Rare earth metal doped ruthenium dioxide nano material as well as preparation method and application thereof

Through rare earth metal-doped ruthenium dioxide nanomaterials, the active sites of the catalyst and the adsorption of nitrate are optimized, and the problem of low catalyst efficiency in the prior art is solved, and the Faraday efficiency and ammonia production rate of electrochemical synthesis are significantly improved.

CN118996516APending Publication Date: 2024-11-22YANGZHOU UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411098013.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-12
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

In the existing methods of nitrate reduction synthesis of ammonia, the low Faraday efficiency of the catalyst and the low ammonia yield are limited, which limits the efficiency of electrochemical synthesis of ammonia.

Method used

Using rare earth metal-doped ruthenium dioxide nanomaterials, the formation of more M-Ru coordination sites by increasing the oxide content of rare earth metals, thereby improving the catalytic activity of the catalyst, optimizing the adsorption of nitrates and inhibiting hydrogen evolution reactions. Improve ammonia production rate and Faraday efficiency.

Benefits of technology

In the process of nitrate reduction and synthesis of ammonia, the Faraday efficiency and rate of ammonia production of rare earth metal-doped ruthenium dioxide nanosheets have been significantly improved. In particular, the Faraday efficiency of Ce doped system can reach 95.6%, and the ammonia production rate can reach 942 mmol h–1g– 1. Significantly improve the selectivity of electrochemical nitrate conversion to ammonia.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118996516A_ABST
    Figure CN118996516A_ABST
Patent Text Reader

Abstract

The invention discloses a rare earth metal doped ruthenium dioxide nano material, the chemical formula of which is Mx-Ru1-XO2, 0lt, x is smaller than or equal to 0.2; the rare earth metal M is one of La, Ce, Eu or Er. The invention also discloses a preparation method of the ruthenium dioxide nano material, which comprises the following steps: (1) mixing and grinding K2CO3, RuO2 and oxide of rare earth metal M to obtain a mixture; (2) calcining the mixture in an oxygen-containing environment at the temperature of 900-1100 DEG C for 55-65 minutes, grinding after calcining, and continuously calcining at the temperature of 900-1100 DEG C for 18-22 hours after grinding; after the step (2) is repeated for 1-2 times, a sample Mx-K0. 2Ru1-xO2, 0lt is obtained; x is smaller than or equal to 0.2; (3) mixing the sample with an HCl solution according to a mass-volume ratio of 0.008-0.012 g / mL, reacting, filtering, washing, and drying to obtain a precipitate; (4) stirring the precipitate in a tetrabutyl ammonium hydroxide aqueous solution to form a colloidal nanosheet suspension; and (5) adding water into the colloidal nanosheet suspension, centrifuging to remove tetrabutylammonium hydroxide in the suspension, and drying to obtain the rare earth metal doped single-layer ruthenium dioxide nanosheet.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a rare earth metal-doped ruthenium dioxide nanomaterial, and also relates to a preparation method of the ruthenium dioxide nanomaterial and its application in electrocatalytic ammonia synthesis. Background Art

[0002] Ammonia is not only an important nitrogen resource for producing fertilizers, but also a promising high-energy carrier. The traditional Haber–Bosch method for producing NH3 needs to be carried out in a high-temperature and high-pressure environment, with an annual carbon emission of 300 million tons and consuming about 2% of the world's energy. The electrochemical method for producing NH3 has mild environmental conditions, low energy consumption, and almost zero CO2 emissions, and is considered the most promising candidate method. However, the nitrogen reduction reaction has a very high dissociation energy of the N≡N triple bond (941 kJ / mol) and extremely low solubility of N2 in water, resulting in a low N2–NH3 conversion efficiency, which greatly limits the electrochemical synthesis of NH3. Electrochemical NO3 - –to–NH3 reduction reaction (NO3RR) is also considered an environmentally friendly method, which can not only degrade NO3 in polluted water - , but also due to the good water solubility of NO3 - , especially the bond energy of the N=O double bond (204 kJ / mol) is much lower than that of the N≡N triple bond. Therefore, the electrocatalytic efficiency of preparing NH3 by electrochemical NO3 - is much higher than that of N2–NH3.

[0003] In the existing methods for nitrate reduction to ammonia synthesis, copper-based or iron-based catalysts are generally used. The use of the above catalysts currently has the problems of low Faraday efficiency and low ammonia yield for catalyzing nitrate reduction to ammonia. Summary of the Invention

[0004] Object of the Invention: The object of the present invention is to provide a rare earth metal-doped ruthenium dioxide nanomaterial. After doping with rare earth metals, the electronic interaction of the catalyst can be made more abundant, thereby enhancing the adsorption ability of the catalyst to nitrate, suppressing the hydrogen evolution reaction while reducing the nitrate reduction potential barrier, and further increasing the ammonia production rate and Faraday efficiency in the process of nitrate reduction to ammonia synthesis; another object of the present invention is to provide a preparation method of the above ruthenium dioxide nanomaterial and its application in electrocatalytic ammonia synthesis.

[0005] Technical Solution: The rare earth metal-doped ruthenium dioxide nanomaterial described in the present invention has the chemical formula: M x -Ru 1-X O2, 0 < x ≤ 0.2; the rare earth metal M is one of La, Ce, Eu or Er.

[0006] The preparation method of the above ruthenium dioxide nanomaterial includes the following steps:

[0007] (1) K2CO3, RuO2 and an oxide of a rare earth metal M are mixed and ground to obtain a mixture;

[0008] (2) calcining the mixture of step (1) at 900°C to 1100°C for 55 to 65 min in an oxygen-containing environment, grinding the mixture after calcination, and further calcining the mixture at 900°C to 1100°C for 18 to 22 hours after grinding; repeating step (2) 1 to 2 times to obtain sample M x –K 0.2 Ru 1–x O2,0 <x≤0.2;

[0009] (3) mixing the sample of step (2) with HCl solution at a mass volume ratio of 0.008 to 0.012 g / mL, filtering and washing after the reaction to remove excess acid, and then drying to obtain a precipitate;

[0010] (4) stirring the precipitate of step (3) in an aqueous solution of tetrabutylammonium hydroxide to form a colloidal nanosheet suspension;

[0011] (5) adding water to the colloidal nanosheet suspension of step (4), then centrifuging to remove tetrabutylammonium hydroxide in the suspension, and drying to obtain a rare earth metal-doped single-layer ruthenium dioxide nanosheet.

[0012] Wherein, in step (1), the oxide of the rare earth metal M is one of La2O3, CeO2, Eu2O3 or Er2O3.

[0013] Wherein, in step (2), the value of x is 0.01 to 0.1.

[0014] Wherein, in step (3), the concentration of the HCl solution is 0.5-1.5 mol / L.

[0015] Wherein, in step (3), the reaction time is 65 to 75 hours.

[0016] Wherein, in step (4), the concentration of the tetrabutylammonium hydroxide aqueous solution is 0.02 to 0.05 mol / L; and the stirring time is 10 to 13 days.

[0017] Wherein, in step (5), the area of ​​the rare earth metal-doped single-layer ruthenium dioxide nanosheet is 1 to 20 μm 2 ; The thickness is 1~2nm.

[0018] Application of the above ruthenium dioxide nanomaterial in electrocatalytic synthesis of ammonia.

[0019] Beneficial effects: Compared with the prior art, the present invention has the following significant advantages: (1) The method for preparing a rare earth metal-doped monolayer ruthenium dioxide nanosheet of the present invention can achieve doping of a relatively high concentration of rare earth metal by increasing the oxide content of the rare earth metal M. The atomic content of the doped rare earth metal element can reach 0.05-12% (100%×M / (Ru+M)). High-concentration doping can form more M-Ru coordination, so that the catalyst has more catalytic active sites, thereby improving the catalytic activity of the catalyst; (2) Compared with undoped monolayer ruthenium dioxide nanosheets, the rare earth metal-doped monolayer ruthenium dioxide nanosheet prepared by the present invention has greatly improved ammonia production Faraday efficiency and ammonia production rate in the process of nitrate reduction to synthesize ammonia. In particular, for a system containing Ce, the ammonia production Faraday efficiency can reach 95.6%, and the ammonia production rate can reach 942 mmol h –1 g –1 This is attributed to the fact that doping with Ce optimizes the adsorption of nitrate ions on RuO2 nanosheets and inhibits their hydrogen evolution reaction, thereby effectively improving their selectivity for electrochemical nitrate conversion to ammonia. BRIEF DESCRIPTION OF THE DRAWINGS

[0020] Figure 1 The XRD diagrams of the ruthenium dioxide nanosheets prepared in Examples 1 to 4 and Comparative Example 1;

[0021] Figure 2 TEM image of the ruthenium dioxide nanosheets prepared in Example 1;

[0022] Figure 3 TEM image of the ruthenium dioxide nanosheets prepared in Example 2;

[0023] Figure 4 TEM image of the ruthenium dioxide nanosheets prepared in Example 3;

[0024] Figure 5 TEM image of the ruthenium dioxide nanosheets prepared in Example 4;

[0025] Figure 6 TEM image of the ruthenium dioxide nanosheets prepared in Comparative Example 1;

[0026] Figure 7 The performance curve of the ruthenium dioxide nanosheets prepared in Example 1 as a catalyst for electrochemical synthesis of ammonia;

[0027] Figure 8 The performance curve of the ruthenium dioxide nanosheets prepared in Example 2 as a catalyst for electrochemical synthesis of ammonia;

[0028] Fig. 9 The performance curve of the ruthenium dioxide nanosheets prepared in Example 3 as a catalyst for electrochemical synthesis of ammonia;

[0029] Fig.10 The performance curve of the ruthenium dioxide nanosheets prepared in Example 4 as a catalyst for electrochemical synthesis of ammonia;

[0030] Fig.11 This is the performance curve of the ruthenium dioxide nanosheets prepared in Comparative Example 1 as a catalyst for electrochemical synthesis of ammonia. DETAILED DESCRIPTION

[0031] Example 1

[0032] The La-doped single-layer ruthenium dioxide nanosheet of the present invention has a chemical formula of La 0.1 –Ru 0.9 O2 is prepared by the following method, the steps are:

[0033] (1) 1.382 g of K2CO3, 1.916 g of RuO2, and 0.19 g of La2O3 were mixed and ground to obtain a mixture;

[0034] (2) The mixture was calcined in air for 60 min at a calcination temperature of 1000°C; after calcination, it was ground and then calcined at 1000°C for 20 h to obtain sample La 0.1 –K 0.2 Ru 0.9 O2;

[0035] (3) 2 g of the obtained sample was immersed in 200 mL of 1 mol / L HCl solution, stirred for 72 h (the mass volume ratio of the sample to the HCl solution was 10 g / L), then filtered, washed to remove excess acid, and air-dried;

[0036] (4) stirring the air-dried solid in a 0.03 mol / L tetrabutylammonium hydroxide aqueous solution for 10 days, so that the obtained precipitate can be peeled off to a single layer to form a colloidal nanosheet suspension;

[0037] (5) adding water to the obtained colloidal nanosheet suspension (the volume ratio of the colloidal nanosheet suspension to water is 1:4), then centrifuging to remove tetrabutylammonium hydroxide in the suspension, and then drying to obtain La-doped single-layer ruthenium dioxide nanosheet powder.

[0038] Example 2

[0039] The Ce-doped single-layer ruthenium dioxide nanosheet of the present invention has the chemical formula Ce 0.1 –Ru 0.9 O2 is prepared by the following method, the steps are:

[0040] (1) 1.382 g of K2CO3, 1.916 g of RuO2, and 0.198 g of CeO2 were mixed and ground to obtain a mixture;

[0041] (2) The mixture was calcined in air for 60 min at a calcination temperature of 1000°C; after calcination, it was ground and then calcined at 1000°C for 20 h to obtain sample Ce. 0.1 –K 0.2 Ru 0.9 O2;

[0042] (3) 2 g of the obtained sample was immersed in 200 mL of 1 mol / L HCl solution, stirred for 72 h (the mass volume ratio of the sample to the HCl solution was 10 g / L), then filtered, washed to remove excess acid, and air-dried;

[0043] (4) stirring the air-dried solid in a 0.03 mol / L tetrabutylammonium hydroxide aqueous solution for 10 days, so that the obtained precipitate can be peeled off to a single layer to form a colloidal nanosheet suspension;

[0044] (5) adding water to the obtained colloidal nanosheet suspension (the volume ratio of the colloidal nanosheet suspension to water is 1:4), then centrifuging to remove tetrabutylammonium hydroxide in the suspension, and then drying to obtain Ce-doped single-layer ruthenium dioxide nanosheet powder.

[0045] Example 3

[0046] The Eu-doped single-layer ruthenium dioxide nanosheet of the present invention has the chemical formula of Eu 0.1 –Ru 0.9 O2 is prepared by the following method, the steps are:

[0047] (1) 1.382 g of K2CO3, 1.916 g of RuO2, and 0.188 g of Eu2O3 were mixed and ground to obtain a mixture;

[0048] (2) The mixture was calcined in air for 60 min at a calcination temperature of 1000°C; after calcination, it was ground and then calcined at 1000°C for 20 h to obtain sample Eu 0.1 –K 0.2 Ru 0.9 O2;

[0049] (3) 2 g of the obtained sample was immersed in 200 mL of 1 mol / L HCl solution, stirred for 72 h (the mass volume ratio of the sample to the HCl solution was 10 g / L), then filtered, washed to remove excess acid, and air-dried;

[0050] (4) stirring the air-dried solid in a 0.03 mol / L tetrabutylammonium hydroxide aqueous solution for 10 days, so that the obtained precipitate can be peeled off to a single layer to form a colloidal nanosheet suspension;

[0051] (5) adding water to the obtained colloidal nanosheet suspension (the volume ratio of the colloidal nanosheet suspension to water is 1:4), then centrifuging to remove tetrabutylammonium hydroxide in the suspension, and then drying to obtain Eu-doped single-layer ruthenium dioxide nanosheet powder.

[0052] Example 4

[0053] The Er-doped single-layer ruthenium dioxide nanosheet of the present invention has the chemical formula Er 0.1 –Ru 0.9 O2 is prepared by the following method, the steps are:

[0054] (1) 1.382 g of K2CO3, 1.916 g of RuO2, and 0.184 g of Er2O3 were mixed and ground to obtain a mixture;

[0055] (2) The mixture was calcined in air for 60 min at a calcination temperature of 1000°C; after calcination, it was ground and then calcined at 1000°C for 20 h to obtain sample Er 0.1 –K 0.2 Ru 0.9 O2;

[0056] (3) 2 g of the obtained sample was immersed in 200 mL of 1 mol / L HCl solution, stirred for 72 h (the mass volume ratio of the sample to the HCl solution was 10 g / L), then filtered, washed to remove excess acid, and air-dried;

[0057] (4) stirring the air-dried solid in a 0.03 mol / L tetrabutylammonium hydroxide aqueous solution for 10 days, so that the obtained precipitate can be peeled off to a single layer to form a colloidal nanosheet suspension;

[0058] (5) adding water to the obtained colloidal nanosheet suspension (the volume ratio of the colloidal nanosheet suspension to water is 1:4), then centrifuging to remove tetrabutylammonium hydroxide in the suspension, and then drying to obtain Er-doped single-layer ruthenium dioxide nanosheet powder.

[0059] Comparative Example 1

[0060] A method for preparing a rare earth metal-free single-layer ruthenium dioxide nanosheet comprises the following steps:

[0061] (1) 1.382 g of K2CO3 and 2.13 g of RuO2 were mixed and ground to obtain a mixture;

[0062] (2) The mixture was calcined in air for 60 min at a calcination temperature of 1000°C; after calcination, it was ground and then calcined at 1000°C for 20 h to obtain sample K 0.2 RuO2;

[0063] (3) 2 g of the obtained sample was immersed in 200 mL of 1 mol / L HCl solution, stirred for 72 h (the mass volume ratio of the sample to the HCl solution was 10 g / L), then filtered, washed to remove excess acid, and air-dried;

[0064] (4) stirring the air-dried solid in a 0.03 mol / L tetrabutylammonium hydroxide aqueous solution for 10 days, so that the obtained precipitate can be peeled off to a single layer to form a colloidal nanosheet suspension;

[0065] (5) adding water to the obtained colloidal nanosheet suspension (the volume ratio of the colloidal nanosheet suspension to water is 1:4), then centrifuging to remove tetrabutylammonium hydroxide in the suspension, and then drying to obtain a single-layer ruthenium dioxide nanosheet powder without rare earth metal doping.

[0066] Electrochemical test: 4.8 mg of ruthenium dioxide nanomaterials prepared in Examples 1 to 4 and Comparative Example 1 were dispersed in 300 μL of ethanol, 30 μL of Nafion solution was added, and 300 μL of deionized water was added after ultrasonic treatment for 20 minutes, and ultrasonic treatment was continued for another 20 minutes to form a uniformly dispersed catalyst slurry. 4.7 μL of the above catalyst slurry was dripped onto a glassy carbon electrode with a diameter of 0.5 mm and dried, and the dripping was repeated three times.

[0067] An H-type closed electrolytic cell was used for electrochemical nitrate reduction to synthesize ammonia test, wherein the working electrode (cathode) was a glassy carbon electrode coated with a catalyst, the reference electrode was a saturated calomel electrode, and the counter electrode was a 1 cm×1 cm Pt sheet; 80 mL of 0.5 M Na2SO4 solution was evenly distributed in the cathode and anode regions of the H-type closed electrolytic cell, wherein NaNO3 was added to the Na2SO4 solution in the cathode region to make the NaNO3 concentration 0.5 M, and NO3 - The counter electrode, reference electrode and working electrode are located on the anode and cathode sides of the H-type electrolytic cell, respectively, separated by a Nafion117 proton exchange membrane. The proton exchange membrane only allows hydrogen ions to pass between the solutions on both sides of the electrolytic cell (the cathode and anode regions), preventing the cathode products from being oxidized at the anode. In an argon atmosphere, the time-current curve of the system at the catalytic potential was tested, with a voltage test range of -0.1V to -0.5V (reversible hydrogen electrode potential), an interval of 0.1V, and a test time of 2h. The total current Q of the process was recorded, and the electrolyte was quickly taken out from the cathode cell, and the ammonia in the electrolyte was quantified by the indophenol blue method.

[0068] (1) Ammonia yield: It measures the reaction rate of NH3 production and can be calculated using the following formula: Yield = (C NH3 ×V) / (M NH3 ×t×M).

[0069] (2) Faradaic efficiency (FE): It measures the selectivity of NH3 production and is calculated as follows: Faradaic efficiency = (8F × C NH3 ×V) / (M NH3 ×Q).

[0070] In the above formula, C NH3 is the NH3 concentration (μg / mL) measured by the indophenol blue method, V is the volume of the electrolyte in the reaction cell (mL), t is the reduction reaction time (h), and M NH3 is the molar mass of ammonia (17 g / mol), M is the mass of the catalyst, F is the Faraday constant (96485 C / mol), and Q is the total charge Q(C).

[0071] pass Figure 1 It can be seen that the layered stacking diffraction peak of Comparative Example 1 indicates that a single-layer ruthenium dioxide nanosheet is successfully synthesized; while there is no obvious change in the XRD between Examples 1-4 and Comparative Example 1, indicating that La, Ce, Eu, and Er are doped into the ruthenium dioxide nanosheet in the form of single atoms. Figures 2 to 6 The ruthenium dioxide nanosheets have high transparency, wrinkles, and sheet-like morphology. Figures 2 to 6 By comparison, it can be seen that the rare earth metal-doped single-layer ruthenium dioxide nanosheets of Examples 1 to 4 were successfully synthesized.

[0072] pass Figures 7 to 11 By comparison, it can be found that the Ce prepared in Example 2 0.1 –Ru 0.9 O2 has the best performance in electrocatalytic reduction of nitrate to ammonia. Compared with single-layer ruthenium dioxide nanosheets that are not doped with rare earth metals, its Faraday efficiency and ammonia yield are greatly improved.

[0073] The performance of the electrochemical synthesis of ammonia by ruthenium dioxide nanosheets of Examples 1 to 4 and Comparative Example 1 is shown in Table 1. It can be seen from Table 1 that after the ruthenium dioxide nanosheets are doped with rare earth metals, the Faraday efficiency and ammonia yield of the electrocatalytic nitrate reduction are significantly improved. Among them, the Ce-doped ruthenium dioxide nanosheet has the best performance. At a potential of -0.4 V, its maximum Faraday efficiency is 95.6%, and the ammonia yield is 942 mmol h –1 g –1 .

[0074] Table 1 is a comparison of the performance of electrochemical synthesis of ammonia by ruthenium dioxide nanosheets in Examples 1 to 4 and Comparative Example 1

[0075] Serial number Maximum Faraday efficiency (%) <![CDATA[Ammonia production rate (mmol h –1 g –1 )]]> Example 1 85.2 683 Example 2 95.6 942 Example 3 68.9 475 Example 4 74.6 572 Comparative Example 1 43.5 245 .

Claims

1. A rare earth metal-doped ruthenium dioxide nanomaterial, characterized in that: Its chemical formula is: M x -Ru 1-X O2, where 0 < x ≤ 0.2; the rare earth metal M is one of La, Ce, Eu or Er.

2. The method for preparing the ruthenium dioxide nanomaterial according to claim 1, wherein: The steps include: (1) K2CO3, RuO2 and an oxide of a rare earth metal M are mixed and ground to obtain a mixture; (2) calcining the mixture of step (1) at 900°C to 1100°C for 55 to 65 min in an oxygen-containing environment, grinding the mixture after calcination, and further calcining the mixture at 900°C to 1100°C for 18 to 22 hours after grinding; repeating step (2) 1 to 2 times to obtain sample M x –K 0.2 Ru 1–x O2,0 <x≤0.2; (3) mixing the sample of step (2) with HCl solution, filtering, washing and drying after the reaction to obtain a precipitate; (4) stirring the precipitate of step (3) in an aqueous solution of tetrabutylammonium hydroxide to form a colloidal nanosheet suspension; (5) adding water to the colloidal nanosheet suspension of step (4), then centrifuging to remove tetrabutylammonium hydroxide in the suspension, and drying to obtain a rare earth metal-doped single-layer ruthenium dioxide nanosheet.

3. The method for preparing ruthenium dioxide nanomaterial according to claim 2, wherein: In step (1), the oxide of the rare earth metal M is one of La2O3, CeO2, Eu2O3 or Er2O3.

4. The method for preparing ruthenium dioxide nanomaterial according to claim 2, characterized in that: In step (2), the value of x is 0.01 to 0.

1.

5. The method for preparing ruthenium dioxide nanomaterial according to claim 2, characterized in that: In step (3), the concentration of the HCl solution is 0.5 to 1.5 mol / L.

6. The method for preparing the ruthenium dioxide nanomaterial according to claim 5, characterized in that: The sample of step (2) was mixed with HCl solution at a mass volume ratio of 0.008 to 0.012 g / mL.

7. The method for preparing ruthenium dioxide nanomaterial according to claim 2, characterized in that: In step (3), the reaction time is 65 to 75 hours.

8. The method for preparing ruthenium dioxide nanomaterial according to claim 2, characterized in that: In step (4), the concentration of the tetrabutylammonium hydroxide aqueous solution is 0.02 to 0.05 mol / L; and the stirring time is 10 to 13 days.

9. The method for preparing ruthenium dioxide nanomaterial according to claim 2, characterized in that: In step (5), the area of ​​the rare earth metal-doped single-layer ruthenium dioxide nanosheet is 1 to 20 μm 2 ; The thickness of the nanosheet is 1 to 2 nm.

10. Use of the ruthenium dioxide nanomaterial according to claim 1 as a catalyst in electrocatalytic synthesis of ammonia.