Self-monitoring cement-based material fracture characteristic high-precision test piece forming method
By adding electrode sheets and prefabricated cracked plates before forming the conductive concrete specimen, combined with high-precision three-point bending method testing, the problem of unused self-monitoring ability of conductive concrete in the traditional concrete fracture test method is solved, and the fracture of conductive concrete is achieved Accurate measurement of parameters and large-scale component load prediction.
Patent Information
- Application Number
- CN202410953116.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-16
- Publication Date
- 2024-11-22
AI Technical Summary
The traditional concrete fracture test method cannot effectively utilize the self-monitoring ability of conductive concrete, resulting in insufficient measurement of fracture parameters, and the loading speed of large-sized test pieces affects the test results.
Before forming the conductive concrete specimen, the electrode sheet is added, and the prefabricated crack plate and electrode mold design is used. The high-precision three-point bending method is used to measure the fracture parameters in real time using the self-monitoring ability of the conductive concrete to avoid delays from external sensors.
High-precision measurement of the fracture parameters of conductive concrete is achieved, and technical support is provided to predict peak fracture loads of large-scale conductive concrete components, improving the accuracy and convenience of testing.
Smart Images

Figure CN119000240A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of high-performance concrete materials and relates to a method for forming a high-precision test specimen for self-monitoring fracture characteristics of cement-based materials. Background Art
[0002] Conductive concrete is a composite material made by adding conductive materials to ordinary concrete. Due to its unique conductive properties, it is widely used in construction, environmental monitoring, electromagnetic shielding and other fields. However, the fracture properties of conductive concrete have an important impact on its application performance.
[0003] The traditional concrete three-point bending test uses external sensors to obtain test parameters such as stress and fracture area of concrete specimens. This method of obtaining test parameters from the outside has a certain delay, especially when judging the cracking and instability of concrete specimens. Conductive concrete is a material whose own resistance will change accordingly when subjected to external loads. Therefore, during the test, the conductive concrete specimen can truly reflect the state of the specimen itself through electrical signals such as the change in its own resistance and the speed of change. This method of measuring relevant test parameters from the inside of the specimen using the self-monitoring ability of conductive concrete is very important for accurately grasping the fracture parameters of conductive concrete. However, the specimens prepared by conventional fracture test specimen molding molds do not have the ability to measure test parameters using the specimen's own self-monitoring ability.
[0004] Conventional concrete fracture tests are conducted using larger specimens, which require larger test loads. This is quite different from the loading speed required for the test, which results in the loading speed affecting the test results. The microscope mechanical testing system is a machine that can conduct three-point bending fracture tests on small-sized conductive concrete. It has a higher accuracy in controlling the loading speed and can reduce the impact of the loading speed on the reliability of the fracture test results to a certain extent. By using the self-monitoring ability of conductive concrete materials through fracture tests on small-sized specimens, the fracture properties of conductive concrete can be studied more accurately, thereby obtaining material fracture parameters that are independent of specimen size and used to predict the fracture parameters of large-sized specimens. However, the conventional specimen molding molds for three-point bending tests of concrete fracture properties are generally larger-sized molds. Using the above molds, it is impossible to prepare small-sized specimens with prefabricated cracks that utilize the self-monitoring ability of conductive concrete, and it is difficult to accurately measure the fracture parameters of small-sized conductive concrete. Summary of the invention
[0005] The technical problem to be solved by the present invention is to provide a method for forming high-precision test specimens for self-monitoring the fracture characteristics of cement-based materials. Electrode sheets are added before the conductive concrete is formed, and the self-monitoring ability of the conductive concrete is used to measure the fracture parameters, revealing the fracture development process of the concrete, and providing technical support for predicting the peak fracture load of large-scale conductive concrete components.
[0006] In order to solve the above technical problems, the technical solution adopted by the present invention is: a high-precision test specimen for self-monitoring the fracture characteristics of cement-based materials, which includes an upper baffle, a lower baffle, mold baffles on both sides, a prefabricated crack plate, an electrode, a bottom plate, a bottom plate expansion plate and a fastening screw; the upper baffle, the lower baffle and the mold baffles on both sides are installed on the bottom plate to form a cavity for preparing the specimen; a through square prefabricated crack plate installation groove is arranged in the middle of the lower bottom surface of the upper baffle, the thickness of the prefabricated crack plate installation groove is consistent with the thickness of the prefabricated crack, and the prefabricated crack plate installation groove is perpendicular to the lower bottom surface; the toe end of the prefabricated crack plate installation groove is a right angle to better engage with the toe end of the prefabricated crack plate to prevent the prefabricated crack plate from shaking; two positioning screw holes are arranged at the corresponding installation positions of the upper baffle and the bottom plate of the mold but do not penetrate the upper baffle to maintain the flatness of the casting surface of the specimen; a mounting screw hole is arranged on each of the left and right sides of the upper baffle; it is applied to the preparation process of the specimen for self-monitoring the fracture characteristics of cement-based materials by the high-precision three-point bending method, and the prefabricated cracks and electrodes for monitoring signals are arranged at designated positions.
[0007] The upper baffle, lower baffle, mold baffles on both sides, prefabricated crack plate, bottom plate, and fastening top screws are made of stainless steel. The upper and lower baffles are of the same thickness as the mold baffles on both sides; the bottom plate expansion plate is made of stainless iron that can be adsorbed by magnets.
[0008] The screw hole on the right side of the upper baffle serves to connect the right mold baffle with the upper baffle, and the length of the screw hole penetrates to the square prefabricated crack plate installation groove at the bottom of the upper baffle, serving to fix the prefabricated crack plate.
[0009] Two electrode mounting grooves are symmetrically arranged on both sides of the upper top surface of the lower baffle plate, the mounting grooves are kept perpendicular to the upper top surface of the lower baffle plate, and the thickness is consistent with the thickness of the electrode; two positioning screw holes are arranged at the connection between the lower baffle plate and the mounting base plate but do not penetrate the lower baffle plate to maintain the flatness of the casting surface of the specimen; two mounting screw holes are arranged on each side of the lower baffle plate to connect with the lower part of the left and right mold baffle plates; the length of the mounting screw holes on both sides of the lower baffle plate penetrates to the electrode mounting grooves on the upper top surface of the lower baffle plate, that is, they serve as mounting holes for the mold baffle plates on both sides, and also as top screw holes for fixing the copper mesh.
[0010] The mold baffles on both sides each have two mounting screw holes, the screw hole on the left baffle is aligned with the mounting screw hole on the left side of the upper baffle, and the lower screw hole is coaxial with the mounting screw hole on the lower baffle; correspondingly, the upper and lower screw holes on the right baffle should also be coaxial with the mounting screw holes on the right sides of the upper and lower baffles.
[0011] The toe end of the prefabricated crack plate is engaged with the prefabricated crack plate installation groove on the lower bottom surface of the upper baffle plate of the mold at a right angle, and the thickness is consistent with the thickness of the prefabricated crack plate installation groove; the head end of the prefabricated crack plate is a pointed end; the height of the prefabricated crack is calculated according to formula (1): (1) in is the length of the prefabricated crack of the specimen; is the length of the prefabricated cracked slab; The depth of the prefabricated crack plate installation groove on the lower bottom surface of the upper baffle of the mold; The seam height ratio of the prepared specimen is calculated according to formula (2): (2) in is the specimen seam height ratio; is the length of the prefabricated cracked slab; The depth of the prefabricated crack plate installation groove on the lower bottom surface of the upper baffle of the mold; Height of the test piece; The electrode is made of conductive material and is installed in an electrode installation groove reserved on the lower baffle of the mold.
[0012] The electrodes are embedded in both sides of the conductive concrete specimen after the specimen is demoulded, and provide contact for collecting the resistance signal caused by the change of the specimen's own state after being loaded during the test. The cracking and instability load of the specimen are judged by the electrical signal of the specimen's own resistance and the rate of resistance change.
[0013] The bottom plate and the bottom plate expansion plate are provided with four screw holes for fixing the upper and lower baffles of the mold; the set of molds includes 8 bolt structures of 4 specifications for installation and fixation of the bottom plate and the front and rear baffles and the left and right baffles.
[0014] The method for forming a high-precision test specimen for self-monitoring fracture characteristics of cement-based materials as described above comprises the following steps: S1, preparing forming mold components, prefabricated crack plates and electrodes; S2, insert four small screws through the mold base expansion plate and the mold base, and install the upper and lower baffles of the mold on the mold base; S3, inserting the prefabricated crack plate into the prefabricated crack plate installation groove of the upper baffle of the mold, so that the prefabricated crack plate and the prefabricated crack plate installation groove are tightly fitted; S4, applying a layer of mold release agent on the mold bottom plate, the mold upper baffle, the lower baffle and the prefabricated crack plate, filling vaseline into the groove of the mold lower baffle until the groove is filled with vaseline, and then inserting the electrode; S5, pass a large screw through the screw hole of the right baffle of the mold and the right mounting screw hole of the upper baffle of the mold, so that the screw presses against the prefabricated crack plate, and take a small screw to connect the upper baffle of the mold and the left baffle of the mold; S6, take two small screws to connect the left and right baffles of the mold with the lower baffle of the mold, and tighten the screws against the electrodes; S7, four magnets are installed on the four sides of the bottom plate expansion plate, the conductive concrete is poured into the forming mold, and adsorbed on the vibration table through the magnets, and vibrated until slurry leaches out from the connection between the baffles on both sides of the mold and the bottom plate of the mold; S8, leaving the mold for 2 days and performing demolding; S9, remove the four screws at the bottom of the forming mold to separate the baffles around the forming mold and the test piece from the bottom plate of the mold; remove the screws connecting the left and right baffles of the mold with the upper baffle, and pull out the prefabricated crack plate; remove the connecting screws of the lower baffle of the mold and the baffles on both sides of the mold, and separate the test piece, electrode and the lower baffle of the mold; S10, moving the specimen into a standard curing room and curing it to the required age for the test, thus obtaining an electrode specimen for testing the fracture performance of conductive concrete using a high-precision three-point bending method.
[0015] The main beneficial effects of the present invention are: Through the above technical scheme, the present invention can prepare small-sized conductive concrete specimens with prefabricated cracks and electrodes, realize accurate measurement of conductive concrete fracture test parameters, and provide technical support for predicting the peak fracture load of large-scale conductive concrete components.
[0016] The position of the prefabricated crack can be accurately controlled to avoid large errors in the test caused by deviations in the position of the prefabricated crack.
[0017] The self-monitoring capability of conductive concrete can also be utilized to implant electrodes before the conductive concrete is formed, so as to achieve real-time measurement of the fracture parameters of the specimen without the need for external sensors, thereby improving the accuracy and convenience of the test. BRIEF DESCRIPTION OF THE DRAWINGS
[0018] The present invention will be further described below in conjunction with the accompanying drawings and embodiments.
[0019] Figure 1 It is a structural schematic diagram of the present invention.
[0020] Figure 2 for Figure 1 Schematic diagram of the main view.
[0021] Figure 3 It is a structural schematic diagram of the upper baffle plate and the prefabricated crack plate installation groove of the mold of the present invention.
[0022] Figure 4It is a structural schematic diagram of the lower baffle plate and electrode mounting groove of the mold of the present invention.
[0023] Figure 5 It is a schematic structural diagram of the baffles on the left and right sides of the mold of the present invention.
[0024] Figure 6 Schematic diagram of mounting screws of different specifications for the mold of the present invention.
[0025] Figure 7 It is a structural schematic diagram of the mold bottom plate of the present invention.
[0026] Figure 8 It is a structural schematic diagram of the mold bottom plate expansion plate of the present invention.
[0027] Fig. 9 It is a schematic structural diagram of the prefabricated crack plate and the crack plate tip of the present invention.
[0028] Fig.10 Schematic diagram of the structure of the electrode of the present invention.
[0029] In the figure: 1 is the upper baffle of the mold, 2 is the lower baffle of the mold, 3 is the left baffle of the mold, 4 is the right baffle of the mold, 5 is the prefabricated crack plate, 6 is the electrode, 7 is the mold bottom plate, 8 is the mold bottom plate expansion plate, 9 is the prefabricated crack plate fastening screw, 10 is the electrode fastening screw, 11 is the mold mounting screw, 12 is the bottom plate mounting screw, 13 is the connecting hole between the upper baffle of the mold and the bottom plate of the mold, 14 is the prefabricated crack plate mounting groove, 15 is the connecting hole between the lower baffle of the mold and the bottom plate of the mold, and 16 is the electrode mounting groove. DETAILED DESCRIPTION
[0030] like Figure 1 to Figure 10 In the invention, a method for forming a high-precision test specimen for self-monitoring fracture characteristics of cement-based materials is disclosed. The method can prepare a small-sized specimen of 50 mm × 15 mm × 8 mm and is applied to the high-precision three-point bending method for testing the fracture characteristics of self-monitoring cement-based materials. Prefabricated cracks and electrodes 6 for monitoring electrical signals can be arranged at designated positions, including a mold upper baffle 1, a mold lower baffle 2, mold baffles 3 and 4 on both sides, a prefabricated crack plate 5, an electrode 6, a bottom plate 7, a bottom plate expansion plate 8, and a fastening screw 9. The mold upper baffle 1, the mold lower baffle 2, and the mold baffles 3 and 4 on both sides are installed on the bottom plate 7 to form a cavity for preparing the specimen.
[0031] Embodiment 1, The mold upper baffle 1, the mold lower baffle 2, the mold baffles 3 and 4 on both sides, the prefabricated crack plate 5, the bottom plate 7, the fastening top screws 9 and 10 are made of stainless steel, and the mold upper and lower baffles 1 and 2 are of the same thickness as the mold baffles 3 and 4 on both sides. The bottom plate expansion plate 8 is made of stainless iron material that can be adsorbed by magnets.
[0032] A through square prefabricated crack plate installation groove 14 is set in the middle of the lower bottom surface of the mold upper baffle 1. The thickness of the prefabricated crack plate installation groove 14 is consistent with the thickness of the prefabricated crack plate 5, and the prefabricated crack plate installation groove 14 is perpendicular to the lower bottom surface of the mold upper baffle 1. The toe end of the prefabricated crack plate installation groove 14 is a right angle to better engage with the toe end of the prefabricated crack plate 5 to prevent the prefabricated crack plate 5 from shaking during vibration. Two positioning screw holes 13 are set at the corresponding installation positions of the mold upper baffle 1 and the bottom plate 7 so that they do not penetrate the upper baffle 1 to maintain the flatness of the casting surface of the test piece. A mounting screw hole is set on each of the left and right sides of the mold upper baffle 1.
[0033] The screw hole on the right side of the mold upper baffle 1 serves to connect the right mold baffle 4 with the mold upper baffle 1. The screw 9 is long enough to penetrate the installation groove of the square prefabricated crack plate 14 at the bottom of the mold upper baffle 1 to fix the prefabricated crack plate 5.
[0034] Two electrode mounting grooves 16 are symmetrically arranged on both sides of the upper top surface of the mold lower baffle 2. The electrode mounting grooves 16 are kept perpendicular to the upper top surface of the mold lower baffle 2, and the thickness is consistent with the thickness of the electrode 6. Two positioning screw holes 15 are arranged at the connection between the mold lower baffle 2 and the mounting bottom plate, but they do not penetrate the lower baffle to maintain the flatness of the casting surface of the test piece. Two mounting screw holes are arranged on both sides of the mold lower baffle to connect with the lower part of the left and right mold baffles.
[0035] The mounting screws 10 on both sides of the mold lower baffle 2 are long enough to penetrate the electrode mounting groove 16 on the top surface of the mold lower baffle 2 , that is, the screws 10 used as the baffles of the molds 3 and 4 on both sides also serve as the top screws for fixing the electrodes 6 .
[0036] Two mounting screw holes are set on the mold baffles 3 and 4 on both sides of the mold. The screw hole on the left baffle is aligned with the axis of the left mounting screw hole of the mold upper baffle 1, and the lower screw hole is aligned with the axis of the mounting screw hole of the mold lower baffle 2. Correspondingly, the upper and lower screw holes of the mold right baffle 4 should also be aligned with the axis of the right mounting screw holes of the mold upper and lower baffles 1 and 2.
[0037] The toe end of the prefabricated crack plate 5 should be at a right angle to engage with the prefabricated crack plate installation groove 14 on the bottom surface of the mold upper baffle 1, and the thickness should be consistent with the thickness of the prefabricated crack plate installation groove 14. The head end of the prefabricated crack plate 5 is a pointed end. The height of the prefabricated crack is calculated according to formula (1): (1) in is the length of the prefabricated crack of the specimen; The length of the prefabricated cracked plate 5; The depth of the prefabricated crack plate installation groove 14 on the lower bottom surface of the mold upper baffle plate 1.
[0038] The seam height ratio of the prepared specimen is calculated according to formula (2): (2) in is the specimen seam height ratio; is the length of the prefabricated cracked slab; The depth of the prefabricated crack plate installation groove on the lower bottom surface of the upper baffle of the mold; Height of the specimen.
[0039] The electrode can be made of a material with good conductivity (such as a copper mesh) and installed in the electrode installation groove 16 reserved on the lower baffle plate 2 of the mold.
[0040] Preferably, after the specimen is demoulded, the electrodes 6 are embedded in both sides of the conductive concrete specimen, providing good contact for collecting signals such as resistance caused by the change in the specimen's own state after being loaded during the test, and judging the cracking and instability load of the specimen by electrical signals such as the specimen's own resistance and the rate of resistance change.
[0041] The bottom plate 7 and the bottom plate enlargement plate 2 are provided with four screw holes for fixing the upper and lower baffles of the mold, which are installation holes for installing screws 12.
[0042] This set of molds includes 8 bolt structures in 4 specifications (30.5mm, 14mm, 10mm, 7mm) for the installation and fixation of the bottom plate 7 and the upper and lower baffles 1 and 2 of the mold, and the left and right baffles 3 and 4 of the mold.
[0043] Embodiment 2, A method for forming a high-precision test specimen for self-monitoring fracture characteristics of cement-based materials comprises the following preparation steps: 1. Prepare molding die parts, prefabricated crack plates and electrodes; 2. Pass four small screws 12 through the mold bottom plate expansion plate 8 and the mold bottom plate 7, and install the mold upper and lower baffles 1 and 2 on the mold bottom plate 7; 3. Insert the prefabricated crack plate 5 into the prefabricated crack plate installation groove 14 of the upper baffle of the mold, so that the prefabricated crack plate 5 fits tightly with the prefabricated crack plate installation groove 14; 4. Apply a layer of release agent on the mold bottom plate 7, the mold upper baffle 1, the mold lower baffle 2 and the prefabricated crack plate 5, fill vaseline into the electrode installation groove 16 of the mold lower baffle, and insert the electrode 6 after the vaseline fills the electrode installation groove 16; 5. Pass a large screw 9 through the screw hole of the mold right baffle 4 and the right mounting screw hole of the mold upper baffle 1, so that the screw 9 presses against the prefabricated crack plate 5, and take a small screw 11 to connect the mold upper baffle and the mold left baffle; 6. Take two small screws 10 to connect the baffles 3 and 4 on the left and right sides of the mold with the lower baffle 2 of the mold, and use the screws 10 to tighten the electrode 6; 7. Install four magnets on the four sides of the bottom plate expansion plate 8, pour the conductive concrete into the forming mold, and adsorb it on the vibration table through the magnets, and vibrate until slurry leaches out from the connection between the baffles 3 and 4 on both sides of the mold and the mold bottom plate 7; 8. Leave the mold for 2 days and remove the mold; 9. Remove the four screws 12 of the bottom plate expansion plate 7 of the forming mold to separate the baffles around the forming mold and the test piece from the bottom plate 7 of the mold; remove the screws 9 and 11 connecting the left and right baffles of the mold with the upper baffle, and pull out the prefabricated crack plate 5; remove the screws 10 connecting the lower baffle 2 of the mold and the baffles 3 and 4 on both sides of the mold, and separate the test piece, electrode 6 and the lower baffle 2 of the mold; The specimen is moved into a standard curing room and cured to the required age for the test, thereby obtaining an electrode specimen for testing the fracture characteristics of conductive concrete using the high-precision three-point bending method.
[0044] The above-mentioned embodiments are only preferred technical solutions of the present invention and should not be regarded as limitations of the present invention. The embodiments and features in the embodiments of the present application can be arbitrarily combined with each other without conflict. The protection scope of the present invention shall be the technical solutions recorded in the claims, including the equivalent replacement solutions of the technical features in the technical solutions recorded in the claims. That is, equivalent replacement improvements within this scope are also within the protection scope of the present invention.
Claims
1. A high-precision test specimen for self-monitoring fracture characteristics of cement-based materials, characterized by: It comprises an upper baffle, a lower baffle, mold baffles on both sides, a prefabricated crack plate, an electrode, a bottom plate, a bottom plate enlargement plate and a fastening screw; the upper baffle, the lower baffle and the mold baffles on both sides are installed on the bottom plate to form a cavity for preparing a test piece; a through square prefabricated crack plate installation groove is arranged in the middle of the lower bottom surface of the upper baffle, the thickness of the prefabricated crack plate installation groove is consistent with the thickness of the prefabricated crack, and the prefabricated crack plate installation groove is perpendicular to the lower bottom surface; the toe end of the prefabricated crack plate installation groove is a right angle to better engage with the toe end of the prefabricated crack plate to prevent the prefabricated crack plate from shaking; two positioning screw holes are arranged at the corresponding installation positions of the upper baffle and the bottom plate of the mold but do not penetrate the upper baffle to maintain the flatness of the casting surface of the test piece; a mounting screw hole is arranged on each of the left and right sides of the upper baffle; it is used in the test piece preparation process of self-monitoring the fracture characteristics of cement-based materials using the high-precision three-point bending method, and prefabricated cracks and electrodes for monitoring signals are arranged at designated positions.
2. The high-precision test specimen for self-monitoring fracture characteristics of cement-based materials according to claim 1 is characterized by: The upper baffle, lower baffle, mold baffles on both sides, prefabricated crack plate, bottom plate, and fastening top screws are made of stainless steel. The upper and lower baffles are of the same thickness as the mold baffles on both sides; the bottom plate expansion plate is made of stainless iron that can be adsorbed by magnets.
3. The high-precision test specimen for self-monitoring fracture characteristics of cement-based materials according to claim 1 is characterized by: The screw hole on the right side of the upper baffle serves to connect the right mold baffle with the upper baffle, and the length of the screw hole penetrates to the square prefabricated crack plate installation groove at the bottom of the upper baffle, serving to fix the prefabricated crack plate.
4. The high-precision test specimen for self-monitoring fracture characteristics of cement-based materials according to claim 1 is characterized by: Two electrode mounting grooves are symmetrically arranged on both sides of the upper top surface of the lower baffle plate, the mounting grooves are kept perpendicular to the upper top surface of the lower baffle plate, and the thickness is consistent with the thickness of the electrode; two positioning screw holes are arranged at the connection between the lower baffle plate and the mounting base plate but do not penetrate the lower baffle plate to maintain the flatness of the casting surface of the specimen; two mounting screw holes are arranged on each side of the lower baffle plate to connect with the lower part of the left and right mold baffle plates; the length of the mounting screw holes on both sides of the lower baffle plate penetrates to the electrode mounting grooves on the upper top surface of the lower baffle plate, that is, they serve as mounting holes for the mold baffle plates on both sides, and also as top screw holes for fixing the copper mesh.
5. The high-precision test specimen for self-monitoring fracture characteristics of cement-based materials according to claim 1 is characterized by: The mold baffles on both sides each have two mounting screw holes, the screw hole on the left baffle is aligned with the mounting screw hole on the left side of the upper baffle, and the lower screw hole is coaxial with the mounting screw hole on the lower baffle; correspondingly, the upper and lower screw holes on the right baffle should also be coaxial with the mounting screw holes on the right sides of the upper and lower baffles.
6. The high-precision test specimen for self-monitoring fracture characteristics of cement-based materials according to claim 1 is characterized by: The toe end of the prefabricated crack plate is engaged with the prefabricated crack plate installation groove on the lower bottom surface of the upper baffle plate of the mold at a right angle, and the thickness is consistent with the thickness of the prefabricated crack plate installation groove; the head end of the prefabricated crack plate is a pointed end; the height of the prefabricated crack is calculated according to formula (1): (1) in is the length of the prefabricated crack of the specimen; is the length of the prefabricated cracked slab; The depth of the prefabricated crack plate installation groove on the lower bottom surface of the upper baffle of the mold; The seam height ratio of the prepared specimen is calculated according to formula (2): (2) in is the specimen seam height ratio; is the length of the prefabricated cracked slab; The depth of the prefabricated crack plate installation groove on the lower bottom surface of the upper baffle of the mold; Height of the specimen.
7. The high-precision test specimen for self-monitoring fracture characteristics of cement-based materials according to claim 1 is characterized by: The electrode is made of conductive material and is installed in an electrode installation groove reserved on the lower baffle of the mold.
8. The high-precision test specimen for self-monitoring fracture characteristics of cement-based materials according to claim 7 is characterized by: The electrodes are embedded in both sides of the conductive concrete specimen after the specimen is demoulded, and provide contact for collecting the resistance signal caused by the change of the specimen's own state after being loaded during the test. The cracking and instability load of the specimen are judged by the electrical signal of the specimen's own resistance and the rate of resistance change.
9. The high-precision test specimen for self-monitoring fracture characteristics of cement-based materials according to claim 1 is characterized by: The bottom plate and the bottom plate expansion plate are provided with four screw holes for fixing the upper and lower baffles of the mold; the set of molds includes 8 bolt structures of 4 specifications for installation and fixation of the bottom plate and the front and rear baffles and the left and right baffles.
10. The method for forming a high-precision test specimen for self-monitoring fracture characteristics of cement-based materials according to any one of claims 1 to 9, characterized in that: The steps include: S1, preparing forming mold components, prefabricated crack plates and electrodes; S2, insert four small screws through the mold base expansion plate and the mold base, and install the upper and lower baffles of the mold on the mold base; S3, inserting the prefabricated crack plate into the prefabricated crack plate installation groove of the upper baffle of the mold, so that the prefabricated crack plate and the prefabricated crack plate installation groove are closely fitted; S4, applying a layer of mold release agent on the mold bottom plate, the mold upper baffle, the lower baffle and the prefabricated crack plate, filling vaseline into the groove of the mold lower baffle until the groove is filled with vaseline, and then inserting the electrode; S5, pass a large screw through the screw hole of the right baffle of the mold and the right mounting screw hole of the upper baffle of the mold, so that the screw presses against the prefabricated crack plate, and take a small screw to connect the upper baffle of the mold and the left baffle of the mold; S6, take two small screws to connect the left and right baffles of the mold with the lower baffle of the mold, and tighten the screws against the electrodes; S7, four magnets are installed on the four sides of the bottom plate expansion plate, the conductive concrete is poured into the forming mold, and adsorbed on the vibration table through the magnets, and vibrated until slurry leaches out from the connection between the baffles on both sides of the mold and the bottom plate of the mold; S8, leaving the mold for 2 days and performing demolding; S9, remove the four screws at the bottom of the forming mold to separate the baffles around the forming mold and the test piece from the bottom plate of the mold; remove the screws connecting the left and right baffles of the mold with the upper baffle, and pull out the prefabricated crack plate; remove the connecting screws of the lower baffle of the mold and the baffles on both sides of the mold, and separate the test piece, electrode and the lower baffle of the mold; S10, moving the specimen into a standard curing room and curing it to the required age for the test, thus obtaining an electrode specimen for testing the fracture performance of conductive concrete using a high-precision three-point bending method.