Method for testing crosslinking degree of packaging adhesive film of photovoltaic module
By measuring the density of the adhesive film sample in water, the crosslinking degree is judged, which solves the problems of slow detection speed and high safety hazards in the prior art, and achieves fast, safe and low-cost adhesive film crosslinking degree testing, which improves production Efficiency and environmental protection.
Patent Information
- Application Number
- CN202411089212.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-09
- Publication Date
- 2024-11-22
AI Technical Summary
The method of detecting the crosslinking degree of EVA adhesive film in the prior art has problems such as slow detection speed, complex operation, large safety hazards, high cost and environmental pollution. It is impossible to quickly and accurately monitor the crosslinking degree of the adhesive film, which affects the timely product. and productivity.
By cutting the film sample and measuring its density change in water, calculate the crosslinking density ratio, and determine whether the crosslinking degree is within the range of 0.80-0.95, it can achieve fast, safe and low-cost crosslinking degree testing, and avoid the use of dangerous chemistry Xylene.
It realizes the rapid and accurate judgment of the degree of crosslinking of the adhesive film, reduces the detection time and cost, improves the process safety and environmental protection, and can adjust the production process in a timely manner, reducing the risks to the environment and personnel.
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of photovoltaic modules, and in particular to a method for testing the cross-linking degree of a photovoltaic module encapsulation film. Background Art
[0002] EVA glue (Ethylene-Vinyl Acetate copolymer) plays a vital role in solar cells and is mainly used as a packaging material for photovoltaic modules. In the photovoltaic module manufacturing process, the solar cell string, backplane and tempered glass are bonded together through EVA film. When the module is laminated, EVA is heated to a certain temperature and is in a molten state. The cross-linking agent in the formula decomposes to produce free radicals that trigger the combination of EVA long-chain molecules, so that it is bonded and cured with the battery cell, tempered glass and backplane, and then the three layers of materials are laminated into one. The cured battery cell no longer moves. EVA glue can resist environmental factors such as high temperature, moisture, and ultraviolet rays, and can ensure the stable operation of solar cell modules.
[0003] The cross-linking degree of EVA film will directly affect the performance and service life of solar cell modules. If the cross-linking is too low, EVA will delaminate from the glass and backplane, causing internal circuit connectivity and reducing mechanical properties; while if the cross-linking is too high, it may cause cracks in the module. At the same time, too high cross-linking will also reduce its anti-ultraviolet aging performance. Therefore, it is necessary to accurately control and monitor the cross-linking degree of EVA film to ensure the long-term stability and efficiency of the module.
[0004] At present, the main method for testing the crosslinking degree of EVA film is the extraction method, that is, the laminated crosslinked EVA is first cut into EVA fragments, and then xylene is used as the extraction solvent to extract at a high temperature of about 140°C for about 5 hours, and then dried. Finally, the crosslinking degree is calculated by the crosslinking degree formula: crosslinking degree = weight difference before and after extraction of the screening bag containing EVA / total amount before extraction. This method has the following defects: (1) The detection speed is slow. The entire detection process takes more than 10 hours, and the test results cannot be obtained quickly, which will affect the timeliness of product use, and quality problems in the production line cannot be discovered in time; (2) The operation process is complicated and must rely on professional facilities, and has high requirements for objective conditions such as sites; (3) Xylene is required during the detection process, which is a hazardous chemical. There is a relatively large safety risk in use. In addition, harmful gases are generated during the xylene extraction process. A gas mask needs to be worn during the detection process, which poses a great health hazard to the operator; (4) Xylene needs to be replaced every three times it is used, which greatly increases the detection cost; (5) Waste gas xylene must be recycled by a professional organization, and the processing cost is relatively high. Therefore, there is an urgent need for a test method for the cross-linking degree of EVA film that is simple to operate, safe, low-cost, environmentally friendly and can accurately measure. Summary of the invention
[0005] In view of the problems of the prior art methods for detecting the cross-linking degree of EVA films, such as long time, complicated operation, high safety risks and high cost, the present invention provides a method for testing the cross-linking degree of photovoltaic module encapsulation films.
[0006] In order to solve the above technical problems, the technical solution provided by the present invention is:
[0007] In a first aspect, the present invention provides a method for testing the crosslinking degree of a photovoltaic module encapsulation film, comprising the following steps:
[0008] S1, cut the film sample A and film sample B to be laminated, weigh them and record them as m A and m B , put the cut film sample A and film sample B into water respectively, and record the volume change V of the water before and after putting the samples into water A and V B , calculate the density of the film sample ρ0=(m A / V A +m B / V B ) / 2;
[0009] S2, laminating the film sample A and the film sample B according to the process parameters, cutting, and obtaining the sample to be tested; weighing the sample to be tested and recording it as m C , then put it into water, record the volume change Vc of the water before and after putting the sample in, and calculate the density of the sample to be tested ρ1=m C / V c ;;
[0010] S3, calculating the cross-linking degree G=ρ1 / ρ0, when 0.80≤G≤0.95, it is determined that the cross-linking degree meets the process requirements, otherwise it is determined that the cross-linking degree does not meet the process requirements.
[0011] Compared with the prior art, the present invention creatively constructs a test method for the crosslinking degree of the encapsulation film of the photovoltaic module. According to whether the density ratio G of the film sample before and after lamination is within the range of 0.80-0.95, it can be intuitively and quantitatively determined whether the crosslinking degree meets the process requirements. According to the test method for the crosslinking degree of the encapsulation film of the photovoltaic module provided by the present invention, not only can the time required for detecting the crosslinking degree be greatly reduced, and the test results can be quickly obtained, but also the use of dangerous chemicals such as xylene can be avoided, and the safety and environmental protection of the process can be improved. No special testing instruments are required, and no additional equipment investment is added. The test results are fast and effective, and the lamination process can be adjusted and improved in time. It can play a positive role in accelerating the production progress, accurately judging the timeliness of product use, and reducing R&D and production costs, and has extremely high practical value.
[0012] It should be noted that the test method for the crosslinking degree of photovoltaic module encapsulation film provided by the present invention is applicable to the judgment of the crosslinking degree of photovoltaic module encapsulation film currently used, such as EVA film, POE film, and other encapsulation films (such as PCMS / Silicon, PVB film, TPU film), etc. It can be used to judge the crosslinking degree of the same film, and can also be used to judge the crosslinking degree of two films with different properties.
[0013] As a specific implementation of the present invention, a precision balance with an accuracy of 0.01 g is used to weigh the mass of each sample.
[0014] Furthermore, the size of the sample to be tested in S2 is the same as the size of the film sample A and the film sample B cut in S1.
[0015] As a specific implementation of the present invention, the size of the sample to be tested is 70 mm×70 mm.
[0016] As a specific implementation of the present invention, in S1, the number of the cut film samples A and B is ≥3.
[0017] In order to improve the accuracy of the test, the film sample before lamination and the sample to be tested after lamination were cut into at least 3 pieces, weighed and tested respectively, and the average value of multiple samples was taken as the final m A 、V A 、m B 、V B 、m C 、V C .
[0018] In order to further improve the accuracy of the measurement, the mass and volume of each sample in step S1 and step S2 are measured 2-3 times respectively, and the average value is taken as the final measurement value.
[0019] Furthermore, in S3, 0.85≤G≤0.95.
[0020] Furthermore, the film sample A and the film sample B are independently selected from EVA film or POE film.
[0021] It should be noted that in order to ensure the accuracy of the test results, the weight and volume values need to be retained to more than two decimal places, and when measuring the volume of the sample, it is necessary to ensure that the sample is completely submerged in water. All calculation results in the calculation formula need to be retained to two decimal places to ensure the accuracy of the calculation results.
[0022] In a second aspect, the present invention provides a method for preparing a photovoltaic module, comprising any of the above-mentioned methods for testing the cross-linking degree of a photovoltaic module encapsulation film.
[0023] In a third aspect, the present invention provides a photovoltaic module, which is prepared by the above-mentioned method for preparing a photovoltaic module.
[0024] Compared with the prior art, the beneficial effect of the present technical solution is that the test method for the cross-linking degree of the photovoltaic module encapsulation film provided by the present invention can quickly and accurately determine whether the lamination process matches the process requirements, and the overall detection time is about 10 minutes, which solves the problem that the time for judging the cross-linking degree of the film in the prior art is too long, which affects the timeliness of product use and cannot accurately and quickly adjust the lamination process. In addition, the test method for the cross-linking degree provided by the present invention is simple to operate, does not require special testing equipment, and does not require the use of high-risk chemicals such as xylene, which not only reduces the detection cost, but also greatly reduces environmental pollution and safety risks, and has extremely high practical value. DETAILED DESCRIPTION
[0025] In order to make the purpose, technical solution and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with the embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention.
[0026] The precision of the precision electronic scale used in the following examples and comparative examples is 0.01 g.
[0027] Example 1
[0028] This embodiment provides a method for testing the crosslinking degree of an EVA film, comprising the following steps:
[0029] S1, cut the EVA sample of 70mm×70mm, put the sample on the precision electronic scale, measure the weight, record it as m1; then put the EVA sample into water, record the volume change V1 of the water before and after putting the sample in, and calculate the density of the film sample ρ1=m1 / V1;
[0030] S2, laminate the EVA sample according to the process parameters, and then cut it into 70mm×70mm test samples; weigh the test sample and record it as m2, then put it into water, record the volume change V2 of water before and after putting the sample in, and calculate the density ρ2=m2 / V2 of the test sample;
[0031] S3, calculate the cross-linking degree G = ρ2 / ρ1, when 0.80≤G≤0.95, it is determined that the cross-linking degree meets the process requirements, otherwise it is determined that the cross-linking degree does not meet the process requirements.
[0032] Example 2
[0033] This embodiment provides a method for testing the crosslinking degree of a POE film, comprising the following steps:
[0034] S1, cut a POE sample of 70mm×70mm, place the sample on a precision electronic scale, measure the weight, record it as m1; then put the POE sample into water, record the volume change V1 of the water before and after putting the sample in, and calculate the density of the film sample ρ1=m1 / V1;
[0035] S2, laminating the POE sample according to the process parameters, and then cutting it into a 70mm×70mm sample to be tested; weighing the sample to be tested as m2, and then putting it into water, recording the volume change V2 of the water before and after putting the sample in, and calculating the density of the sample to be tested ρ2=m2 / V2;
[0036] S3, calculate the cross-linking degree G = ρ2 / ρ1, when 0.80≤G≤0.95, it is determined that the cross-linking degree meets the process requirements, otherwise it is determined that the cross-linking degree does not meet the process requirements.
[0037] Example 3
[0038] This embodiment provides a method for testing the crosslinking degree of EVA and POE films, comprising the following steps:
[0039] S1, cut EVA samples and POE samples into 70mm×70mm pieces, place the EVA samples and POE samples on precision electronic scales respectively, weigh them and record them as m A and m B , put the cut EVA samples and POE samples into water respectively, and record the volume change V of the water before and after putting the samples into water A and V B , calculate the density of the film sample ρ0=(m A / V A +m B / V B ) / 2;
[0040] S2, laminate the EVA sample and the POE sample according to the process parameters, and then cut them into 70mm×70mm samples to be tested; weigh the samples to be tested and record them as m C , and then put it into water, record the volume change Vc of the water before and after the sample is put in, and calculate the density of the sample to be tested ρ1=mc / V c ;;
[0041] S3, calculating the cross-linking degree G=ρ1 / ρ0, when 0.80≤G≤0.95, it is determined that the cross-linking degree meets the process requirements, otherwise it is determined that the cross-linking degree does not meet the process requirements.
[0042] Comparative Example 1
[0043] This comparative example provides a method for testing the crosslinking degree of a photovoltaic module film (xylene extraction method), which specifically comprises the following steps:
[0044] S1, put the film sample into a vacuum laminator for lamination according to the process parameters, use a wallpaper knife to remove about 0.5g of the cross-linked and cured film in the middle of the sample, and cut it into pieces;
[0045] S2, wash, dry and weigh the stainless steel wire mesh, record it as W1 (accurate to 0.001g), take 0.5±0.01g of sample (accurate to 0.001g), put it into the stainless steel wire mesh, and get the sample bag;
[0046] S3, fold the sample package, tie it firmly with thin wire, then insert it from the side of the three-necked flask and seal it with a rubber stopper, add 1 / 2 volume of xylene into the flask, immerse the sample package in xylene, heat it to 140℃, and heat it for 5h;
[0047] S4, take out the sample package, place it to remove the xylene droplets, then put it into a vacuum drying oven and dry it at 140°C for 3 hours. Take out the sample package from the oven, remove the iron wire, put it into a dryer to cool for 20 minutes, take it out, weigh W2 (accurate to 0.001g), and then calculate the cross-linking degree G=W2 / W1.
[0048] After EVA film is used on both the front and back sides, or POE film is used on both the front and back sides, and the front EVA film and the back POE film are laminated using the same lamination process, the crosslinking degree is tested according to the above-mentioned xylene extraction method and compared with Examples 1 to 3. The results are shown in Table 1.
[0049] Table 1
[0050] Example Methods Comparative Example Method (Xylene Extraction Method) EVA-EVA film 87.5547% 87.5528% POE-POE film 86.3929% 86.3948% EVA-POE film 88.5217% 88.5236%
[0051] From the above results, it can be seen that there is no significant difference between the test results of the cross-linking degree test method provided by the present invention and the traditional xylene extraction method, which proves that the cross-linking degree test method provided by the present invention has good practicality and reliability, can replace the existing xylene extraction method, and provides a new method for photovoltaic module packaging that is fast, accurate, safer and more environmentally friendly.
[0052] Examples 1-3 can also be used to test the crosslinking degree of other identical films after lamination, and can also be used to test the crosslinking degree of other films with different properties after lamination. The test results have no significant difference compared with the xylene extraction method.
[0053] In summary, the test method for the cross-linking degree of the solar photovoltaic module encapsulation film provided by the present invention does not require additional funds to purchase testing equipment, saves money and is convenient and fast, can quickly determine whether the lamination process meets the process requirements, and can achieve intuitive and quantitative accurate judgment, which solves the problem of long testing time and inability to adjust the lamination process in time in the prior art, and does not require the use of high-risk chemicals such as xylene, which not only reduces the detection cost but also greatly reduces environmental pollution and safety risks, and has a very high value for promotion and application.
[0054] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modification, equivalent substitution or improvement made within the spirit and principle of the present invention should be included in the protection scope of the present invention.
Claims
1. A method for testing the crosslinking degree of a photovoltaic module encapsulation film, characterized in that: The steps include: S1, cut the film sample A and film sample B to be laminated, weigh them and record them as m A and m B , put the cut film sample A and film sample B into water respectively, and record the volume change V of the water before and after putting the samples into water A and V B , calculate the density of the film sample ρ0=(m A / V A +m B / V B ) / 2; S2, laminating the film sample A and the film sample B according to the process parameters, cutting, and obtaining the sample to be tested; weighing the sample to be tested and recording it as m C , then put it into water, record the volume change Vc of the water before and after putting the sample in, and calculate the density of the sample to be tested ρ1=m C / V c ;; S3, calculating the cross-linking degree G=ρ1 / ρ0, when 0.80≤G≤0.95, it is determined that the cross-linking degree meets the process requirements, otherwise it is determined that the cross-linking degree does not meet the process requirements.
2. The method for testing the crosslinking degree of the photovoltaic module encapsulation film according to claim 1, characterized in that: The size of the sample to be tested in S2 is the same as the size of the film sample A and the film sample B cut in S1.
3. The method for testing the crosslinking degree of the photovoltaic module encapsulation film according to claim 2, characterized in that: The size of the sample to be tested is 70 mm×70 mm.
4. The method for testing the crosslinking degree of the photovoltaic module encapsulation film according to claim 1, characterized in that: In S1, the number of the cut film samples A and B is ≥3.
5. The method for testing the crosslinking degree of the photovoltaic module encapsulation film according to claim 1, characterized in that: In S3, 0.85≤G≤0.
95.
6. The method for testing the crosslinking degree of the photovoltaic module encapsulation film according to claim 1, characterized in that: The film sample A and the film sample B are independently selected from EVA film or POE film.
7. A method for preparing a photovoltaic module, characterized in that: A method for testing the crosslinking degree of a photovoltaic module encapsulation film as described in any one of claims 1 to 6.
8. A photovoltaic module, characterized in that: The photovoltaic module is prepared by the method for preparing the photovoltaic module according to claim 7.