst has good catalytic activity and has a strong binding force with the metal substrate. This method can relatively easily prepare large-area sulfide electrode materials, improve the utilization rate of raw materials, and enhance the activity and stability of the anode in electrolysis of water and oxygen evolution.
[0035] The reducing agent may be citric acid, sodium citrate or ascorbic acid. The preferred reducing agent is a hydroxyl-containing small molecule, which is reducing and slightly acidic, avoids reacting with metal salts to form precipitation, and can buffer the alkaline environment formed by the dissolution of the sulfur source. The reducing agent is citric acid or ascorbic acid, and more preferably, the reducing agent is citric acid.
[0036] The sulfur source may be thiourea, sulfur powder or sodium thiosulfate. Preferably, the sulfur source is thiourea.
[0037] The nickel salt in the metal salt may be nickel chloride hexahydrate or nickel nitrate hexahydrate, and the iron salt may be ferric chloride hexahydrate or ferric nitrate nonahydrate. Nitrates have certain explosion risks and are not as easy to decompose and volatilize as chlorides during calcination. Preferably, the nickel salt is nickel chloride hexahydrate and the iron salt is ferric chloride hexahydrate.
[0038] The metal substrate can be a nickel mesh, nickel foam or nickel fiber felt. Preferably, the metal substrate is a nickel mesh, which is cheap, has excellent conductivity, high mechanical strength, and is resistant to strong alkali corrosion. The specifications of the metal substrate can be, for example, 2cm*2cm or 100cm*100cm.
[0039] When preparing materials in step S1, the molar ratio of the total amount of metal salt to the reducing agent can be 1:0.1-10. Preferably, the molar ratio of the metal salt to the reducing agent is 1:0.5-5.
[0040] The molar ratio of the metal salt to the thiourea may be 1:0.2-20, preferably, the molar ratio of the metal salt to the thiourea may be 1:1-10.
[0041] The molar ratio of the metal salt to the ethanol is 1:500 to 5000. Preferably, the molar ratio of the metal salt to the ethanol is 1:500 to 2000.
[0042] The temperature of the prepared solution is 20°C-30°C, and ultrasound can be used to assist dissolution, and the ultrasound time is 1 minute to 10 minutes.
[0043] The specific operation of step S2 may be, for example: placing the metal substrate on the heating table of the ultrasonic sprayer, transferring the mixed solution into a syringe, preheating the heating table at high temperature for a period of time, and then using the sprayer to evenly and slowly spray the liquid onto the metal substrate until the solution is exhausted, continuing to heat for a period of time, and stopping heating after the solvent is completely evaporated.
[0044] The heating temperature of the heating table is 50℃~100℃, the preheating time is 3 minutes to 20 minutes, and the vertical distance between the spray outlet and the metal substrate is 100mm~300mm. Taking the 18cm*18cm metal substrate as an example, the liquid pushing speed of the syringe is 0.1ml / min-2ml / min, and the entire mixed solution can be sprayed 1 to 5 times (that is, divided into 1 to 5 sprays), and the time spent waiting for the solvent to evaporate each time is 1 minute to 10 minutes.
[0045] In step S3, the calcination temperature is 200°C to 400°C, the temperature rise rate is 2°C / min to 10°C / min, and the holding time is preferably 0.5 to 3 hours. The calcination equipment can be a vacuum oven or a tubular furnace. Preferably, the calcination is directly carried out in a vacuum oven, which can prepare a larger area of sulfide electrodes, with low cost and simple operation.
[0046] Example 1 Cut a nickel mesh of 18cm*18cm and place it on the heating table of the ultrasonic sprayer. Preheat it at 80 degrees Celsius for 5 minutes. The metal salt preparation process is as follows: 1mmol ferric chloride hexahydrate, 1mmol citric acid and 2mmol thiourea are added to 20ml ethanol and ultrasonicated for 5 minutes to obtain a clear solution. Use the ultrasonic sprayer to evenly spray a total of 5mL of solution on the nickel mesh each time. After heating for 5 minutes, continue spraying until all the solution is sprayed.
[0047] The nickel mesh covered with the metal salt and sulfur source coating is transferred to a vacuum oven. After evacuating for half an hour, the temperature is raised from room temperature to 300°C at a rate of 10°C per minute and kept at this temperature for 1 hour. After the end of the heat preservation, the nickel mesh is naturally cooled. The nickel mesh is cleaned with pure water and ethanol and dried naturally to obtain a large-area sulfide electrode for catalytic water electrolysis, which is recorded as FeS electrode. Figure 1 As shown, from Figure 1 It can be seen that the nickel mesh is uniformly loaded with a black catalyst layer. The electrode is observed under a scanning electron microscope. Figures 2 to 4 As shown in the figure, it is proved that the nickel mesh is loaded with a dense coating. The element mapping image analysis (element mapping) of the electrode is performed, and the results are as follows Figure 5 ( Figure 5 As shown in the first picture "Ch1" in the figure (the original scanning electron microscope image), it can be found that Fe and S elements are evenly distributed in the outer catalytic layer.
[0048] Example 2 Cut a nickel mesh of 18cm*18cm and place it on the heating table of the ultrasonic sprayer. Preheat it at 80 degrees Celsius for 5 minutes. The metal salt preparation process is as follows: 1mmol nickel chloride hexahydrate, 1mmol citric acid and 2mmol thiourea are added to 20ml ethanol and ultrasonicated for 5 minutes to obtain a clear solution. Use the ultrasonic sprayer to evenly spray a total of 5mL of solution on the nickel mesh each time. After heating for 5 minutes, continue spraying until all the solution is sprayed.
[0049] The nickel mesh covered with metal salt and sulfur source coating was transferred to a vacuum oven. After evacuation for half an hour, the temperature was raised from room temperature to 300°C at a rate of 10°C per minute and kept at that temperature for 1 hour. After the end of the heat preservation, the nickel mesh was naturally cooled. The nickel mesh was cleaned with pure water and ethanol and dried naturally to obtain a large-area sulfide electrode for catalytic water electrolysis, which was recorded as NiS electrode. The electrode was observed under a scanning electron microscope. Figures 6 to 8 As shown in Figure 2, it is proved that the nickel mesh is loaded with a dense coating. The element distribution image analysis of the electrode is shown in Figure 2. Fig. 9 ( Fig. 9As shown in the first picture (Ch1 in the figure indicates the original SEM image), it can be found that Ni and S elements are evenly distributed in the outer catalyst layer. It should be noted that since the substrate is a nickel mesh, the Ni signal will be more obvious at the nickel mesh position, and the outer Ni signal will appear weaker in contrast.
[0050] Control sample 1 Cut a nickel mesh of 18cm*18cm and place it on the heating table of the ultrasonic sprayer. Preheat it at 80 degrees Celsius for 5 minutes. Add 1mmol of ferric chloride hexahydrate and 1mmol of citric acid to 20ml of ethanol and ultrasonicate for 5 minutes to obtain a clear solution. Use the ultrasonic sprayer to evenly spray a total of 5mL of solution on the nickel mesh each time. After heating for 5 minutes, continue spraying until all the solution is sprayed.
[0051] Weigh 1g of thiourea on a porcelain boat and place it on the upper air outlet of the tube furnace. Cut a 9cm*9cm sample obtained in the first step into a porcelain boat and place it on the lower air outlet of the tube furnace. Encapsulate the tube furnace, evacuate for half an hour, introduce nitrogen until the tube returns to normal pressure, open the gas outlet and connect the tail gas absorption solution. Heat up from room temperature to 300℃ at a rate of 10 degrees Celsius per minute, keep warm for 1 hour, cool naturally after the end of the insulation, clean the nickel mesh with pure water and ethanol, and dry naturally to obtain the FeS-CVD electrode.
[0052] Control sample 2 The sulfide electrodes were prepared using a conventional hydrothermal method.
[0053] Cut a 2cm*5cm copper mesh and put it into a 50ml polytetrafluoroethylene liner. Dissolve 1mmol ferric chloride hexahydrate, 1mmol citric acid and 2mmol thiourea in 20ml ethanol and transfer to the polytetrafluoroethylene liner containing the nickel mesh. After sealing the hydrothermal reactor shell, put it into an oven and heat it at 120 degrees Celsius for 10 hours. After the reaction is completed, cool it naturally, take out the sample, wash it with water and ethanol, and dry it naturally to obtain the FeS-SR electrode control sample.
[0054] The activity of FeS electrode, NiS electrode, FeS-CVD electrode, FeS-SR electrode and pure nickel mesh substrate in electrolysis of water and oxygen evolution was tested. The electrochemical test conditions were: electrode area of 1cm*1cm, 25℃, 1mol / L KOH. The working electrodes were FeS electrode, NiS electrode, FeS-CVD electrode, FeS-SR electrode, pure nickel mesh substrate (only one of them was used each time), the reference electrode was Hg / HgO, and the counter electrode was a platinum sheet electrode. First, a cyclic voltammetry test was performed on the working electrode to achieve the activation effect. The scan range was 0.8V~1.7V vs RHE, and the scan rate was 0.1V / s. The test was stopped when the electrode was stable. Then the electrochemical activity of the electrode was tested using linear scanning voltammetry. The scan range was 1.2V~1.7V vs RHE, and the scan rate was 5mV / s. The results are as follows: Fig.10 and Fig.11 shown.
[0055] from Fig.10 It can be seen that the FeS electrode only needs 377mV overpotential to reach 100mAcm -2 . Slightly better than NiS electrode and much better than pure nickel mesh substrate.
[0056] from Fig.11 It can be seen that the performance of the electrode prepared by the method of the present application is slightly better than that of the vapor deposition method, and the amount of sulfur source used in the present application is much lower than that of the traditional vapor deposition method, which further highlights the superiority of the method of the present application. On the other hand, the vapor deposition method requires the use of a tubular furnace to provide gas transportation conditions, and the tube diameter limits the area of the electrode. The common quartz tube inner diameter is currently about 5cm~15cm, and it is impossible to prepare a large-area sulfide electrode. The electrode made by the hydrothermal method has the worst performance, which may be because the amount of in-situ growth on the substrate is far less than the amount of raw material added, and the catalytic sites are far less than the electrodes in the embodiments of the present application.
[0057] The stability test diagram of FeS electrode and NiS electrode. Constant current test conditions: 25℃, 1mol / LKOH. The working electrode is FeS electrode and NiS electrode (only one of them is used at a time), the counter electrode is platinum sheet, and the current is set to 100mA. The results are as follows Fig.12 As shown, it can be seen that the electrode performance is basically stable within 25 hours.
[0058] The present application adopts liquid phase spraying to volatilize the solvent on the metal substrate and retain a coating containing polymetallic salts and a sulfur source. The metal substrate is pre-attached with a sulfur source, eliminating the need to additionally introduce a sulfur source and an inert gas during high-temperature calcination. The amount of the sulfur source and the ratio of elements can be strictly controlled. This solution is suitable for preparing large-area electrodes, while improving the utilization rate of raw materials, which is beneficial to reducing the cost of preparing large-area electrodes.
[0059] In the description of this specification, the description with reference to the terms "one embodiment", "certain embodiments", "illustrative embodiments", "examples", "specific examples", or "some examples" means that the specific features, structures, materials, or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representation of the above terms does not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials, or characteristics described may be combined in any one or more embodiments or examples in a suitable manner.
[0060] The above is a preferred embodiment of the present invention. It should be pointed out that a person skilled in the art can make several improvements and modifications without departing from the principle of the present invention. These improvements and modifications are also considered to be within the scope of protection of the present invention.
Claims
1. A method for preparing a large-area sulfide electrode for catalytic water electrolysis, characterized in that: The following steps are involved: Using ethanol as solvent, a sulfur source, a reducing agent and a metal salt are prepared into a mixed solution; the metal salt is at least one of a nickel salt and an iron salt; Placing the metal substrate in a heating environment, spraying the mixed solution onto the metal substrate while volatilizing the mixed solution until the mixed solution is completely volatilized; The metal substrate is calcined under a vacuum environment, and after natural cooling, the large-area sulfide electrode for catalyzing water electrolysis is obtained.
2. The method for preparing a large-area sulfide electrode for catalytic water electrolysis according to claim 1, characterized in that: The temperature of the heating environment is 50°C to 100°C.
3. The method for preparing a large-area sulfide electrode for catalytic water electrolysis according to claim 1 or 2, characterized in that: In the step of spraying the mixed solution onto the metal substrate while volatilizing, an intermittent operation is adopted to divide the mixed solution into multiple spray liquids. After each spray liquid is sprayed, the spray liquid is evaporated before spraying the next spray liquid.
4. The method for preparing a large-area sulfide electrode for catalytic water electrolysis according to claim 3, characterized in that: When spraying the spray liquid, the spraying speed per square centimeter of the metal substrate is 18.5 μL / s to 37.2 μL / s.
5. The method for preparing a large-area sulfide electrode for catalytic water electrolysis according to claim 2, characterized in that: The nozzle outlet is 100 mm to 300 mm away from the metal substrate.
6. The method for preparing a large-area sulfide electrode for catalytic water electrolysis according to claim 1, characterized in that: The step of calcining the metal substrate under a vacuum environment comprises: heating to 200° C. to 400° C. at a rate of 2° C. / min to 10° C. / min, and calcining for 0.5 h to 5 h.
7. The method for preparing a large-area sulfide electrode for catalytic water electrolysis according to claim 1, characterized in that: In the step of calcining the metal substrate under a vacuum environment, the vacuum degree of the environment in which the metal substrate is located is below 0.1 bar.
8. The method for preparing a large-area sulfide electrode for catalytic water electrolysis according to claim 1, characterized in that: In the step of preparing a mixed solution by using ethanol as solvent, preparing the sulfur source, the reducing agent and the metal salt, dissolving them by ultrasonication for 1 min to 10 min, and the molar ratio of the metal salt: the reducing agent: the sulfur source: the ethanol is 1: 0.1 to 10: 0.2 to 20: 500 to 5000.
9. The method for preparing a large-area sulfide electrode for catalytic water electrolysis according to claim 1, characterized in that: The sulfur source is sulfur powder, thiourea or sodium thiosulfate, the reducing agent is citric acid, sodium citrate or ascorbic acid, the nickel salt is nickel chloride hexahydrate, and the iron salt is ferric chloride hexahydrate.
10. A large-area sulfide electrode for catalytic water electrolysis, characterized in that: The large-area sulfide electrode for catalytic water electrolysis is prepared by the preparation method of any one of claims 1 to 9.
Citation Information
Patent Citations
Method for preparing CoS electrocatalyst by using ultrasonic spraying technology
CN107744817A
Preparation method and application of metal sulfide
CN109574096A
Bimetal sulfuration integrated electrode with surface modified by square meter grade stainless steel, preparation method and application of bimetal sulfuration integrated electrode
CN118480805A
