Preparation method of large-area two-dimensional alpha-phase molybdenum trioxide single crystal
By controlling the growth temperature and cooling rate on the mica substrate by CVD one-step method, a high-purity and high crystallinity two-dimensional large-a-phase molybdenum trioxide single crystal was prepared, which solved the preparation problems in the prior art and realized nanoelectronics Development of devices and ultra-short channel field effect transistors.
Patent Information
- Application Number
- CN202411119754.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-15
- Publication Date
- 2024-11-22
AI Technical Summary
The prior art is difficult to prepare large-area high-quality two-dimensional alpha-phase molybdenum trioxide single crystals, which hinders its application in low-power nanoelectronic devices and ultra-short channel field effect transistors.
Using the one-step chemical vapor deposition (CVD) method, two-dimensional α-phase molybdenum trioxide single crystals are grown on the mica substrate by controlling the growth temperature and cooling rate, and the nucleation density and Gibb are regulated by the bending of metal molybdenum sheets and the mica spacing. This free energy induced, achieving the preparation of two-dimensional large-area α-phase molybdenum trioxide single crystals at the millimeter level.
A high-purity and high crystallinity two-dimensional large-a-a-phase molybdenum trioxide single crystal was successfully prepared, with good air stability and high dielectric properties, and promoted the future development of nanoelectronic devices and ultra-short channel field effect transistors.
Smart Images

Figure CN118996618A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of materials and relates to a method for preparing a large-area two-dimensional alpha-phase molybdenum trioxide single crystal. Background Art
[0002] Large-area preparation of two-dimensional high-k dielectric materials is crucial for the construction of low-power nanoelectronic devices and the future development of ultrashort channel field-effect transistors that are immune to short-channel effects. The growing interest in using two-dimensional (2D) semiconductors as channel materials in transistors has prompted the integration of these materials with large-area high-quality dielectric materials. However, such integration remains a challenge, and the low dielectric constant and high leakage current of traditional three-dimensional dielectrics such as h-BN, which require deposition processes, hinder their full potential in future transistors. As a high-k van der Waals material, α-phase MoO3 has been demonstrated to be used as a dielectric layer for two-dimensional field-effect transistors (FETs), demonstrating its potential as a promising high-k 2D van der Waals gate dielectric. However, current reports on the preparation of α-phase MoO3 materials mainly focus on bulk or micron-sized types. Therefore, the controllable preparation technology of large-area 2D α-phase MoO3 single crystals remains a huge challenge. Summary of the invention
[0003] Purpose of the invention: Based on the existing problems in the synthesis process of two-dimensional large-area α-phase molybdenum trioxide single crystals, the present invention aims to provide a method for regulating and preparing two-dimensional large-area α-phase molybdenum trioxide single crystals. The method has simple process, low requirements for tube furnaces, short production cycle, and the sample can be prepared at normal pressure under an inert gas atmosphere.
[0004] Technical solution: The present invention discloses a method for preparing a large-area two-dimensional α-phase molybdenum trioxide single crystal, which utilizes a one-step CVD method to prepare a two-dimensional large-area α-phase molybdenum trioxide single crystal, and controls the growth temperature and the cooling rate to control the thickness and area to synthesize a two-dimensional large-area α-phase molybdenum trioxide single crystal with a lateral size of millimeters. During the growth of the two-dimensional large-area α-phase molybdenum trioxide single crystal, the growth temperature is 520-550°C, and the cooling rate is 4.6°C / min-127°C / min.
[0005] Furthermore, the CVD one-step method specifically comprises the following steps:
[0006] (1) The metal molybdenum sheet is uniformly bent to a certain curvature, and then the peeled mica is covered on the upper surface of the metal molybdenum sheet. The curvature of the bending of the metal molybdenum sheet is used to control the distance between the metal molybdenum sheet and the mica, and the distance is controlled within 0.5 mm;
[0007] (2) Preparation of two-dimensional large-area α-phase molybdenum trioxide single crystals: In a slidable tubular furnace, a combination of mica and metal molybdenum sheets is placed in the center of a long cooling zone furnace. Under oxygen gas, the growth of α-phase molybdenum trioxide is controlled by using the effects of growth temperature and cooling rate on the growth of α-phase molybdenum trioxide to prepare two-dimensional large-area α-phase molybdenum trioxide single crystals.
[0008] Furthermore, in step (1), the layered mica is peeled off to expose a flat surface as a substrate for growing α-phase molybdenum trioxide, the metal molybdenum sheet is polished, and the peeled mica is covered on the upper surface of the metal molybdenum sheet, with the spacing controlled within 0.5 mm.
[0009] Furthermore, in step (1), after the metal molybdenum sheet is cut, it is evenly bent into an arc with a curvature of 0.08, and the peeled mica is covered on the upper surface of the metal molybdenum sheet, and the spacing is controlled within 0.2-0.5 mm.
[0010] Furthermore, in step (2), when the maximum growth temperature is reached, the mica and metal molybdenum sheet combination is pushed into the heating zone in the tube furnace.
[0011] Furthermore, in step (2), the cooling zone of the tubular furnace is 10-15 cm long.
[0012] Furthermore, in step (2), the gas introduced into the tube furnace is high-purity oxygen, and preferably, the gas flow rate is 600-800 sccm.
[0013] Furthermore, in step (2), the growth time of α-MoO3 is 120-360 min.
[0014] On the other hand, the present invention provides a method for preparing the above-mentioned large-area two-dimensional α-phase molybdenum trioxide single crystal.
[0015] The present invention discloses a method for preparing a two-dimensional large-area α-phase molybdenum trioxide single crystal, comprising the following steps: uniformly bending a metal molybdenum sheet to a certain curvature, covering the peeled mica on the upper surface of the metal molybdenum sheet, that is, controlling the spacing between the metal molybdenum sheet and the mica within 0.2-0.5 mm, placing the mica and the metal molybdenum sheet in a tube furnace, and then controlling the growth parameters (including temperature, gas flow rate, cooling rate, and holding time) by a one-step chemical vapor deposition method (CVD) to grow α-phase molybdenum trioxide crystals on a mica substrate (mica). The curvature of the metal molybdenum sheet makes the distance between the substrate and the source different, thereby making the saturated vapor pressure difference distribution during the period, and using the multiple control strategies induced by nucleation density and Gibbs free energy to control the thickness and area to synthesize a two-dimensional α-phase molybdenum trioxide single domain, so as to obtain a two-dimensional large-area α-phase molybdenum trioxide single crystal with a lateral size of millimeter level, and they all show good air stability.
[0016] The CVD growth method shows unique advantages in the large-area preparation of two-dimensional materials due to its simple operation process and low cost. In the CVD system, the effective control of the large-area growth of two-dimensional α-phase molybdenum trioxide depends to a large extent on the thermodynamic driving force between the target two-dimensional material and the substrate surface. Since the binding energy between the epitaxial growth of the target two-dimensional material and the substrate interface is regulated by macroscopic conditions, the CVD growth method has great potential in synthesizing two-dimensional large-area α-phase molybdenum trioxide single crystals. The preparation method of a large-area two-dimensional α-phase molybdenum trioxide single crystal of the present invention prepares a two-dimensional large-area α-phase molybdenum trioxide single crystal with a size of millimeter level, which has high dielectric properties and high stability and repeatability. The present invention has a very great prospect for promoting the future construction of low-power nanoelectronic devices and the future development trend of preparing ultra-short channel field effect transistors that are immune to short channel effects.
[0017] Beneficial effects: Compared with the prior art, the present invention has the following significant advantages: The present invention develops a method for preparing a large-area two-dimensional α-phase molybdenum trioxide single crystal, and adopts a van der Waals epitaxial growth method to achieve the growth of a two-dimensional large-area α-phase molybdenum trioxide single crystal with high purity and high crystallinity. Large-area thin film epitaxy is driven by the thermodynamic driving force caused by the synergistic effect of nucleation density regulation and Gibbs free energy induction. The layered mica material as a substrate provides a platform for van der Waals epitaxy and induces the formation of a large-area thin film of two-dimensional molybdenum trioxide with an α phase. It provides a valuable reference in guiding the regulation and preparation of large-area thin films of other two-dimensional materials. BRIEF DESCRIPTION OF THE DRAWINGS
[0018] Figure 1 It is a schematic diagram of a CVD device and a growth control schematic diagram of a two-dimensional large-area α-phase molybdenum trioxide single crystal prepared by the method of the present invention;
[0019] Figure 2It is an optical microscope image of a two-dimensional large-area α-phase molybdenum trioxide single crystal prepared by the method of the present invention;
[0020] Figure 3 It is an XRD phase characterization diagram of the α crystal phase of a two-dimensional large-area α-phase molybdenum trioxide single crystal prepared by the method of the present invention;
[0021] Figure 4 These are Raman and Raman area scanning characterization images of a two-dimensional large-area α-phase molybdenum trioxide single crystal prepared by the method of the present invention, wherein Figure a is a Raman spectrum; Figure b is a Raman area scanning characterization image.
[0022] Figure 5 The optical microscope images of the effect of growth temperature on the growth of two-dimensional large-area α-phase molybdenum trioxide single crystals using the method of the present invention are shown in FIG. a, wherein FIG. b is an optical microscope image at 570°C; FIG. b is an optical microscope image at 560°C; FIG. c is an optical microscope image at 550°C; FIG. d is an optical microscope image at 540°C; FIG. e is an optical microscope image at 530°C; FIG. f is an optical microscope image at 520°C; FIG. g is an optical microscope image at 510°C; and FIG. h is a graph showing thickness changing with temperature.
[0023] Figure 6 The optical microscope images of the influence of the cooling rate in the method of the present invention on the growth of two-dimensional large-area α-phase molybdenum trioxide single crystals are shown, wherein Figure a is an optical microscope image at a cooling rate of 4.6°C / min; Figure b is an optical microscope image at a cooling rate of 17.5°C / min; Figure c is an optical microscope image at a cooling rate of 26.9°C / min; Figure d is an optical microscope image at a cooling rate of 127°C / min; and Figure e is a graph of temperature change over time.
[0024] Figure 7 It is a thickness statistical distribution of a two-dimensional large-area α-phase molybdenum trioxide single crystal sample prepared by the method of the present invention, wherein Figure a is an atomic force microscopy image of selected area one; Figure b is an atomic force microscopy image of selected area two; Figure c is an atomic force microscopy image of selected area three; Figure d is an atomic force microscopy image of selected area four; Figure e is an atomic force microscopy image of selected area five; Figure f is an atomic force microscopy image of selected area six; Figure g is an atomic force microscopy image of selected area seven; and Figure h is an atomic force microscopy image of selected area eight.
[0025] Figure 8 This is an optical microscope image of the growth of a two-dimensional large-area α-phase molybdenum trioxide single crystal prepared by the method of Comparative Example 1.
[0026] Fig. 9 This is an optical microscope image of the growth of a two-dimensional large-area α-phase molybdenum trioxide single crystal prepared by the method of Comparative Example 2.
[0027] Fig.10 This is an optical microscope image of the growth of a two-dimensional large-area α-phase molybdenum trioxide single crystal prepared by the method of Comparative Example 3.
[0028] Fig.11 This is an optical microscope image of the growth of a two-dimensional large-area α-phase molybdenum trioxide single crystal prepared by the method of Comparative Example 4. DETAILED DESCRIPTION
[0029] In order to further understand the content of the present invention, the present invention is described in detail in conjunction with the accompanying drawings and embodiments.
[0030] like Figure 1 As shown, an embodiment of the present invention provides a method for preparing a large-area two-dimensional α-phase molybdenum trioxide single crystal, comprising the following steps:
[0031] (1) Covering the peeled mica on the upper surface of the metal molybdenum sheet with a spacing of less than 0.5 mm: peeling the layered mica to expose a flat surface as a substrate for growing α-phase molybdenum trioxide, polishing the metal molybdenum sheet, cutting the metal molybdenum sheet, and evenly bending it into an arc with a curvature of 0.08, and covering the peeled mica on the upper surface of the metal molybdenum sheet with a spacing of less than 0.2-0.5 mm.
[0032] (2) Preparation of two-dimensional large-area α-phase molybdenum trioxide single crystals: In a slidable long-range tubular furnace, a combination of mica and metal molybdenum flakes is placed in the center of a long cooling zone furnace. Under oxygen gas, the effects of gas flow rate, growth temperature and cooling rate on the growth of α-phase molybdenum trioxide are used to control the thickness and area of the synthesized two-dimensional α-phase molybdenum trioxide single domains, thereby obtaining a two-dimensional large-area α-phase molybdenum trioxide single crystal with a lateral size of millimeters. The cooling zone length of the tubular furnace is 10 cm. After the growth is completed, the combination of mica and metal molybdenum flakes is moved to a rapid cooling zone. The gas flow rate is 500-800sccm, the growth temperature is 520-550°C, and the growth time is 120-360min.
[0033] In order to further understand the content of the present invention, the present invention is described in detail in conjunction with the accompanying drawings and embodiments.
[0034] Example 1
[0035] A method for regulating and preparing a two-dimensional large-area α-phase molybdenum trioxide single crystal - a process in which growth temperature affects the growth of a two-dimensional large-area α-phase molybdenum trioxide single crystal, specifically comprising the following steps:
[0036] (1) Use scissors to cut the mica sheet and the metal molybdenum sheet into 2 cm × 2 cm pieces;
[0037] (2) Use a blade to peel off the surface of the mica sheet to expose a smooth and clean surface;
[0038] (3) polishing the metal molybdenum thin slice with sandpaper to remove the molybdenum oxide layer produced on the surface;
[0039] (4) After cutting the metal molybdenum sheet, evenly bend it into an arc with a curvature of 0.08, and cover the peeled mica on the upper surface of the metal molybdenum sheet with a spacing of 0.2-0.5 mm. Figure 1 ;
[0040] (5) The mica and metal molybdenum flakes are placed in the center of the long cooling zone furnace, such as Figure 1 ;
[0041] (6) setting the oxygen gas flow rate to a fixed value of 660 sccm;
[0042] (7) The growth temperature range was set to 510°C-570°C (α-MoO3) and the effect of growth temperature on the α-phase MoO3 film was studied in increments of 10°C.
[0043] (8) The growth temperature of the α-phase molybdenum trioxide thin film is specifically set to 510°C, 520°C, 530°C, 540°C, 550°C, 560°C, and 570°C.
[0044] (9) The growth parameters were set as follows: initial temperature 30 °C, heating rate 20 °C / min, and after reaching the growth temperature, keeping warm for 660 min;
[0045] (10) When the growth temperature is reached, the heating zone is moved to the combination of mica and metal molybdenum sheet, such as Figure 1 After the growth process is completed, the heating zone is quickly removed and the tube furnace is cooled at a rate of 127°C / min.
[0046] (12) After rapid cooling to room temperature, take out the sample. Figure 1 ;
[0047] (13) The prepared samples were characterized by optical microscopy (OM). It can be seen from the figure that the size of the prepared two-dimensional large-area α-phase MoO3 single crystal reached the millimeter level. Figure 2 Shown
[0048] (14) The prepared samples were characterized by X-ray diffractometer (XRD) and Raman spectroscopy to confirm the phase structure and high-quality uniformity of the prepared two-dimensional large-area α-phase MoO3 single crystal. The results are as follows: Figure 3-4 shown.
[0049] Figure 5This is an optical microscope image of the effect of growth temperature on the growth of a two-dimensional large-area α-phase molybdenum trioxide single crystal. It can be seen from the figure that as the growth temperature increases from a high growth temperature of 570°C to a low growth temperature of 510°C, the thickness of the two-dimensional large-area α-phase molybdenum trioxide single crystal grown on mica gradually changes from thick to thin, and there is an obvious color change on the surface of the material, from the characteristic blue-purple and goose yellow when thick to grayish white when thin. And from a slender shape when thick to a flake shape when thin, there is a trend of epitaxial film. Among them, at 520°C, the growth of two-dimensional α-phase molybdenum trioxide on mica has the best thickness.
[0050] Example 2
[0051] A method for controlling the preparation of a two-dimensional large-area α-phase molybdenum trioxide single crystal—a process in which a cooling rate affects the growth of a two-dimensional large-area α-phase molybdenum trioxide single crystal, specifically comprising the following steps:
[0052] (1) Use scissors to cut the mica sheet and the metal molybdenum sheet into 2 cm × 2 cm pieces;
[0053] (2) Use a blade to peel off the surface of the mica sheet to expose a smooth and clean surface;
[0054] (3) polishing the metal molybdenum thin slice with sandpaper to remove the molybdenum oxide layer produced on the surface;
[0055] (4) After cutting the metal molybdenum sheet, evenly bend it into an arc with a curvature of 0.08, and cover the peeled mica on the upper surface of the metal molybdenum sheet with a spacing of 0.2-0.5 mm. Figure 1 ;
[0056] (5) The mica and metal molybdenum flakes are placed in the center of the long cooling zone furnace, such as Figure 1 ;
[0057] (6) setting the oxygen gas flow rate to a fixed value of 660 sccm;
[0058] (7) The cooling rate range was set to 4.6°C / min-127°C / min by using a cooling device, and the effect of the cooling rate on the α-phase MoO2 film was studied according to the increasing cooling rate.
[0059] (8) Among them, the cooling rate of the α-phase molybdenum trioxide film is specifically controlled to be 4.6℃ / min, 17.5℃ / min, 26.9℃ / min, and 127℃ / min.
[0060] (9) The growth parameters were set as follows: initial temperature 30°C, heating rate 20°C / min, and after reaching the growth temperature 520°C, heat preservation for 660 min;
[0061] (10) When the growth temperature is reached, the heating zone is moved to the combination of mica and metal molybdenum sheet, such as Figure 1 ;
[0062] (11) After the growth process is completed, the heating zone is quickly removed, and the tube furnace is quickly cooled to room temperature at different cooling rates, and then the sample is taken out. Figure 1 ;
[0063] (12) The prepared samples were characterized by optical microscopy (OM). It can be seen from the figure that the size of the prepared two-dimensional large-area α-phase MoO3 single crystal reached the millimeter level. Figure 2 Shown
[0064] (13) The prepared samples were characterized by X-ray diffractometer (XRD) and Raman spectroscopy to confirm the phase structure and high-quality uniformity of the prepared two-dimensional large-area α-phase MoO3 single crystal. The results are as follows: Figure 3-4 shown.
[0065] Figure 6 The optical microscope image of the effect of cooling rate on the growth of two-dimensional large-area α-phase molybdenum trioxide single crystals. It can be seen from the figure that as the cooling rate increases from a low cooling rate of 4.6℃ / min to a high cooling rate of 127℃ / min, the size of the two-dimensional large-area α-phase molybdenum trioxide single crystals grown on mica gradually increases from more than ten microns to the millimeter level. It is obvious that with the increase in cooling rate, the size of the molybdenum trioxide crystal has a significant increasing trend. Among them, at a cooling rate of 127℃ / min, the size of the two-dimensional α-phase molybdenum trioxide crystal reached 1448 microns, with the optimal length.
[0066] The characterization means involved in the above embodiments are: X-ray diffractometer (XRD) and Raman spectrometer (Raman) are used to perform physical characterization on the prepared samples to determine whether the samples are α-phase molybdenum trioxide crystals. The morphological characteristics of all samples in the experiment are recorded by optical microscope (OM). The thickness of the samples is recorded by atomic force microscope (ΑFM), and the thickness distribution of the prepared samples is statistically analyzed.
[0067] Example 3
[0068] It can be seen from Examples 1-2 that the preferred growth parameters of two-dimensional large-area α-phase molybdenum trioxide crystals are: initial temperature 30°C, heating rate 20°C / min, and after reaching the growth temperature of 520°C, keeping warm for 660 minutes; this example is carried out according to the above conditions.
[0069] This embodiment provides a control method for a two-dimensional large-area α-phase molybdenum trioxide crystal, which specifically includes the following steps:
[0070] (1) Use scissors to cut the mica sheet and the metal molybdenum sheet into 2 cm × 2 cm pieces;
[0071] (2) Use a blade to peel off the surface of the mica sheet to expose a smooth and clean surface;
[0072] (3) polishing the metal molybdenum thin slice with sandpaper to remove the molybdenum oxide layer produced on the surface;
[0073] (4) After cutting the metal molybdenum sheet, evenly bend it into an arc with a curvature of 0.08, and cover the peeled mica on the upper surface of the metal molybdenum sheet with a spacing of 0.2-0.5 mm. Figure 1 ;
[0074] (5) The mica and metal molybdenum flakes are placed in the center of the long cooling zone furnace, such as Figure 1 ;
[0075] (6) setting the oxygen gas flow rate to a fixed value of 660 sccm;
[0076] (7) The growth temperature was set to 520°C;
[0077] (8) The growth parameters were set as follows: initial temperature 30°C, heating rate 20°C / min, and after reaching the growth temperature, keeping warm for 660 min;
[0078] (9) When the growth temperature is reached, the heating zone is moved to the combination of mica and metal molybdenum sheet, such as Figure 1 ;
[0079] (10) After the growth process is completed, the heating zone is quickly removed, and the tube furnace is rapidly cooled to room temperature at a cooling rate of 127°C / min, and the sample is taken out. Figure 1 ;
[0080] (11) The prepared samples were characterized by optical microscopy (OM). It can be seen from the figure that the size of the prepared two-dimensional large-area α-phase MoO3 single crystal reached the millimeter level. Figure 2 Shown
[0081] (12) The prepared samples were characterized by X-ray diffractometer (XRD) and Raman spectroscopy to confirm the phase structure and high-quality uniformity of the prepared two-dimensional large-area α-phase MoO3 single crystal. The results are as follows: Figure 3-4 shown.
[0082] Figure 7Shown is a two-dimensional large-area α-phase molybdenum trioxide single crystal prepared under the growth parameter conditions of a growth temperature of 520°C, a cooling rate of 127°C / min, and a holding time of 660 minutes, with other conditions remaining unchanged. It can be seen from the figure that the prepared two-dimensional large-area α-phase molybdenum trioxide single crystals can reach a few-layer thickness of ~4 nanometers.
[0083] Comparative Example 1
[0084] Compared with Example 1, the difference is that the growth temperature in step (7-8) is 450 degrees, and the remaining steps are the same as Example 1. Figure 8 Shown is a two-dimensional large-area α-phase molybdenum trioxide single crystal prepared under the growth parameter conditions of a growth temperature of 450°C, a cooling rate of 127°C / min, and a holding time of 660 minutes, with other conditions remaining unchanged. It can be seen from the figure that unformed molybdenum trioxide pre-materials are scattered on the substrate, and most of them are less than 10 microns in size, and a well-crystallized large-area molybdenum trioxide single crystal cannot be formed.
[0085] Comparative Example 2
[0086] Compared with Example 1, the difference is that the growth temperature in step (7-8) is 600 degrees, and the remaining steps are the same as Example 1. Fig. 9 Shown is a two-dimensional large-area α-phase molybdenum trioxide single crystal prepared under the growth parameter conditions of a growth temperature of 600°C, a cooling rate of 127°C / min, and a holding time of 660 minutes, with other conditions remaining unchanged. It can be seen from the figure that the prepared molybdenum trioxide single crystal is a bulk material, and is densely covered on the entire substrate surface, and cannot be extended into a thin film.
[0087] Comparative Example 3
[0088] Compared with Example 3, the difference is that the bending curvature of the metal molybdenum sheet in step (4) is 0.02, and the remaining steps are the same as Example 3. Fig.10 The preparation was carried out under the growth parameter conditions of growth temperature of 520°C, cooling rate of 127°C / min, holding time of 660 minutes, and other conditions remained unchanged. It can be seen from the figure that black-brown strip materials appeared on the surface of the substrate, showing a strip distribution. The distance between the substrate and the source material is too small, which limits the participation of oxygen in the reaction, resulting in the formation of sub-oxide molybdenum material that is not completely oxidized.
[0089] Comparative Example 4
[0090] Compared with Example 3, the difference is that the bending curvature of the metal molybdenum sheet in step (4) is 0.2, and the remaining steps are the same as Example 3. Fig.11The figure shows the preparation under the growth parameter conditions of growth temperature of 520°C, cooling rate of 127°C / min, holding time of 660 minutes, and other conditions remaining unchanged. It can be seen from the figure that no material is formed on the substrate surface, the distance between the substrate and the source material is too large, and the source material is difficult to supply to the substrate surface.
Claims
1. A method for preparing a large-area two-dimensional α-phase molybdenum trioxide single crystal, characterized in that: Two-dimensional large-area α-phase molybdenum trioxide single crystals were prepared by a one-step CVD method. By controlling the growth temperature and matching the temperature gradient of the cooling process, the two-dimensional α-phase molybdenum trioxide single crystals were synthesized by controlling the thickness and area, and a two-dimensional large-area α-phase molybdenum trioxide single crystal with a lateral size of millimeter level was obtained. During the growth of the two-dimensional large-area α-phase molybdenum trioxide single crystal, the growth temperature was 520-550℃, and the cooling rate was 4.6℃ / min-127℃ / min.
2. The method for preparing a large-area two-dimensional α-phase molybdenum trioxide single crystal according to claim 1, characterized in that: The CVD one-step method specifically includes the following steps: (1) The metal molybdenum sheet is evenly bent to a certain curvature, and then the peeled mica is covered on the upper surface of the metal molybdenum sheet. The curvature of the bending of the metal molybdenum sheet is used to control the distance between the metal molybdenum sheet and the mica, and the distance is controlled within 0.5 mm; (2) Preparation of two-dimensional large-area α-phase molybdenum trioxide single crystals: In a slidable tubular furnace, a combination of mica and metal molybdenum sheets is placed in the center of a long cooling zone furnace. The effects of growth temperature and cooling rate on the growth of α-phase molybdenum trioxide are used to control the preparation of two-dimensional large-area α-phase molybdenum trioxide single crystals.
3. The method for preparing a large-area two-dimensional α-phase molybdenum trioxide single crystal according to claim 2, characterized in that: In step (1), the layered mica is peeled off to expose a flat surface as a substrate for growing α-phase molybdenum trioxide, the molybdenum foil is polished, and the peeled mica is covered on the upper surface of the metal molybdenum sheet, with the spacing controlled within 0.5 mm.
4. The method for preparing a large-area two-dimensional α-phase molybdenum trioxide single crystal according to claim 3, characterized in that: In step (1), the distance between the metal molybdenum sheet and the mica is 0.2-0.5 mm.
5. The method for preparing a large-area two-dimensional α-phase molybdenum trioxide single crystal according to claim 2, characterized in that: In step (2), when the maximum growth temperature is reached, the mica and metal molybdenum sheet combination is pushed into the heating zone in the tube furnace.
6. The method for preparing a large-area two-dimensional α-phase molybdenum trioxide single crystal according to claim 3, characterized in that: In step (2), the cooling zone of the tubular furnace is 10-15 cm long.
7. The method for preparing a large-area two-dimensional α-phase molybdenum trioxide single crystal according to claim 1, characterized in that: The gas introduced into the tube furnace is high-purity oxygen.
8. The method for preparing a large-area two-dimensional α-phase molybdenum trioxide single crystal according to claim 7, characterized in that: In step (2), the flow rate of high purity oxygen is 600-800 sccm.
9. The method for preparing a large-area two-dimensional α-phase molybdenum trioxide single crystal according to claim 3, characterized in that: In step (2), the growth time of α-MoO3 is 120-360 min.
10. A two-dimensional large-area α-phase molybdenum trioxide single crystal prepared according to the method for preparing a large-area two-dimensional α-phase molybdenum trioxide single crystal according to any one of claims 1 to 9.