Thin film lithium niobate electro-optical modulator and manufacturing method thereof
By making optical waveguides and metal electrodes on the silicon nitride layer compatible with the CMOS process, and bonding the thin-film lithium niobate layer to the silicon oxide layer by heterogeneous bonding from chip to wafer, the thin-film lithium niobate battery photolithography is solved The problem of difficult manufacturing of modulators has achieved industrial application and performance improvement of large-scale electro-optical integrated chips.
Patent Information
- Application Number
- CN202410990827.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-23
- Publication Date
- 2024-11-22
AI Technical Summary
The existing thin-film lithium niobate electro-optical modulators are difficult to manufacture and are incompatible with the CMOS process, resulting in complex manufacturing processes and high cost.
Optical waveguides and metal electrodes are made on silicon nitride layer compatible with CMOS process, and bonding the thin film lithium niobate layer to the silicon oxide layer through heterogeneous bonding from chip to wafer, reducing alignment errors and manufacturing difficulties .
It reduces manufacturing difficulty and production costs, realizes the industrial application of large-scale electro-optical integrated chips, and improves device performance and process stability.
Smart Images

Figure CN119002103A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of electro-optic modulators, and in particular to a thin-film lithium niobate electro-optic modulator and a manufacturing method thereof. Background Art
[0002] Photonic systems require modulators with complementary metal oxide semiconductor (CMOS)-compatible drive voltages, large bandwidth, low optical insertion loss, high extinction ratio, excellent signal quality, and compatibility with large-scale manufacturing. Lithium niobate (LN) electro-optic modulators (EOMs) are widely used in long-distance optical communications due to their excellent material properties, including temperature stability and a wide range of optical transparency windows. Furthermore, ultra-low-loss thin-film lithium niobate (TFLN) waveguide platforms offer excellent performance, including a small footprint, low half-wave voltage (Vπ), and a 3-dB bandwidth exceeding 100 GHz. However, current thin-film lithium niobate EOMs are difficult to manufacture.
[0003] How to solve the problem of difficulty in manufacturing thin-film lithium niobate electro-optical modulators has become a technical problem that needs to be urgently solved by those skilled in the art. Summary of the Invention
[0004] This application provides a thin-film lithium niobate electro-optic modulator and a method for manufacturing the same. This method first fabricates an optical waveguide and metal electrodes on a CMOS-compatible silicon nitride layer, then bonds the thin-film lithium niobate layer as a subsequent step. This reduces incompatibility with the CMOS process and allows alignment errors of up to 100 μm for the bonded thin-film lithium niobate layer, reducing manufacturing complexity. The thin-film lithium niobate electro-optic modulator utilizes chip-to-wafer heterogeneous bonding, facilitating the realization of silicon-based electro-optical integrated systems and the industrial application of large-scale electro-optical integrated chips.
[0005] According to a first aspect of the present invention, there is provided a method for manufacturing a thin-film lithium niobate electro-optical modulator, comprising:
[0006] Providing a substrate wafer, the substrate wafer comprising a silicon layer and a first insulating dielectric layer disposed on an upper end of the silicon layer;
[0007] forming a silicon nitride layer, wherein the silicon nitride layer is disposed on a side of the first insulating dielectric layer away from the silicon layer;
[0008] forming a plurality of optical waveguides, wherein the plurality of optical waveguides are arranged on a side of the first insulating dielectric layer away from the silicon layer;
[0009] forming a plurality of metal electrodes, wherein portions of the metal electrodes are embedded in the first insulating dielectric layer and located between the two optical waveguides;
[0010] A second insulating dielectric layer is formed, wherein the second insulating dielectric layer is located on the side of the first insulating dielectric layer, the optical waveguide, and the metal electrode away from the silicon layer;
[0011] forming a plurality of thin-film lithium niobate layers and a plurality of silicon oxide layers, wherein the thin-film lithium niobate layers are bonded to a side of the second insulating dielectric layer away from the silicon layer, and the silicon oxide layers are located on a side of the thin-film lithium niobate layers away from the silicon layer, with the thin-film lithium niobate layers and the silicon oxide layers corresponding one to one;
[0012] A passivation layer is formed, wherein the passivation layer is arranged on the surface of the thin-film lithium niobate layer away from the silicon layer, and on the side walls of the thin-film lithium niobate layer and the oxide layer; the surface of the passivation layer away from the silicon layer is higher than the surface of the thin-film lithium niobate layer away from the silicon layer.
[0013] In some embodiments, the step of forming a plurality of optical waveguides includes:
[0014] The silicon nitride layer is etched to form multiple optical waveguides.
[0015] In some embodiments, the step of forming a plurality of metal electrodes includes:
[0016] Etching the first insulating dielectric layer between the two optical waveguides to form a groove;
[0017] Photoresist is formed on the surface of the first insulating dielectric layer away from the silicon layer, excluding the groove, and on the surface of the optical waveguide away from the silicon layer.
[0018] forming a metal layer in the groove and on the surface of the photoresist away from the silicon layer;
[0019] The photoresist is stripped off, and the remaining metal layer forms a metal electrode.
[0020] In some embodiments, the step of forming the second insulating dielectric layer includes:
[0021] growing an insulating oxide material on a surface of the first insulating dielectric layer away from the silicon layer, and on surfaces of the optical waveguide and the metal electrode exposed from the first insulating dielectric layer;
[0022] The insulating oxide material is thinned to obtain a second insulating dielectric layer.
[0023] In some embodiments, the step of forming a plurality of thin-film lithium niobate layers and a plurality of silicon oxide layers includes:
[0024] A plurality of thin-film lithium niobate wafers are provided, wherein the thin-film lithium niobate wafer includes a silicon substrate and a bonding material, the bonding material including a thin-film lithium niobate and silicon oxide disposed between the thin-film lithium niobate and the silicon substrate;
[0025] activating the material to be bonded of the thin-film lithium niobate wafer to obtain an activated thin-film lithium niobate wafer;
[0026] The material to be bonded in the activated thin-film lithium niobate wafer is bonded to the side of the second insulating dielectric layer away from the silicon layer;
[0027] A protective layer is formed on the surface of the second insulating dielectric layer on the side away from the silicon layer, excluding the portion that is bonded to the activated thin-film lithium niobate wafer.
[0028] removing the silicon substrate;
[0029] The protective layer is removed, and the activated thin-film lithium niobate wafer forms a thin-film lithium niobate layer and a silicon oxide layer with thin-film lithium niobate and silicon oxide.
[0030] In some embodiments, the step of forming the passivation layer includes:
[0031] Passivation material is grown on the surface of the thin-film lithium niobate layer away from the silicon layer, as well as on the sidewalls of the thin-film lithium niobate layer and the sidewalls of the silicon oxide layer;
[0032] The passivation material is thinned to form a passivation layer.
[0033] In some embodiments, the step of activating the material to be bonded to the thin film lithium niobate wafer includes:
[0034] Radio frequency plasma was used to activate the bonding material of thin-film lithium niobate wafers.
[0035] In some embodiments, the step of bonding the material to be bonded in the activated thin-film lithium niobate wafer to a side of the second insulating dielectric layer away from the silicon layer includes:
[0036] The material to be bonded in the activated thin-film lithium niobate wafer is bonded to the side of the second insulating dielectric layer away from the silicon layer, and then immersed in deionized water for a preset time. After that, it is dried with nitrogen gas, so that the material to be bonded and the second insulating dielectric layer are bonded together.
[0037] In some embodiments, prior to the step of forming the protective layer, the method further includes cyclic annealing via a preset temperature gradient.
[0038] The present application also provides a thin-film lithium niobate electro-optic modulator, comprising:
[0039] A substrate wafer, the substrate wafer comprising a silicon layer and a first insulating dielectric layer disposed on an upper end of the silicon layer;
[0040] a plurality of optical waveguides, wherein the plurality of optical waveguides are arranged on a side of the first insulating dielectric layer away from the silicon layer;
[0041] a plurality of metal electrodes, wherein portions of the metal electrodes are embedded in the first insulating dielectric layer and located between the two optical waveguides;
[0042] a second insulating dielectric layer, wherein the second insulating dielectric layer is located on a side of the first insulating dielectric layer, the optical waveguide, and the metal electrode away from the silicon layer;
[0043] Multiple thin-film lithium niobate layers and multiple silicon oxide layers are provided. The thin-film lithium niobate layers are bonded to the side of the second insulating dielectric layer away from the silicon layer. The silicon oxide layers are located on the side of the thin-film lithium niobate layers away from the silicon layer. The thin-film lithium niobate layers and silicon oxide layers correspond one-to-one.
[0044] A passivation layer is disposed on the surface of the thin-film lithium niobate layer away from the silicon layer, and on the sidewalls of the thin-film lithium niobate layer and the oxide layer; the surface of the passivation layer away from the silicon layer is higher than the surface of the thin-film lithium niobate layer away from the silicon layer.
[0045] The above embodiments provide a thin-film lithium niobate electro-optic modulator and its manufacturing method. In this method, optical waveguides and metal electrodes are first fabricated on a silicon nitride layer compatible with CMOS processes. Bonding the thin-film lithium niobate layer is then performed as a subsequent step, reducing incompatibility with CMOS processes. Furthermore, the bonded thin-film lithium niobate layer allows for alignment errors down to 100 μm, reducing manufacturing difficulty. The thin-film lithium niobate electro-optic modulator employs a chip-to-wafer heterogeneous bonding method, which is beneficial for realizing silicon-based electro-optic integrated systems and achieving industrial applications of large-scale electro-optic integrated chips. The method includes: providing a substrate wafer; forming a silicon nitride layer; forming multiple optical waveguides; forming multiple metal electrodes; forming a second insulating dielectric layer; forming multiple thin-film lithium niobate layers and multiple silicon oxide layers; and forming a passivation layer.
[0046] The above description is only an overview of the technical solution of the present invention. In order to more clearly understand the technical means of the present invention, it can be implemented in accordance with the contents of the specification. In order to make the above and other purposes, features and advantages of the present invention more obvious and easy to understand, the specific implementation methods of the present invention are specifically listed below. BRIEF DESCRIPTION OF THE DRAWINGS
[0047] Figure 1An exemplary flowchart illustrates a method for manufacturing a thin-film lithium niobate electro-optic modulator according to some embodiments;
[0048] Figure 2 A schematic diagram of a structure including a substrate wafer and a silicon nitride layer provided in accordance with some embodiments is exemplarily shown;
[0049] Figure 3 Schematic diagram of a structure including an optical waveguide provided according to some embodiments is exemplarily shown;
[0050] Figure 4 An exemplary schematic diagram of a structure including a groove is shown according to some embodiments;
[0051] Figure 5 A schematic diagram of a structure including a photoresist according to some embodiments is exemplarily shown;
[0052] Figure 6 Schematic diagram of a structure including a metal layer provided according to some embodiments is exemplarily shown;
[0053] Figure 7 An exemplary schematic diagram of a structure including a metal electrode is shown according to some embodiments;
[0054] Figure 8 Schematic diagram of a structure including an insulating oxide material provided according to some embodiments is exemplarily shown;
[0055] Figure 9 illustratively shows a schematic structural diagram including a second insulating dielectric layer provided according to some embodiments;
[0056] Figure 10 Schematic diagram of a structure including a thin-film lithium niobate wafer provided according to some embodiments is exemplarily shown;
[0057] Figure 11 A schematic structural diagram of a bonding structure provided according to some embodiments is exemplarily shown;
[0058] Figure 12 An exemplary schematic diagram of a structure including a protective layer is shown according to some embodiments;
[0059] Figure 13 An exemplary schematic diagram of a structure for removing a silicon substrate is shown according to some embodiments;
[0060] Figure 14 A schematic structural diagram of removing a protective layer according to some embodiments is exemplarily shown;
[0061] Figure 15Schematic diagram of a structure including a passivation material provided according to some embodiments is exemplarily shown;
[0062] Figure 16 Schematic diagram of a structure including a passivation layer provided according to some embodiments is exemplarily shown;
[0063] Figure 17 A schematic structural diagram of a thin-film lithium niobate electro-optic modulator provided according to some embodiments is exemplarily shown. DETAILED DESCRIPTION
[0064] The technical solutions in the embodiments of this application will be clearly and completely described below with reference to the accompanying drawings. Obviously, the described embodiments are only some embodiments of this application, and not all embodiments.
[0065] It should be noted that, in the description of this application, the terms "on...", "above...", "above...", and "above..." should be interpreted in the broadest sense, meaning that the description containing these terms is interpreted as "the component can be set on another component in direct contact, or there can be an intermediate component or layer between the components". In addition, for the convenience of description, this application may also use spatially relative terms such as "under...", "under...", "under...", "on...", "above...", "above...", "lower", "upper", etc. to describe the relationship between one element or component and another element or component shown in the drawings. In addition to the orientations described in the figures, the spatially relative terms are also intended to cover different orientations of the device in use or operation. The device can be oriented in other ways (rotated 90° or in other orientations), and the spatially relative descriptors used in this application can be interpreted accordingly.
[0066] As used herein, the term "layer" refers to a portion of a material comprising an area having a certain thickness. A layer may extend over the entire underlying or superstructure, or may extend over a localized area of the underlying or superstructure. Furthermore, a layer may be a region of a continuous structure, either homogeneous or heterogeneous, whose thickness is less than that of the continuous structure. For example, a layer may be located between the top and bottom surfaces of a continuous structure, or between any pair of horizontal planes therebetween. A layer may extend horizontally, vertically, and / or along a tapered surface.
[0067] Photonic systems require modulators with complementary metal oxide semiconductor (CMOS)-compatible drive voltages, large bandwidth, low optical insertion loss, high extinction ratio, excellent signal quality, and compatibility with large-scale manufacturing. Lithium niobate (LN) electro-optic modulators (EOMs) are widely used in long-distance optical communications due to their excellent material properties, including temperature stability and a wide range of optical transparency windows. Furthermore, ultra-low-loss thin-film lithium niobate (TFLN) waveguide platforms offer excellent performance, including a small footprint, low half-wave voltage (Vπ), and a 3-dB bandwidth exceeding 100 GHz. However, current thin-film lithium niobate EOMs are difficult to manufacture.
[0068] How to solve the problem of difficulty in manufacturing thin-film lithium niobate electro-optical modulators has become a technical problem that needs to be urgently solved by those skilled in the art.
[0069] The present invention provides a method for manufacturing a thin-film lithium niobate electro-optical modulator. This method first fabricates an optical waveguide and metal electrodes on a CMOS-compatible silicon nitride layer. Bonding the thin-film lithium niobate layer is then performed as a subsequent step, reducing incompatibility with the CMOS process. Furthermore, the bonded thin-film lithium niobate layer can tolerate alignment errors of up to 100 μm, reducing manufacturing complexity. The thin-film lithium niobate electro-optical modulator utilizes chip-to-wafer heterogeneous bonding, facilitating the realization of silicon-based electro-photonic integrated systems and the industrial application of large-scale electro-optical integrated chips.
[0070] Figure 1 The flowchart of a method for manufacturing a thin-film lithium niobate electro-optical modulator according to some embodiments is exemplarily shown. The method includes S100-S700.
[0071] S100, providing a substrate wafer. Figure 2 An exemplary schematic diagram of a structure including a substrate wafer and a silicon nitride layer according to some embodiments is shown. The substrate wafer includes a silicon layer 101 and a first insulating dielectric layer 102 disposed on the upper end of the silicon layer 101. Exemplarily, the first insulating dielectric layer is SiO2.
[0072] S200, forming a silicon nitride layer, wherein the silicon nitride layer 201 is disposed on a side of the first insulating dielectric layer 102 away from the silicon layer 101, and referring again to Figure 2 .
[0073] S300, forming multiple optical waveguides 202, Figure 3 An exemplary schematic diagram of a structure including optical waveguides is shown according to some embodiments. The plurality of optical waveguides 202 are disposed on the side of the first insulating dielectric layer 102 away from the silicon layer 101. In one example, the optical waveguides are strip-shaped.
[0074] In some embodiments, the step of forming a plurality of optical waveguides includes:
[0075] The silicon nitride layer 201 is etched to form a plurality of optical waveguides 202. Figure 3 .
[0076] In some embodiments, a silicon nitride layer is grown on the side of the first insulating dielectric layer 102 away from the silicon layer 101 by low-pressure chemical vapor deposition (LPCVD) to realize a low-loss optical transmission channel. For example, the thickness of the silicon nitride layer can be in the range of 100-300 nm.
[0077] S400: A plurality of metal electrodes are formed, wherein a portion of the metal electrodes is embedded in the first insulating dielectric layer and located between the two optical waveguides.
[0078] Since LN is not a CMOS-compatible material, TFLN cannot manufacture large-sized wafers (only 4 or 6 inches) and requires processes such as EBL (Electron Beam Lithography). The etching process has poor uniformity and the waveguide steepness is around 70°, which increases the optical transmission loss and is not conducive to integration with other devices. Therefore, in the embodiment of the present application, the optical waveguide and metal electrodes are first made on the silicon nitride layer compatible with the CMOS process, and the bonding thin-film lithium niobate layer is used as a subsequent step, which reduces the incompatibility with the CMOS process. At the same time, the allowable alignment error of the bonded thin-film lithium niobate layer can be up to 100μm, reducing the manufacturing difficulty. If the metal electrode is made after bonding, the alignment error of the metal electrode needs to be as small as possible. Less than 1μm, which increases the challenge of the process.
[0079] In some embodiments, the step of forming a plurality of metal electrodes includes:
[0080] Figure 4 An exemplary schematic diagram of a structure including grooves according to some embodiments is shown. A first insulating dielectric layer 102 located between the two optical waveguides 202 is etched to form a groove 1021. To make the structure in the figure clearer, Figure 4 This is only a schematic diagram of a portion of the structure during the fabrication of the thin-film lithium niobate electro-optic modulator. It can be understood that the thin-film lithium niobate electro-optic modulator does not only include... Figure 4 The two optical waveguides shown in Figure 4 The grooves include not only the grooves between the two optical waveguides, but also the grooves provided between the two optical waveguides and other optical waveguides. Figure 4The substrate includes three grooves 1021. Of course, the number of grooves may actually be greater. For example, the grooves have a depth of 300 nm to 900 nm and a width of 15 to 25 μm or 60 to 100 μm. The width of the grooves can be determined based on the required width of the subsequent metal electrode.
[0081] Figure 5 A schematic diagram of a structure including photoresist according to some embodiments is shown. Photoresist 301 is formed on the surface of the first insulating dielectric layer 102 facing away from the silicon layer 101, excluding the groove 1021, and on the surface of the optical waveguide 202 facing away from the silicon layer 101. In some embodiments, the steps of forming the photoresist include spin coating, exposure, development, and baking.
[0082] Figure 6 A schematic diagram of a structure including a metal layer according to some embodiments is shown. A metal layer 401 is formed within the groove 1021 and on the surface of the photoresist 301 facing away from the silicon layer 101. In some embodiments, magnetron sputtering of a metal such as aluminum or gold is used to deposit it within the groove 1021 and on the surface of the photoresist 301 facing away from the silicon layer 101 to achieve electric field microwave control. In one example, the thickness of the metal layer is 500-1500 nm.
[0083] Figure 7 The schematic diagram of a structure including a metal electrode according to some embodiments is exemplarily shown. The photoresist 301 is stripped off, and the remaining metal layer forms a metal electrode 402.
[0084] S500 , forming a second insulating dielectric layer, wherein the second insulating dielectric layer is located on a side of the first insulating dielectric layer, the optical waveguide, and the metal electrode away from the silicon layer.
[0085] In some embodiments, the step of forming the second insulating dielectric layer includes:
[0086] Figure 8 A schematic diagram of a structure including an insulating oxide material according to some embodiments is shown. An insulating oxide material 501 is grown on a surface of the first insulating dielectric layer 102 facing away from the silicon layer 101, and on surfaces of the optical waveguide 202 and metal electrode 402 where the first insulating dielectric layer 102 is exposed.
[0087] Figure 9 An exemplary schematic diagram of a structure including a second insulating dielectric layer is shown according to some embodiments. The second insulating dielectric layer 502 is obtained by thinning the insulating oxide material 501.
[0088] In some embodiments, chemical mechanical planarization (CMP) is used to thin the insulating oxide material 501. The side of the optical waveguide 202 away from the silicon layer 101 is lower than the side of the second insulating dielectric layer 502 away from the silicon layer 101, and the distance between the two can be 30-100 nm.
[0089] S600: Form multiple thin-film lithium niobate layers and multiple silicon oxide layers. The thin-film lithium niobate layers are bonded to the side of the second insulating dielectric layer away from the silicon layer. The silicon oxide layers are located on the side of the thin-film lithium niobate layers away from the silicon layer. The thin-film lithium niobate layers and silicon oxide layers correspond one-to-one.
[0090] Since the single crystal submicron thick TFLN is bonded to a low refractive index insulating substrate (silicon dioxide, SiO2), it provides a high refractive index contrast, and the optical mode is limited to a very small range. It is difficult to achieve vertical side walls when etching TFLN, and form a good ridge waveguide. The bonding method in the embodiment of the present application does not need to etch the thin film lithium niobate layer, avoiding the problem that it is difficult to achieve vertical side walls when etching the thin film lithium niobate, and form a good ridge waveguide, and avoids the problem of tilted side walls and large light loss, giving full play to the excellent characteristics of lithium niobate, and achieving a cross-generational improvement in device performance. At the same time, the metal electrodes and passive optical waveguide structures are manufactured on a silicon nitride platform compatible with the CMOS process, and the process is more mature. In addition, it reduces production costs and is suitable for large-scale production. After completing step S500, a silicon nitride wafer is formed. The thin-film lithium niobate electro-optic modulator adopts the form of chip (i.e., thin-film lithium niobate wafer) to wafer (die-wafer, i.e., silicon nitride wafer). Unlike die-die (chip-chip) bonding, the bonding of the thin-film lithium niobate layer only occurs in a designated area, and the device structure in other areas is not affected by the bonding. In addition to integration with other electro-optical devices, it is also suitable for multi-material integration. The introduction of certain materials with better optical properties is conducive to integration with other electro-optical devices such as detectors, lasers, filters, etc., realizing a truly silicon-based electro-photonic monolithic integrated system and realizing the industrial application of large-scale electro-optical integrated chips. The use of wafer-level technology can greatly improve process stability, increase output and reduce costs. In the embodiment of the present application, after making optical waveguides and metal electrodes on the silicon nitride wafer and bonding them to the thin-film lithium niobate layer, both system reliability and process feasibility can be taken into account.
[0091] In some embodiments, the step of forming a plurality of thin-film lithium niobate layers and a plurality of silicon oxide layers includes:
[0092] Figure 10A schematic diagram of a structure including a thin-film lithium niobate wafer according to some embodiments is shown. A plurality of thin-film lithium niobate wafers 601 are provided, wherein each thin-film lithium niobate wafer 601 includes a silicon substrate 6011 and a material to be bonded 6012. The material to be bonded 6012 includes a thin-film lithium niobate 60121 and silicon oxide 60122 disposed between the thin-film lithium niobate 60121 and the silicon substrate 6011.
[0093] In some embodiments, the step of providing a thin film lithium niobate wafer includes:
[0094] Thin-film lithium niobate wafers are cut into small pieces and cleaned with RCA-1 solvent, which contains NH₄OH, H₂O₂, and H₂O in a volume ratio of 1:1:5. Cleaning with RCA-1 removes dust particles and contaminants.
[0095] Activating the material to be bonded on the thin-film lithium niobate wafer to obtain an activated thin-film lithium niobate wafer. In some embodiments, the step of activating the material to be bonded on the thin-film lithium niobate wafer includes activating the material to be bonded on the thin-film lithium niobate wafer using radio frequency plasma (RF plasma). In one example, the activation can be performed at 150 W and 1.103 mbar for 180 seconds.
[0096] The material to be bonded in the activated thin-film lithium niobate wafer is bonded to a side of the second insulating dielectric layer away from the silicon layer.
[0097] In some embodiments, the step of bonding the material to be bonded in the activated thin-film lithium niobate wafer to a side of the second insulating dielectric layer away from the silicon layer includes:
[0098] Figure 11 A schematic diagram of a bonded structure according to some embodiments is shown. The bonded material 6021 in the activated thin-film lithium niobate wafer 602 is bonded to the side of the second insulating dielectric layer 502 facing away from the silicon layer 101. The bonded material 6021 is then immersed in deionized water for a predetermined period of time and then dried with nitrogen gas, thereby bonding the bonded material 6021 to the second insulating dielectric layer 502.
[0099] Figure 12A schematic diagram of a structure including a protective layer according to some embodiments is shown. A protective layer 701 is formed and disposed on the surface of the second insulating dielectric layer 502 facing away from the silicon layer 101, excluding the portion in contact with the activated thin-film lithium niobate wafer 602. In one example, the protective layer can be several microns thick.
[0100] Figure 13 A schematic diagram of a structure for removing a silicon substrate according to some embodiments is shown. The silicon substrate 6011 is removed. In some embodiments, dry etching is used to remove the silicon substrate of the activated thin-film lithium niobate wafer.
[0101] Figure 14 The protective layer 701 is removed, and the activated thin-film lithium niobate wafer 602 and silicon oxide form a thin-film lithium niobate layer 60211 and a silicon oxide layer 60212 .
[0102] In some embodiments, before the step of forming the protective layer, the method further comprises: annealing the film through a preset temperature gradient cycle. For example, under certain pressure conditions, such as 9.8Ncm -2 Under the applied pressure, the bonded sample is annealed by setting a temperature gradient cycle, and the annealing temperature range can be 100-300°C.
[0103] S700. Form a passivation layer, wherein the passivation layer is disposed on a surface of the thin-film lithium niobate layer away from the silicon layer, and on side walls of the thin-film lithium niobate layer and the oxide layer; a surface of the passivation layer away from the silicon layer is higher than a surface of the thin-film lithium niobate layer away from the silicon layer.
[0104] In some embodiments, the step of forming the passivation layer includes:
[0105] Figure 15 A schematic diagram of a structure including a passivation material according to some embodiments is shown. Passivation material 801 is grown on the surface of the thin-film lithium niobate layer 60211 facing away from the silicon layer 101, as well as on the sidewalls of the thin-film lithium niobate layer 60211 and the silicon oxide layer 60212. In one example, the passivation material is silicon oxide.
[0106] Figure 16A schematic diagram of a structure including a passivation layer according to some embodiments is shown. The passivation material 801 and silicon oxide layer 60212 are thinned to form a passivation layer 802. In this embodiment, excess passivation material is removed. Depending on device design requirements, a certain thickness of passivation material and / or silicon oxide layer may be retained as a passivation layer. Specific methods may include HF wet etching or chemical mechanical polishing (CMP).
[0107] In an embodiment of the present application, a thin-film lithium niobate electro-optic modulator is provided. In this method, an optical waveguide and a metal electrode are first fabricated on a silicon nitride layer compatible with a CMOS process, and bonding of the thin-film lithium niobate layer is performed as a subsequent step, thereby reducing the incompatibility with the CMOS process. At the same time, the allowable alignment error of the bonded thin-film lithium niobate layer can be as low as 100 μm, reducing the difficulty of manufacturing. In addition, the thin-film lithium niobate does not need to be etched during the bonding process, reducing the production cost and being suitable for large-scale production. The thin-film lithium niobate electro-optic modulator adopts the form of chip-to-wafer heterogeneous bonding, which is conducive to the realization of silicon-based electro-photonic integrated systems and the industrial application of large-scale electro-optical integrated chips. The method includes: providing a substrate wafer; forming a silicon nitride layer; forming a plurality of optical waveguides; forming a plurality of metal electrodes; forming a second insulating dielectric layer; forming a plurality of thin-film lithium niobate layers and a plurality of silicon oxide layers; and forming a passivation layer.
[0108] A growing number of applications, such as artificial intelligence optical computing, are placing higher demands on process platforms, requiring high-performance devices and larger networks. As hybrid electro-optical modulator designs continue to be refined and validated, the capabilities of existing silicon foundry processes can be leveraged to integrate increasingly complex and multifunctional components with TFLNs. The crystalline properties of the silicon layer can be exploited to incorporate dopants to create diodes and detectors. Combined, these designs and fabrication processes will benefit numerous applications in both classical and quantum photonics.
[0109] The present application also provides a thin film lithium niobate electro-optic modulator. Figure 17 A schematic structural diagram of a thin-film lithium niobate electro-optic modulator provided according to some embodiments is exemplarily shown. Figure 16 The structure shown in the figure is a partial structure of a thin film lithium niobate electro-optical modulator, mainly to facilitate a clearer view of the structural details of the thin film lithium niobate electro-optical modulator. The thin film lithium niobate electro-optical modulator includes:
[0110] A substrate wafer, the substrate wafer comprising a silicon layer and a first insulating dielectric layer disposed on an upper end of the silicon layer;
[0111] a plurality of optical waveguides, wherein the plurality of optical waveguides are arranged on a side of the first insulating dielectric layer away from the silicon layer;
[0112] a plurality of metal electrodes, wherein portions of the metal electrodes are embedded in the first insulating dielectric layer and located between the two optical waveguides;
[0113] a second insulating dielectric layer, wherein the second insulating dielectric layer is located on a side of the first insulating dielectric layer, the optical waveguide, and the metal electrode away from the silicon layer;
[0114] Multiple thin-film lithium niobate layers and multiple silicon oxide layers are provided. The thin-film lithium niobate layers are bonded to the side of the second insulating dielectric layer away from the silicon layer. The silicon oxide layers are located on the side of the thin-film lithium niobate layers away from the silicon layer. The thin-film lithium niobate layers and silicon oxide layers correspond one-to-one.
[0115] A passivation layer is provided on the surface of the thin-film lithium niobate layer away from the silicon layer, and on the sidewalls of the thin-film lithium niobate layer and the oxide layer; the surface of the passivation layer away from the silicon layer is higher than the surface of the thin-film lithium niobate layer away from the silicon layer.
[0116] It should be noted that the device structure, shape, and materials in the embodiments of the thin-film lithium niobate electro-optic modulator in this application can refer to the above-mentioned embodiments of the manufacturing method of the thin-film lithium niobate electro-optic modulator, and will not be repeated here.
[0117] The above embodiments merely illustrate several implementations of the present invention, and while the descriptions are relatively specific and detailed, they should not be construed as limiting the scope of the patent. It should be noted that a person skilled in the art would be able to make various modifications and improvements without departing from the spirit of the present invention, all of which fall within the scope of protection of the present invention. Therefore, the scope of protection of the patent for this invention shall be determined by the appended claims.
Claims
1. A method for manufacturing a thin film lithium niobate electro-optic modulator, characterized in that: include: Providing a substrate wafer, the substrate wafer comprising a silicon layer and a first insulating dielectric layer disposed on an upper end of the silicon layer; forming a silicon nitride layer, wherein the silicon nitride layer is disposed on a side of the first insulating dielectric layer away from the silicon layer; forming a plurality of optical waveguides, wherein the plurality of optical waveguides are arranged on a side of the first insulating medium layer away from the silicon layer; forming a plurality of metal electrodes, wherein parts of the metal electrodes are embedded in the first insulating medium layer and located between the two optical waveguides; forming a second insulating dielectric layer, wherein the second insulating dielectric layer is located on a side of the first insulating dielectric layer, the optical waveguide, and the metal electrode away from the silicon layer; forming a plurality of thin-film lithium niobate layers and a plurality of silicon oxide layers, wherein the thin-film lithium niobate layers are bonded to a side of the second insulating dielectric layer away from the silicon layer, the silicon oxide layers are located on a side of the thin-film lithium niobate layers away from the silicon layer, and the thin-film lithium niobate layers and the silicon oxide layers correspond one to one; A passivation layer is formed, wherein the passivation layer is disposed on the surface of the thin-film lithium niobate layer away from the silicon layer, and on the side walls of the thin-film lithium niobate layer and the oxide layer; the surface of the passivation layer away from the silicon layer is higher than the surface of the thin-film lithium niobate layer away from the silicon layer.
2. The method according to claim 1, characterized in that The step of forming a plurality of optical waveguides includes etching the silicon nitride layer to form a plurality of optical waveguides.
3. The method according to claim 1, characterized in that: The step of forming a plurality of metal electrodes comprises: Etching the first insulating dielectric layer between the two optical waveguides to form a groove; forming a photoresist on a portion of a surface of the first insulating dielectric layer away from the silicon layer except the groove, and on a surface of the optical waveguide away from the silicon layer; forming a metal layer in the groove and on the surface of the photoresist away from the silicon layer; The photoresist is stripped off, and the remaining metal layer forms a metal electrode.
4. The method according to claim 1, characterized in that: The step of forming the second insulating dielectric layer comprises: Growing an insulating oxide material on a surface of the first insulating dielectric layer away from the silicon layer and on surfaces of the optical waveguide and the metal electrode exposed from the first insulating dielectric layer; The insulating oxide material is thinned to obtain a second insulating dielectric layer.
5. The method according to claim 1, characterized in that The step of forming a plurality of thin-film lithium niobate layers and a plurality of silicon oxide layers comprises: Providing a plurality of thin-film lithium niobate wafers, wherein the thin-film lithium niobate wafers include a silicon substrate and a material to be bonded, and the material to be bonded includes thin-film lithium niobate and silicon oxide disposed between the thin-film lithium niobate and the silicon substrate; activating the material to be bonded of the thin-film lithium niobate wafer to obtain an activated thin-film lithium niobate wafer; Bonding the material to be bonded in the activated thin-film lithium niobate wafer to a side of the second insulating dielectric layer away from the silicon layer; forming a protective layer, wherein the protective layer is disposed on a portion of the surface of the second insulating dielectric layer on a side away from the silicon layer except for a portion in contact with the activated thin-film lithium niobate wafer; removing the silicon substrate; The protective layer is removed, and the thin film lithium niobate and silicon oxide in the activated thin film lithium niobate wafer form a thin film lithium niobate layer and a silicon oxide layer.
6. The method according to claim 1, characterized in that The step of forming a passivation layer comprises: Growing a passivation material on the surface of the thin-film lithium niobate layer on the side away from the silicon layer, and on the sidewalls of the thin-film lithium niobate layer and the sidewalls of the silicon oxide layer; The passivation material is thinned to form a passivation layer.
7. The method according to claim 1, characterized in that The step of activating the material to be bonded of the thin film lithium niobate wafer comprises: Radio frequency plasma is used to activate the material to be bonded on the thin film lithium niobate wafer.
8. The method according to claim 1, characterized in that The step of bonding the material to be bonded in the activated thin-film lithium niobate wafer to a side of the second insulating dielectric layer away from the silicon layer comprises: The material to be bonded in the activated thin-film lithium niobate wafer is laminated to the side of the second insulating dielectric layer away from the silicon layer, and immersed in deionized water for a preset time, and then blown dry with nitrogen to bond the material to be bonded to the second insulating dielectric layer.
9. The method according to claim 8, characterized in that Before the step of forming the protective layer, the method further includes: annealing through a preset temperature gradient cycle.
10. A thin film lithium niobate electro-optic modulator, characterized in that: include: A substrate wafer, the substrate wafer comprising a silicon layer and a first insulating dielectric layer disposed on an upper end of the silicon layer; A plurality of optical waveguides, wherein the plurality of optical waveguides are arranged on a side of the first insulating medium layer away from the silicon layer; a plurality of metal electrodes, parts of which are embedded in the first insulating medium layer and located between the two optical waveguides; a second insulating dielectric layer, wherein the second insulating dielectric layer is located on a side of the first insulating dielectric layer, the optical waveguide, and the metal electrode away from the silicon layer; A plurality of thin-film lithium niobate layers and a plurality of silicon oxide layers, wherein the thin-film lithium niobate layers are bonded to a side of the second insulating dielectric layer away from the silicon layer, the silicon oxide layers are located on a side of the thin-film lithium niobate layers away from the silicon layer, and the thin-film lithium niobate layers and the silicon oxide layers correspond one to one; A passivation layer is provided on the surface of the thin film lithium niobate layer away from the silicon layer, and on the side walls of the thin film lithium niobate layer and the oxide layer; the surface of the passivation layer away from the silicon layer is higher than the surface of the thin film lithium niobate layer away from the silicon layer.
Citation Information
Patent Citations
Low-power consumption double module integrated humidity sensitive chip with heating function and its manufacture method
CN101308110A
Pressure, flow and temperature integrated chip and method for manufacturing same
CN103496665A
Silicon-based photoelectron monolithic heterogeneous integration method
CN112764158A
Monocrystal piezoelectric film and preparation method thereof
CN115084352A
Electro-optical modulator and preparation method thereof
CN115793294A
Cited By
Heterogeneous integrated electro-optical modulator and preparation method thereof
CN119828363A
A heterogeneous integrated electro-optical modulation device and its preparation method
CN119828363B
Electro-optical film wafer and preparation method thereof, and preparation method of heterogeneous integrated electro-optical modulator