Quantitative detection method for passive film content of nickel tab / nickel-plated copper tab for lithium ion battery

Through solution heating, cooking and weight loss ratio calculation, the problem of detection of passivation film content in the lithium-ion battery electrode is solved, and the accuracy and simplicity of detection before the electrode production is achieved, avoiding the problem of unqualified sealing in production .

CN119000401AInactive Publication Date: 2024-11-22DONGGUAN XIANNUO ELECTRONIC MATERIALS CO LTD
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202411035100.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-31
Publication Date
2024-11-22
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

The prior art cannot effectively detect the passivation film content of nickel ears/copper nickel ears before the production of lithium-ion battery ears, resulting in unqualified sealing and economic losses in mass production.

Method used

The solution heating and cooking treatment method is used to calculate the weight loss ratio by weighing and repeating weighing, and the passivation film content of nickel ears/copper plated nickel ears is quantitatively detected, and whether it is qualified is determined based on the reference standards.

Benefits of technology

Quantitative inspection is carried out before the finished product of the ear, avoiding batch failure, reducing economic losses, and improving the accuracy of inspection and simplicity of operation.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119000401A_ABST
    Figure CN119000401A_ABST
Patent Text Reader

Abstract

The invention discloses a quantitative detection method for the passive film content of a nickel tab / nickel-plated copper tab for a lithium ion battery, and belongs to the technical field of new energy testing, the quantitative detection method comprises the following steps: S1, preparing a solution; s2, weighing is conducted, specifically, the passivated nickel strip or the copper-plated nickel strip is weighed and recorded as m0; s3, solution treatment: putting the weighed nickel strip or copper-plated nickel strip into the solution prepared in the step S1, taking out the nickel strip or copper-plated nickel strip after cooking, weighing the nickel strip or copper-plated nickel strip after cleaning and drying treatment, recording the nickel strip or copper-plated nickel strip as m1, and calculating the weight loss ratio; s4, repeated processing: repeating the operation of the step S3 at least once; s5, checking: comparing the weight loss ratios of the last two times until the weight loss ratios are equal, stopping repeated processing, and comparing the weight loss ratio of the last time with a reference standard. According to the method, the content of the passivation film of the tab can be tested before the tab is manufactured, the test is simple and convenient, and the cost is low.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of new energy testing, and in particular relates to a quantitative detection method for the content of a passivation film of a nickel tab / copper-plated nickel tab for a lithium-ion battery. Background Art

[0002] Lithium batteries are composed of multiple components, including positive electrode materials, negative electrode materials, electrolytes, separators, conductive agents, etc. Among them, the tab is a crucial part of soft-pack lithium-ion batteries. It is divided into positive tabs and negative tabs, which bear the dual functions of battery charging and discharging channels and battery sealing. The positive tab is usually made of aluminum, and the negative tab is usually made of nickel or copper-plated nickel. Figure 1 The structure of the pole ear includes a passivated metal strip (the metal strip used for the positive pole ear is an aluminum strip, and the metal strip used for the negative pole ear is a nickel strip or a nickel-plated copper strip), and a modified PP plastic film on the upper and lower surfaces of the metal strip. The three are heated and bonded together to form the pole ear.

[0003] The performance of the tab material directly affects the performance and stability of the battery. Its main performance requirements include conductivity, corrosion resistance, mechanical properties, temperature stability, etc. In the production process of lithium batteries, the sealing of the tab is very important, and the quality of the tab sealing is directly related to the thickness and density of the passivation film on the surface of the tab metal strip. The greater the thickness / density of the passivation film, the better the sealing of the tab. However, the thickness of the passivation film is too small (less than 1um), and in the actual production process, conventional measurement methods cannot be used for quantitative detection.

[0004] At present, in the lithium-ion battery industry, the quality of the tab sealing is tested by the method of the tab's resistance to electrolyte corrosion at high temperature. The specific operation method is to put the tab into the lithium battery electrolyte, add a small amount of water to produce more hydrofluoric acid, heat it to a certain high temperature (such as 85°C), and after a certain period of time (such as 24 hours), take the tab out of the electrolyte, tear off the modified PP on the surface of the tab, and observe whether the modified PP is easy to tear, whether it turns white when torn, or the strength of the tearing. However, this is a destructive test, and it must be tested after the tab is made, and it cannot be tested during the passivation process. Therefore, once the tab sealing test fails, batch failure will occur, resulting in great waste of production.

[0005] After searching the prior art, the applicant has not found any effective testing method. Therefore, the present invention is proposed. Summary of the invention

[0006] In view of the shortcomings of the prior art, the purpose of the present invention is to provide a method for quantitatively detecting the passivation film content of a nickel tab / copper-plated nickel tab for a lithium-ion battery, which can complete the test of the passivation film content of the tab after passivation and before the tab is made, and the test is simple and low-cost.

[0007] In order to achieve the above object, the present invention adopts the following technical solution:

[0008] A method for quantitatively detecting the content of a passivation film of a nickel tab / copper-plated nickel tab for a lithium-ion battery comprises the following steps:

[0009] S1. Prepare solution;

[0010] S2. Weighing: weigh the passivated nickel strip or copper-plated nickel strip, recorded as m0;

[0011] S3, solution treatment: placing the weighed nickel strip or copper-plated nickel strip in the solution prepared in step S1, taking it out after steaming, and weighing it again after washing and drying, recorded as m1, and calculating the weight loss ratio;

[0012] S4, repeat processing: repeat the operation of step S3 at least once;

[0013] S5. Verification: Compare the last two weight loss ratios until they are equal, then stop the repeated treatment, define the last weight loss ratio as the passive film content, and compare it with the reference standard.

[0014] As a preferred embodiment of the technical solution of the present invention, in step S1, the solution is at least one of sodium hydroxide and potassium hydroxide.

[0015] As a preferred embodiment of the technical solution of the present invention, in step S1, the concentration of the solution is 10-40 wt%.

[0016] As a further preferred embodiment of the technical solution of the present invention, in step S1, the concentration of the solution is 30-40 wt%.

[0017] As a preferred embodiment of the technical solution of the present invention, in step S2, the mass of the passivated nickel strip or the copper-plated nickel strip is not less than 30 g.

[0018] As a preferred embodiment of the technical solution of the present invention, in step S3, the volume of the solution is 300 to 1000 mL.

[0019] As a preferred embodiment of the technical solution of the present invention, in step S3, the cooking temperature is 40-80° C., and the cooking time is 3-10 minutes.

[0020] As a further preferred embodiment of the technical solution of the present invention, in step S3, the cooking temperature is 60-80° C., and the cooking time is 3-5 min.

[0021] As a preferred embodiment of the technical solution of the present invention, in step S3 or S4, the weight loss ratio is calculated as follows:

[0022] Weight loss ratio = (m0-m N ) / m0×100%;

[0023] Among them, m N It is the weight value obtained by weighing the solution after N times of treatment.

[0024] As a preferred embodiment of the technical solution of the present invention, the reference standard is: for a nickel strip or a nickel-plated copper strip with a thickness of 0.10 mm, the weight loss ratio is greater than or equal to 0.02%, which is qualified.

[0025] Compared with the prior art, the present invention has the following beneficial effects:

[0026] 1. The quantitative detection method provided by the present invention overcomes the shortcomings of the traditional method of testing the passivation effect after the metal strip is made into a tab. The test can be performed before the tab is made into a finished product, thereby avoiding the phenomenon of batch passivation failure of products and reducing potential economic losses.

[0027] 2. The quantitative detection method provided by the present invention can be tested on the first piece before passivation or after passivation, and the test stage can be flexibly selected.

[0028] 3. The quantitative detection method provided by the present invention has common raw materials, strong operability, high accuracy, and is effective, and has excellent prospects for promotion and application. BRIEF DESCRIPTION OF THE DRAWINGS

[0029] Figure 1 It is a schematic diagram of the lug structure; in the figure, the dots represent the passivation film.

[0030] Figure 2 This is a test result diagram of Example 1.

[0031] Figure 3 Schematic diagram of the quantitative detection method of the present invention. DETAILED DESCRIPTION

[0032] Embodiments of the present invention are described in detail below. All embodiments are exemplary and intended to be used to explain the present invention, but should not be construed as limiting the present invention.

[0033] Unless otherwise specified, the nickel strip or nickel-plated copper strip and related chemical reagents involved in the present invention are purchased from the market.

[0034] See also Figure 1 In the present invention, a method for quantitatively detecting the content of the passivation film of a nickel tab / copper-plated nickel tab for a lithium-ion battery is provided, comprising the following steps:

[0035] S1. Prepare solution;

[0036] S2. Weighing: weigh the passivated nickel strip or copper-plated nickel strip, recorded as m0;

[0037] S3, solution treatment: placing the weighed nickel strip or copper-plated nickel strip in the solution prepared in step S1, taking it out after steaming, and weighing it again after washing and drying, recorded as m1, and calculating the weight loss ratio;

[0038] S4, repeat processing: repeat the operation of step S3 at least once;

[0039] S5. Verification: Compare the last two weight loss ratios until they are equal, then stop the repeated treatment, define the last weight loss ratio as the passive film content, and compare it with the reference standard.

[0040] In the above technical solution, the nickel strip or copper-plated nickel strip used for the tab is directly tested, avoiding the insufficiency of testing after the tab is made; by adopting a simple solution heating and boiling treatment, repeated multiple times, calculating the weight loss ratio, and based on the change of the weight loss ratio, the content of the passivation film is determined, and finally based on the comparison with the reference standard, it can be known whether the content of the passivation film is qualified. The whole process is simple, convenient and easy to implement.

[0041] It should be noted that the number of repeated treatments in step S4 is based on the comparison of weight loss ratios. The solution treatment in step S3 is the first time, and the weight loss ratio is (m0-m1) / m0×100%.

[0042] Repeat the treatment once, the solution is treated twice cumulatively, the mass is recorded as m2, and the weight loss ratio is (m0-m2) / m0×100%;

[0043] Repeat the treatment twice, the solution is treated 3 times cumulatively, the mass is recorded as m3, and the weight loss ratio is (m0-m3) / m0×100%;

[0044] Repeat the treatment N-1 times, the total solution treatment is N times, and the mass is recorded as m N , the weight loss ratio is (m0-m N ) / m0×100%.

[0045] Obviously, the calculation of the weight loss ratio is the cumulative weight loss value compared with the initial mass; and it should be emphasized that in step S5, the stop of repeated treatment is judged by comparing the weight loss ratios of the last two times, but due to the influence of test accuracy and test environment, "until the two are equal" does not mean that the two are absolutely equal, but equal in a broad sense, that is, when the values ​​of the weight loss ratios of the two are the same at two or three decimal places, it can be considered that the weight loss ratio of the passivation film after repeated treatment has no longer changed, and what is obtained at this time is the content of the passivation film of the metal strip; for example, when the weight loss ratio after the last two solution treatments is 0.262%, 0.263% or 0.262%, 0.262%, the treatment can be stopped.

[0046] In some embodiments, in step S1, the solution is at least one of sodium hydroxide and potassium hydroxide.

[0047] In some embodiments, in step S1, the solution concentration is 10-40wt%; it can be understood that the concentration of the solution can be flexibly selected according to actual needs, such as the solution concentration can be 10wt%, 15wt%, 20wt%, 25wt%, 30wt%, 35wt%, 40wt% or any specific value within the above range; preferably, the solution concentration is 30-40wt%.

[0048] In some embodiments, in step S2, the mass of the passivated nickel strip or copper-plated nickel strip is not less than 30 g; more preferably, it is 30 to 50 g; in step S3, the volume of the solution is 300 to 1000 mL. It can be understood that the mass of the nickel strip or the copper-plated nickel strip is related to the volume of the solution. The more mass, the greater the amount of solution used, taking into account both test convenience and test accuracy. The metal mass in the present invention can be 30g, 31g, 32g, 33g, 34g, 35g, 36g, 37g, 38g, 39g, 40g, 41g, 42g, 43g, 44g, 45g, 46g, 47g, 48g, 49g, 50g or any specific value within the above range; correspondingly, the volume of the solution can be 300mL, 350mL, 400mL, 450mL, 500mL, 550mL, 600mL, 650mL, 700mL, 750mL, 800mL, 850mL, 900mL, 950mL, 1000mL or any specific value within the above range.

[0049] In some embodiments, in step S3, the cooking temperature is 40-80°C, and the cooking time is 3-10 min; preferably, the cooking temperature is 60-80°C, and the cooking time is 3-5 min; it can be understood that the above cooking temperature can be a value among 40°C, 45°C, 50°C, 55°C, 60°C, 65°C, 70°C, 75°C, 80°C or any specific value within the above range; correspondingly, the cooking time can be a value among 3min, 4min, 5min, 6min, 7min, 8min, 9min, 10min or any specific value within the above range.

[0050] In some embodiments, after the content of the passivation film is finally determined, it is necessary to judge whether its content is qualified. For a nickel strip or nickel-plated copper strip with a thickness of 0.1 mm, the weight loss ratio is greater than or equal to 0.02%, which is qualified. It should be particularly noted that since the thickness of the passivation film is very small (usually between 1 nm and 1 um), the weight loss of the passivation film is directly related to the thickness of the metal strip. Therefore, for metal strips of different specifications (such as 0.06 mm, 0.08 mm, 0.10 mm, 0.15 mm, 0.20 mm, etc.), the same weight loss ratio cannot be used as a standard, but a separate standard should be formulated through experiments, and the specific standard value needs to be scientifically determined through repeated experiments.

[0051] The technical solution of the present invention is further described below with reference to specific embodiments.

[0052] Example 1

[0053] A method for quantitatively detecting the content of a passivation film of a nickel tab / copper-plated nickel tab for a lithium-ion battery comprises the following steps:

[0054] S1, prepare 25wt% sodium hydroxide solution;

[0055] S2. Weighing: weigh the passivated nickel strip of 0.1×6 mm, recorded as m0;

[0056] S3, solution treatment: the weighed nickel strip is placed in the solution (500 mL) prepared in step S1, boiled at 50°C for 5 min, taken out, washed and dried, and weighed again, recorded as m1, and the weight loss ratio is calculated;

[0057] S4, repeat processing: repeat the operation of step S3 at least once;

[0058] S5. Verification: Compare the weight loss ratios of the last two times until they are equal, and process 6 times in total.

[0059] For detailed test results, see Figure 1 .from Figure 1It can be seen that the weight loss ratio of the nickel strip remains unchanged at 0.25% after 5 cumulative treatments, and remains unchanged at 0.25% after the 6th treatment. Therefore, it can be determined that the content of the passivation film of the nickel strip is 0.25%. Referring to the reference standard "weight loss ratio greater than or equal to 0.02% is qualified", the content of the passivation film of this nickel strip is qualified.

[0060] Example 2

[0061] A method for quantitatively detecting the content of a passivation film of a nickel tab / copper-plated nickel tab for a lithium-ion battery comprises the following steps:

[0062] S1, prepare 28wt% sodium hydroxide solution;

[0063] S2. Weighing: weigh the passivated nickel strip of 0.1×6 mm, recorded as m0;

[0064] S3, solution treatment: the weighed nickel strip is placed in the solution (500 mL) prepared in step S1, boiled at 55°C for 5 min, taken out, washed and dried, and weighed again, recorded as m1, and the weight loss ratio is calculated;

[0065] S4, repeat processing: repeat the operation of step S3 at least once;

[0066] S5. Verification: Compare the last two weight loss ratios until they are equal, and define the last weight loss ratio as the passive film content.

[0067] Example 3

[0068] A method for quantitatively detecting the content of a passivation film of a nickel tab / copper-plated nickel tab for a lithium-ion battery comprises the following steps:

[0069] S1, prepare 35wt% sodium hydroxide solution;

[0070] S2. Weighing: weigh the passivated nickel strip of 0.1×6 mm, recorded as m0;

[0071] S3, solution treatment: the weighed nickel strip is placed in the solution (500 mL) prepared in step S1, boiled at 65°C for 6 min, taken out, washed and dried, and weighed again, recorded as m1, and the weight loss ratio is calculated;

[0072] S4, repeat processing: repeat the operation of step S3 at least once;

[0073] S5. Verification: Compare the last two weight loss ratios until they are equal, and define the last weight loss ratio as the passive film content.

[0074] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.

Claims

1. A method for quantitatively detecting the content of passivation film of nickel tabs / copper-plated nickel tabs for lithium-ion batteries, It is characterized in that The steps include: S1. Prepare solution; S2. Weighing: Weigh the passivated nickel strip or copper-plated nickel strip, recorded as m 0 ; S3, solution treatment: the weighed nickel strip or copper-plated nickel strip is placed in the solution prepared in step S1, taken out after steaming, washed and dried, and weighed again, recorded as m 1 , calculate the weight loss ratio; S4, repeat processing: repeat the operation of step S3 at least once; S5. Verification: Compare the last two weight loss ratios until they are equal, then stop the repeated treatment, define the last weight loss ratio as the passive film content, and compare it with the reference standard.

2. A method for quantitatively detecting the content of a passivation film of a nickel tab / copper-plated nickel tab for a lithium-ion battery according to claim 1, It is characterized in that In step S1, the solution is at least one of sodium hydroxide and potassium hydroxide.

3. A method for quantitatively detecting the content of a passivation film of a nickel tab / copper-plated nickel tab for a lithium-ion battery according to claim 2, It is characterized in that In step S1, the concentration of the solution is 10-40 wt%.

4. A method for quantitatively detecting the content of a passivation film of a nickel tab / copper-plated nickel tab for a lithium-ion battery according to claim 3, It is characterized in that In step S1, the solution concentration is 30-40 wt%.

5. A method for quantitatively detecting the content of a passivation film of a nickel tab / copper-plated nickel tab for a lithium-ion battery according to claim 1, It is characterized in that In step S2, the mass of the passivated nickel strip or the copper-plated nickel strip is not less than 30 g.

6. A method for quantitatively detecting the content of a passivation film of a nickel tab / copper-plated nickel tab for a lithium-ion battery according to claim 1, It is characterized in that In step S3, the volume of the solution is 300 to 1000 mL.

7. A method for quantitatively detecting the content of a passivation film of a nickel tab / copper-plated nickel tab for a lithium-ion battery according to claim 1, It is characterized in that In step S3, the cooking temperature is 40-80° C., and the cooking time is 3-10 minutes.

8. A method for quantitatively detecting the content of a passivation film of a nickel tab / copper-plated nickel tab for a lithium-ion battery according to claim 7, It is characterized in that In step S3, the cooking temperature is 60-80° C., and the cooking time is 3-5 minutes.

9. A method for quantitatively detecting the content of a passivation film of a nickel tab / copper-plated nickel tab for a lithium-ion battery according to claim 1, It is characterized in that In step S3 or S4, the weight loss ratio is calculated as: Weight loss ratio = (m 0 -m N ) / m 0 ×100%; Among them, m N It is the weight value obtained by weighing the solution after N times of treatment.

10. A method for quantitatively detecting the content of a passivation film of a nickel tab / copper-plated nickel tab for a lithium-ion battery according to claim 1, It is characterized in that In step S5, the reference standard is: for a nickel strip or a nickel-plated copper strip with a thickness of 0.10 mm, a weight loss ratio greater than or equal to 0.02% is qualified.

Citation Information

Patent Citations

  • Surface processing method of tab easily plated with tin

    CN106328880A

  • Production process of nickel tab of lithium ion battery

    CN106356491A

  • Method, device and equipment for detecting qualification rate of battery pole piece and medium

    CN118294310A

  • Lithium ion battery electrode lug

    CN206849932U