Nickel-cobalt co-doped ruthenium-based metal nanoparticle catalyst as well as preparation method and application thereof
The electronic structure of ruthenium oxide is regulated by co-doping nickel-cobalt ruthenium-based metal nanoparticle catalyst, which solves the problems of nitrogen-nitrogen triple bond fracture and competition reaction in electrocatalytic nitrogen oxide reaction, and achieves efficient and stable nitrate preparation, which improves the Selectivity and stability of catalysts.
Patent Information
- Application Number
- CN202410973631.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-19
- Publication Date
- 2024-11-22
AI Technical Summary
In the existing electrocatalytic nitrogen oxide reaction, the destruction of the nitrogen-nitrogen triple bond needs to overcome the high reaction energy barrier, and there is competition between the electrocatalytic oxygen evolution reaction and the nitrogen oxide reaction, resulting in insufficient catalyst selectivity and stability.
Ni-cobalt co-doped ruthenium-based metal nanoparticle catalyst is used to prepare nickel-cobalt co-doped ruthenium-based metal nanoparticle catalyst by hydrothermal method, regulate the electronic structure of ruthenium oxide, enhance the adsorption and activation of nitrogen, and regulate the electrocatalytic oxygen evolution reaction. strength.
The performance of electrocatalytic nitrogen oxide preparation is significantly improved, achieving high selectivity and stability, with the highest nitrate yield of 726.46μg h-1mg-1 and the highest Faraday efficiency is 59.65%.
Smart Images

Figure CN118996498A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of nanomaterials and electrocatalysis, and in particular to a nickel-cobalt co-doped ruthenium-based metal nanoparticle catalyst and a preparation method and application thereof. Background Art
[0002] Nitrate is one of the most important inorganic chemicals in the world's agriculture, medicine and industry, and plays an important role in human daily life and economic construction. At present, the industrial production of nitrate mainly relies on the "two-step method", including the Ostwald process and the Haber-Bosch process. Both processes are energy-intensive processes, resulting in the consumption of a large amount of energy in the manufacture of nitrate, and the emission of greenhouse gases into the atmosphere at an alarming rate. Therefore, from the perspectives of energy saving and environmental protection, it is necessary to find an efficient, low-energy, and environmentally friendly nitrate synthesis route. In recent years, the preparation of nitrate by electrocatalytic oxidation at room temperature and pressure using water as a proton source and nitrogen as a nitrogen source has gradually become a research hotspot at home and abroad.
[0003] Research has found that precious metals such as Ru, Pt, and Pd can serve as true catalytically active species to adsorb and activate nitrogen, thereby achieving electrocatalytic oxidation of nitrogen to synthesize nitrate. For example, the Chinese patent document with publication number CN116177627A discloses a Sr(Ti / Zr / Hf / Sn / Ru)O3 high-entropy perovskite oxide and its preparation method and application. The method uses strontium carbonate, titanium oxide, zirconium oxide, hafnium oxide, tin oxide, and ruthenium oxide as raw materials and is prepared through high-speed ball milling, drying, and roasting to obtain Sr(Ti / Zr / Hf / Sn / Ru)O3 high-entropy perovskite oxide: the prepared high-entropy perovskite oxide has abundant active sites, which can enhance the adsorption and activation of nitrogen on its surface and show better electrocatalytic activity; the highest nitrate yield and the highest Faraday efficiency of the catalyst under normal temperature and pressure conditions are 52.5μmol mg -1 h -1 and 65.6%.
[0004] As reported by Nie et al., a ruthenium nanocluster coupled Mn3O4 (Ru-Mn3O4) electrocatalyst was prepared by salt fractionation strategy for nitrogen oxidation reaction. The synergistic effect between ruthenium nanocluster and Mn3O4 effectively reduced the energy barrier of nitrogen-nitrogen triple bond breaking, enhanced nitrogen activation, and improved the performance of electrocatalytic nitrogen oxidation. The Ru-Mn3O4 catalyst has an electrocatalytic nitrogen oxidation production rate of 35.34 μg h at 1.6 V vs. RHE under normal temperature and pressure conditions. -1 cm -2, the Faraday efficiency reaches 28.87% (Adv.Mater.2022,34,2108180).
[0005] Since the nitrogen-nitrogen triple bond has extremely strong structural stability, it is necessary to overcome a high reaction energy barrier to destroy the nitrogen-nitrogen triple bond during the electrocatalytic oxidation of nitrogen. At the same time, the oxidation potentials of the electrocatalytic oxygen evolution reaction and the electrocatalytic oxidation of nitrogen are very similar, resulting in a competitive reaction between the two. Although some research progress has been made in the electrocatalytic oxidation of nitrogen to prepare nitrate, further research is needed to develop electrocatalysts with high selectivity, superior performance and good stability. Summary of the invention
[0006] The purpose of the present invention is to provide a method for preparing a nickel-cobalt co-doped ruthenium-based metal nanoparticle catalyst with high catalytic activity, high selectivity and good stability. The method can obtain a catalyst with uniform size and nanoparticle structure, and is applied to the electrocatalytic oxidation of nitrogen to prepare nitrate systems, showing good catalytic selectivity and stability.
[0007] To achieve the above object, the technical solution adopted by the present invention is:
[0008] A method for preparing a nickel-cobalt co-doped ruthenium-based metal nanoparticle catalyst comprises the following steps:
[0009] (1) ultrasonically dissolving metal ruthenium salt, nickel salt and cobalt salt in ultrapure water to obtain a homogeneous solution;
[0010] (2) adding sodium hydroxide solution to the homogeneous solution of step (1), stirring to obtain a precipitated mixture of ruthenium hydroxide, nickel hydroxide and cobalt hydroxide;
[0011] (3) subjecting the precipitated mixture obtained in step (2) to hydrothermal treatment, and then filtering and drying to obtain a nickel-cobalt co-doped ruthenium-based metal nanoparticle catalyst precursor;
[0012] (4) calcining the precursor prepared in step (3) to obtain a nickel-cobalt co-doped ruthenium-based metal nanoparticle catalyst.
[0013] The preparation principle of the nickel-cobalt co-doped ruthenium-based metal nanoparticle catalyst provided by the present invention is: heating and pressurizing an aqueous solution reaction system in an autoclave by a hydrothermal method to create a relatively high-temperature, high-pressure reaction environment, so that a precipitated mixture of ruthenium hydroxide, nickel hydroxide, and cobalt hydroxide is dissolved and recrystallized to form a nickel-cobalt co-doped ruthenium-based metal nanoparticle catalyst precursor; then, the precursor is oxidized by air heat treatment to obtain a nickel-cobalt co-doped ruthenium-based metal nanoparticle catalyst.
[0014] The nickel and cobalt species in the nickel-cobalt co-doped ruthenium-based metal nanoparticle catalyst can regulate the electronic structure of the active site of ruthenium oxide, which is beneficial to the breaking of the nitrogen-nitrogen triple bond, enhances the adsorption and activation of nitrogen during the reaction, and can regulate the strength of the electrocatalytic oxygen evolution reaction on ruthenium dioxide, thereby improving the performance of the catalyst in the electrocatalytic oxidation of nitrogen to produce nitrate. In general, the ruthenium oxide species in the catalyst, as the real catalytic active component, plays a role in adsorbing and activating nitrogen, while the nickel and cobalt species, as dopants, effectively regulate the electronic structure of the ruthenium oxide species, making nitrogen easier to activate, regulating the strength of the electrocatalytic oxygen evolution reaction, and thus promoting the electrocatalytic oxidation of nitrogen.
[0015] The metal ruthenium salt is a soluble inorganic salt. Preferably, the ruthenium salt is hydrated ruthenium chloride.
[0016] The metal nickel salt is a soluble inorganic salt. Preferably, the nickel salt is nickel chloride hexahydrate.
[0017] The metal cobalt salt is a soluble inorganic salt. Preferably, the cobalt salt is cobalt chloride hexahydrate.
[0018] Compared with other transition metals, the catalyst of the present invention can more accurately control the electronic structure of ruthenium oxide by co-doping with nickel and cobalt. This control not only significantly enhances its nitrogen adsorption capacity and improves its activation efficiency, but also controls the strength of the oxygen evolution reaction, thereby helping to increase the yield of nitrate and the Faraday efficiency.
[0019] In step (1), the molar ratio of the metal ruthenium salt, the nickel salt and the cobalt salt is 0.5-0.9:0.05-0.25:0.05-0.25. When the content of nickel and cobalt salts is too low, the metal doping amount is too small, the electronic structure of the ruthenium oxide active site in the catalyst is adjusted less, and the electrocatalytic nitrogen oxidation performance is not significantly improved. When the content of nickel and cobalt salts is too high, a composite metal oxide of nickel and cobalt is easily formed, resulting in a change in the catalyst structure, a decrease in the electrocatalytic nitrogen oxidation performance and a decrease in stability.
[0020] The molar ratio of the metal ruthenium salt, the nickel salt and the cobalt salt is 0.7:0.1-0.15:0.15-0.2. The electronic structure of the nickel-cobalt co-doped ruthenium-based metal nanoparticle catalyst can be further optimized by limiting the above ratio.
[0021] In step (1), in the homogeneous solution after the metal ruthenium salt, nickel salt and cobalt salt are dissolved, the molar concentration of the ruthenium salt is 17 to 30 mmol / L, the molar concentration of the nickel salt is 1.7 to 8.3 mmol / L, and the molar concentration of the cobalt salt is 1.7 to 8.3 mmol / L;
[0022] In step (1), the ultrasonic time is 0.5 to 1 h, so that the metal ruthenium salt, nickel salt and cobalt salt are completely dissolved and evenly dispersed in pure water;
[0023] In step (2), after sodium hydroxide solution is added to the homogeneous solution of step (1), the molar concentration of sodium hydroxide is 85-150 mmol / L, which promotes the precipitation of ruthenium salt, nickel salt and cobalt salt to form a precipitated mixture of ruthenium hydroxide, nickel hydroxide and cobalt hydroxide.
[0024] Preferably, the molar ratio of the sodium hydroxide to the total amount of metal elements of the metal ruthenium salt, nickel salt and cobalt salt is 5:1. When the sodium hydroxide content is too low, the total amount of hydroxide in the solution is small, and the metal elements cannot be completely precipitated, which affects the synthesis of the catalyst precursor. When the sodium hydroxide content is too high, it is easy to affect the precipitation-dissolution equilibrium in the subsequent hydrothermal process, thereby affecting the recrystallization of the catalyst, resulting in catalyst phase separation, and affecting the electrocatalytic oxidation performance of the catalyst.
[0025] In step (3), the temperature of the hydrothermal reaction is 100 to 150° C., and the time of the hydrothermal reaction is 4 to 12 hours.
[0026] In step (4), the calcination temperature is 300-900° C., the atmosphere is air, and the calcination time is 1-6 hours.
[0027] The present invention also provides a nickel-cobalt co-doped ruthenium-based metal nanoparticle catalyst synthesized by the above preparation method.
[0028] The catalyst provided by the present invention has the chemical formula: Ni x Co y Ru (1-x-y) O2 represents (x is the molar number of nickel element in the catalyst, x is 0.05-0.25; y is the molar number of cobalt element in the catalyst, y is 0.05-0.25), the catalyst is composed of a ruthenium oxide substrate and metal nickel and cobalt doped in the ruthenium oxide (or expressed as nickel and cobalt doped in the ruthenium oxide in the form of oxides). In the catalyst provided by the present invention, due to the co-doping of nickel and cobalt and the presence of ruthenium oxide species, the adsorption and activation of nitrogen molecules by the active sites of ruthenium oxide are significantly improved, thereby improving the performance of the electrocatalytic oxidation of nitrogen to prepare nitrates.
[0029] The nickel-cobalt co-doped ruthenium-based metal nanoparticle catalyst provided by the invention has uniform size and ultra-small nanoparticle morphology, and the particle size ranges from 3 to 6 nm.
[0030] The present invention also provides an application of the nickel-cobalt co-doped ruthenium-based metal nanoparticle catalyst in the electrocatalytic oxidation of nitrogen to prepare nitrate.
[0031] Preferably, the nickel-cobalt co-doped ruthenium-based metal nanoparticle catalyst is used as a working electrode in an alkaline solution for the electrocatalytic oxidation of nitrogen to produce nitrate.
[0032] Preferably, the catalyst Ni x Co y Ru (1-x-y) In O2: x is 0.1 to 0.15, y is 0.15 to 0.2. The application of the working electrode in the electrocatalytic oxidation of nitrogen to prepare nitrate in an alkaline solution has a higher nitrate yield and Faraday efficiency.
[0033] In the reaction of electrocatalytic oxidation of nitrogen to synthesize nitrate, a three-electrode system is used, specifically, a Hg / HgO electrode is used as a reference electrode, a carbon rod is used as a counter electrode, a carbon paper covered with a nickel-cobalt co-doped ruthenium-based metal nanoparticle catalyst provided by the present invention is used as a working electrode, and 0.1M potassium hydroxide is used as an electrolyte.
[0034] Compared with the prior art, the nickel-cobalt co-doped ruthenium-based metal nanoparticle catalyst provided by the present invention has the following beneficial effects:
[0035] (1) The method for preparing the nickel-cobalt co-doped ruthenium-based metal nanoparticle catalyst provided by the present invention has the advantages of being simple, efficient, highly controllable, and reproducible, and has good commercial application prospects;
[0036] (2) The nickel-cobalt co-doped ruthenium-based metal nanoparticle catalyst provided by the present invention has a uniform size and ultra-small nanoparticle morphology, and the particle size ranges from 3 to 6 nm. The nickel-cobalt co-doping optimizes the electronic structure of ruthenium oxide, which can effectively improve the adsorption and activation of nitrogen, thereby facilitating the electrocatalytic oxidation of nitrogen to synthesize nitrate ions.
[0037] (3) The nickel-cobalt co-doped ruthenium-based metal nanoparticle catalyst provided by the present invention has both high electrocatalytic nitrogen oxidation activity and good stability in alkaline electrolyte for electrocatalytic oxidation of nitrogen to synthesize nitrate, and the highest nitrate yield is 726.46 μg h -1 mg -1 , the highest Faradaic efficiency is 59.65%, which has good prospects for synthetic applications. BRIEF DESCRIPTION OF THE DRAWINGS
[0038] Figure 1 The catalyst Ni prepared in Example 1 0.1 Co 0.2 Ru 0.7 Scanning electron microscope SEM image of O2;
[0039] Figure 2 The catalyst Ni prepared in Example 1 0.1 Co 0.2Ru 0.7 High magnification transmission electron microscopy HRTEM image of O2;
[0040] Figure 3 The catalyst Ni prepared in Example 1 0.1 Co 0.2 Ru 0.7 X-ray diffraction XRD pattern of O2;
[0041] Figure 4 The catalyst Ni prepared in Example 1 0.1 Co 0.2 Ru 0.7 X-ray photoelectron spectroscopy XPS graph of O2;
[0042] Figure 5 The catalyst Ni prepared in Example 1 0.1 Co 0.2 Ru 0.7 Energy dispersion spectrum EDX image of O2;
[0043] Figure 6 The electrocatalytic oxidation of nitrogen to produce nitrate by the catalysts prepared in Examples 1-5 and Comparative Examples 1-3;
[0044] Figure 7 The catalyst Ni prepared in Example 1 0.1 Co 0.2 Ru 0.7 Stability test diagram of electrocatalytic oxidation of nitrogen gas by O2 to produce nitrate. DETAILED DESCRIPTION
[0045] In order to make the purpose, technical scheme and advantages of the present invention clearer, the present invention is further described in detail below in conjunction with embodiment. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not intended to limit the present invention. Those skilled in the art can make modifications or equivalent substitutions based on the understanding of the technical scheme of the present invention without departing from the spirit and scope of the technical scheme of the present invention, and all should be included in the protection scope of the present invention.
[0046] Example 1
[0047] (1) Weigh 145.18 mg of ruthenium chloride hydrate, 23.77 mg of nickel chloride hexahydrate, and 47.59 mg of cobalt chloride hexahydrate, dissolve them in 30 mL of ultrapure water, and treat with ultrasound for 0.5 h;
[0048] (2) weighing 200 mg of sodium hydroxide, dissolving it in 5 mL of ultrapure water, and then adding the obtained sodium hydroxide solution to step (1) to obtain a homogeneous solution, stirring and mixing for 0.5 h to form a precipitated mixture of ruthenium hydroxide, nickel hydroxide, and cobalt hydroxide;
[0049] (3) hydrothermaling the precipitate mixture prepared in step (2) at 150° C. for 10 h, filtering and drying to obtain a nickel-cobalt co-doped ruthenium-based metal nanoparticle catalyst precursor;
[0050] (4) Placing the catalyst precursor prepared in step (3) in air and subjecting it to thermal decomposition treatment at 450° C. for 6 h to obtain a nickel-cobalt co-doped ruthenium-based metal nanoparticle catalyst.
[0051] The macroscopic morphology of the prepared nickel-cobalt co-doped ruthenium-based metal nanoparticle catalyst was observed by scanning electron microscopy (SEM) and transmission electron microscopy (TEM). Figure 1 As shown, the TEM results are Figure 2 As shown. Figure 1-Figure 2 It can be seen that the nickel-cobalt co-doped ruthenium-based metal nanoparticle catalyst presents a uniformly distributed nanoparticle morphology with a particle size range of 3 to 6 nm.
[0052] The XRD results of the nickel-cobalt co-doped ruthenium-based metal nanoparticle catalyst prepared in this example are as follows: Figure 3 As shown, it can be seen that the catalyst prepared in this example has the characteristic diffraction peak of ruthenium oxide, and does not have the diffraction peaks of metallic nickel, metallic cobalt and their compounds.
[0053] The XPS results of the nickel-cobalt co-doped ruthenium-based metal nanoparticle catalyst prepared in this example are as follows: Figure 4 As shown: Figure 4 a in the figure is the high-resolution spectrum of ruthenium, and the spectral peak at the binding energy of 462.4 eV is Ru 4+ Characteristic peaks of Figure 4 b in the figure is the high-resolution spectrum of nickel element, and the spectral peak at the binding energy of 854.1 eV is Ni 2+ The characteristic peak of Ni 3+ The characteristic peaks of , the spectral peaks at 860.7eV and 864.5eV are its satellite peaks; Figure 4 The c in the figure is the high-resolution spectrum of cobalt element, and the spectral peak at the binding energy of 779.2 eV is Co 3+ The characteristic peak of Co is at a binding energy of 781.1 eV. 2+ The peak at 786.1eV is its satellite peak. The above results prove that the catalyst is composed of nickel and cobalt doped in ruthenium oxide in the form of oxides.
[0054] Example 2
[0055] According to the preparation process of Example 1, except that the amount of nickel chloride hexahydrate added in step (1) is changed to 11.88 mg, and the amount of cobalt chloride hexahydrate is changed to 59.48 mg, a nickel-cobalt co-doped ruthenium-based metal nanoparticle catalyst is obtained, denoted as Ni0.05 Co 0.25 Ru 0.7 O2.
[0056] Example 3
[0057] According to the preparation process of Example 1, except that the amount of nickel chloride hexahydrate added in step (1) is changed to 35.65 mg, and the amount of cobalt chloride hexahydrate is changed to 35.69 mg, a nickel-cobalt co-doped ruthenium-based metal nanoparticle catalyst is obtained, denoted as Ni 0.15 Co 0.15 Ru 0.7 O2.
[0058] Example 4
[0059] According to the preparation process of Example 1, except that the amount of nickel chloride hexahydrate added in step (1) is changed to 47.54 mg, and the amount of cobalt chloride hexahydrate is changed to 23.79 mg, a nickel-cobalt co-doped ruthenium-based metal nanoparticle catalyst is obtained, denoted as Ni 0.2 Co 0.1 Ru 0.7 O2.
[0060] Example 5
[0061] According to the preparation process of Example 1, except that the amount of nickel chloride hexahydrate added in step (1) is changed to 59.42 mg, and the amount of cobalt chloride hexahydrate is changed to 11.90 mg, a nickel-cobalt co-doped ruthenium-based metal nanoparticle catalyst is obtained, denoted as Ni 0.25 Co 0.05 Ru 0.7 O2.
[0062] Comparative Example 1
[0063] According to the preparation process of Example 1, except that the amount of nickel chloride hexahydrate added in step (1) is changed to 71.31 mg, and cobalt chloride hexahydrate is not added, a nickel-doped ruthenium-based metal nanoparticle catalyst is obtained, which is denoted as Ni 0.3 RuO2.
[0064] Comparative Example 2
[0065] The preparation process of Example 1 was followed, except that the amount of cobalt chloride hexahydrate added in step (1) was changed to 71.38 mg, and nickel chloride hexahydrate was not added, to obtain a cobalt-doped ruthenium-based metal nanoparticle catalyst, denoted as Co 0.3 RuO2.
[0066] Comparative Example 3
[0067] According to the preparation process of Example 1, except that nickel chloride hexahydrate and cobalt chloride hexahydrate are not added in step (1), a ruthenium-based metal nanoparticle catalyst without nickel and cobalt doping is obtained, which is recorded as RuO2.
[0068] Application Examples
[0069] (1) A three-electrode system was used, with the catalyst-loaded carbon paper prepared in Examples 1-5 or Comparative Examples 1-3 as the working electrode, the carbon rod as the counter electrode, the Hg / HgO electrode as the reference electrode, and the electrolyte being 0.1 M potassium hydroxide;
[0070] (2) Cyclic voltammetry (CV) activation: Shanghai Chenhua CHI 760E electrochemical workstation was used. Nitrogen was introduced into the electrolyte for 30 min before testing. The CV program was used, with the test interval at 0.87-1.67 V vs. RHE and a scan rate of 50 mV s -1 After 30 cycles, the electrode reaches a stable state.
[0071] The catalysts prepared in Examples 1-5 and Comparative Examples 1-3 were first activated by CV tests, and then their performance was tested. The switching procedure was constant voltage-time test. During the constant voltage test, N2 was continuously introduced into the electrolyte. The test time at different voltages was 2h. The results are shown in Table 1. Figure 6 As shown: Figure 6 a in is the Faraday efficiency, Figure 6 Where b is the nitrate yield. Figure 6 It can be seen that the Ni prepared in Example 1 0.1 Co 0.2 Ru 0.7 The O2 catalyst exhibited the best electrochemical activity in the electrocatalytic oxidation of nitrogen to nitrate, that is, at 1.5 V vs. RHE, the highest nitrate yield was 726.46 μg h -1 mg -1 , the highest Faradaic efficiency is 59.65%.
[0072] The catalyst prepared in Example 1 was tested for stability. Figure 7 The stability test results of the catalyst in Example 1 show that in 50 cycle tests (the test time for one cycle is 2 hours), the nitrate yield and Faraday efficiency obtained by the catalyst in the reaction of electrocatalytic oxidation of nitrogen to prepare nitrate did not change significantly, demonstrating its good catalytic stability.
[0073] It should be noted that the specific implementation method described above provides a detailed description of the technical scheme and application results of the present invention. Please understand that the above embodiments are only the most preferred embodiments and are not used to limit the present invention. Modifications or equivalent substitutions made by relevant technical personnel within the core theoretical scope of the present invention should all fall within the protection scope of the present invention.
Claims
1. A method for preparing a nickel-cobalt co-doped ruthenium-based metal nanoparticle catalyst, characterized in that: The preparation method comprises the following steps: (1) dissolving metal ruthenium salt, nickel salt and cobalt salt to obtain a homogeneous solution; (2) adding a sodium hydroxide solution to the homogeneous solution of step (1), and stirring to obtain a precipitated mixture of ruthenium hydroxide, nickel hydroxide, and cobalt hydroxide; (3) subjecting the precipitated mixture obtained in step (2) to hydrothermal treatment to obtain a nickel-cobalt co-doped ruthenium-based metal nanoparticle catalyst precursor; (4) calcining the precursor prepared in step (3) to obtain a nickel-cobalt co-doped ruthenium-based metal nanoparticle catalyst.
2. The method for preparing the nickel-cobalt co-doped ruthenium-based metal nanoparticle catalyst according to claim 1, characterized in that: In step (1), the molar ratio of the metal ruthenium salt, the nickel salt and the cobalt salt is 0.5-0.9:0.05-0.25:0.05-0.
25.
3. The method for preparing the nickel-cobalt co-doped ruthenium-based metal nanoparticle catalyst according to claim 2, characterized in that: The molar ratio of the metal ruthenium salt, the nickel salt and the cobalt salt is 0.7:0.1-0.15:0.15-0.
2.
4. The method for preparing the nickel-cobalt co-doped ruthenium-based metal nanoparticle catalyst according to claim 1, characterized in that: In step (3), the temperature of the hydrothermal treatment is 100 to 150° C., and the time of the hydrothermal treatment is 4 to 12 hours.
5. The method for preparing the nickel-cobalt co-doped ruthenium-based metal nanoparticle catalyst according to claim 1, characterized in that: In step (4), the calcination temperature is 300-900° C., the atmosphere is air, and the calcination time is 1-6 hours.
6. A nickel-cobalt co-doped ruthenium-based metal nanoparticle catalyst prepared by the preparation method according to any one of claims 1 to 5.
7. The nickel-cobalt co-doped ruthenium-based metal nanoparticle catalyst according to claim 6, characterized in that: In the catalyst, nickel and cobalt are doped in ruthenium oxide in the form of oxides, and the chemical formula is: Ni x Co y Ru (1-x-y) O2, x is the molar number of nickel element in the catalyst, x is 0.05-0.25; y is the molar number of cobalt element in the catalyst, y is 0.05-0.
25.
8. The nickel-cobalt co-doped ruthenium-based metal nanoparticle catalyst according to claim 6, characterized in that: The particle size of the catalyst is 3-6 nm.
9. Use of the nickel-cobalt co-doped ruthenium-based metal nanoparticle catalyst according to claim 6 in the electrocatalytic oxidation of nitrogen to produce nitrate.
10. The use according to claim 9, characterized in that: The catalyst is used as a working electrode to electrocatalytically oxidize nitrogen in an alkaline solution to prepare nitrate.
Citation Information
Cited By
Methane reforming catalyst with high carbon deposition resistance as well as preparation method and application of methane reforming catalyst
CN120885236A