Boron-nitrogen co-doped monatomic catalyst and preparation and application thereof
By co-doping boron and nitrogen porous carbon materials, the problems of low CO selectivity and high cost of precious metals in electrochemical carbon dioxide reduction reaction are solved, and the efficient and low-cost CO2 conversion effect is achieved.
Patent Information
- Application Number
- CN202310569677.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-05-19
- Publication Date
- 2024-11-22
AI Technical Summary
In the existing electrochemical carbon dioxide reduction reaction, high activation energy and competitive hydrogen evolution reactions lead to low CO selectivity and high cost of precious metal catalysts, which limits its commercial application.
A single-atom catalyst is loaded with boron and nitrogen co-doped porous carbon material, and prepared by mixing metal precursors, nitrogen sources, boron sources and chelates with porous carbon support and then calcining them to obtain a non-precious metal catalyst with high CO selectivity. Inhibit side reaction hydrogen evolution reaction.
It achieves high CO selectivity and activity at lower costs, avoids the use of precious metals, is suitable for large-scale industrial applications, and significantly improves the efficiency of CO2 conversion into CO.
Smart Images

Figure CN118996497A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of catalyst development, and in particular to the preparation of a single-atom catalyst and its application in an electrochemical carbon dioxide reduction reaction, and belongs to the relevant technology of comprehensive utilization of carbon dioxide. Technical Background
[0002] Excessive use of fossil fuels leads to excessive CO 2 The emission of carbon dioxide will cause global warming. 2 RR) is the use of renewable energy to convert CO 2 It is converted into various industrial chemicals (propanol, acetic acid, ethanol, ethylene, formic acid and CO, etc.), which is used to reduce CO in the air. 2 Due to the high activation energy barrier, a larger overpotential is usually required to activate CO 2 molecules. Meanwhile, the competitive hydrogen evolution reaction (HER) has a kinetic advantage at negative potentials, which significantly reduces the selectivity of the product. Among the products of the CO2 reduction reaction, carbon monoxide (CO) is an ideal CO2 reduction product and has attracted much attention because it can be further converted into high value-added commercial chemicals through Fischer-Tropsch synthesis. Precious metal catalysts such as gold (Au), silver (Ag), and palladium (Pd) exhibit excellent CO production capabilities, but their high cost limits their commercial application. Therefore, there is an urgent need to develop low-yield catalysts that maintain high CO selectivity over a wide potential range.
[0003] In recent years, nitrogen-doped carbon-supported transition metal single-atom catalysts (MNC SACS, M = Fe, Co, Ni, Cu, etc.) have been widely used as alternatives to noble metal catalysts due to their abundant element reserves and high atomic utilization efficiency. 4 The structure is the recognized active center of this type of catalyst. Heteroatom doping without changing the coordination number of the central metal is an effective means to change the activity of this type of catalyst. It can change the symmetry of the MNC single atom catalyst while adjusting the electronic structure of the central metal. Heteroatoms such as O, P, S, and Cl have been successfully introduced into MNC single atom catalysts to achieve efficient carbon dioxide reduction activity and selectivity. Summary of the invention
[0004] The object of the present invention is to provide a method for preparing a single-atom catalyst supported by a porous carbon material co-doped with boron and nitrogen. The single-atom catalyst prepared by the present invention is used under the reaction conditions of the electrochemical carbon dioxide reduction reaction (-0.4 to -1.4 V vs. RHE, 10 to 30 ml·min -1) has good carbon monoxide selectivity. The use of boron-nitrogen co-doped single-atom catalysts can inhibit the side reaction of hydrogen evolution reaction, while not using precious metals and reducing the cost of the catalyst.
[0005] To achieve the above object, the present invention adopts the following scheme:
[0006] The present invention provides a method for preparing a boron-nitrogen co-doped single-atom catalyst, the method comprising the following steps:
[0007] (1) A certain amount of metal precursor, nitrogen source, boron source, chelate, solvent and porous carbon support are fully mixed by stirring or ultrasonication, and after the solvent is evaporated, the insoluble matter is dried in an oven to obtain a supported single atom catalyst precursor;
[0008] (2) calcining the prepared supported single atom catalyst precursor in a specific atmosphere to obtain a boron-nitrogen co-doped supported single atom catalyst;
[0009] Based on the above technical scheme, in step (1), the preparation method of a single atom catalyst according to claim 1 is characterized in that, in step (1), the metal precursor is one or more of acetate, chloride, nitrate and sulfate of metal Fe, Co, Ni, Cu, preferably one or more of acetate, chloride and nitrate; the chelating agent is one or more of D-glucose, o-phenanthroline, ethylenediaminetetraacetic acid, D-xylose, preferably D-glucose; o-phenanthroline, ethylenediaminetetraacetic acid; the nitrogen source is one or more of urea, dicyandiamide, melamine, triethylamine, glycine, glutamic acid, preferably urea, dicyandiamide, melamine, triethylamine, glycine, glutamic acid; The invention relates to a method for preparing the present invention in accordance with the present invention. The invention relates to a method for preparing the present invention in accordance with the present invention. The invention relates to a method for preparing the present invention in accordance with the present invention. The invention relates to a method for preparing the present invention in accordance with the present invention. The invention relates to a method for preparing the present invention in accordance with the present invention. The invention relates to a method for preparing the present invention in accordance with the present invention. The invention relates to a method for preparing the present invention in accordance with the present invention. The invention relates to a method for preparing the present invention in accordance with the present invention.
[0010] Based on the above technical solution, in step (2), the calcination atmosphere is one or more of nitrogen, argon, helium, hydrogen, and carbon monoxide, preferably one or more of nitrogen, argon, and helium; the calcination gas flow rate is 10 to 500 mL min -1 , preferably 20 to 200 mL min -1; Calcination temperature is 500-1000°C, preferably 700-1000°C; Heating rate is 1-20°C·min -1 , preferably 2~15℃·min -1 ; Constant temperature roasting time 0.5 ~ 6.0h, preferably 1.0 ~ 5.0h;
[0011] Based on the above technical solution, the catalyst is a porous carbon carrier loaded with a non-precious metal single atom catalyst, and the metal loading (calculated as metal) is 1 to 10 wt%, preferably 1 to 5 wt%;
[0012] Another aspect of the present invention provides the use of the above single-atom catalyst in an electrochemical carbon dioxide reduction reaction.
[0013] Based on the above technical solution, it is characterized in that, in the application, the reaction potential is: 0.0~-1.6V vs.RHE (preferably -0.3~-1.4V vs.RHE), the electrolyte is: one or more of potassium carbonate, potassium bicarbonate, potassium phosphate, potassium sulfate, potassium nitrate (preferably one or more of potassium carbonate, potassium bicarbonate, potassium phosphate), the electrolyte concentration is: 0.01~3M (preferably 0.05~1M), the electrolyte volume is: 5~100ml (10~50mL), and the gas flow rate (by mass): 5~100mL·min -1 (Preferably 10 to 50 mL min -1 ), the reactor adopts an H-type electrolytic cell, separated by a proton exchange membrane, the gas phase product is analyzed by gas chromatography, and the liquid phase product is detected by nuclear magnetic resonance hydrogen spectrum.
[0014] Compared with the prior art, the beneficial effects of the present invention are:
[0015] (1) A method for preparing a single-atom catalyst supported by a porous carbon material co-doped with boron and nitrogen was developed, which can obtain a non-precious metal single-atom catalyst with a high loading amount. The method is simple and easy to operate, with a wide range of raw materials, and is suitable for large-scale industrial applications;
[0016] (2) Single-atom catalysts prepared by co-doping with boron and nitrogen can significantly inhibit the side reaction of hydrogen evolution reaction (HER), and can obtain higher carbon monoxide Faraday efficiency compared with catalysts and nanocatalysts doped with nitrogen only; at the same time, the single atoms on the catalyst surface are anchored by nitrogen atoms and boron atoms on the surface of the carrier, which can prevent metal agglomeration at a more negative potential. At the same time, no precious metals are used, which saves costs on the one hand and has a basis for large-scale preparation on the other.
[0017] Therefore, the present invention has broad application prospects in the large-scale preparation of non-precious metal single-atom catalysts and in electrochemical carbon dioxide reduction reaction systems.
[0018] The present invention adopts a calcination method to prepare a non-precious metal single-atom catalyst supported on a porous carbon material, wherein the metal loading is 1 to 10 wt% (in terms of metal), and has good activity and selectivity in the electroreduction of carbon dioxide into carbon monoxide. The present invention utilizes the characteristics of the single-atom isolated site to avoid the occurrence of the side reaction hydrogen evolution reaction; at the same time, the heteroatoms on the surface of the carrier can anchor the metal single atom, making it have good stability. The present invention develops a preparation method for a boron-nitrogen co-doped single-atom catalyst supported on a porous carbon material, which does not use precious metals, has a wide source of raw materials, is low in cost, and is suitable for large-scale preparation. BRIEF DESCRIPTION OF THE DRAWINGS
[0019] Figure 1 . HAADF-STEM images of Catalysts AF and Comparative Examples 1 and 2. DETAILED DESCRIPTION
[0020] The present invention will be further described below in conjunction with embodiments, but the scope of the present invention is not limited in any way.
[0021] Example 1
[0022] 0.200 g of ferric acetate, 0.200 g of D-glucose, 0.500 g of urea, 0.5 g of boric acid, 0.200 g of activated carbon and 10.0 g of tetrahydrofuran were placed in a 250 mL beaker, stirred and mixed thoroughly, and the solvent was evaporated. The insoluble matter was dried in an oven at 80 ° C for 5 h to prepare a supported single-atom catalyst precursor; the prepared supported single-atom catalyst precursor was calcined at 700 ° C in an argon atmosphere for 1 h (the heating rate was 2.0 ° C·min -1 , gas flow rate 50mL·min -1 ), a supported single-atom catalyst A was prepared, and HAADF-STEM confirmed that the active component iron in catalyst A existed in the form of a single atom, such as Figure 1 As shown in a.
[0023] The prepared single-atom catalyst was used to conduct an electrochemical carbon dioxide reduction reaction evaluation test. The specific evaluation conditions are as follows: reaction potential: -1.0V vs. RHE, electrolyte: potassium carbonate, electrolyte (aqueous solution of electrolyte) concentration: 0.05M, electrolyte volume: 20mL per cell, gas flow rate (by mass): 10mL min -1The reactor uses an H-type electrolytic cell with a single cell cavity volume of 30 mL. The reference electrode is a saturated Ag / AgCl electrode, the counter electrode is a platinum electrode, and the working electrode is a single-atom catalyst A supported on carbon paper. The working electrode preparation conditions are as follows: 10 mg of the prepared single-atom catalyst A is dispersed in 1 mL of a mixed solution of ethanol and Nafion (the volume ratio of ethanol to Nafion is 9:1). After ultrasonication for 30 minutes, 100 uL of the mixed solution is dropped on a 1*1 cm long*width=1 cm 2 On one side of the carbon paper, the solvent was dried to obtain a working electrode (mass loading 1 mg / cm 2 ). The electrolytic cell uses a proton exchange membrane (N117) to separate the two cells of the H-type electrolytic cell. The working electrode and the reference electrode are located on one side of the electrolytic cell (in one cell), and the counter electrode is located on the other side of the electrolytic cell (in another cell). During the test, a set reaction potential is applied between the working electrode and the counter electrode. The H-type electrolytic cell and electrodes are purchased from Gaoshi Ruilian Technology Co., Ltd. The gas phase products are analyzed by gas chromatography, and the liquid phase products are detected by nuclear magnetic resonance hydrogen spectrum. The current density of the product CO and the Faraday efficiency of each product CO are listed in Table 1.
[0024] Example 2
[0025] 0.200 g of cobalt chloride, 0.200 g of o-phenanthroline, 0.500 g of dicyandiamide, 0.5 g of sodium borate, 0.200 g of carbon nanotubes and 10.0 g of water were placed in a 250 mL beaker, stirred and mixed thoroughly, and the solvent was evaporated. The insoluble matter was dried in an oven at 90 ° C for 7 h to prepare a supported single-atom catalyst precursor; the prepared supported single-atom catalyst precursor was calcined at 800 ° C in an argon atmosphere for 2 h (the heating rate was 3.0 ° C·min -1 , gas flow rate 100mL·min -1 ), a supported single-atom catalyst B was prepared, and HAADF-STEM confirmed that the active component cobalt in catalyst B existed in the form of a single atom, such as Figure 1 As shown in b.
[0026] The prepared single-atom catalyst was used to conduct an electrochemical carbon dioxide reduction reaction evaluation test. The specific evaluation conditions are as follows: reaction potential: -1.0V vs. RHE, electrolyte: potassium carbonate, electrolyte (aqueous solution of electrolyte) concentration: 0.05M, electrolyte volume: 20mL per cell, gas flow rate (by mass): 10mL min -1The reactor uses an H-type electrolytic cell with a single cell cavity volume of 30 mL. The reference electrode is a saturated Ag / AgCl electrode, the counter electrode is a platinum electrode, and the working electrode is a single-atom catalyst B supported on carbon paper. The working electrode preparation conditions are as follows: 10 mg of the prepared single-atom catalyst B is dispersed in 1 mL of a mixed solution of ethanol and Nafion (the volume ratio of ethanol to Nafion is 9:1). After ultrasonication for 30 minutes, 100 uL of the mixed solution is dropped on a 1*1 cm long*width=1 cm 2 On one side of the carbon paper, the solvent was dried to obtain a working electrode (mass loading 1 mg / cm 2 ). The electrolytic cell uses a proton exchange membrane (N117) to separate the two cells of the H-type electrolytic cell. The working electrode and the reference electrode are located on one side of the electrolytic cell, and the counter electrode is located on the other side of the electrolytic cell. During the test, a set reaction potential is applied between the working electrode and the counter electrode. The electrolytic cell and electrodes are purchased from Gaoshi Ruilian Technology Co., Ltd. The gas phase product is analyzed by gas chromatography, and the liquid phase product is detected by nuclear magnetic resonance hydrogen spectrum. The current density of the product CO and the Faraday efficiency of each product are listed in Table 1.
[0027] Example 3
[0028] 0.200 g nickel nitrate, 0.200 g D-xylose, 0.500 g triethylamine, 0.5 g ammonium borate, 0.200 g mesoporous carbon and 10.0 g ethanol were placed in a 250 mL beaker, stirred and mixed thoroughly, and then the solvent was evaporated. The insoluble matter was dried in an oven at 100 ° C for 10 h to prepare a supported single-atom catalyst precursor. The prepared supported single-atom catalyst precursor was calcined in a nitrogen atmosphere at 1000 ° C for 3 h (the heating rate was 4.0 ° C·min -1 , gas flow rate 150mL·min -1 ), a supported single-atom catalyst C was prepared, and HAADF-STEM confirmed that the active component nickel in catalyst C existed in the form of a single atom, such as Figure 1 As shown in c.
[0029] The prepared single-atom catalyst was used to conduct an electrochemical carbon dioxide reduction reaction evaluation test. The specific evaluation conditions are as follows: reaction potential: -1.0V vs. RHE, electrolyte: potassium carbonate, electrolyte (aqueous solution of electrolyte) concentration: 0.05M, electrolyte volume: 20mL per cell, gas flow rate (by mass): 10mL min -1The reactor uses an H-type electrolytic cell with a single cell cavity volume of 30 mL. The reference electrode is a saturated Ag / AgCl electrode, the counter electrode is a platinum electrode, and the working electrode is a single-atom catalyst C supported on carbon paper. The working electrode preparation conditions are as follows: 10 mg of the prepared single-atom catalyst C is dispersed in 1 mL of a mixed solution of ethanol and Nafion (the volume ratio of ethanol to Nafion is 9:1). After ultrasonication for 30 minutes, 100 uL of the above mixed solution is dropped on a 1*1 cm long * width = 1 cm 2 On one side of the carbon paper, the solvent was dried to obtain a working electrode (mass loading 1 mg / cm 2 ). The electrolytic cell uses a proton exchange membrane (N117) to separate the two cells of the H-type electrolytic cell. The working electrode and the reference electrode are located on one side of the electrolytic cell, and the counter electrode is located on the other side of the electrolytic cell. During the test, a set reaction potential is applied between the working electrode and the counter electrode. The electrolytic cell and electrodes are purchased from Gaoshi Ruilian Technology Co., Ltd. The gas phase product is analyzed by gas chromatography, and the liquid phase product is detected by nuclear magnetic resonance hydrogen spectrum. The current density of the product CO and the Faraday efficiency of each product are listed in Table 1.
[0030] Example 4
[0031] 0.200 g of copper sulfate, 0.200 g of ethylenediaminetetraacetic acid, 0.500 g of melamine, 0.5 g of cobalt borate, 0.200 g of carbon black and 10.0 g of isopropanol were placed in a 250 mL beaker, stirred and mixed thoroughly, and the solvent was evaporated. The insoluble matter was dried in an oven at 110° C. for 12 h to prepare a supported single-atom catalyst precursor. The prepared supported single-atom catalyst precursor was calcined in a carbon monoxide atmosphere at 1000° C. for 4 h (heating rate was 5° C. min -1 , gas flow rate 200mL·min -1 ), a supported single-atom catalyst D was prepared, and HAADF-STEM confirmed that the active component copper in catalyst D existed in the form of a single atom, such as Figure 1 As shown in d.
[0032] The prepared single-atom catalyst was used to conduct an electrochemical carbon dioxide reduction reaction evaluation test. The specific evaluation conditions are as follows: reaction potential: -1.0V vs. RHE, electrolyte: potassium carbonate, electrolyte (aqueous solution of electrolyte) concentration: 0.05M, electrolyte volume: 20mL per cell, gas flow rate (by mass): 10mL min -1The reactor uses an H-type electrolytic cell with a single cell cavity volume of 30 mL. The reference electrode is a saturated Ag / AgCl electrode, the counter electrode is a platinum electrode, and the working electrode is a single-atom catalyst D supported on carbon paper. The working electrode preparation conditions are as follows: 10 mg of the prepared single-atom catalyst D is dispersed in 1 mL of a mixed solution of ethanol and Nafion (the volume ratio of ethanol to Nafion is 9:1). After ultrasonication for 30 minutes, 100 uL of the above mixed solution is dropped on a 1*1 cm long*width=1 cm 2 On one side of the carbon paper, the solvent was dried to obtain a working electrode (mass loading 1 mg / cm 2 ). The electrolytic cell uses a proton exchange membrane (N117) to separate the two single cells of the H-type electrolytic cell. The working electrode and the reference electrode are located on one side of the electrolytic cell, and the counter electrode is located on the other side of the electrolytic cell. During the test, a set reaction potential is applied between the working electrode and the counter electrode. The electrolytic cell and electrodes are purchased from Gaoshi Ruilian Technology Co., Ltd. The gas phase product is analyzed by gas chromatography, and the liquid phase product is detected by nuclear magnetic resonance hydrogen spectrum. The partial current density of the product CO and the partial current density of each product are listed in Table 1.
[0033] Example 5
[0034] 0.200 g nickel chloride, 0.200 g triethylamine, 0.500 g dicyandiamide, 0.5 g sodium borohydride, 0.200 g carbon sphere and 10.0 g methanol were placed in a 250 mL beaker, stirred and mixed thoroughly, and then the solvent was evaporated. The insoluble matter was dried in an oven at 80 ° C for 10 h to prepare a supported single-atom catalyst precursor. The prepared supported single-atom catalyst precursor was calcined in a hydrogen atmosphere at 900 ° C for 3 h (the heating rate was 6 ° C min -1 , gas flow rate 100mL·min -1 ), a supported single-atom catalyst E was prepared, and HAADF-STEM confirmed that the active component nickel in the catalyst E existed in the form of a single atom, such as Figure 1 As shown in e.
[0035] The prepared single-atom catalyst was used to conduct an electrochemical carbon dioxide reduction reaction evaluation test. The specific evaluation conditions are as follows: reaction potential: -1.0V vs. RHE, electrolyte: potassium carbonate, electrolyte (aqueous solution of electrolyte) concentration: 0.05M, electrolyte volume: 20mL per cell, gas flow rate (by mass): 10mL min -1The reactor uses an H-type electrolytic cell with a single cell cavity volume of 30 mL. The reference electrode is a saturated Ag / AgCl electrode, the counter electrode is a platinum electrode, and the working electrode is a single-atom catalyst E supported on carbon paper. The working electrode preparation conditions are as follows: 10 mg of the prepared single-atom catalyst E is dispersed in 1 mL of a mixed solution of ethanol and Nafion (the volume ratio of ethanol to Nafion is 9:1). After ultrasonication for 30 minutes, 100 uL of the above mixed solution is dropped on a 1*1 cm long*width=1 cm 2 On one side of the carbon paper, the solvent was dried to obtain a working electrode (mass loading 1 mg / cm 2 ). The electrolytic cell uses a proton exchange membrane (N117) to separate the two cells of the H-type electrolytic cell. The working electrode and the reference electrode are located on one side of the electrolytic cell, and the counter electrode is located on the other side of the electrolytic cell. During the test, a set reaction potential is applied between the working electrode and the counter electrode. The electrolytic cell and electrodes are purchased from Gaoshi Ruilian Technology Co., Ltd. The gas phase product is analyzed by gas chromatography, and the liquid phase product is detected by nuclear magnetic resonance hydrogen spectrum. The current density of the product CO and the Faraday efficiency of each product are listed in Table 1.
[0036] Example 6
[0037] 0.200 g of ferric acetate, 0.200 g of D-xylose, 0.500 g of o-phenanthroline, 0.5 g of boric acid, 0.200 g of mesoporous carbon and 10.0 g of methanol were placed in a 250 mL beaker, stirred and mixed thoroughly, and then the solvent was evaporated. The insoluble matter was dried in an oven at 120 ° C for 5 h to prepare a supported single-atom catalyst precursor. The prepared supported single-atom catalyst precursor was calcined in a helium atmosphere at 800 ° C for 4 h (the heating rate was 5.0 ° C·min -1 , gas flow rate 150mL·min -1 ), a supported single-atom catalyst F was prepared, and HAADF-STEM confirmed that the active component iron in catalyst F existed in the form of a single atom, such as Figure 1 f.
[0038] The prepared single-atom catalyst was used to conduct an electrochemical carbon dioxide reduction reaction evaluation test. The specific evaluation conditions are as follows: reaction potential: -1.0V vs. RHE, electrolyte: potassium carbonate, electrolyte (aqueous solution of electrolyte) concentration: 0.05M, electrolyte volume: 20mL per cell, gas flow rate (by mass): 10mL min -1The reactor uses an H-type electrolytic cell with a single cell cavity volume of 30 mL. The reference electrode is a saturated Ag / AgCl electrode, the counter electrode is a platinum electrode, and the working electrode is a single-atom catalyst F supported on carbon paper. The working electrode preparation conditions are as follows: 10 mg of the prepared single-atom catalyst F is dispersed in 1 mL of a mixed solution of ethanol and Nafion (the volume ratio of ethanol to Nafion is 9:1). After ultrasonication for 30 minutes, 100 uL of the mixed solution is dropped on a 1*1 cm long*width=1 cm 2 On one side of the carbon paper, the solvent was dried to obtain a working electrode (mass loading 1 mg / cm 2 ). The electrolytic cell uses a proton exchange membrane (N117) to separate the two cells of the H-type electrolytic cell. The working electrode and the reference electrode are located on one side of the electrolytic cell, and the counter electrode is located on the other side of the electrolytic cell. During the test, a set reaction potential is applied between the working electrode and the counter electrode. The electrolytic cell and electrodes are purchased from Gaoshi Ruilian Technology Co., Ltd. The gas phase product is analyzed by gas chromatography, and the liquid phase product is detected by nuclear magnetic resonance hydrogen spectrum. The current density of the product CO and the Faraday efficiency of each product are listed in Table 1.
[0039] Comparative Example 1
[0040] 0.200 g nickel chloride, 0.200 g ethylenediaminetetraacetic acid, 0.500 g urea, 0.200 g carbon black and 10.0 g ethanol were placed in a 250 mL beaker, stirred and mixed thoroughly, and then the solvent was evaporated. The insoluble matter was dried in an oven at 120 ° C for 5 h to prepare a supported single-atom catalyst precursor. The prepared supported single-atom catalyst precursor was calcined in a nitrogen atmosphere at 1000 ° C for 4 h (the heating rate was 5 ° C·min -1 , gas flow rate 100mL·min -1 ), a supported single-atom catalyst comparative example 1 was prepared, and HAADF-STEM confirmed that the active component nickel in the catalyst comparative example 1 existed in the form of a single atom, such as Figure 1 As shown in g.
[0041] The prepared single-atom catalyst was used to conduct an electrochemical carbon dioxide reduction reaction evaluation test. The specific evaluation conditions are as follows: reaction potential: -1.0V vs. RHE, electrolyte: potassium carbonate, electrolyte (aqueous solution of electrolyte) concentration: 0.05M, electrolyte volume: 20mL per cell, gas flow rate (by mass): 10mL min -1The reactor uses an H-type electrolytic cell with a single cell cavity volume of 30 mL. The reference electrode is a saturated Ag / AgCl electrode, the counter electrode is a platinum electrode, and the working electrode is a single-atom catalyst G supported on carbon paper. The working electrode preparation conditions are as follows: 10 mg of the prepared single-atom catalyst G is dispersed in 1 mL of a mixed solution of ethanol and Nafion (the volume ratio of ethanol to Nafion is 9:1). After ultrasonication for 30 minutes, 100 uL of the above mixed solution is dropped on a 1*1 cm long*width=1 cm 2 On one side of the carbon paper, the solvent was dried to obtain a working electrode (mass loading 1 mg / cm 2 ). The electrolytic cell uses a proton exchange membrane (N117) to separate the two cells of the H-type electrolytic cell. The working electrode and the reference electrode are located on one side of the electrolytic cell, and the counter electrode is located on the other side of the electrolytic cell. During the test, a set reaction potential is applied between the working electrode and the counter electrode. The electrolytic cell and electrodes are purchased from Gaoshi Ruilian Technology Co., Ltd. The gas phase product is analyzed by gas chromatography, and the liquid phase product is detected by nuclear magnetic resonance hydrogen spectrum. The current density of the product CO and the Faraday efficiency of each product are listed in Table 1.
[0042] Comparative Example 2
[0043] 0.200 g of copper nitrate, 0.200 g and 0.500 g of melamine, 0.200 g of carbon spheres and 10.0 g of water were placed in a 250 mL beaker, stirred and mixed thoroughly, and then the solvent was evaporated. The insoluble matter was dried in an oven at 100 ° C for 4 h to prepare a supported single-atom catalyst precursor. The prepared supported single-atom catalyst precursor was calcined in a hydrogen atmosphere at 900 ° C for 5 h (the heating rate was 8 ° C·min -1 , gas flow rate 100mL·min -1 ), a supported single-atom catalyst comparative example 2 was prepared, and HAADF-STEM confirmed that the active component copper in the catalyst comparative example 2 existed in the form of a single atom, such as Figure 1 h.
[0044] The prepared single-atom catalyst was used to conduct an electrochemical carbon dioxide reduction reaction evaluation test. The specific evaluation conditions are as follows: reaction potential: -1.0V vs. RHE, electrolyte: potassium carbonate, electrolyte (aqueous solution of electrolyte) concentration: 0.05M, electrolyte volume: 20mL per cell, gas flow rate (by mass): 10mL min -1The reactor uses an H-type electrolytic cell with a single cell cavity volume of 30 mL. The reference electrode is a saturated Ag / AgCl electrode, the counter electrode is a platinum electrode, and the working electrode is a single-atom catalyst H supported on carbon paper. The working electrode preparation conditions are as follows: 10 mg of the prepared single-atom catalyst H is dispersed in 1 mL of a mixed solution of ethanol and Nafion (the volume ratio of ethanol to Nafion is 9:1). After ultrasonication for 30 minutes, 100 uL of the above mixed solution is dropped on a 1*1 cm long*width=1 cm 2 On one side of the carbon paper, the solvent was dried to obtain a working electrode (mass loading 1 mg / cm 2 ). The electrolytic cell uses a proton exchange membrane (N117) to separate the two cells of the H-type electrolytic cell. The working electrode and the reference electrode are located on one side of the electrolytic cell, and the counter electrode is located on the other side of the electrolytic cell. During the test, a set reaction potential is applied between the working electrode and the counter electrode. The electrolytic cell and electrodes are purchased from Gaoshi Ruilian Technology Co., Ltd. The gas phase product is analyzed by gas chromatography, and the liquid phase product is detected by nuclear magnetic resonance hydrogen spectrum. The current density of the product CO and the Faraday efficiency of each product are listed in Table 1.
[0045] Table 1 Electrochemical CO2 reduction performance of different single-atom catalysts
[0046]
[0047] It can be seen from the table:
[0048] This paper proposes a new method for preparing boron-nitrogen co-doped single-atom catalysts. The prepared catalysts have good catalytic activity and selectivity for the electroreduction of carbon dioxide to CO. Compared with the comparative catalyst containing only nitrogen source in the precursor, the catalyst containing both boron source and nitrogen source has higher CO Faraday efficiency and larger CO partial current density, indicating that the boron-nitrogen co-doped catalyst is more conducive to CO 2 to CO, leading to higher catalytic activity.
[0049] The raw materials and equipment used in the present invention, unless otherwise specified, are all commonly used raw materials and equipment in the art; the methods used in the present invention, unless otherwise specified, are all conventional methods in the art.
[0050] The above description is only a preferred embodiment of the present invention and does not limit the present invention in any way. Any simple modification, change and equivalent transformation made to the above embodiment based on the technical essence of the present invention still falls within the protection scope of the technical solution of the present invention.
Claims
1. A method for preparing a boron-nitrogen co-doped single-atom catalyst, characterized in that: The method comprises the following steps: (1) mixing a metal precursor, a nitrogen source, a boron source, a chelate, a solvent and a porous carbon support by stirring or ultrasonication, evaporating the solvent and drying the insoluble matter in an oven to obtain a supported single-atom catalyst precursor; (2) calcining the prepared supported single atom catalyst precursor in a specific calcination atmosphere to obtain a boron-nitrogen co-doped supported single atom catalyst; The calcination atmosphere is one or more of nitrogen, argon, helium, hydrogen, and carbon monoxide, preferably one or more of nitrogen, argon, and helium.
2. The preparation method according to claim 1, characterized in that: In step (1), The metal precursor is one or more of acetate, chloride, nitrate and sulfate of one or more of metals Fe, Co, Ni and Cu, preferably one or more of acetate, chloride and nitrate; The chelating agent is one or more of D-glucose, o-phenanthroline, ethylenediaminetetraacetic acid, and D-xylose, preferably one or more of D-glucose, o-phenanthroline, and ethylenediaminetetraacetic acid; The nitrogen source is one or more of urea, dicyandiamide, melamine, triethylamine, glycine, and glutamic acid, preferably one or more of urea, dicyandiamide, melamine, and triethylamine; The boron source is one or more of boric acid, sodium borate, ammonium borate, cobalt borate, sodium borohydride, and calcium borate, preferably one or more of boric acid, sodium borate, ammonium borate, and sodium borohydride; The solvent is one or more of tetrahydrofuran, water, isopropanol, methanol, and ethanol, preferably one or more of water, methanol, and ethanol; The porous carbon carrier is one or more of activated carbon, carbon nanotubes, mesoporous carbon, carbon black, and carbon spheres, preferably one or more of carbon nanotubes, mesoporous carbon, and carbon black; The drying temperature is 40 to 120° C., preferably 60 to 120° C.; the drying time is 1 to 24 hours, preferably 5 to 20 hours.
3. The preparation method according to claim 1 or 2, characterized in that: The mass ratio of the metal precursor, the chelate, the nitrogen source, the boron source, the porous carbon carrier and the solvent is in the range of (1:0.1:1:1:0.1:10 to 1:10:50:50:10:100), and the preferred mass ratio is in the range of (1:0.5:1:1:0.5:20 to 1:5:10:10:5:80).
4. The preparation method according to claim 1, 2 or 3, characterized in that: In step (2), 1.6 g of supported single-atom catalyst precursor is calcined at a gas flow rate of 10 to 500 mL min -1 , preferably 20 to 200 mL min -1 ; The calcination temperature is 500-1000°C, preferably 600-900°C; the heating rate from room temperature or drying temperature to the calcination temperature is 1-10°C·min -1 , preferably 2~8℃·min -1 ; The constant temperature calcination time is 0.5 to 6.0 hours, preferably 1.0 to 5.0 hours.
5. A boron-nitrogen co-doped single-atom catalyst supported on a porous carbon material prepared by the preparation method according to any one of claims 1 to 4.
6. The single atom catalyst according to claim 5, characterized in that The catalyst is a non-noble metal single-atom catalyst supported by a porous carbon carrier, and the metal loading (calculated as metal) is 1 to 10 wt %, preferably 1 to 5 wt %.
7. Use of the boron-nitrogen co-doped single-atom catalyst supported by the porous carbon material according to claim 5 or 6 in an electrochemical carbon dioxide reduction reaction.
8. The use according to claim 7, characterized in that: In the application, the reaction potential is 0.0 to -1.6 V vs. RHE (preferably -0.3 to -1.4 V vs. RHE), the electrolyte is one or more of potassium carbonate, potassium bicarbonate, potassium phosphate, potassium sulfate, and potassium nitrate (preferably one or more of potassium carbonate, potassium bicarbonate, and potassium phosphate), the electrolyte concentration is 0.01 to 3 M (preferably 0.05 to 1 M), the electrolyte volume is 5 to 100 ml (10 to 50 mL), and the gas flow rate (by mass) is 5 to 100 mL min -1 (Preferably 10 to 50 mL min -1 ), the reactor adopts an H-type electrolytic cell, separated by a proton exchange membrane, the gas phase product is analyzed by gas chromatography, and the liquid phase product is detected by nuclear magnetic resonance hydrogen spectrum.
Citation Information
Cited By
Modified bismuth-based catalyst as well as preparation method and application thereof
CN119553309A