Magnetic field focusing orientation neodymium iron boron permanent magnet and preparation method thereof

By partitioning and arranging mixed alloy powders of different components in the NdFeB permanent magnet, the leakage flux and manufacturing process complexity problems in the magnetization direction design are solved, and efficient magnetic field focusing orientation design is achieved, and the finished product pass rate and magnetic flux are improved. , simplifies the process flow.

CN119008158AActive Publication Date: 2024-11-22JING CI MATERIAL SCI CO LTD

Patent Information

Application Number
CN202411227353.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-03
Publication Date
2024-11-22
Estimated Expiration
2044-09-03

AI Technical Summary

Technical Problem

In the magnetization direction design of sintered NdFeB permanent magnets, there are problems such as increased leakage flux and complex magnet manufacturing process, and the difference in expansion characteristics caused by orientation magnetization under non-uniform magnetic fields leads to low yield.

Method used

By partitioning mixed alloy powders of different components in the permanent magnet, adjusting the content gradient and carbon content of RE and Co, controlling the difference in thermal expansion coefficients, and using magnetic field orientation molding and sintering heat treatment processes to achieve the overall forming magnetic field focusing orientation permanent magnet.

Benefits of technology

It improves the magnetic reconstruction effect of magnets, reduces internal stress, improves the qualification rate of finished products, simplifies the manufacturing process, reduces the low material utilization and process complexity, and enhances the magnetic flux and reliability of magnets.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119008158A_ABST
    Figure CN119008158A_ABST
Patent Text Reader

Abstract

The invention discloses a magnetic field focusing orientation neodymium iron boron permanent magnet and a preparation method thereof. The permanent magnet comprises a central region and at least one group of side regions, and each group of side regions comprises two side regions which are symmetrically distributed on two sides of the central region; the RE content in the permanent magnet is reduced one by one from the central region to the edge region, and the Co content is gradually increased; the carbon content of the permanent magnet is gradually increased from the central area to the edge area; the thermal expansion coefficient in the permanent magnet vertical to the orientation direction is increased one by one from the central region to the edge region; the difference between the coefficients of thermal expansion of the permanent magnets perpendicular to the orientation direction and parallel to the orientation direction decreases region by region from the central region to the edge region. The magnetic gathering effect of the permanent magnet can be improved, the internal stress of the permanent magnet is reduced, and the qualified rate of finished products is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of rare earth permanent magnet material manufacturing, in particular to a magnetic field focusing oriented NdFeB permanent magnet and a preparation method thereof. Background Art

[0002] Sintered NdFeB permanent magnet materials are widely used in new energy vehicles, consumer electronics, wind power generation and other important fields due to their excellent comprehensive magnetic properties. Permanent magnet motors or generators are devices that realize the conversion of electrical energy and mechanical energy, and are one of the areas where sintered NdFeB is used the most. The permanent magnets in the motor are usually installed on the rotor. There is a certain air gap between the rotor and the stator. The magnetic flux generated by the permanent magnet is divided into two parts. One part is cross-linked with the armature winding through the air gap, which is called the main magnetic flux, and the other part is not cross-linked with the armature winding, which is called the leakage magnetic flux. When designing permanent magnets, the main magnetic flux should be increased and the leakage magnetic flux should be reduced to maximize the performance of the permanent magnet material. The magnetization directions of permanent magnets are usually parallel, such as Figure 1 As shown in the figure, after the permanent magnet is magnetized, its magnetic field lines are distributed as follows Figure 2 As shown, from Figure 2 It can be seen that at a certain air gap from the permanent magnet, the magnetic lines of force diverge. This structure inevitably leads to an increase in leakage flux. The solution of the prior art is to add two magnets on both sides of the permanent magnet to form a Haier shell structure. Figure 3 shown. Figure 4 This is the distribution of magnetic lines of force of the Halbach structure permanent magnet assembly. It can be seen that for this structure magnet, the magnetic lines of force form a magnetic concentration effect in the upper space of the permanent magnet, and the density of magnetic lines of force in the upper part of the permanent magnet is significantly greater than that in the lower part. However, the new problem brought by this structure is that the magnet manufacturing process is relatively complicated, especially the magnets on both sides and the magnets in the middle have a large repulsive force, which often requires special fixtures and high-strength adhesives to achieve.

[0003] Another method is to carry out focused orientation magnetization when the permanent magnet is pressed into the green body, so that the magnetic powder is focused and rotated toward a certain point, and then sintering heat treatment is carried out to obtain a densified magnet. This method can make a single permanent magnet have the effect of a Haier shell array made of multiple pieces. Chinese patent CN 116761689A discloses a device and method for a single permanent magnet with focused and parallel magnetic flux areas. This method modifies the magnetic circuit structure in the mold so that the mold cavity has a magnetic circuit structure with parallel lower part and focused upper part. For example, Chinese patent CN 218041167 U provides a focused magnetization scheme, which is mainly to arrange mutually repelling magnetic fields on both sides of the mold so that the magnetic powder in the mold cavity presents the characteristics of focused distribution. Although the above scheme provides a method for the magnetic field distribution in the mold, for sintered NdFeB magnetic powder, when the oriented magnetic field is non-uniform, the magnetic powder particles are of different sizes, so the flipping effect in the mold cavity has significant differences. In addition, sintered NdFeB magnets have anisotropic expansion characteristics, that is, positive expansion parallel to the orientation direction and negative expansion perpendicular to the orientation direction. This non-parallel orientation will lead to greater internal stress inside the magnet, and when the magnet blank is cooled during the sintering process, it will inevitably shrink unevenly and even cause the magnet to crack. Summary of the invention

[0004] An object of the present invention is to solve at least the above problems and / or disadvantages and to provide at least the advantages which will be described hereinafter.

[0005] An object of the present invention is to provide a permanent magnet with magnetic field focusing orientation and a preparation method thereof, which can improve the magnetic field focusing effect of the permanent magnet, reduce the internal stress of the permanent magnet, and improve the qualified rate of finished products.

[0006] In order to achieve these purposes and other advantages according to the present invention, the permanent magnet includes a central region and at least one group of side regions, wherein the permanent magnet has a symmetry plane in the central region, each group of side regions includes two side regions symmetrically distributed on both sides of the central region, and the outermost group of side regions in the at least one group of side regions is a group of edge regions;

[0007] The composition and magnet properties of each set of side regions remain consistent;

[0008] The composition of the permanent magnet in the central area or the side area is calculated by mass percentage: RE L a RE H b Co c Cu d M e Fe bal B f, 24≤a≤31, 0≤b≤4, 0≤c≤30, 0.1≤d≤0.8, 0.2≤e≤3, 0.86≤f≤1.2, 28≤a+b≤35, bal is the margin; RE L is one or a combination of light rare earth elements Pr, Nd, La, Ce and Y, RE H is one or a combination of heavy rare earths Gd, Ho, Dy and Tb, and M is one or a combination of Al, Cr, Nb, Zr, Ga, Ti, V, Mo and Mn;

[0009] The RE content in the permanent magnet decreases from the central region to the edge region, and the Co content gradually increases. The composition distribution of the central region is rich in RE and poor in Co, and the composition distribution of the edge region is poor in RE and rich in Co. The difference in RE content between the central region and the edge region is ≤1%, and the difference in Co content between the edge region and the central region is ≤30%. The RE content is RE L and RE H sum;

[0010] The carbon content of the permanent magnet increases from the central region to the edge region, and the difference in carbon content between the central region and the edge region is ≥400 ppm;

[0011] The thermal expansion coefficient perpendicular to the orientation direction in the permanent magnet increases from the central region to the edge region; the thermal expansion coefficient parallel to the orientation direction of the permanent magnet has no obvious difference between the central region and the at least one group of side regions; the difference between the thermal expansion coefficient perpendicular to the orientation direction and the thermal expansion coefficient parallel to the orientation direction of the permanent magnet decreases from the central region to the edge region;

[0012] The permanent magnet has a focusing plane perpendicular to the symmetry plane, and on the focusing plane, the magnetic field strength of the permanent magnet increases from the edge region to the central region.

[0013] Preferably, in the permanent magnet with magnetic field focusing orientation, the permanent magnet includes two or four side regions symmetrically distributed on both sides of the central region.

[0014] The present invention also provides a method for preparing a permanent magnet with magnetic field focusing orientation, comprising:

[0015] Step (1) preparing an alloy powder I rich in RE and poor in Co, wherein the composition of the alloy powder I is as follows by mass percentage: L a1 RE H b1 Co c1 Cud1 Fe bal M e1 B f1 , where 30≤a1≤33, 0≤b1≤4, 0≤c1≤3, 0≤d1≤0.3, 0.2≤e1≤3, 0.86≤f1≤1.2;

[0016] Step (2) preparing an alloy powder II which is low in RE and rich in Co. The composition of the alloy powder II is as follows by mass percentage: L a2 RE H b2 Co c2 Cu d2 Fe bal M e2 B f2 , where 26≤a2≤31, 0≤b2≤4, 3<c2≤40, 0≤d2≤2, 0.2≤e2≤3, 0.86≤f2≤1.2;

[0017] Step (3) powder proportioning: the alloy powder I and the alloy powder II are mixed in at least two proportions to prepare at least two mixed alloy powders, wherein at least one of the at least two mixed alloy powders has a composition of rich RE and poor Co, and at least one of the mixed alloy powders has a composition of poor RE and rich Co, the RE content of the at least two mixed alloy powders decreases in sequence, and the Co content increases in sequence, the difference in RE content between the mixed alloy powder with the highest RE content and the mixed alloy powder with the lowest RE content in the at least two mixed alloy powders is ≤1%, and the difference in Co content between the mixed alloy powder with the highest Co content and the mixed alloy powder with the lowest Co content in the at least two mixed alloy powders is ≤30%, wherein the RE content is RE L and RE H sum;

[0018] Step (4) adding lubricant and mixed powder: adding lubricant to the at least two mixed alloy powders respectively, so that the carbon content of the at least two mixed alloy powders increases successively, the difference in carbon content between the mixed alloy powder with the highest carbon content and the mixed alloy powder with the lowest carbon content in the at least two mixed alloy powders is ≥400ppm, and the carbon content in each mixed alloy powder is 500-2000ppm;

[0019] Step (5) magnetic field orientation molding: divide the internal space of the mold into a central space and at least one group of side spaces, each group of side spaces includes two side spaces symmetrically distributed on both sides of the central space, and the outermost group of side spaces in the at least one group of side spaces is a group of edge spaces; put the at least two mixed alloy powders into the central space and the at least one group of side spaces respectively, put mixed alloy powders of the same composition into each group of side spaces, and make the RE content of the mixed alloy powders placed in the central space to the edge space one by one decrease successively, and the Co content increase successively, the composition distribution of the mixed alloy powder placed in the central space is rich in RE and poor in Co, the composition distribution of the mixed alloy powder placed in the edge space is poor in RE and rich in Co, the difference in RE content between the mixed alloy powders placed in the central space and the edge space is ≤1%, and the difference in Co content between the mixed alloy powders placed in the edge space and the central space is ≤30%, wherein the RE content is RE L and RE H The RE content of the mixed alloy powder placed in the middle space to the edge space increases successively, and the difference in carbon content between the mixed alloy powder placed in the middle space and the edge space is ≥400ppm; then, the mold is placed in a magnetic field for orientation and shaping;

[0020] Step (6) sintering and tempering heat treatment;

[0021] Step (7) machining;

[0022] Step (8) magnetization.

[0023] Preferably, in the method for preparing the magnetic field focusing oriented permanent magnet, the average particle size of the alloy powder I is 1 to 5 μm; the average particle size of the alloy powder II is 2 to 6 μm.

[0024] Preferably, in the method for preparing the permanent magnet with magnetic field focusing orientation, in the step (4), the lubricant is added in a ratio of 0.1% to 1%.

[0025] Preferably, in the method for preparing a permanent magnet with magnetic field focusing orientation, in the step (5), the density of the mixed alloy powder placed in the middle space and the at least one set of side spaces in the internal space of the mold is 1.6-2 g / cm 3 The mold is placed in a magnetic field for orientation shaping, which is specifically achieved by the following process: orientation shaping is carried out in a non-uniform magnetic field of 1.2-2.2T, and then placed in an isostatic press for secondary pressing, the isostatic pressure is 150-300MPa, and the green density obtained is 3.9-4.5g / cm 3 .

[0026] Preferably, in the preparation method of the magnetic field focusing oriented permanent magnet, in the step (6), the sintering and tempering heat treatment are specifically achieved by the following process: placing the green body in a vacuum sintering furnace set at a temperature of 1000-1100°C for sintering and densification, and the insulation time is 2-10 hours; after the insulation is completed, stopping heating, slowly cooling to 800-900°C, filling with argon and turning on the fan to quickly cool to room temperature to obtain a sintered magnet; subjecting the sintered magnet to secondary tempering treatment, the treatment conditions are insulation at 800-950°C for 2-6 hours and then rapidly cooling to room temperature, and then insulation at 400-650°C for 2-10 hours and then rapidly cooling to room temperature; the atmosphere of the tempering heat treatment is a vacuum or argon protection state.

[0027] Preferably, in the method for preparing the permanent magnet with magnetic field focusing orientation, the magnetization is specifically achieved by the following process: the magnet machined in step (7) is placed in a magnetization coil for magnetization, the magnetization method is to magnetize in parallel with the symmetry plane of the magnet machined in step (7), and the magnetization magnetic field is 3 to 10T.

[0028] The present invention has at least the following beneficial effects:

[0029] (1) The present invention solves the problems of poor magnet focusing effect and low yield rate caused by uneven magnet shrinkage in the prior art by regulating the composition of the magnet. In addition, the present invention adjusts the composition ratio of the alloy powder mixed at different positions of the mold and the ratio of the powder lubricant to make the magnetic powder rotate more uniformly under the non-uniform orientation field, and solves the problem of excessive difference in magnet expansion characteristics at the edge. Therefore, the magnet yield rate of the present invention is higher.

[0030] (2) The present invention solves the problems of complex process and low material utilization caused by focusing through the Haier shell array. The permanent magnet of the present invention is integrally formed, does not require complicated processing and bonding steps, is easy to implement, has high material utilization, and is more reliable.

[0031] (3) On the one hand, the present invention can obtain a higher degree of orientation under the same magnetic field conditions by zoning and controlling the composition of the mixed alloy powder, thereby increasing the remanence Br in each area and finally obtaining a high magnetic flux; on the other hand, under the same degree of orientation, the powder particles have better adaptability to the oriented magnetic field, the internal stress of the magnet is smaller, the stray magnetic field caused by grain crushing is smaller, and the whole permanent magnet can maintain a higher magnetic flux. The focused oriented permanent magnet of the present invention reduces the leakage flux and increases the main magnetic flux, so it can reduce the amount of permanent magnets in the motor or increase the motor torque.

[0032] Other advantages, objectives and features of the present invention will be embodied in part through the following description, and in part will be understood by those skilled in the art through study and practice of the present invention. BRIEF DESCRIPTION OF THE DRAWINGS

[0033] Figure 1 Schematic diagram of the magnetization direction of a conventional permanent magnet.

[0034] Figure 2 This is the magnetic field line distribution diagram of a conventional parallel magnetized permanent magnet.

[0035] Figure 3 Schematic diagram of a permanent magnet assembly with a Halbach structure.

[0036] Figure 4 This is the magnetic field line distribution diagram of the Halbach permanent magnet assembly.

[0037] Figure 5 The present invention provides a flow chart of a method for preparing a permanent magnet with magnetic field focusing orientation.

[0038] Figure 6 Schematic diagram of the distribution of mixed alloy powder in the mold in Example 1 of the present invention.

[0039] Figure 7 This is a cloud diagram of the magnetic field distribution on the focusing surface of the permanent magnet prepared in Example 1 of the present invention.

[0040] Figure 8 Schematic diagram of the distribution of mixed alloy powder in the mold in Example 2 of the present invention.

[0041] Fig. 9 This is a cloud diagram of the magnetic field distribution on the focusing surface of the permanent magnet prepared in Example 2 of the present invention. DETAILED DESCRIPTION

[0042] The present invention is further described in detail below in conjunction with the accompanying drawings so that those skilled in the art can implement the invention with reference to the description.

[0043] The present invention provides a permanent magnet with a magnetic field focusing orientation, the permanent magnet comprising a central region and at least one group of side regions, the permanent magnet having a symmetric plane in the central region, each group of side regions comprising two side regions symmetrically distributed on both sides of the central region, the outermost group of side regions in the at least one group of side regions being a group of edge regions; the composition of each group of side regions and the magnet performance are consistent; the composition of the permanent magnet in the central region or the side region is calculated as follows by mass percentage: RE L a RE H b Co c Cu d Me Fe bal B f , 24≤a≤31, 0≤b≤4, 0≤c≤30, 0.1≤d≤0.8, 0.2≤e≤3, 0.86≤f≤1.2, 28≤a+b≤35, bal is the margin; RE L is one or a combination of light rare earth elements Pr, Nd, La, Ce and Y, RE H is one or more of the heavy rare earth Gd, Ho, Dy and Tb, M is one or more of the heavy rare earth Al, Cr, Nb, Zr, Ga, Ti, V, Mo and Mn, wherein the RE content in the permanent magnet decreases from the central region to the edge region, and the Co content gradually increases, the composition distribution of the central region is rich in RE and poor in Co, the composition distribution of the edge region is poor in RE and rich in Co, the difference in RE content between the central region and the edge region is ≤1%, and the difference in Co content between the edge region and the central region is ≤30%, wherein the RE content is RE L and RE H The sum of the carbon content of the permanent magnet increases from the central area to the edge area, and the difference in carbon content between the central area and the edge area is ≥400ppm; the thermal expansion coefficient perpendicular to the orientation direction in the permanent magnet increases from the central area to the edge area; there is no obvious difference in the thermal expansion coefficient parallel to the orientation direction of the permanent magnet between the central area and the at least one group of side areas; the difference between the thermal expansion coefficient perpendicular to the orientation direction and the thermal expansion coefficient parallel to the orientation direction of the permanent magnet decreases from the central area to the edge area; the permanent magnet has a focusing plane perpendicular to the symmetry plane, and the magnetic field strength of the permanent magnet on the focusing plane increases from the edge area to the central area.

[0044] Due to its own physical properties, NdFeB materials have different expansion characteristics parallel to the orientation direction (C∥) and perpendicular to the orientation direction (C⊥). In the C∥ direction, the magnet has a positive thermal expansion coefficient, while in the C⊥ direction, due to the magnetostrictive effect, it has a negative thermal expansion coefficient. In the traditional method, when magnetic powder is oriented and formed under a non-uniform magnetic field with focusing characteristics, different positions in the mold have different magnetic field sizes, so the rotation angles of the magnetic powder at the corresponding positions will also be different. This situation will lead to different internal expansion characteristics of the magnet during sintering and tempering, which will lead to a large stress concentration problem inside the magnet. Therefore, the focused oriented blank is prone to cracking and the yield rate is very low. The present invention controls the composition ratio of different regions of the permanent magnet, so that the magnetic powder can rotate more consistently under the non-uniform orientation field (that is, the mixed alloy powder filled in each space in the mold cavity can rotate consistently in the non-uniform orientation field), thereby solving the problem of poor magnet focusing effect caused by non-uniform magnetization in the prior art, and solving the problem of excessive difference in expansion characteristics of the permanent magnet at the edge, thereby reducing the internal stress of the permanent magnet and achieving a higher yield rate.

[0045] Specifically, the thermal expansion coefficient perpendicular to the orientation direction in the permanent magnet increases from the central area to the edge area, and the thermal expansion coefficient perpendicular to the orientation direction in the central area is -4 to 3×10 -6 K -1 The thermal expansion coefficient of the edge region perpendicular to the orientation direction is -1.5 to 5×10 -6 K -1 The thermal expansion coefficient of the permanent magnet parallel to the orientation direction has no significant difference between the central region and at least one set of side regions, and is 6 to 9.9×10 -6 K -1 The difference between the thermal expansion coefficient of the permanent magnet perpendicular to the orientation direction and the thermal expansion coefficient parallel to the orientation direction decreases from the central area to the edge area. As a result, the internal stress of the permanent magnet is lower and the qualified rate of the finished product is higher.

[0046] In a preferred embodiment, in the permanent magnet with magnetic field focusing orientation, the permanent magnet includes two or four side regions symmetrically distributed on both sides of the central region.

[0047] like Figure 5 As shown, the present invention also provides a method for preparing a permanent magnet with magnetic field focusing orientation, comprising:

[0048] Step (1) preparing an alloy powder I rich in RE and poor in Co, wherein the composition of the alloy powder I is as follows by mass percentage: L a1 RE H b1 Co c1 Cu d1 Febal M e1 B f1 , where 30≤a1≤33, 0≤b1≤4, 0≤c1≤3, 0≤d1≤0.3, 0.2≤e1≤3, 0.86≤f1≤1.2;

[0049] Step (2) preparing an alloy powder II which is low in RE and rich in Co. The composition of the alloy powder II is as follows by mass percentage: L a2 RE H b2 Co c2 Cu d2 Fe bal M e2 B f2 , where 26≤a2≤31, 0≤b2≤4, 3<c2≤40, 0≤d2≤2, 0.2≤e2≤3, 0.86≤f2≤1.2;

[0050] Step (3) powder proportioning: the alloy powder I and the alloy powder II are mixed in at least two proportions to prepare at least two mixed alloy powders, wherein at least one of the at least two mixed alloy powders has a composition of rich RE and poor Co, and at least one of the mixed alloy powders has a composition of poor RE and rich Co, the RE content of the at least two mixed alloy powders decreases in sequence, and the Co content increases in sequence, the difference in RE content between the mixed alloy powder with the highest RE content and the mixed alloy powder with the lowest RE content in the at least two mixed alloy powders is ≤1%, and the difference in Co content between the mixed alloy powder with the highest Co content and the mixed alloy powder with the lowest Co content in the at least two mixed alloy powders is ≤30%, wherein the RE content is RE L and RE H sum;

[0051] Step (4) adding lubricant and mixed powder: adding lubricant to the at least two mixed alloy powders respectively, so that the carbon content of the at least two mixed alloy powders increases successively, the difference in carbon content between the mixed alloy powder with the highest carbon content and the mixed alloy powder with the lowest carbon content in the at least two mixed alloy powders is ≥400ppm, and the carbon content in each mixed alloy powder is 500-2000ppm;

[0052] Step (5) magnetic field orientation molding: divide the internal space of the mold into a central space and at least one group of side spaces, each group of side spaces includes two side spaces symmetrically distributed on both sides of the central space, and the outermost group of side spaces in the at least one group of side spaces is a group of edge spaces; put the at least two mixed alloy powders into the central space and the at least one group of side spaces respectively, put mixed alloy powders of the same composition into each group of side spaces, and make the RE content of the mixed alloy powders placed in the central space to the edge space one by one decrease successively, and the Co content increase successively, the composition distribution of the mixed alloy powder placed in the central space is rich in RE and poor in Co, the composition distribution of the mixed alloy powder placed in the edge space is poor in RE and rich in Co, the difference in RE content between the mixed alloy powders placed in the central space and the edge space is ≤1%, and the difference in Co content between the mixed alloy powders placed in the edge space and the central space is ≤30%, wherein the RE content is RE L and RE H The RE content of the mixed alloy powder placed in the middle space to the edge space increases successively, and the difference in carbon content between the mixed alloy powder placed in the middle space and the edge space is ≥400ppm; then, the mold is placed in a magnetic field for orientation and shaping;

[0053] Step (6) sintering and tempering heat treatment;

[0054] Step (7) machining;

[0055] Step (8) magnetization.

[0056] When NdFeB permanent magnets are used, in order to achieve the magnetic focusing effect, Halbach arrays are usually used to achieve this, but this method requires bonding and assembly, the manufacturing process is complicated, and it is difficult to mass produce. Another method is to perform focused oriented magnetization when the permanent magnet is prepared. However, when focusing magnetization is performed during green compact pressing, since the oriented magnetic field belongs to a non-uniform field, it is difficult for the magnetic powder particles to rotate in unison, resulting in inconsistent sintering shrinkage after sintering of the permanent magnet, causing problems such as internal cracks in the blank, and resulting in a very low material qualification rate. On the other hand, due to the deviation in the rotation angle of the magnetic powder, the magnetic focusing effect is poor, and it is difficult to give play to the advantages of concentrated magnetization. Based on this, the present invention provides a method for preparing a permanent magnet with magnetic field focused orientation. The method provided by the present invention divides the internal space (mold cavity) of the mold into multiple spaces, controls the composition of the magnetic powder filled in each space, and enables the magnetic powder to rotate more consistently with the oriented magnetic field in the mold cavity, thereby improving the magnetic focusing effect of the permanent magnet and reducing the internal stress of the permanent magnet.

[0057] The traditional method achieves the effect of focused magnetization by splicing multiple magnets, but each unit of the permanent magnet needs to be processed separately, and complex tooling and fixtures are required for bonding. In addition, when the permanent magnet is used at high temperature or in a scene with large centrifugal force, the adhesive layer is prone to failure, causing the motor to be scrapped. The permanent magnet manufacturing process provided by the present invention is simple, the permanent magnet is integrally formed, does not require complex processing and bonding steps, is easy to implement, has high material utilization, and has higher reliability.

[0058] In addition, the present invention achieves a higher orientation degree of magnetic powder under the same magnetic field conditions by arranging the powder partitions and controlling the composition, thereby increasing the remanence Br in each region of the permanent magnet, and finally obtaining a high magnetic flux. The permanent magnet prepared by the present invention reduces the leakage flux and increases the main magnetic flux, which helps to reduce the amount of permanent magnets or can increase the motor torque.

[0059] The carbon content of the magnet is low in the center and high in the edge, because more lubricant is added to the powder in the edge, while less lubricant is added in the middle. The magnetic field in the mold is low in the edge and high in the center, so by improving the lubricity of the powder in the edge, it is possible to ensure that the edge maintains a high degree of orientation, thereby obtaining a higher remanent magnetism Br.

[0060] In step (5), when at least two kinds of mixed alloy powders are placed in the internal space of the mold, a plurality of partition plates can be used to divide the internal space of the mold into a middle space and at least one set of side spaces, and then the corresponding mixed alloy powders are placed in each space according to the design, and then each partition plate is withdrawn, so that there is no physical separation between the mixed alloy powders in adjacent spaces. In this way, during subsequent processing, the mixed alloy powders in the mold are processed into a permanent magnet as a whole.

[0061] In a preferred embodiment, in the method for preparing a permanent magnet with magnetic field focusing orientation, the average particle size of the alloy powder I is 1 to 5 μm; the average particle size of the alloy powder II is 2 to 6 μm.

[0062] The present invention selects the particle size of the alloy powder so that the powder particles have better adaptability to the oriented magnetic field under the same orientation degree, thereby reducing the internal stress of the permanent magnet, reducing the stray magnetic field caused by grain crushing, and allowing the entire permanent magnet to maintain a higher magnetic flux.

[0063] In a preferred embodiment, in the method for preparing the permanent magnet with magnetic field focusing orientation, in the step (4), the addition ratio of the lubricant is 0.1% to 1%.

[0064] Specifically, the addition ratio of the lubricant can be adjusted according to the composition of the mixed alloy powder. The present invention can adjust the lubricant ratio of the mixed alloy powder in different spaces in the internal space of the mold, so that the powder rotates more uniformly under the non-uniform orientation field, thereby further enhancing the focusing effect, improving the magnet yield rate, and better solving the problem of poor magnet focusing effect caused by non-uniform magnetization and low yield rate caused by uneven magnet shrinkage.

[0065] In a preferred embodiment, in the method for preparing a permanent magnet with magnetic field focusing orientation, in step (5), the density of the mixed alloy powder placed in the middle space and the at least one set of side spaces in the internal space of the mold is 1.6-2 g / cm 3 The mold is placed in a magnetic field for orientation shaping, which is specifically achieved by the following process: orientation shaping is carried out in a non-uniform magnetic field of 1.2-2.2T, and then placed in an isostatic press for secondary pressing, the isostatic pressure is 150-300MPa, and the green density obtained is 3.9-4.5g / cm 3 .

[0066] In a preferred embodiment, in the method for preparing the magnetic field focusing oriented permanent magnet, in the step (6), the sintering and tempering heat treatment are specifically achieved by the following process: placing the green body in a vacuum sintering furnace set at a temperature of 1000-1100°C for sintering and densification, and the insulation time is 2-10 hours; after the insulation is completed, heating is stopped, and after slowly cooling to 800-900°C, argon is filled and a fan is turned on to quickly cool to room temperature to obtain a sintered magnet; the sintered magnet is subjected to secondary tempering treatment, and the treatment conditions are insulation at 800-950°C for 2-6 hours and then rapidly cooled to room temperature, and then insulation at 400-650°C for 2-10 hours and then rapidly cooled to room temperature; the atmosphere of the tempering heat treatment is a vacuum or argon protection state.

[0067] In a preferred embodiment, in the method for preparing the permanent magnet with magnetic field focusing orientation, the magnetization is specifically achieved by the following process: the magnet machined in step (7) is placed in a magnetization coil for magnetization, the magnetization method is to magnetize parallel to the symmetry plane of the magnet machined in step (7), and the magnetization magnetic field is 3 to 10T.

[0068] In a preferred embodiment, the machining process in step (7) is as follows: the permanent magnet blank obtained in step (6) is machined into a desired shape. In order to ensure symmetry during machining, the blank is first marked and then ground. The processed black sheet magnet is surface treated, and the surface treatment method includes phosphating, passivation, Zn, Ni plating or epoxy.

[0069] Specific examples are provided below to further illustrate the magnetic field focusing and oriented permanent magnet and the preparation method thereof provided by the present invention.

[0070] Example 1

[0071] S1: Prepare RE-rich and Co-poor alloy powder I, the composition of the alloy powder by mass percentage is: (PrNd) 30 Dy 0.5 Co 1.5 Cu 0.2 Fe bal Al 0.3 Zr 0.15 B 0.90 According to the process of batching - rapid solidification belt spinning - hydrogen crushing - air flow milling, alloy fine powder with an average particle size of 3.5 μm was obtained.

[0072] S2: Prepare RE-poor Co-rich alloy powder II, the composition of the alloy powder is as follows by mass percentage: PrNd 29 Dy 0.5 Co5Cu 0.8 Fe bal Al 0.3 Zr 0.15 B 0.90 According to the process of batching - rapid solidification belt spinning or ingot casting - hydrogen crushing - air flow milling or high energy ball milling, alloy fine powder with an average particle size of 4.5 μm is obtained.

[0073] S3: Powder proportioning: alloy powders I and II are mixed in a ratio of 4:6 and 1:9 respectively to obtain mixed powders in two ratios.

[0074] S4: Add 0.1% lubricant to the powder with a mixing ratio of 4:6, and add 0.2% lubricant to the powder with a mixing ratio of 1:9, and then mix the powder in a V-type mixer for 4 hours. In order to reduce the activity of the powder, it needs to be left to stand for 2 hours to 2.5 hours after mixing.

[0075] S5: Magnetic field orientation molding: The above two powders are injected into the mold. The mold is divided into three areas. The middle area is injected with powders in a ratio of 4:6, and the two side areas are injected with powders in a ratio of 1:9. The distribution of the mixed alloy powder in the mold is shown in Figure 6 . The powder bulk density is 1.8g / cm 3 The magnetic powder was then oriented and formed in a non-uniform magnetic field of 1.9 T, and then placed in an isostatic press for secondary pressing. The green density obtained at an isostatic pressure of 200 MPa was 4.30 g / cm 3 .

[0076] S6: Sintering and tempering heat treatment: Place the green body in a vacuum sintering furnace set at 1080°C for sintering and densification, and keep it warm for 6 hours; after the end of the heat preservation, stop heating, slowly cool to 850°C, fill with argon and turn on the fan to quickly cool to room temperature to obtain a sintered magnet; perform secondary tempering treatment on the sintered magnet, the treatment process is to keep it warm at 920°C for 6 hours and then quickly cool it to room temperature, and then keep it warm at 450°C for 4 hours and then quickly cool it to room temperature; the atmosphere of the tempering heat treatment is a vacuum state.

[0077] S7: Machining: The permanent magnet blank obtained in step S6 is processed according to the required shape and size. Its specific size is 90*40*30↑, where 30 is the magnetization direction. The permanent magnet surface treatment method is Zn plating.

[0078] S8: Magnetization and inspection: Place the processed permanent magnet into the magnetization coil for magnetization. The magnetization method is parallel magnetization and the magnetization magnetic field is 3 T. After magnetization, a permanent magnet with focusing orientation can be obtained.

[0079] Comparative Example 1

[0080] The single-component magnet powder is prepared according to the conventional process. The composition of the magnet powder is (PrNd) 29.5 Dy 0.5 Co 1.5 Cu 0.2 Fe bal Al 0.3 Zr 0.15 B 0.90 According to the process of batching, rapid solidification, belt spinning, hydrogen crushing and air flow milling, an alloy fine powder with an average particle size of 3.5 μm was obtained; then 0.15% additives were added to the powder, the powder was mixed for 4 hours, and then the powder was allowed to stand for 2 hours. Then the powder was injected into the mold cavity shown in the figure above. The magnetic powder was oriented and formed in a non-uniform magnetic field of 1.2 T, and then placed in an isostatic press for secondary pressing. The green density obtained at an isostatic pressure of 200 MPa was 4.30 g / cm 3 ; The permanent magnet is obtained by using steps S6 to S8 which are exactly the same as those in Example 1.

[0081] Sample processing and testing: Use a surface magnetic tester to measure the surface magnetic values ​​of different positions of the magnetic steel, recorded as Bs. Use a NIM permanent magnetic property tester to test the magnetic properties of the central area and edge area of ​​the permanent magnet. The sample size is D10*10mm. Prepare a D6*20mm cylinder, test the thermal expansion coefficient of the central area and edge area of ​​the permanent magnet, and calculate the difference in thermal expansion coefficient perpendicular to the orientation direction and parallel to the orientation direction, recorded as Δα. Calculate the difference in carbon content between the edge area and the center area of ​​the permanent magnet. For the permanent magnet prepared in Comparative Example 1, it can be divided into 3 equal parts, corresponding to the central area and a group of edge areas on both sides of the central area. The overall qualified rate of permanent magnets prepared by the two methods is calculated, and the qualified rate = number of good products / total number * 100%. The qualified rate includes the blank, processing and electroplating links.

[0082] Table 1 Surface magnetic intensity of permanent magnets at different measurement positions of Example 1 and Comparative Example 1

[0083]

[0084] Table 2 Magnetic performance parameters and qualified rates of permanent magnets in various regions of Example 1 and Comparative Example 1

[0085]

[0086] Table 3 Thermal expansion coefficients and differences of various regions of the permanent magnets of Example 1 and Comparative Example 1

[0087]

[0088] Table 4 Composition distribution of each region of the permanent magnet of Example 1 and Comparative Example 1

[0089]

[0090]

[0091] It can be seen from Example 1 and Comparative Example 1 that the focused magnetized permanent magnet prepared by the present invention has a significant focusing effect on the focusing surface after the magnet is magnetized. As shown in Table 1, within a certain distance range of the focusing surface, the magnetic field Bs of Example 1 is increased by more than 10% compared with Comparative Example 1 at the same position. It can be seen from Table 2 that the edge of the magnet of Example 1 of the present invention has a higher Br, indicating that the magnet has a higher degree of orientation. It can be seen from the comparison of thermal expansion data that the expansion difference of the magnet of Example 1 is smaller, indicating that the internal stress of the magnet is smaller. The qualified rate data show that the qualified rate of the permanent magnet prepared by the method of the present invention reaches 96%, while the qualified rate of Comparative Example 1 using conventional technology only reaches 82%. It can be seen from Table 3 that the thermal expansion coefficients at different positions of the comparative example are the same, and the difference is 11.5, while the thermal expansion coefficients of different regions of Example 1 of the present invention are not the same by adjusting the component distribution, the difference in the central area is 10.5, and the edge area is 9.2. The smaller the thermal expansion difference at the edge, the smaller the internal stress of the magnet. It can be seen from Table 4 that the rare earth RE content, carbon content and cobalt content of Comparative Example 1 are uniform, while those of Example 1 are gradient distributed. This is the fundamental reason why the permanent magnet of the present invention has better magnetic concentration effect and higher qualified rate. Figure 7 This is a cloud diagram of the surface magnetic distribution outside the focusing surface of the permanent magnet in Example 1 of the present invention. Figure 7 It can be seen that on the focusing surface, the magnetic field presents a focusing magnetization characteristic with a large center and small sides, which indicates that the method of the present invention achieves a better magnetic focusing effect.

[0092] Example 2

[0093] S1: Prepare RE-rich and Co-poor alloy powder I, the composition of the alloy powder by mass percentage is: (PrNd) 30 Tb3Co 1.5 Cu 0.2 Fe bal Al 0.3 Zr 0.15 B 0.86 According to the process of batching - rapid solidification belt spinning - hydrogen crushing - air flow milling, alloy fine powder with an average particle size of 1 μm was obtained.

[0094] S2: Prepare RE-poor Co-rich alloy powder II, the composition of the alloy powder is as follows by mass percentage: PrNd 25 Tb1 40 Cu 1.5 Fe bal Al 0.3 Zr 0.15 B 1.00 According to the process of batching - rapid solidification belt spinning or ingot casting - hydrogen crushing - air flow milling or high energy ball milling, alloy fine powder with an average particle size of 6 μm is obtained.

[0095] S3: Powder proportioning: alloy powders I and II are mixed in proportions of 3:7, 4:6 and 5:5 respectively to obtain mixed powders of three proportions.

[0096] S4: Add 0.3% lubricant to the powder with a mixing ratio of 3:7, add 0.2% lubricant to the powder with a mixing ratio of 4:6, and add 0.1% lubricant to the powder with a mixing ratio of 5:5. Then mix the powder in a V-type mixer for 4 hours. In order to reduce the activity of the powder, it needs to be left to stand for 2 hours to 2.5 hours after mixing.

[0097] S5: Magnetic field orientation molding: The above two powders are injected into the mold. The mold is divided into 5 areas. The powders are injected into areas A and E at a ratio of 3:7, into areas B and D at a ratio of 4:6, and into area C at a ratio of 5:5. The distribution of the mixed alloy powder in the mold is shown in Figure 8 . The powder bulk density is 2g / cm 3 The magnetic powder was then oriented and formed in a non-uniform magnetic field of 2.2 T, and then placed in an isostatic press for secondary pressing. The green density obtained at an isostatic pressure of 300 MPa was 4.50 g / cm 3 .

[0098] S6: Sintering and tempering heat treatment: Place the green body in a vacuum sintering furnace set at 1095°C for sintering and densification, and keep it warm for 8 hours; after the end of the heat preservation, stop heating, slowly cool to 800°C, fill with argon and turn on the fan to quickly cool to room temperature to obtain a sintered magnet; perform secondary tempering treatment on the sintered magnet, the treatment process is to keep it warm at 870°C for 6 hours and then quickly cool it to room temperature, and then keep it warm at 500°C for 4 hours and then quickly cool it to room temperature; the atmosphere of the tempering heat treatment is a vacuum state.

[0099] S7: Machining: The permanent magnet blank obtained in step S6 is processed according to the required shape and size. Its specific size is 80*40*30, where 30 is the magnetization direction. The arrow points to the focusing surface, and the tail of the arrow is the non-focusing surface. The surface treatment method of the permanent magnet is spraying epoxy.

[0100] S8: Magnetization and inspection: Place the processed permanent magnet into the magnetization coil for magnetization. The magnetization method is parallel magnetization and the magnetization magnetic field is 9 T. After magnetization, a permanent magnet with focusing orientation can be obtained.

[0101] Detect the composition distribution of each area of ​​the permanent magnet. Test the thermal expansion coefficient and magnetic properties of each area of ​​the permanent magnet.

[0102] Table 5 Composition distribution of each region of permanent magnet

[0103]

[0104]

[0105] Table 6 Thermal expansion coefficient of each region of permanent magnet

[0106] Area A Zone B Zone C Area D Zone E <![CDATA[α c∥ (K -1 )]]> <![CDATA[7.5×10 -6 ]]> <![CDATA[7.4×10 -6 ]]> <![CDATA[7.5×10 -6 ]]> <![CDATA[7.4×10 -6 ]]> <![CDATA[7.4×10 -6 ]]> <![CDATA[α c⊥ (K -1 )]]> <![CDATA[4.9×10 -6 ]]> <![CDATA[3.7×10 -6 ]]> <![CDATA[1.8×10 -6 ]]> <![CDATA[3.8×10 -6 ]]> <![CDATA[4.9×10 -6 ]]> <![CDATA[Δα(K -1 )]]> <![CDATA[2.6×10 -6 ]]> <![CDATA[3.7×10 -6 ]]> <![CDATA[5.7×10 -6 ]]> <![CDATA[3.6×10 -6 ]]> <![CDATA[2.5×10 -6 ]]>

[0107] Table 7 Magnetic properties of each region of permanent magnet

[0108] Area A Zone B Zone C Area D Zone E Br(kGs) 12.55 12.54 12.64 12.59 12.58 Hcj(kOe) 16.89 16.74 17.31 16.90 16.87

[0109] From the data of Table 5 to Table 7 of Example 2, it can be seen that the internal composition of the magnet presents a gradient distribution, that is, the total amount of rare earth in the central area of ​​the magnet is high, and the total amount at the edge is low. This distribution can ensure that the Br in the edge area remains high; the cobalt content in the central area of ​​the magnet is low and the cobalt content in the edge area is high, which can improve the reduction of the thermal expansion difference, help reduce the internal stress of the magnet, and reduce the probability of grains being crushed by backlog, thereby improving the qualified rate. The carbon content of the magnet is low in the central area and high in the edge area. This is because more lubricants are added to the powder in the edge area, while less lubricants are added in the middle. The magnetic field in the mold is low in the edge area and high in the center area. Therefore, by improving the lubricity of the powder in the edge area, it is possible to ensure that the edge area maintains a high degree of orientation, thereby obtaining a higher remanent magnetization Br. Figure 8 This is a cloud diagram of the magnetic field distribution on the focusing surface of the permanent magnet of Example 2. It can be seen that the magnetic field exhibits an obvious characteristic of converging toward the center line, which indicates that the present invention has achieved a better focusing magnetization effect.

[0110] Although the embodiments of the present invention have been disclosed above, they are not limited to the applications listed in the specification and the embodiments. It can be fully applied to various fields suitable for the present invention. For those familiar with the art, additional modifications can be easily realized. Therefore, without departing from the general concept defined by the claims and equivalent scope, the present invention is not limited to the specific details and the illustrations shown and described here.

Claims

1. A magnetic field focusing oriented NdFeB permanent magnet, characterized in that: The permanent magnet comprises a central region and at least one group of side regions, wherein the permanent magnet has a symmetry plane in the central region, each group of side regions comprises two side regions symmetrically distributed on both sides of the central region, and the outermost group of side regions in the at least one group of side regions is a group of edge regions; The composition and magnet properties of each set of side regions remain consistent; The composition of the permanent magnet in the central area or the side area is calculated by mass percentage: RE L a RE H b Co c Cu d M e Fe bal B f , 24≤a≤31, 0≤b≤4, 0≤c≤30, 0.1≤d≤0.8, 0.2≤e≤3, 0.86≤f≤1.2, 28≤a+b≤35, bal is the margin; RE L is one or a combination of light rare earth elements Pr, Nd, La, Ce and Y, RE H is one or a combination of heavy rare earths Gd, Ho, Dy and Tb, and M is one or a combination of Al, Cr, Nb, Zr, Ga, Ti, V, Mo and Mn; The RE content in the permanent magnet decreases from the central region to the edge region, and the Co content gradually increases. The composition distribution of the central region is rich in RE and poor in Co, and the composition distribution of the edge region is poor in RE and rich in Co. The difference in RE content between the central region and the edge region is ≤1%, and the difference in Co content between the edge region and the central region is ≤30%, wherein the RE content is RE L and RE H sum; The carbon content of the permanent magnet increases from the central region to the edge region, and the difference in carbon content between the central region and the edge region is ≥400 ppm; The thermal expansion coefficient perpendicular to the orientation direction in the permanent magnet increases from the central region to the edge region; the thermal expansion coefficient parallel to the orientation direction of the permanent magnet has no obvious difference between the central region and the at least one group of side regions; the difference between the thermal expansion coefficient perpendicular to the orientation direction and the thermal expansion coefficient parallel to the orientation direction of the permanent magnet decreases from the central region to the edge region; The permanent magnet has a focusing plane perpendicular to the symmetry plane, and on the focusing plane, the magnetic field strength of the permanent magnet increases region by region from the edge region to the central region.

2. The magnetic field focusing oriented NdFeB permanent magnet according to claim 1, characterized in that: The permanent magnet includes two or four side regions symmetrically distributed on both sides of the central region.

3. A method for preparing a magnetic field focusing oriented NdFeB permanent magnet as claimed in claim 1 or 2, characterized in that: include: Step (1) preparing an alloy powder I rich in RE and poor in Co, wherein the composition of the alloy powder I is as follows by mass percentage: L a1 RE H b1 Co c1 Cu d1 Fe bal M e1 B f1 , where 30≤a1≤33, 0≤b1≤4, 0≤c1≤3, 0≤d1≤0.3, 0.2≤e1≤3, 0.86≤f1≤1.2; Step (2) preparing an alloy powder II which is low in RE and rich in Co. The composition of the alloy powder II is as follows by mass percentage: L a2 RE H b2 Co c2 Cu d2 Fe bal M e2 B f2 , where 26≤a2≤31, 0≤b2≤4, 3<c2≤40, 0≤d2≤2, 0.2≤e2≤3, 0.86≤f2≤1.2; Step (3) powder proportioning: the alloy powder I and the alloy powder II are mixed in at least two proportions to prepare at least two mixed alloy powders, wherein at least one of the at least two mixed alloy powders has a composition of rich RE and poor Co, and at least one of the mixed alloy powders has a composition of poor RE and rich Co, the RE content of the at least two mixed alloy powders decreases in sequence, and the Co content increases in sequence, the difference in RE content between the mixed alloy powder with the highest RE content and the mixed alloy powder with the lowest RE content in the at least two mixed alloy powders is ≤1%, and the difference in Co content between the mixed alloy powder with the highest Co content and the mixed alloy powder with the lowest Co content in the at least two mixed alloy powders is ≤30%, wherein the RE content is RE L and RE H sum; Step (4) adding lubricant and mixed powder: adding lubricant to the at least two mixed alloy powders respectively, so that the carbon content of the at least two mixed alloy powders increases successively, the difference in carbon content between the mixed alloy powder with the highest carbon content and the mixed alloy powder with the lowest carbon content in the at least two mixed alloy powders is ≥400ppm, and the carbon content in each mixed alloy powder is 500-2000ppm; Step (5) magnetic field orientation molding: divide the internal space of the mold into a central space and at least one group of side spaces, each group of side spaces includes two side spaces symmetrically distributed on both sides of the central space, and the outermost group of side spaces in the at least one group of side spaces is a group of edge spaces; put the at least two mixed alloy powders into the central space and the at least one group of side spaces respectively, put mixed alloy powders of the same composition into each group of side spaces, and make the RE content of the mixed alloy powders placed in the central space to the edge space one by one decrease successively, and the Co content increase successively, the composition distribution of the mixed alloy powder placed in the central space is rich in RE and poor in Co, the composition distribution of the mixed alloy powder placed in the edge space is poor in RE and rich in Co, the difference in RE content between the mixed alloy powders placed in the central space and the edge space is ≤1%, and the difference in Co content between the mixed alloy powders placed in the edge space and the central space is ≤30%, wherein the RE content is RE L and RE H The RE content of the mixed alloy powder placed in the middle space to the edge space increases successively, and the difference in carbon content between the mixed alloy powder placed in the middle space and the edge space is ≥400ppm; then, the mold is placed in a magnetic field for orientation and shaping; Step (6) sintering and tempering heat treatment; Step (7) machining; Step (8) magnetization.

4. The method for preparing a magnetic field focusing oriented NdFeB permanent magnet according to claim 3, characterized in that: The average particle size of the alloy powder I is 1 to 5 μm; the average particle size of the alloy powder II is 2 to 6 μm.

5. The method for preparing a magnetic field focusing oriented NdFeB permanent magnet according to claim 3, characterized in that: In the step (4), the lubricant is added in an amount of 0.1% to 1%.

6. The method for preparing a magnetic field focusing oriented NdFeB permanent magnet according to claim 3, characterized in that: In the step (5), the density of the mixed alloy powder placed in the middle space and the at least one set of side spaces in the internal space of the mold is 1.6 to 2 g / cm 3 The mold is placed in a magnetic field for orientation shaping, which is specifically achieved by the following process: orientation shaping is carried out in a non-uniform magnetic field of 1.2-2.2T, and then placed in an isostatic press for secondary pressing, the isostatic pressure is 150-300MPa, and the green density obtained is 3.9-4.5g / cm 3 .

7. The method for preparing a magnetic field focusing oriented NdFeB permanent magnet according to claim 6, characterized in that: In the step (6), the sintering and tempering heat treatment is specifically achieved through the following process: placing the green body in a vacuum sintering furnace set at a temperature of 1000-1100°C for sintering and densification, and the insulation time is 2-10 hours; after the insulation is completed, stopping heating, slowly cooling to 800-900°C, filling with argon and turning on the fan to quickly cool to room temperature to obtain a sintered magnet; subjecting the sintered magnet to a secondary tempering treatment, the treatment conditions are: keeping at 800-950°C for 2-6 hours and then quickly cooling to room temperature, and then keeping at 400-650°C for 2-10 hours and then quickly cooling to room temperature; the atmosphere of the tempering heat treatment is a vacuum or argon protection state.

8. The method for preparing a magnetic field focusing oriented NdFeB permanent magnet according to claim 7, characterized in that: The magnetization is specifically achieved through the following process: the magnet machined in step (7) is placed in a magnetization coil for magnetization, the magnetization method is parallel to the symmetry plane of the magnet machined in step (7), and the magnetization magnetic field is 3 to 10T.

Citation Information

Patent Citations

  • Gradient functionality rare earth permanent magnet

    CN101030467A

  • Gradient neodymium iron boron magnet and manufacturing method thereof

    CN108899190A

  • Sintered neodymium-iron-boron magnet and preparation method thereof

    CN115346746A

  • Neodymium-iron-boron magnet and preparation method thereof

    CN116313350A

  • Functionally graded rare earth permanent magnet

    CN1838344A

Cited By

  • Preparation method of magnetism-gathering magnetic steel, magnetism-gathering magnetic steel and loudspeaker

    CN119993730A

  • Preparation of mold with surface magnetism gathering function and magnet

    CN120072504A

  • Magnetic steel forming accurate control method and system based on magnetic field orientation