Graphene packaged metal nanowire composite transparent electrode and preparation method thereof
By using graphene to encapsulate the metal nanowire composite structure in transparent electrodes, combining the thermal insulation layer and conductive dielectric, the metal migration problem in the unbonded surface of the metal nanowire and high temperature and high humidity environment is solved, and the conductivity of the electrode is improved. stability.
Patent Information
- Application Number
- CN202410933855.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-12
- Publication Date
- 2024-11-22
AI Technical Summary
The surface of metal nanowires is not fully bonded to affect the conductivity of the electrode, and metal migration is prone to occur in high temperature and high humidity environments, resulting in a degradation of electrode performance.
Graphene encapsulated metal nanowire composite transparent electrode, by setting the insulation layer and conductive dielectric inside the outer protective film, and applying anti-diffusing reflection coating on the surface of the metal nanowire, forming a conductive grid to improve conductivity, while using transparent external protection. The membrane and thermal insulation layer are used to block water and oxygen.
It improves the conductivity and durability of the electrode, reduces the risk of metal migration in high temperature and high humidity environments, and enhances the stability and service life of the electrode.
Smart Images

Figure CN119008083A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of electronic materials, and in particular to a graphene-encapsulated metal nanowire composite transparent electrode and a preparation method thereof. Background Art
[0002] Transparent electrodes are important components of various optoelectronic devices and have been widely used in sensors, displays, light-emitting diodes, solar cells, etc. With the development of science and technology, new high-performance optoelectronic devices require electrodes with higher conductivity and better transparency.
[0003] There are three main types of transparent electrodes at present. The first is transparent conductive oxides, such as indium tin oxide; the second is ultrathin metal film; and the third is nanometal structure. Compared with precious metals, indium tin oxide has higher transparency but relatively lower conductivity, and the scarcity of indium leads to higher cost of indium tin oxide. Ultrathin metal films with a thickness of less than 5nm show higher reasonable transmission performance, but the thickness of ultrathin metal films will lead to higher resistivity, and ultrathin metal films have high requirements for manufacturing processes, such as film continuity and surface roughness, which have high processing requirements. For nanometal structures, the atoms on the surface of nanometal wires are not fully bonded, and the resistivity of nanometal wires is affected by boundary effects. In addition, metal particles in nanometal wires are very prone to metal migration in high temperature, high humidity and electrification environments, which causes metal nanowires to be destroyed and affects the conductivity of the electrode. For this reason, a graphene encapsulated metal nanowire composite transparent electrode and a preparation method are proposed. Summary of the invention
[0004] The present invention provides a graphene-encapsulated metal nanowire composite transparent electrode and a preparation method thereof, which solves the problem that the unbonded atoms on the surface of the metal nanowires mentioned in the above background technology affect the conductivity of the electrode and metal migration is prone to occur in a high temperature and high humidity environment.
[0005] The present invention provides the following technical solution: a graphene-encapsulated metal nanowire composite transparent electrode, comprising an outer protective film, the inner wall of the outer protective film is fixedly connected to a heat insulation layer, the inner cavity of the heat insulation layer is provided with an isolation plate, a packaging plate, a conductive medium, a conductive mesh and a substrate from top to bottom, the top of the substrate is inlaid with a conductive mesh, the outer surface of the conductive mesh is coated with an anti-diffuse reflection coating, the top of the conductive mesh is covered with a conductive medium, the top of the conductive medium is fixedly connected to a packaging plate, and the top of the packaging plate is fixedly connected to an isolation plate.
[0006] Preferably, a mesh groove adapted to the conductive mesh is provided on the top of the substrate, and conductive pillars are evenly and fixedly connected to the bottom of the substrate.
[0007] Preferably, the conductive mesh comprises metal nanowires, and the outer surfaces of the metal nanowires are coated with an anti-diffuse reflection coating.
[0008] Preferably, the packaging plate is made of graphene, and the outer protective film is made of a transparent conductive material.
[0009] Preferably, the thermal insulation layer is mesh-shaped, and a conductive medium is filled between the thermal insulation layer and the outer protective film, the conductive column is adapted to the mesh of the thermal insulation layer, and the bottom of the conductive column is in contact with the outer protective film through the mesh of the thermal insulation layer.
[0010] A method for preparing a graphene-encapsulated metal nanowire composite transparent electrode comprises the following steps:
[0011] Step 1: prepare a transparent substrate, wherein the top of the transparent substrate is horizontal and the bottom of the transparent substrate has protruding conductive columns;
[0012] Step 2: etching a mesh groove on the top of the transparent substrate;
[0013] Step 3: spraying a hydrophilic coating on the top of the transparent substrate;
[0014] Step 4: prepare metal nanowires, apply an anti-diffuse reflection coating on the outer surface of the metal nanowires, apply a hydrophilic coating on the outer surface of the anti-diffuse reflection coating, fill the metal nanowires into the mesh slots, and form a conductive mesh with the metal nanowires;
[0015] Step 5: spray the conductive medium onto the structure formed in step 4;
[0016] Step 6: Encapsulate the structure formed in step 5 with an encapsulation plate, and fix an isolation plate on the top of the encapsulation plate;
[0017] Step 7: Wrap the structure formed in step 6 with a heat-insulating layer, and spray a conductive medium on the outer surface of the heat-insulating layer.
[0018] Step 8: Fix a transparent outer protective film on the outer surface of the thermal insulation layer.
[0019] Preferably, in step seven, the conductive column contacts the outer protective film through the mesh holes of the thermal insulation layer.
[0020] Compared with the prior art, the present invention has the following beneficial effects:
[0021] 1. The graphene-encapsulated metal nanowire composite transparent electrode and preparation method can intercept heat by setting a heat-insulating layer, so that the electrode has a heat-insulating function and reduces the influence of the external environment on the electrode. The outer protective film can play a role in water and oxygen barrier, which is convenient for the use of the electrode.
[0022] 2. The graphene-encapsulated metal nanowire composite transparent electrode and preparation method can reduce the boundary effect of the metal nanowires, improve the conductivity of the motor, and facilitate the use of the electrode by applying an anti-diffuse reflection coating on the outer surface of the power grid. BRIEF DESCRIPTION OF THE DRAWINGS
[0023] Figure 1 It is a front schematic diagram of the structure of the present invention;
[0024] Figure 2 Schematic diagram of the structural base of the present invention.
[0025] In the figure: 1. outer protective film; 2. substrate; 3. conductive mesh; 4. conductive medium; 5. thermal insulation layer; 6. isolation plate; 7. packaging plate; 8. conductive column; 9. mesh slot. DETAILED DESCRIPTION
[0026] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0027] The present invention provides an embodiment: please refer to Figure 1 and Figure 2 ,, a graphene encapsulated metal nanowire composite transparent electrode, including an outer protective film 1. The outer protective film 1 can play a role in water and oxygen barrier, prevent moisture from corroding the electrode, and facilitate the use of the electrode.
[0028] The inner surface of the outer protective film 1 is adhered with a heat insulation layer 5, which is woven into a mesh from a transparent material, and the outer surface of the glass fiber is coated with a conductive medium, so that the heat insulation layer 5 has a conductive function, which facilitates the operation of the electrode.
[0029] The bottom of the inner cavity of the thermal insulation layer 5 is fixedly connected to a substrate 2 made of a transparent conductive material, and the top of the substrate 2 is horizontal. The bottom of the substrate 2 is evenly provided with protruding conductive columns 8, and the conductive columns 8 are located in the mesh of the thermal insulation layer 5, and the bottom of the conductive columns 8 is in contact with the inner surface of the outer protective film 1.
[0030] After a mesh groove 9 is opened on the top of the substrate 2, a hydrophilic coating is applied on the top of the substrate 2, and the inner cavity of the mesh groove 9 is filled with metal nanowires. The metal nanowires in the mesh groove 9 form a conductive mesh 3, and an anti-diffuse reflection coating is applied on the outer surface of the metal nanowires, and a hydrophilic coating is applied on the outer surface of the anti-diffuse reflection coating.
[0031] A conductive medium 4 is applied on the conductive mesh 3, and the conductive medium 4 connects the metal nanowires together to facilitate the wiring of the electrode.
[0032] The top of the conductive medium 4 is fixedly connected with a packaging plate 7, and the top of the packaging plate 7 is fixedly connected with an isolation plate 6, which protects the packaging plate 7. The top of the isolation plate 6 is provided with a convex column adapted to the mesh of the thermal insulation layer 5.
[0033] A method for preparing a graphene-encapsulated metal nanowire composite transparent electrode comprises the following steps:
[0034] Step 1: prepare a transparent substrate 2, wherein the top of the transparent substrate 2 is horizontal and the bottom of the transparent substrate 2 has a protruding conductive column 8;
[0035] Step 2: etching a mesh groove 9 on the top of the transparent substrate 2;
[0036] Step 3: spraying a hydrophilic coating on the top of the transparent substrate 2;
[0037] Step 4: prepare metal nanowires, apply an anti-diffuse reflection coating on the outer surface of the metal nanowires, apply a hydrophilic coating on the outer surface of the anti-diffuse reflection coating, fill the metal nanowires into the mesh slots 9, and the metal nanowires form a conductive mesh 3;
[0038] Step 5: spray the conductive medium 4 on the structure formed in step 4, and dry it to speed up the drying speed of the conductive medium 4;
[0039] Step 6: Encapsulate the structure formed in step 5 with an encapsulation plate 7, and fix an isolation plate 6 on the top of the encapsulation plate 7;
[0040] Step seven: Wrap the structure formed in step six with a heat insulation layer 5 , and spray a conductive medium 4 on the outer surface of the heat insulation layer 5 .
[0041] Step eight: fix the transparent outer protective film 1 on the outer surface of the heat insulation layer 5.
[0042] In step seven, the conductive pillars 8 are in contact with the outer protective film 1 through the mesh holes of the thermal insulation layer 5 .
[0043] Embodiment 1:
[0044] The material of the outer protective film is ITO transparent waterproof conductive film, the material of the substrate 2 is conductive glass film, and the material of the conductive mesh 3 is silver nanowires; the conductive medium 4 is a graphene oxide solution with a concentration of 8 mg / ml, the thermal insulation layer 5 is woven into a mesh by glass fibers, and the size of the mesh is the same as the diameter of the conductive column 8, the thickness of the thermal insulation layer 5 is the same as the height of the conductive column 8, the material of the packaging plate 7 is graphene, and the material of the isolation plate 6 is quartz film.
[0045] The preparation steps of the electrode are as follows: grid lines are drawn on the top of a transparent substrate 2 with paraffin wax, an etchant is sprayed on the grid lines, and a mesh groove 9 is drawn on the top of the substrate 2 by etching; the substrate 2 is cleaned, and a hydrophilic graphene oxide coating is sprayed on the top of the transparent substrate 2; the outer surface of the silver nanowire is coated with a conductive coating composed of conductive graphite for anti-diffuse reflection, and a hydrophilic graphene oxide coating is applied on the outer surface of the anti-diffuse reflection coating, and the treated silver nanowires are filled into the mesh groove 9, so that the silver nanowires form a conductive mesh 3; a conductive medium 4 is covered on the conductive mesh 3 by spraying; the structure formed in the above steps is encapsulated with a packaging plate 7, and an isolation plate 6 is adhered to the top of the packaging plate 7; the structure formed in the above steps is wrapped with a heat insulation layer 5, and a transparent outer protective film 1 is fixed on the outer surface of the heat insulation layer 5.
[0046] Embodiment 2:
[0047] The material of the outer protective film is ITO transparent waterproof conductive film, the material of the substrate 2 is PA flexible film, and the material of the conductive mesh 3 is copper nanowires; the conductive medium 4 is a graphene oxide solution with a concentration of 8 mg / ml, the thermal insulation layer 5 is woven into a mesh by glass fibers, and the size of the mesh is the same as the diameter of the conductive column 8, the thickness of the thermal insulation layer 5 is the same as the height of the conductive column 8, the material of the packaging board 7 is graphene, and the material of the isolation board 6 is PC flexible film.
[0048] The preparation steps of the electrode are as follows: a mesh groove 9 is formed by a flexible film of the same material as the substrate 2, and the mesh groove 9 is bonded to the top of the substrate 2, and a hydrophilic graphene oxide coating is sprayed on the top of the transparent substrate 2; the outer surface of the copper nanowire is wrapped with a conductive coating composed of conductive graphite for anti-diffuse reflection, and a hydrophilic graphene oxide coating is applied on the outer surface of the anti-diffuse reflection coating, and the treated copper nanowire is filled into the mesh groove 9, and the copper nanowire forms a conductive mesh 3; a conductive medium 4 is covered on the conductive mesh 3 by a spraying method; the structure formed in the above steps is encapsulated with a packaging plate 7, and an isolation plate 6 is adhered to the top of the packaging plate 7; the structure formed in the above steps is wrapped with a heat insulation layer 5, and a transparent outer protective film 1 is fixed on the outer surface of the heat insulation layer 5.
[0049] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.
Claims
1. A graphene-encapsulated metal nanowire composite transparent electrode, comprising an outer protective film (1), characterized in that: The inner wall of the outer protective film (1) is fixedly connected to a heat insulating layer (5); the inner cavity of the heat insulating layer (5) is provided with an isolation plate (6), a packaging plate (7), a conductive medium (4), a conductive mesh (3) and a base (2) from top to bottom; the top of the base (2) is inlaid with a conductive mesh (3); the outer surface of the conductive mesh (3) is coated with an anti-diffuse reflection coating; the top of the conductive mesh (3) is covered with a conductive medium (4); the top of the conductive medium (4) is fixedly connected to a packaging plate (7); and the top of the packaging plate (7) is fixedly connected to the isolation plate (6).
2. The graphene-encapsulated metal nanowire composite transparent electrode according to claim 1, characterized in that: The top of the base (2) is provided with a mesh groove (9) adapted to the conductive mesh (3), and the bottom of the base (2) is evenly and fixedly connected with conductive pillars (8).
3. The graphene-encapsulated metal nanowire composite transparent electrode according to claim 1, characterized in that: The conductive mesh (3) comprises metal nanowires, and the outer surfaces of the metal nanowires are coated with an anti-diffuse reflection coating.
4. The graphene-encapsulated metal nanowire composite transparent electrode according to claim 1, characterized in that: The packaging plate (7) is made of graphene, and the outer protective film (1) is made of a transparent conductive material.
5. The graphene-encapsulated metal nanowire composite transparent electrode according to claim 2, characterized in that: The thermal insulation layer (5) is in mesh shape, and a conductive medium (4) is filled between the thermal insulation layer (5) and the outer protective film (1); the conductive column (8) is adapted to the mesh of the thermal insulation layer (5), and the bottom of the conductive column (8) is in contact with the outer protective film (1) through the mesh of the thermal insulation layer (5).
6. A method for preparing a graphene-encapsulated metal nanowire composite transparent electrode according to any one of claims 1 to 5, characterized in that: The following steps are involved: Step 1: prepare a transparent substrate (2), wherein the top of the transparent substrate (2) is horizontal and the bottom of the transparent substrate (2) has a protruding conductive column (8); Step 2: etching a mesh groove (9) on the top of the transparent substrate (2); Step 3: spraying a hydrophilic coating on the top of the transparent substrate (2); Step 4: prepare metal nanowires, apply an anti-diffuse reflection coating on the outer surface of the metal nanowires, apply a hydrophilic coating on the outer surface of the anti-diffuse reflection coating, fill the metal nanowires into the mesh grooves (9), and the metal nanowires form a conductive mesh (3); Step 5, spraying the conductive medium (4) onto the structure formed in step 4; Step 6: Encapsulate the structure formed in step 5 with an encapsulation plate (7), and fix the isolation plate (6) on the top of the encapsulation plate (7); Step 7: Wrap the structure formed in step 6 with a heat-insulating layer (5), and spray the conductive medium (4) on the outer surface of the heat-insulating layer (5). Step 8: Fix a transparent outer protective film (1) on the outer surface of the heat insulation layer (5).
7. The method for preparing a graphene-encapsulated metal nanowire composite transparent electrode according to claim 6, characterized in that: In step seven, the conductive column (8) contacts the outer protective film (1) through the mesh of the thermal insulation layer (5).