Monatomic catalyst-containing electrolytic tank system for preparing glycollate through electro-catalysis of ethylene glycol and method for preparing glycollate through electro-catalysis of ethylene glycol
By using the single-atom catalyst Pd-Ni(OH)x-SAC in the electrolytic cell system for electrocatalyzed ethylene glycol preparation, the Pd distribution is regulated by using Ni2+ vacancy defects of Ni(OH)x and atomic layer deposition method to regulate the Pd distribution to solve the problem of The problem of high cost of precious metal catalysts is achieved, and high electrocatalytic activity and low cost production are achieved.
Patent Information
- Application Number
- CN202411078445.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-07
- Publication Date
- 2024-11-22
AI Technical Summary
In existing electrocatalytic technologies, the high cost and high Pd loading of precious metal Pd or Pt catalysts limit the low-cost mass production of glycolates.
The single-atom catalyst Pd-Ni(OH)x-SAC is used to regulate the growth and distribution of Pd through Ni2+ vacancy defects and atomic layer deposition method of Ni(OH)x, reduce the load of Pd, and improve the electrocatalytic activity.
The electrocatalytic activity is significantly improved under relatively lower Pd load, with a maximum current density of >2A/cm2, reducing the cost of catalyst preparation, and is suitable for industrialization and large-scale promotion.
Smart Images

Figure CN118996492A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the field of electrochemical catalysis technology, and more specifically, to an electrolytic cell system for preparing glycolate from ethylene glycol using a single-atom catalyst and a method for preparing glycolate from ethylene glycol using a single-atom catalyst. Background Art
[0002] As a common chemical raw material, glycolic acid is widely used in many industrial fields, such as chemical cleaning, disinfectants, daily chemicals, biodegradable materials, electroplating surface treatment agents, etc. However, the synthesis cost of glycolic acid is relatively high. The main reason is that the current preparation of industrial glycolic acid starts with chloroacetic acid as the raw material, then esterifies with methanol to produce methyl glycolate, and then purifies by distillation and hydrolysis. The raw material chloroacetic acid is highly toxic and corrosive, belonging to Class 6 hazardous chemicals, so low-cost and large-scale production of glycolic acid has insurmountable difficulties. In the current research, ethylene glycol (or ethylene glycol, a hydrolysis derivative of waste plastic PET) can be converted into sodium glycolate by electrocatalytic oxidation, thereby solving the problem of highly toxic raw materials for the production of glycolic acid. However, the catalyst for converting ethylene glycol into sodium glycolate by electrocatalytic technology is basically a precious metal Pd or Pt catalyst, which has a relatively high content of precious metals and faces the problem of high cost of electrocatalysts. For this reason, it is urgent to develop a new high-activity electrocatalytic ethylene glycol preparation glycolate system to solve the cost problem. Summary of the invention
[0003] One object of the present invention is to provide an electrolytic cell system for electrocatalytically preparing glycolate from ethylene glycol. The electrolytic cell system disclosed in the present invention is used in the electrocatalytic reaction of preparing glycolate from ethylene glycol. It can be found that the electrolytic cell system can exhibit high electrocatalytic activity at a relatively lower Pd loading (the Pd loading of the present invention is 0.1-0.2 mg / cm 2 , conventional Pd nanocatalyst loading>1mg / cm 2 ), maximum current density>2A / cm 2 , compared with the current density of conventional Pd nanocatalysts <1A / cm 2 , the electrocatalytic activity is significantly improved.
[0004] Another object of the present invention is to provide a method for preparing glycolate from ethylene glycol via electrocatalysis.
[0005] In order to achieve the above first object, the present invention adopts the following technical scheme:
[0006] The present invention provides an electrolytic cell system for preparing glycolate from ethylene glycol by electrocatalysis, wherein the electrolytic cell system comprises a working electrode and an alkaline electrolyte containing ethylene glycol; the working electrode comprises a single-atom catalyst Pd-Ni(OH) x -SAC;
[0007] The single-atom catalyst is based on a foamed metal as a conductive substrate, and the single-atom catalyst is based on Ni(OH) x As the main support, the electrocatalyst with single-atom Pd as the guest catalytic center, wherein x is Ni(OH) x Ni 2+ The degree of vacancy defect is 2<x≤2.1.
[0008] In the present invention, using Ni 2+ Vacancy defect Ni(OH) x Inducing single-atom catalyst occupancy and combining it with atomic layer deposition to achieve the growth of Ni(OH) x The single-atom Pd on the surface is regulated to make it grow and distribute evenly, which inhibits Pd-Pd bonding and prevents Pd atomic agglomeration. At the same time, the Pd loading amount is controlled by regulating the number of deposition cycles to ensure high electrocatalytic activity even at a relatively lower Pd loading amount, thereby reducing the preparation cost of the catalyst.
[0009] The electrolytic cell system catalyzes the oxidation of ethylene glycol in an alkaline solution through electrocatalysis under the action of a self-made working electrode. The generated oxidation product, glycolate, achieves the electrocatalytic oxidation of ethylene glycol in an alkaline solution under the action of a self-made working electrode. x -The purpose of converting ethylene glycol into high value-added products driven by SAC.
[0010] Furthermore, the loading amount of Pd in the foam metal in the single atom catalyst is 0.1-0.2 mg / cm 2 .
[0011] Furthermore, the single atom catalyst is prepared according to the following steps:
[0012] The nickel salt, urea and reducing agent are dissolved in water, and the foam metal is immersed in the above solution, wherein the foam metal is a conductive substrate, and the Ni-containing foam metal is prepared by a hydrothermal method. 2+ Defective Ni(OH) x Nanosheet arrays are prepared and single-atom Pd is then loaded on them using atomic layer deposition to obtain single-atom catalysts.
[0013] Further, the nickel salt is selected from one or more of nickel nitrate, nickel acetate, nickel chloride, nickel sulfate and nickel acetylacetonate;
[0014] The reducing agent is selected from triethylene glycol;
[0015] The foam metal is selected from one of foam nickel, foam copper, foam iron and foam cobalt.
[0016] Compared with inorganic alkaline sources, organic alkaline source urea releases OH - The rate is slower, which can inhibit the rapid growth of Ni(OH)2 to a certain extent, avoid the appearance of large blocks of Ni(OH)2, and facilitate the reduction of small-sized Ni(OH)2 by the reducing agent, thereby producing Ni 2+ Vacancy defects: The formation of vacancy defects is beneficial to the regulation of the growth of single-atom Pd. x Growth, on the one hand, by adjusting the type of reducing agent in the reaction system to regulate Ni(OH) x The thermodynamic driving force of growth, on the other hand, can be tuned by changing the hydrothermal conditions. x The growth kinetics and the ratio of raw materials are also critical. By optimizing the above reaction conditions, two-dimensional Ni(OH) sheets with a length of 0.3-1 μm were obtained. x .
[0017] Furthermore, the molar ratio of the nickel salt, urea and reducing agent is 1-5:2-10:50-200.
[0018] Further, the molar ratio of the nickel salt to water is 1:2000-5000. Exemplarily, the molar ratio of the nickel salt to water can be 1:2000, 1:3000, 1:4000, 1:5000, etc.
[0019] Further, the atomic layer deposition method specifically comprises the following steps:
[0020] Loading Ni(OH) x The foam metal of the nanosheet array is placed in an atomic layer deposition reaction chamber, hexafluoroacetylacetonate palladium vapor is injected into the atomic layer deposition reaction chamber, and at least one atomic layer deposition cycle is performed. After the reaction is completed, a single atom catalyst is obtained.
[0021] Furthermore, the atomic layer deposition method further comprises using Ar gas to purge the unreacted hexafluoroacetylacetonate palladium molecules, and using formaldehyde-methanol mixed vapor to remove the remaining ligands of the Pd atoms.
[0022] Furthermore, the hydrothermal reaction temperature is 120-180° C., and the hydrothermal reaction time is 8-24 h.
[0023] Further, the temperature in the atomic layer deposition reaction chamber is 100-400° C., and illustratively, the temperature in the atomic layer deposition reaction chamber can be 100° C., 150° C., 200° C., 250° C., 300° C., 350° C., 400° C., etc.; the number of atomic layer deposition cycles is 1-5 times, and the concentration of hexafluoroacetylacetonate palladium molecular vapor in the atomic layer deposition reaction chamber is 0.2-2×10 -7 mol / cm 3 .
[0024] Furthermore, in one atomic layer deposition cycle, the Ar gas purge time is 10-30 minutes, and the formaldehyde-methanol mixed vapor purge time is 10-30 minutes.
[0025] Furthermore, the electrolytic cell system further comprises a counter electrode and a reference electrode, which are assembled into a three-electrode electrolytic cell with the working electrode and an alkaline electrolyte containing ethylene glycol. In a specific embodiment, the counter electrode is a Pt sheet, and the reference electrode is Hg / HgO.
[0026] In order to achieve the above second purpose, the present invention adopts the following technical solutions:
[0027] The present invention provides a method for preparing glycolate from ethylene glycol by electrocatalysis, wherein the electrolytic cell system as described above is used for electrocatalytic reaction, wherein the ethylene glycol is oxidized at the working electrode to generate glycolate, and at the same time, high-purity hydrogen with the same coulomb quantity can be generated at the counter electrode.
[0028] Furthermore, the alkaline electrolyte containing ethylene glycol is obtained by hydrolyzing waste plastic PET or by directly adding ethylene glycol into an alkaline solution.
[0029] When the alkaline electrolyte is obtained by hydrolyzing waste plastic PET, the specific preparation steps of the alkaline electrolyte may be:
[0030] The waste plastic PET is dissolved in alkaline solution, and subjected to heating reflux treatment (i.e. alkaline hydrolysis reaction) in the range of 50-100°C for 5-20h. After the reflux, solid-liquid separation is performed to obtain an alkaline electrolyte containing ethylene glycol.
[0031] Furthermore, the waste plastic PET includes but is not limited to one or more of bottle-grade PET, film-grade PET and fiber-grade PET.
[0032] Furthermore, in the alkaline electrolyte containing ethylene glycol, the molar concentration ratio of ethylene glycol to alkali is 1:1-5.
[0033] Furthermore, the base is potassium hydroxide and / or sodium hydroxide. When the base is sodium hydroxide, it is more conducive to the separation and purification of the product.
[0034] Furthermore, during the electrocatalytic reaction, the applied voltage ranges from 0.6-1 V vs. RHE.
[0035] Furthermore, after the electrocatalytic reaction, technicians can separate and purify the oxidation products according to experimental needs, which specifically includes the following steps:
[0036] The solution after electrolysis (electrolyte containing glycolate) is subjected to activated carbon decolorization, drying, washing, dissolution filtration, and recrystallization to obtain separated and purified glycolate; wherein, the separation and purification operation of the present invention can not only effectively separate glycolate from the electrolyte after the reaction, but also obtain high-purity glycolate, which can be directly used for the industrial manufacture of glycolic acid without other purification treatments.
[0037] Furthermore, the washing liquid used for washing is at least one of dichloromethane, methanol, ethanol and water.
[0038] The beneficial effects of the present invention are as follows:
[0039] The present invention provides an electrolytic cell system for preparing glycolate from ethylene glycol by electrocatalysis. The electrolytic cell system comprises a working electrode, a counter electrode, a reference electrode and an alkaline electrolyte containing ethylene glycol, wherein the working electrode comprises a single-atom catalyst Pd-Ni(OH) x -SAC, the single-atom catalyst can show high electrocatalytic activity at a relatively lower Pd loading (the Pd loading of the present invention is 0.1-0.2 mg / cm 2 , conventional Pd nanocatalyst loading>1mg / cm 2 ), reducing the preparation cost of the catalyst, the maximum current density> 2A / cm 2 , compared with the current density of conventional Pd nanocatalysts <1A / cm 2 , the electrocatalytic activity is significantly improved. Therefore. Compared with the existing electrocatalysts, this technology has greater economic benefits and better catalytic performance, so it is suitable for industrialization and large-scale promotion.
[0040] The single-atom catalyst provided by the present invention can regulate the Ni(OH) by adjusting the reducing agent and organic base types of the reaction system. x Thermodynamic driving force of growth, regulation of Ni(OH) by changing hydrothermal conditions x The growth kinetics process, in obtaining Ni 2+ Vacancy defect Ni(OH) x After the nanosheet array, the atomic layer deposition method was combined to achieve the growth of Ni(OH) x The single-atom Pd on the surface is regulated to make it grow and distribute evenly, which inhibits Pd-Pd bonding and prevents Pd atomic agglomeration. At the same time, the Pd loading amount is controlled by regulating the number of deposition cycles to ensure high electrocatalytic activity even at a relatively lower Pd loading amount, thereby reducing the preparation cost of the catalyst. BRIEF DESCRIPTION OF THE DRAWINGS
[0041] The specific implementation modes of the present invention are further described in detail below in conjunction with the accompanying drawings.
[0042] Figure 1 The single atom catalyst Pd-Ni(OH) x -Synthetic preparation route of SAC.
[0043] Figure 2 The Pd-Ni(OH) prepared in Example 1 is shown x -Scanning electron microscopy image of SAC catalyst.
[0044] Figure 3 The Pd-Ni(OH) prepared in Example 1 is shown x -Spherical aberration electron microscopy image of SAC catalyst.
[0045] Figure 4 The commercially available Pd / C in Test Example 1 and the Pd-Ni(OH) x -Comparison of cyclic voltammetry curves of SAC catalyst in ethylene glycol solution.
[0046] Figure 5 The Pd-Ni(OH) of Example 1 is shown x -Chronoamperometric curves of the electrocatalytic oxidation of ethylene glycol solution by SAC catalyst.
[0047] Figure 6 The results show that the ethylene glycol solution in Test Example 1 after electrocatalytic oxidation 1 H NMR spectrum.
[0048] Figure 7 The results show that the ethylene glycol solution in Test Example 1 after electrocatalytic oxidation 13 C NMR spectrum. DETAILED DESCRIPTION
[0049] In order to explain the present invention more clearly, the present invention is further described below in conjunction with preferred embodiments and drawings. It should be understood by those skilled in the art that the content described below is illustrative rather than restrictive, and should not be used to limit the scope of protection of the present invention.
[0050] In addition, unless otherwise specified, the raw materials used in the present invention can be obtained commercially, and any range recorded in the present invention includes the end value and any numerical value between the end values and any sub-range formed by the end value or any numerical value between the end values.
[0051] In the specific embodiment, there is no particular limitation on the time of the electrocatalytic reaction. Those skilled in the art can 1 H spectrum and gas chromatography are used to qualitatively or quantitatively analyze the electrolysis product glycolate, thereby determining the progress and completion time of the reaction.
[0052] Example 1: Pd-Ni(OH) x-SAC preparation
[0053] Figure 1 The single atom catalyst Pd-Ni(OH) x -Synthetic preparation route of SAC.
[0054] Foam Ni (1cm×2cm) was used as the carrier and Ni(NO3)2 was used as the Ni 2+ Ni(OH) was prepared by hydrothermal method using urea as alkaline source and triethylene glycol as reducing agent. x Nanosheet array: 120 mg Ni(NO3)2, 70 mg urea, 10 mL triethylene glycol and 40 mL water were mixed, and after mixing evenly, the foamed Ni was immersed in the above solution and subjected to hydrothermal reaction at 160 °C for 12 h to obtain Ni(OH)2 supported by the foamed Ni. x Nanosheet array, x was 2.08 after ICP test.
[0055] Ni(OH) x Surface Ni 2+ Vacancy defects are used as anchoring sites to prepare Pd-Ni(OH) by atomic layer deposition x -SAC: Loading Ni(OH) x The foamed Ni carrier was placed in an atomic layer deposition reaction chamber, and hexafluoroacetylacetonate palladium molecular vapor was injected into the atomic layer deposition reaction chamber. The temperature in the atomic layer deposition reaction chamber was 240 °C, and the hexafluoroacetylacetonate palladium vapor concentration was 0.8×10 -7 mol / cm 3 After the deposition reaction, the unreacted hexafluoroacetylacetonate palladium molecules were purged with Ar gas for 10 minutes, and then the formaldehyde-methanol mixed vapor was injected into the reaction chamber to remove the remaining ligands of the Pd atoms. The purge time was 10 minutes, and Ar gas was used for purging to complete an atomic layer deposition cycle. The deposition cycle was performed twice to obtain the single atom catalyst Pd-Ni(OH) x -SAC, Pd loading is 0.15 mg / cm 2 .
[0056] Figure 2 The prepared Pd-Ni(OH) x -Scanning electron microscope image of SAC catalyst. Figure 2 It can be seen that Pd-Ni(OH) x -SAC is presented in a two-dimensional flake morphology with a length between 0.3-1 μm.
[0057] Figure 3 The prepared Pd-Ni(OH) x -SAC catalyst spherical aberration electron microscope image. Figure 3 It can be seen that Pd is loaded onto Ni(OH) in the form of single atoms. x Carrier surface.
[0058] Example 2: Pd-Ni(OH) x -SAC preparation
[0059] Foamed Ni (1cm×2cm) was used as the carrier and NiCl2 as the Ni 2+ Ni(OH) was prepared by hydrothermal method using urea as alkaline source and triethylene glycol as reducing agent. x Nanosheet array: 90 mg NiCl2, 60 mg urea, 12 mL triethylene glycol and 40 mL water were mixed, and after mixing evenly, the foamed Ni was immersed in the above solution and subjected to hydrothermal reaction at 140 °C for 12 h to obtain Ni(OH) x Nanosheet array, x was 2.08 after ICP test.
[0060] Ni(OH) x Surface Ni 2+ Vacancy defects are used as anchoring sites to prepare Pd-Ni(OH) by atomic layer deposition x -SAC: Loading Ni(OH) x The foamed Ni carrier was placed in an atomic layer deposition reaction chamber, and hexafluoroacetylacetonate palladium molecular vapor was injected into the atomic layer deposition reaction chamber. The temperature in the atomic layer deposition reaction chamber was 260°C, and the hexafluoroacetylacetonate palladium vapor concentration was 0.8×10 -7 mol / cm 3 After the deposition reaction, the unreacted hexafluoroacetylacetonate palladium molecules were purged with Ar gas for 10 minutes, and then the formaldehyde-methanol mixed vapor was injected into the reaction chamber to remove the remaining ligands of the Pd atoms. The purge time was 10 minutes, and Ar gas was used for purging to complete an atomic layer deposition cycle. The deposition cycle was performed twice to obtain the single atom catalyst Pd-Ni(OH) x -SAC, Pd loading is 0.15 mg / cm 2 .
[0061] Example 3: Pd-Ni(OH) x -SAC preparation
[0062] Foamed Ni (1cm×2cm) was used as the carrier and NiSO4 as the Ni 2+ Ni(OH) was prepared by hydrothermal method using urea as alkaline source and triethylene glycol as reducing agent. xNanosheet array: 100 mg NiSO4, 90 mg urea, 10 mL triethylene glycol and 40 mL water were mixed, and after mixing evenly, the foamed Ni was immersed in the above solution and subjected to hydrothermal reaction at 180 °C for 12 h to obtain Ni(OH)2+ loaded on the foamed Ni. x Nanosheet array, x was 2.08 after ICP test.
[0063] Ni(OH) x Surface Ni 2+ Vacancy defects are used as anchoring sites to prepare Pd-Ni(OH) by atomic layer deposition x -SAC: Loading Ni(OH) x The foamed Ni carrier was placed in an atomic layer deposition reaction chamber, and hexafluoroacetylacetonate palladium molecular vapor was injected into the atomic layer deposition reaction chamber. The temperature in the atomic layer deposition reaction chamber was 260°C, and the hexafluoroacetylacetonate palladium vapor concentration was 0.8×10 -7 mol / cm 3 After the deposition reaction, the unreacted hexafluoroacetylacetonate palladium molecules were purged with Ar gas for 10 minutes, and then the formaldehyde-methanol mixed vapor was injected into the reaction chamber to remove the remaining ligands of the Pd atoms. The purge time was 10 minutes, and Ar gas was used for purging to complete a deposition cycle. The deposition cycle was performed twice to obtain the single atom catalyst Pd-Ni(OH) x -SAC, Pd loading is 0.15 mg / cm 2 .
[0064] Comparative Example 1: Pd-Co(OH) x -SAC preparation
[0065] Pd-Co(OH) x -SAC preparation conditions and Pd-Ni(OH) x -SAC preparation conditions are similar, and the specific experimental steps are:
[0066] Use Ni foam as carrier (e.g. 1cm×2cm) and Co(NO3)2 as Co 2+ Co(OH) was prepared by hydrothermal method using urea as alkaline source and triethylene glycol as reducing agent. x Nanosheet array: 120 mg Co(NO3)2, 70 mg urea, 10 mL triethylene glycol and 40 mL water were mixed, and after mixing evenly, the foamed Ni was immersed in the above solution and subjected to hydrothermal reaction at 160 °C for 12 h to obtain the foamed Ni-supported Co(OH) x Nanosheet array, x was 2.1 after ICP test.
[0067] Co(OH)x Surface Co 2+ Defects are used as anchoring sites to prepare Pd-Co(OH) by atomic layer deposition x -SAC. First, Co(OH) x The foamed Ni carrier was placed in the atomic layer deposition reaction chamber, and then the hexafluoroacetylacetonate palladium molecular vapor was injected into the reaction chamber. The temperature in the atomic layer deposition reaction chamber was 260°C, and the hexafluoroacetylacetonate palladium vapor concentration was 0.8×10 -7 mol / cm 3 , and a deposition reaction was carried out. After the deposition reaction was completed, the unreacted hexafluoroacetylacetonate palladium molecules were purged with Ar gas for 10 minutes, and then the formaldehyde-methanol mixed vapor was injected into the reaction chamber to remove the remaining ligands of the Pd atoms. The purging time was 10 minutes, and finally Ar gas was used for purging to complete a deposition cycle. This deposition cycle was carried out twice to obtain the single-atom catalyst Pd-Co(OH) x -SAC, Pd loading is 0.15 mg / cm 2 .
[0068] Comparative Example 2: Pd-MnO x -SAC preparation
[0069] Pd-MnO x -SAC preparation conditions and Pd-Ni(OH) x -SAC preparation conditions are similar, and the specific experimental steps are: using Ni foam as the carrier (e.g. 1cm×2cm), KMnO4 as the Mn 7+ The MnO was prepared by hydrothermal method using hydrazine monohydrate as the base source and reducing agent. x : 100 mg KMnO4, 5 mL hydrazine monohydrate and 45 mL water were mixed, and after mixing evenly, the foamed Ni was immersed in the above solution and subjected to hydrothermal reaction at 140 °C for 12 h to obtain the MnO4 supported by the foamed Ni. x , after ICP testing, x is 2.1.
[0070] MnO x Surface Mn 4+ Defects are used as anchoring sites to prepare Pd-MnO by atomic layer deposition x -SAC. First, load MnO x The foamed Ni carrier was placed in the atomic layer deposition reaction chamber, and then the hexafluoroacetylacetonate palladium molecular vapor was injected into the reaction chamber. The temperature in the atomic layer deposition reaction chamber was 260°C, and the hexafluoroacetylacetonate palladium vapor concentration was 0.8×10 -7 mol / cm 3, a deposition reaction was carried out, and after the deposition reaction, the unreacted hexafluoroacetylacetonate palladium molecules were purged with Ar gas for 10 minutes, and then the formaldehyde-methanol mixed vapor was injected into the reaction chamber to remove the remaining ligands of the Pd atoms for 10 minutes, and finally Ar gas was used for purging to complete an atomic layer deposition cycle. This deposition cycle was carried out twice to obtain the single-atom catalyst Pd-MnO x -SAC, Pd loading is 0.15 mg / cm 2 .
[0071] Test Example 1: Electrocatalytic Preparation of Glycolate from Ethylene Glycol
[0072] The electrocatalytic oxidation of ethylene glycol was controlled by a CHI660E electrochemical workstation connected to a high current amplifier. An H-type electrolytic cell was used with a three-electrode setup. The working electrode was the catalyst sample prepared in each scheme, the counter electrode was a Pt sheet electrode, the reference electrode was a Hg / HgO electrode, and the electrolyte was an alkaline electrolyte containing ethylene glycol (volume 40 ml). In the alkaline electrolyte, the concentration of ethylene glycol was controlled to be 1 M, and the concentration of NaOH was controlled to be 5 M. In the CV test, the scan rate was 10 mV / s, and commercially available Pd / C was used as the control group.
[0073] All potentials in the electrocatalytic oxidation of ethylene glycol were calibrated with reference to the reversible hydrogen electrode (RHE). The geometric surface area of the catalyst sample was 1 cm 2 (only half of the area is inserted into the electrolyte) and use 1cm 2 The current density is calculated from the geometric surface area. All experiments were carried out at room temperature and pressure. Figure 4 Commercially available Pd / C and Pd-Ni(OH) x -SAC catalyst cyclic voltammetry curve of ethylene glycol solution is shown. When the applied voltage is controlled at 0.75Vvs.RHE, the electrolysis curve is as follows Figure 5 As shown. Figure 4 It can be seen that compared with Pd / C catalyst, Pd-Ni(OH) x -SAC catalyst activity for ethylene glycol oxidation was significantly improved. At 0.85V vs.RHE, Pd-Ni(OH) x -The peak current of SAC for ethylene glycol oxidation is 2.17 A / cm 2 , which is 5.7 times the catalytic activity of Pd / C. Figure 5 It can be seen that at 0.75V vs. RHE bias oxidation electrolysis, the initial current is 1000mA / cm 2 As the electrolysis proceeds, the current density gradually decreases, which is due to the decrease in the concentration of ethylene glycol in the electrolyte.
[0074] Qualitative and quantitative analysis of sodium glycolate
[0075] After 2.2 hours of electrocatalytic oxidation, 300ul of the electrolyte sample to be tested + 300uL of heavy water + 10uL of DMSO (internal standard) were taken. 1 H and 13 The product sodium glycolate was qualitatively and quantitatively analyzed by method C. The results are shown in Figure 6 and Figure 7 , the results are shown in Table 1.
[0076] Table 1
[0077] sample Example 1 Commercially available Pd / C Example 2 Example 3 Comparative Example 1 Comparative Example 2 Selectivity / % 96 75 95 94 81 67 Conversion rate / % 46 18 47 43 23 27
[0078] from Figure 6 It can be seen that Pd-Ni(OH) x The main product of ethylene glycol oxidation driven by -SAC catalyst is sodium glycolate, and dimethyl sulfoxide (DMSO) is used as the internal standard. 1 Quantitative calculation of H NMR spectrum shows that, taking Example 1 as an example, the amount of ethylene glycol oxidized is 0.0185 mol, and the amount of sodium glycolate generated is 0.0178 mol, so the selectivity of sodium glycolate is 96%.
[0079] Obviously, the above embodiments of the present invention are merely examples for clearly illustrating the present invention, and are not limitations on the implementation methods of the present invention. For ordinary technicians in the relevant field, other different forms of changes or modifications can be made based on the above description. It is impossible to list all the implementation methods here. All obvious changes or modifications derived from the technical solution of the present invention are still within the protection scope of the present invention.
Claims
1. An electrolytic cell system for preparing glycolate from ethylene glycol electrocatalyzed by electrocatalysis, characterized in that: The electrolytic cell system comprises a working electrode and an alkaline electrolyte containing ethylene glycol; the working electrode comprises a single-atom catalyst Pd-Ni(OH) x -SAC; The single-atom catalyst is based on a foam metal as a conductive substrate and Ni(OH) x The electrocatalyst is a main carrier and a single-atom Pd is a guest catalytic center, and the value range of x is 2<x≤2.
1.
2. The electrolytic cell system according to claim 1, characterized in that The loading amount of Pd in the foam metal in the single atom catalyst is 0.1-0.2 mg / cm 2 .
3. The electrolytic cell system according to claim 1, characterized in that The single atom catalyst is prepared according to the following steps: The nickel salt, urea and reducing agent are dissolved in water, and then the foam metal is immersed in the above solution, and the Ni-containing foam metal is prepared by a hydrothermal method. 2+ Defective Ni(OH) x Nanosheet arrays are prepared and single-atom Pd is then loaded on them using atomic layer deposition to obtain single-atom catalysts.
4. The electrolytic cell system according to claim 3, characterized in that The nickel salt is selected from one or more of nickel nitrate, nickel acetate, nickel chloride, nickel sulfate and nickel acetylacetonate; The reducing agent is selected from triethylene glycol; The foam metal is selected from one of foam nickel, foam copper, foam iron and foam cobalt.
5. The electrolytic cell system according to claim 3, characterized in that The molar ratio of the nickel salt, urea and reducing agent is 1-5:2-10:50-200.
6. The electrolytic cell system according to claim 3, characterized in that: The specific steps of the atomic layer deposition method are: Loading Ni(OH) x The foam metal of the nanosheet array is placed in an atomic layer deposition reaction chamber, hexafluoroacetylacetonate palladium vapor is injected into the atomic layer deposition reaction chamber, and at least one atomic layer deposition cycle is performed. After the reaction is completed, a single atom catalyst is obtained.
7. The electrolytic cell system according to claim 1, characterized in that The hydrothermal reaction temperature is 120-180°C, and the hydrothermal reaction time is 8-24h.
8. The electrolytic cell system according to claim 1, characterized in that The temperature in the atomic layer deposition reaction chamber is 100-400° C., the number of atomic layer deposition cycles is 1-5 times, and the concentration of hexafluoroacetylacetonate palladium vapor in the atomic layer deposition reaction chamber is 0.2-2×10 -7 mol / cm 3 .
9. A method for preparing glycolate from ethylene glycol by electrocatalysis, characterized in that: The electrolytic cell system according to any one of claims 1 to 8 is used to carry out an electrocatalytic reaction, wherein the ethylene glycol is oxidized at the working electrode to generate glycolate.
10. The method according to claim 9, characterized in that During the electrocatalytic reaction, the applied voltage ranges from 0.6-1V vs. RHE.