Method for preparing large-size single crystal metal foil through strain synergy

Through the strain collaborative preparation method, the high cost and equipment complexity of preparing large-size single crystal metal foils in the prior art are solved, and efficient preparation of low-purity metal foils is achieved and substrates suitable for new two-dimensional materials are realized. It has strong universality and low cost characteristics.

CN118996597AActive Publication Date: 2024-11-22HARBIN INST OF TECH
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202411110600.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-13
Publication Date
2024-11-22
Estimated Expiration
2044-08-13

Smart Images

  • Figure CN118996597A_ABST
    Figure CN118996597A_ABST
Patent Text Reader

Abstract

The invention belongs to the technical field of metal foil single crystallization, and particularly relates to a method for preparing large-size single crystal metal foil through strain synergy. The method comprises the following steps: carrying out primary annealing treatment on an original metal foil to obtain a recrystallized polycrystalline metal foil, carrying out rolling treatment on the polycrystalline metal foil, and carrying out compression strain on the polycrystalline metal foil in the thickness direction to obtain a strain metal foil; and carrying out secondary annealing treatment on the strained metal foil to obtain the large-size single crystal metal foil with the low-index crystal face. The method provided by the invention can be suitable for the metal foil with low purity (99% or above), the single-crystal metal foil with the low-index crystal face is obtained, the method is high in universality, simple, efficient, high in repeatability and low in cost, and the method can be widely used for preparing the large-size high-quality single-crystal metal foil substrate with the low-index crystal face. The method has huge application potential in the field of novel two-dimensional photoelectric material epitaxial preparation.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of metal foil single crystalization, and in particular relates to a method for preparing large-size single crystal metal foil in a strain-cooperative manner. Background Art

[0002] At present, most commercial metal foils are polycrystalline foils, but single-crystal metal foils have better physical properties, such as better electrical and thermal conductivity, better flexibility and ductility. At the same time, because single-crystal metal foils have no grain boundaries, the surface atoms are oriented in the same way, and some individual crystal planes of metals have a small lattice mismatch with graphene [Cu(111): ~3~4%; Ni(111): ~1%; Co(0001): ~2%], they can be used as epitaxial growth substrates for large-size single-crystal new two-dimensional materials (graphene, hexagonal boron nitride, transition metal sulfides, etc.), such as copper foil, nickel foil, gold foil, etc. For example, graphene single crystal films are epitaxially grown on Cu(111) single crystal substrates, and single-layer MoS is epitaxially grown on Au(111) substrates. 2 Transition metal sulfide two-dimensional materials such as single crystal films, preparation of multilayer hexagonal boron nitride single crystal films and multilayer graphene single crystal films on Ni (111) substrates, etc.

[0003] The traditional method of synthesizing single crystal metals is to grow single crystals through bulk crystal growth (Czochralski method or Bridgman method), using the seed crystal of the single crystal as the initial growth surface, and slowly pulling the material in a molten state by rotation to achieve the growth of single crystals. At present, there are also research reports on depositing copper films on sapphire or annealing copper foil to form single crystal foil, such as temperature gradient annealing, contactless annealing and cyclic polishing annealing. These research works have achieved good results in the preparation of single crystal substrates.

[0004] However, depositing metal films such as copper on sapphire faces problems such as expensive sapphire substrates, rare magnetron sputtering equipment, and the easy condensation of copper films to form discontinuous films during high-temperature annealing. Among the methods for annealing single crystal metal foils, temperature gradient annealing requires precise temperature control experimental equipment. Both this method and contactless annealing require the original copper foil to have a specific texture in order to anneal into a single crystal copper foil. Cyclic polishing annealing has complex operations. The complexity of the operations, equipment, or use of polycrystalline metal foils with specific textures involved in these studies has hindered the widespread application of single crystal metal preparation methods.

[0005] How to increase the size of metal single crystals and reduce the preparation cost is of great significance for the application of various metal single crystals. Therefore, the current domestic metal material research field still needs to provide key technologies that can prepare metal single crystals on a large scale. Summary of the invention

[0006] The purpose of the present invention is to provide a method for strain-synergistically preparing large-sized single-crystalline metal foils. The method provided by the present invention can be adapted to metal foils with relatively low purity (99% or more) to obtain single-crystalline metal foils with low-index crystal planes. The method has strong universality, simplicity, high efficiency, high repeatability, and low cost. It can be widely used to prepare large-sized, high-quality single-crystalline metal foil substrates with low-index crystal planes, and has great application potential in the field of epitaxial preparation of new two-dimensional optoelectronic materials.

[0007] In order to achieve the above object, the present invention provides the following technical solutions:

[0008] The present invention provides a method for strain-synergistically preparing a large-size single crystal metal foil, comprising the following steps:

[0009] The original metal foil is subjected to a first annealing treatment to obtain a recrystallized polycrystalline metal foil, wherein the surface of the original metal foil is provided with pressing stripes, and the width of the original metal foil is ≥0.5 cm;

[0010] The polycrystalline metal foil is subjected to a rolling process, so that the polycrystalline metal foil generates a compressive strain in a thickness direction, thereby obtaining a strained metal foil;

[0011] The deformed metal foil is subjected to a second annealing treatment, abnormal grain growth occurs, and single crystal growth is performed to obtain a large-sized single crystal metal foil, wherein the large-sized single crystal metal foil is a single crystal metal foil having a low-index crystal plane.

[0012] Preferably, the original metal foil includes copper foil, gold foil, nickel foil, silver foil, cobalt foil, platinum foil or ruthenium foil.

[0013] Preferably, the purity of the original metal foil is ≥99wt%.

[0014] Preferably, the original metal foil has a thickness of ≥10 μm, a width of 0.5 to 30 cm, and a length of 1 to 100 cm.

[0015] Preferably, the temperature of the first annealing treatment is 850-2000° C., and the time is 0.5-12 hours.

[0016] Preferably, the compression deformation is 0.1 to 15%.

[0017] Preferably, the temperature of the second annealing treatment is 850-2000° C., and the time is 0.5-16 hours.

[0018] Preferably, the first annealing treatment and the second annealing treatment are performed in a reducing gas atmosphere, and the reducing gas includes an inert gas and hydrogen.

[0019] The present invention provides a large-sized single-crystal metal foil, which is prepared by the method described in the above technical solution. The large-sized single-crystal metal foil is a single-crystal metal foil with a low-index crystal plane.

[0020] Preferably, the single crystal plane of the large-size single crystal metal foil is a 111 crystal plane or a 100 crystal plane.

[0021] The present invention provides a method for preparing a large-size single-crystalline metal foil by strain synergy, comprising the following steps: subjecting an original metal foil to a first annealing treatment to obtain a recrystallized polycrystalline metal foil, wherein the surface of the original metal foil is distributed with rolling stripes, and the width of the original metal foil is ≥0.5 cm; subjecting the polycrystalline metal foil to a rolling treatment to cause a compressive strain in the thickness direction of the polycrystalline metal foil to obtain a strained metal foil; subjecting the deformed metal foil to a second annealing treatment to cause abnormal grain growth to perform single crystal growth to obtain a large-size single-crystalline metal foil, wherein the large-size single-crystalline metal foil is a single-crystalline metal foil with a low-index crystal plane. The method provided by the present invention first subjects the original metal foil to a first annealing treatment, and subjecting the polycrystalline metal foil obtained after the first annealing to a rolling treatment to apply a certain amount of strain to the metal foil, using the strain to form storage energy, and then subjecting the metal foil to a second annealing treatment to cause the strain energy to promote abnormal grain growth, thereby obtaining a large-size single-crystalline metal foil, which can be used as a growth substrate for a new type of two-dimensional material. The method provided by the present invention can be adapted to metal foils with relatively low purity (above 99%) to obtain single crystal metal foils with low-index crystal planes. The method has strong universality, simplicity, high efficiency, high repeatability and low cost. It can be widely used to prepare large-size, high-quality single crystal metal foil substrates with low-index crystal planes, and has great application potential in the field of epitaxial preparation of new two-dimensional optoelectronic materials.

[0022] At the same time, the method provided by the present invention is not limited by the specific original texture of the original metal foil and the precision temperature gradient of the tube furnace. It can process a variety of original metal foils of any size and anneal to obtain large-sized single crystal metal foils. It has the characteristics of strong universality, simplicity, high efficiency, and high repeatability, and has important practical application value.

[0023] Furthermore, in the present invention, the purity of the original metal foil is ≥99wt%. Compared with the prior art, only high-purity (99.99% or more) commercial nickel foil can be used, and stress treatment is directly applied, and then high-temperature annealing is performed to obtain a single-crystalline nickel foil with a high-index crystal plane. The method provided by the present invention is suitable for preparing large-size single-crystalline metal foils from metal foils with lower purity (99% or more). The present invention first anneals the metal foil of the commercial metal foil (purity of 99% or more) to obtain a polycrystalline metal foil with a multi-grain distribution after recrystallization, and then applies roller pressure stress treatment, and finally performs annealing to obtain a single-crystalline metal foil with a low-index crystal plane (such as 111 crystal plane or 100 crystal plane). The method provided by the present invention is also suitable for metal foils with lower purity (99% or more). In a polycrystalline metal foil composed of multiple grains, the grain boundaries reach a state of equilibrium and stability, and the surface energy is insufficient to drive grain boundary migration and cause abnormal grain growth. The introduction of strain energy can break this equilibrium state. The strain energy and surface energy work synergistically to enable the grains on the low-index crystal planes to expand and migrate, thereby forming a large-sized single crystal metal foil. BRIEF DESCRIPTION OF THE DRAWINGS

[0024] Figure 1 Digital images and optical microscope images of the polycrystalline copper foil prepared by the conventional annealing method and the single crystal copper foil prepared by the rolling re-annealing method involved in the present invention;

[0025] Figure 2 The XRD diffraction pattern of the single crystal copper foil prepared by the present invention;

[0026] Figure 3 EBSD spectra of four random positions of the single crystal copper foil prepared by the present invention;

[0027] Figure 4 This is an optical microscope image of graphene grown on the single crystal copper foil prepared by the present invention;

[0028] Figure 5 Digital images, optical microscope images and XRD diffraction patterns of the polycrystalline gold foil prepared by the conventional annealing method and the single crystal gold foil prepared by the rolling re-annealing method involved in the present invention;

[0029] Figure 6 This is an optical microscope image of a polycrystalline copper foil with a purity of 99% after direct roll annealing involved in the present invention;

[0030] Figure 7 It is an operation flow chart and product characterization diagram of the method involved in the present invention. DETAILED DESCRIPTION

[0031] The present invention provides a method for strain-synergistically preparing a large-size single crystal metal foil, comprising the following steps:

[0032] The original metal foil is subjected to a first annealing treatment to obtain a recrystallized polycrystalline metal foil, wherein the surface of the original metal foil is provided with pressing stripes, and the width of the original metal foil is ≥0.5 cm;

[0033] The polycrystalline metal foil is subjected to a rolling process, so that the polycrystalline metal foil generates a compressive strain in a thickness direction, thereby obtaining a strained metal foil;

[0034] The deformed metal foil is subjected to a second annealing treatment, abnormal grain growth occurs, and single crystal growth is performed to obtain a large-sized single crystal metal foil, wherein the large-sized single crystal metal foil is a single crystal metal foil having a low-index crystal plane.

[0035] In the present invention, unless otherwise specified, all preparation raw materials / components are commercially available products well known to those skilled in the art.

[0036] The present invention performs a first annealing treatment on the original metal foil to obtain a recrystallized polycrystalline metal foil, wherein the surface of the original metal foil is distributed with rolling stripes, and the width of the original metal foil is ≥0.5 cm. In the present invention, the original metal foil is preferably a commercial metal foil, and the original metal foil is directly purchased from the market. The original metal foil preferably includes copper foil, gold foil, nickel foil, silver foil, cobalt foil, platinum foil, tungsten foil, iron foil or ruthenium foil, and more preferably copper foil, gold foil, nickel foil or silver foil. The purity of the original metal foil is preferably ≥99wt%, and specifically preferably 99wt%.

[0037] In the present invention, the thickness of the original metal foil is preferably ≥10 μm, more preferably 10 to 300 μm, further preferably 10 to 200 μm, and most preferably 20 to 120 μm. The width of the original metal foil is preferably 0.5 to 30 cm, more preferably 1 to 20 cm. The length of the original metal foil is preferably 1 to 100 cm, more preferably 1 to 40 cm. In a specific embodiment of the present invention, the width of the original metal foil is 10 cm, the length is 30 cm, and the thickness is 30 to 100 μm.

[0038] In the present invention, the first annealing treatment is preferably carried out in a chemical vapor deposition tube furnace. The temperature of the first annealing treatment is preferably 850-2000°C, more preferably 900-1500°C, and specifically preferably 1050°C; the time of the first annealing treatment is 0.5-12h, more preferably 1-10h. In the present invention, the heating time from room temperature to the temperature of the first annealing treatment is preferably 100-150min. The first annealing treatment is preferably carried out under normal pressure or negative pressure, and is further preferably carried out under normal pressure. The first annealing treatment is preferably carried out in a reducing gas atmosphere, and the reducing gas preferably includes an inert gas and hydrogen. The inert gas is preferably argon. In the present invention, the reducing gas is preferably a flowing gas, and the flow rate of the inert gas in the reducing gas is preferably 400-450sccm, and the flow rate of hydrogen is preferably 80-90sccm.

[0039] In the present invention, during the first annealing treatment, the original metal foil is recrystallized, and grain boundaries are distributed all over the surface, thereby obtaining a recrystallized polycrystalline metal foil.

[0040] After obtaining the polycrystalline metal foil, the present invention performs a rolling process on the polycrystalline metal foil, and the polycrystalline metal foil undergoes compressive strain in the thickness direction to obtain a strained metal foil. In the present invention, the rolling process preferably uses a pressure roller to apply pressure to the surface of the polycrystalline metal foil, so that the polycrystalline metal foil undergoes compressive strain in the thickness direction. In the present invention, the compressive deformation amount is preferably 0.1 to 15%, more preferably 0.2 to 12%, and most preferably 0.5 to 10%. The compressive deformation amount is the deformation amount of the polycrystalline metal foil in the thickness direction. In the present invention, the rolling process preferably uses an upper pressure roller and a lower pressure roller to achieve rolling of the polycrystalline metal foil in the form of self-rotation. The upper pressure roller and the lower pressure roller are located at the upper and lower surfaces of the polycrystalline metal foil. The moving speed of the polycrystalline metal foil during the rolling process is preferably 0.1 to 0.2 m / s.

[0041] After obtaining the strained metal foil, the present invention performs a second annealing treatment on the strained metal foil to obtain a large-sized single-crystalline metal foil, wherein the large-sized single-crystalline metal foil is a single-crystalline metal foil with a low-index crystal plane. In the present invention, the second annealing treatment is performed in a chemical vapor deposition tube furnace. The temperature of the second annealing treatment is preferably 850-2000°C, more preferably 900-1800°C, most preferably 900-1500°C, and specifically preferably 1050°C; the time of the second annealing treatment is preferably 0.5-16h, more preferably 0.5-14h, most preferably 0.2-12h, and specifically preferably 6h. In the present invention, the heating time from room temperature to the temperature of the second annealing treatment is preferably 100-150min. The second annealing treatment is preferably performed under normal pressure or negative pressure, and more preferably under normal pressure. The second annealing treatment is preferably performed in a reducing gas atmosphere, and the reducing gas preferably includes an inert gas and hydrogen. The inert gas is preferably argon. The present invention has no special requirements on the volume ratio of the inert gas to hydrogen.

[0042] The method provided by the present invention can effectively solve the problem that the existing method for preparing single crystal metal foil is limited by the texture, thickness, etc. of the original copper foil. Large-sized single crystal metal foil can be prepared efficiently and stably. For individual metal foils, the crystal plane can be regulated to obtain single crystal metal foil with low-index crystal plane, thereby ultimately realizing the epitaxial growth of single crystal thin films of two-dimensional materials.

[0043] The present invention provides a large-sized single-crystal metal foil, which is prepared by the method described in the above technical solution. The large-sized single-crystal metal foil is a single-crystal metal foil with a low-index crystal plane.

[0044] In the present invention, the single crystal plane of the large-size single crystal metal foil is a 111 crystal plane or a 100 crystal plane.

[0045] In order to further illustrate the present invention, the technical solutions provided by the present invention are described in detail below in conjunction with embodiments, but they should not be construed as limiting the protection scope of the present invention.

[0046] The following examples are based on Figure 7 Large-size single crystal metal foils are prepared using the preparation process in .

[0047] Example 1

[0048] This example provides a method for strain-synergistically preparing a large-size single crystal metal foil, taking copper foil as an example, including the following steps:

[0049] A commercial copper foil with a width of 10 cm, a length of 30 cm, and a thickness of 30 microns, with a purity of 99%, was subjected to the first annealing treatment in a chemical vapor deposition tube furnace. The annealing treatment was carried out under normal pressure conditions in a reducing atmosphere containing a mixture of argon and hydrogen. 400 sccm of argon and 80 sccm of hydrogen were introduced into the chemical vapor deposition tube furnace. After the air was exhausted, the temperature was raised to 1050°C within 100 minutes, and a constant temperature annealing treatment was carried out at normal pressure for 1 hour. The metal foil was recrystallized, and grain boundaries were distributed all over the surface; a polycrystalline copper foil after recrystallization was obtained;

[0050] The polycrystalline copper foil is then rolled on a double-axis roller press, and the distance between the rollers is adjusted to control the deformation of the copper foil. The polycrystalline copper foil is then passed between the two rollers at a speed of 0.1 m / s, and the deformation is between 1.5 and 2%.

[0051] The copper foil after rolling treatment is subjected to a second annealing treatment. 400sccm argon and 80sccm hydrogen are introduced into a chemical vapor deposition tube furnace. After exhausting the air, the temperature is raised to 1050°C within 100 minutes and constant temperature annealing is performed under normal pressure for 6 hours. After natural cooling, a large-size single crystal copper foil can be obtained.

[0052] Comparative Example 1

[0053] The method is basically the same as that of Example 1, except that the rolling process between the first annealing and the second annealing in Example 1 is omitted. In the method provided in this comparative example, no strain is applied, and a polycrystalline copper foil is obtained without large-area single crystal growth.

[0054] The digital images and optical microscope images of the polycrystalline copper foil prepared by the conventional annealing method in Comparative Example 1 and the single crystal copper foil prepared by the annealing treatment-rolling-reannealing method in Example 1 are as follows: Figure 1 As shown, Figure 1 (a) is a digital image of the polycrystalline metal foil prepared in Comparative Example 1. Figure 1 (f) is a digital image of the large-size single crystal copper foil prepared in Example 1. Figure 1 (b), (c), (d) and (e) are optical microscope images of the polycrystalline metal foil prepared in Comparative Example 1. Figure 1 (g), (h), (i) and (j) are optical microscope images of the large-sized single crystal copper foil prepared in Example 1. Figure 2 The XRD diffraction pattern of the single crystal copper foil obtained in Example 1 is as follows: Figure 2 The four XRD diffraction curves in are Figure 1 The test results of four random positions in (f) are given by Figure 2It can be seen that the test results at any position of the large-size single-crystal copper foil prepared in Example 1 are all 111 crystal plane diffraction peaks, which can further illustrate the single crystal nature of the large-area copper foil prepared in Example 1. Figure 3 EBSD spectra of four random positions of the single crystal copper foil prepared in Example 1. Figures 1 to 3 This reflects the single crystal characteristics of the large-sized single crystal copper foil prepared in Example 1. Figure 4 This is an optical microscope image of graphene grown on the large-size single-crystal copper foil prepared in Example 1. The graphene is grown by chemical vapor deposition, where the single-crystal copper foil is heated to 1050°C in an atmosphere of 250 sccm argon and 20 sccm hydrogen, and 3 sccm methane is introduced for 10 minutes. Figure 4 It can be seen that the large-size single-crystal copper foil prepared in Example 1 can realize the epitaxial growth of single-crystal thin films of two-dimensional materials.

[0055] Example 2

[0056] This embodiment provides a method for large-size single crystal gold foil. The difference from Embodiment 1 is that the commercial copper foil in Embodiment 1 is replaced by commercial gold foil. The thickness of the gold foil is 100 μm. The second annealing temperature is 1050° C. The remaining steps and parameters are the same as those in Embodiment 1.

[0057] The XRD diffraction pattern and optical microscope image of the large-size single crystal gold foil prepared in this example are as follows: Figure 5 As shown in the right figure of the middle part, the crystal plane of the large-sized single crystal gold foil prepared in this embodiment is a 111 crystal plane.

[0058] Comparative Example 2

[0059] The method is basically the same as that of Example 2, except that the rolling process between the first annealing and the second annealing in Example 2 is omitted. In the method provided in this comparative example, no strain is applied, and a polycrystalline gold foil is obtained without large-area single crystal growth.

[0060] The digital images, optical microscope images and XRD diffraction patterns of the polycrystalline gold foil prepared by the conventional annealing method in Comparative Example 2 and the single crystal gold foil prepared by the annealing treatment-rolling-reannealing method in Example 2 are as follows: Figure 5 As shown, Figure 5 The left picture in the figure is the XRD diffraction pattern and optical microscope image of the polycrystalline gold foil prepared in Comparative Example 2. Figure 5 The right figure in the figure is the XRD diffraction pattern and optical microscope image of the large-size single crystal gold foil prepared in Example 2. Figure 5 It can be seen that the crystal plane of the large-sized single-crystalline gold foil prepared in Example 2 is a 111 crystal plane, while the product prepared in Comparative Example 2 is a polycrystalline gold foil.

[0061] Comparative Example 3

[0062] The method provided in Comparative Example 3 is basically the same as that in Example 1, except that the commercial copper foil with a purity of 99% in Example 1 is subjected to roller pressing and second annealing without the first annealing treatment. The optical microscope image of the obtained metal foil product is as follows: Figure 6 shown. Figure 6 This is an optical microscope image of the polycrystalline copper foil of 99% purity after direct roll annealing in Comparative Example 3. Figure 6 It can be seen that commercial copper foil with a purity of 99% cannot be subjected to direct roll-pressing annealing to obtain single-crystal copper foil, but only polycrystalline copper foil.

[0063] From the above embodiments, it can be seen that the present invention performs a first annealing treatment on the original metal foil, the original metal foil undergoes recrystallization, and obtains a polycrystalline metal foil. The polycrystalline metal foil is subjected to a rolling treatment, and the polycrystalline metal foil undergoes compressive strain in the thickness direction, and obtains a strained metal foil; the strained metal foil is subjected to a second annealing treatment to obtain a large-sized single-crystalline metal foil with a low-index crystal plane. The method provided by the present invention can be adapted to metal foils with low purity (99% or more) to obtain a single-crystalline metal foil with a low-index crystal plane. The method has strong universality, is simple and efficient, has high repeatability, and is low in cost. It can be widely used to prepare large-sized, high-quality single-crystalline metal foil substrates with low-index crystal planes, and has great application potential in the field of epitaxial preparation of new two-dimensional optoelectronic materials.

[0064] Although the above embodiment describes the present invention in detail, it is only a part of the embodiments of the present invention, not all of the embodiments. Other embodiments can be obtained based on this embodiment without creativity, and these embodiments all fall within the protection scope of the present invention.

Claims

1. A method for strain-synergistically preparing large-size single-crystal metal foil, characterized in that: The following steps are involved: Performing a first annealing treatment on the original metal foil to obtain a recrystallized polycrystalline metal foil, wherein the surface of the original metal foil has rolling stripes, and the width of the original metal foil is greater than or equal to 0.5 cm; Rolling the recrystallized polycrystalline metal foil to generate compressive strain in the thickness direction of the polycrystalline metal foil to obtain a strained metal foil; The strained metal foil is subjected to a second annealing treatment to generate abnormal grain growth and perform single crystal growth to obtain a large-sized single crystal metal foil. The large-sized single crystal metal foil is a single crystal metal foil having a low-index crystal plane.

2. The method according to claim 1, characterized in that The original metal foil includes copper foil, gold foil, nickel foil, silver foil, cobalt foil, platinum foil, tungsten foil, iron foil or ruthenium foil.

3. The method according to claim 2, characterized in that The purity of the original metal foil is ≥99 wt %.

4. The method according to any one of claims 1 to 3, characterized in that The original metal foil has a thickness of ≥10 μm, a width of 0.5 to 30 cm, and a length of 1 to 100 cm.

5. The method according to claim 1, characterized in that The temperature of the first annealing treatment is 850-2000° C., and the time is 0.5-12 hours.

6. The method according to claim 1 or 5, characterized in that The compressive strain deformation is 0.1 to 15%.

7. The method according to claim 1, characterized in that The temperature of the second annealing treatment is 850-2000° C., and the time is 0.5-16 hours.

8. The method according to claim 1, 5 or 7, characterized in that The first annealing treatment and the second annealing treatment are performed in a reducing gas atmosphere, and the reducing gas includes an inert gas and hydrogen.

9. A large-sized single crystal metal foil, characterized in that: Prepared by the method according to any one of claims 1 to 8, the large-sized single crystal metal foil is a single crystal metal foil having a low-index crystal plane.

10. The large-sized single crystal metal foil according to claim 9, characterized in that The single crystal plane of the large-size single crystal metal foil is a 111 crystal plane or a 100 crystal plane.

Citation Information

Patent Citations

  • Preparation method of large-size Cu(100) single-crystal copper foil

    CN105714382A

  • Method for preparing monocrystal metal foil

    CN108950684A

  • Preparation method of ultra-large-area single crystal metal foil

    CN114561696A

  • Rolled copper foil and manufacturing method thereof

    US20080099110A1