Flexible composite film for high-frequency current measurement and preparation method thereof
By using 3D printing technology to prepare flexible composite films on silica nanoaerogel felt, the problems of large core size and high manufacturing cost of high frequency current transformer are solved, and low-cost and high-performance high-frequency current measurement solutions are achieved plan.
Patent Information
- Application Number
- CN202411051037.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-01
- Publication Date
- 2024-11-22
AI Technical Summary
The existing high-frequency current transformers have large cores, which are difficult to connect in a narrow space, and have high manufacturing costs, which cannot meet the application needs of multiple scenarios.
Using silica nanoaerogel felt as a support, 3D printing technology is used to form a flexible composite film on its surface to form a low-cost, high-permeability magnetic core material to achieve the density and controllability of the magnetic core. .
The prepared flexible composite film has high starting permeability, quality factor and transmission impedance value, is small in size and light in weight, and is suitable for high-frequency current measurement of power equipment such as transformers and cables, reducing manufacturing costs.
Smart Images

Figure CN119008187A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of high-frequency current measurement, and in particular relates to a flexible composite film for high-frequency current measurement and a preparation method thereof. Background Art
[0002] When the insulation of power equipment such as transformers and cables fails, high-frequency pulse current will be generated and introduced into the earth through the ground wire. Therefore, connecting a high-frequency current transformer to the ground wire to measure the high-frequency current component can determine the operating status of the power equipment and avoid major accidents.
[0003] At present, high-frequency current transformers mainly use soft ferrite cores and winding coils for measurement. The inner diameter of the transformer is between 0.02m and 0.2m, and is used for various grounding wires and cable bodies. In order to ensure that there is enough magnetic flux to improve the sensitivity of the transformer, the core of the transformer generally needs to be 4cm 2 The above cross-sectional area results in a large volume and heavy mass of the transformer, which cannot be connected by through-hole clamping in some places where the grounding wire is laid along the ground. As for the clamping of the cable body, due to the large diameter of cables such as 220kV, the transformer needs to have a large inner diameter. The manufacturing cost of the transformer is very high, and the selling price generally exceeds 30,000 yuan, which cannot be applied on a large scale. Therefore, by developing flexible thin film sensing materials as magnetic cores, a low-cost flexible transformer that can be simply through-hole clamped in various scenarios is formed and applied.
[0004] Prior art document 1 (CN 101299378 B) discloses a magnetic core of a printed circuit board transformer made of flexible magnetic material. The structural features of the PCB transformer using flexible magnetic material are as follows: (1) using flexible magnetic conductive material or other new magnetic material with high magnetic permeability; (2) the magnetic core structure can adopt a multi-core long magnetic wire structure; (3) the magnetic core structure can adopt a magnetic braided tape structure; (4) the magnetic core structure can also adopt a thin film layered flexible magnetic tape structure; (5) the magnetic core and coil of the PCB transformer adopt a matrix structure. However, the shortcomings of this prior art document are that it does not provide a specific preparation method of the flexible magnetic material, and there are a large number of gaps inside the flexible magnetic core body formed by multi-core, braided tape or thin film layered magnetic materials, resulting in low overall magnetic permeability.
[0005] 3D printing is a rapid preparation method that uses a specific nozzle or nozzle to extrude materials directly out of the nozzle to form a solid structure. The 3D printing method has the advantages of low cost, high efficiency, simple preparation method and environmental protection. At the same time, it can also achieve precise control of the structure, size and performance of flexible composite films and meet the needs of customized preparation of size and structure.
[0006] Therefore, there is an urgent need for a flexible composite film for high-frequency current measurement prepared using 3D printing technology. Summary of the invention
[0007] In order to solve the deficiencies in the prior art, the present invention provides a solution to the problem that the existing high-frequency mutual inductor magnetic core is large in size and difficult to be connected in a narrow space. Silica nano aerogel felt is selected as a support body, and a flexible composite film is prepared by forming on its surface using a 3D printing method, so as to promote the low cost of high-frequency current testing and industrial application in various scenarios, thereby providing a flexible composite film for high-frequency current measurement and a preparation method thereof.
[0008] To achieve the above object, the present invention is implemented according to the following steps:
[0009] The first aspect of the present invention discloses a method for preparing a flexible composite film for high-frequency current measurement, comprising the following steps:
[0010] Step 1, pretreatment of the flexible substrate material: using silica nano-aerogel felt as the substrate material, washing it with an organic solvent of a set proportion, and obtaining a substrate material with a clean surface after drying;
[0011] Step 2, preparation of 3D printing slurry: mixing materials in a set ratio to obtain a mixture A, calcining and ball-milling the mixture A to obtain a mixture B, and mixing the mixture B with polydimethylsiloxane to obtain a 3D printing slurry;
[0012] Step 3, 3D printing to obtain a flexible composite film: The 3D printing slurry obtained in step 2 is 3D printed on the surface of the base material obtained in step 1 to obtain a flexible composite film for high-frequency current measurement after processing.
[0013] Preferably, in step 1, the matrix material is a silica nano-aerogel felt with a pore size range of 20-50 nm and a porosity of 85% to 95%;
[0014] Preferably, in step 1, the organic solvent comprises: anhydrous ethanol and acetone, wherein the mass ratio of the matrix material to anhydrous ethanol and acetone is (2-5):3:(1-3).
[0015] Preferably, step 2 specifically includes:
[0016] Step 2.1, Fe2O3, ZnO, NiO, CuO, SiO2, B2O3, and Co2O3 are mixed with pure water in a set ratio to obtain a mixture A, and the mixture A is ball-milled;
[0017] Step 2.2, calcining the ball-milled mixed material A at a set temperature and ball-milling again to obtain mixed material B;
[0018] Step 2.3, mixing the mixture B with polydimethylsiloxane to obtain a 3D printing slurry.
[0019] Preferably, in step 2.1, the set ratio is 21.3-24.7% Fe2O3, 15.3-18.7% ZnO, 5.6-8.3% NiO, 5.2-6.7% CuO, 1.5-3.0% SiO2, 0.5-1.2% B2O3, 0.5-0.8% Co2O3 and the balance pure water.
[0020] Preferably, the ball milling speed in step 2.1 is 320-400 r / min for 2.5-4 hours, and the ball milling speed in step 2.2 is 380-450 r / min for 4-5 hours.
[0021] Preferably, in step 2.3, the mass fraction of the mixture B is 35-65%.
[0022] Preferably, step 3 specifically includes: transferring the 3D printing slurry into the printer slurry cylinder, and spreading the base material on the 3D printer workbench, controlling the 3D printer to print and form a rectangular shape on the surface of the base material, and then sintering at a set sintering temperature, and finally rolling to obtain a flexible composite film prepared by 3D printing for high-frequency current measurement.
[0023] Preferably, the 3D printing speed is 15 to 25 mm / s, the nozzle diameter of the 3D printer is 0.2 to 1.5 mm, and the thickness of the 3D printed composite film is 3 to 8 mm; the sintering temperature is 900 to 950° C., and the sintering time is 15 to 20 hours.
[0024] The second aspect of the present invention discloses a flexible composite film for high-frequency current measurement, which is prepared by the method for preparing a flexible composite film for high-frequency current measurement. The flexible composite film includes: a substrate layer and a high-frequency current sensing material layer, and the substrate layer plays a supporting role for the composite film.
[0025] The beneficial effect of the present invention is that, compared with the prior art,
[0026] (1) The present invention uses silicon dioxide nano-aerogel felt as a flexible base material, adopts an optimal raw material ratio and processing technology, and uses 3D printing technology to print and shape the configured 3D printing slurry on the surface of the base material, and then heats it at high temperature to prepare a high-permeability flexible magnetic core material with controllable structure and size, thereby obtaining a flexible composite film prepared by 3D printing for high-frequency current measurement;
[0027] (2) The composite film of the present invention has good flexibility and soft magnetic properties. According to actual tests, the initial magnetic permeability of the flexible composite film of the present invention is greater than 100, the quality factor is greater than 50, and the transmission impedance value is greater than 8mV / mA. At the same time, it has the characteristics of small magnetic core thickness, small volume and light weight, which can meet the needs of high-frequency current measurement of grounding current of power equipment such as transformers and cables. BRIEF DESCRIPTION OF THE DRAWINGS
[0028] In order to more clearly illustrate the specific implementation methods of the present invention or the technical solutions in the prior art, the drawings required for use in the specific implementation methods or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are some implementation methods of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0029] Figure 1 is the initial magnetic permeability of the flexible composite film for high-frequency current measurement prepared in Examples 1 to 4;
[0030] Figure 2 is the quality factor of the flexible composite film for high-frequency current measurement prepared in Examples 1 to 4;
[0031] Figure 3 is the transmission impedance of the flexible composite film for high-frequency current measurement prepared in Examples 1 to 4;
[0032] Figure 4 It is a flexible composite film used for high-frequency current measurement. DETAILED DESCRIPTION
[0033] In order to make the purpose, technical scheme and advantages of the present invention clearer, the technical scheme of the present invention will be clearly and completely described below in conjunction with the drawings in the embodiments of the present invention. The embodiments described in this application are only part of the embodiments of the present invention, not all of them. Based on the spirit of the present invention, other embodiments obtained by ordinary technicians in this field without creative work are all within the scope of protection of the present invention.
[0034] The present invention provides a flexible composite film for high-frequency current measurement and a preparation method thereof, the steps of which are as follows:
[0035] Step 1, pretreatment of the flexible substrate material: using silica nano-aerogel felt as the substrate material, washing it with an organic solvent of a set proportion, and obtaining a substrate material with a clean surface after drying;
[0036] In a preferred but non-limiting embodiment of the present invention, the matrix material is a silica nano-aerogel felt with a pore size range of 20-50 nm and a porosity of 85% to 95%;
[0037] It is worth noting that the existing flexible magnetic core preparation technology is to first prepare the magnetic core separately by high-temperature sintering, and then use a polymer film material, such as polydimethylsiloxane film, as a matrix material, and glue the obtained magnetic core to the polymer film to form a flexible magnetic core. The main reason for preparing the magnetic core first and then gluing it to the flexible matrix is that the polymer film is not resistant to high temperature and will basically melt at temperatures above 200°C. The flexible magnetic core material prepared in this way is affected by the gluing process, resulting in its reliability and magnetic properties are not ideal.
[0038] The applicant of the present invention has found that the silica nano aerogel felt has excellent high temperature resistance, which can withstand high temperatures up to 1000°C. Therefore, the magnetic core is directly printed on the silica nano aerogel felt flexible substrate, and then the whole is subjected to high temperature sintering treatment. This can improve the bonding strength and density of the magnetic core and the substrate, and omit the gluing step.
[0039] Further preferably, the organic solvent includes anhydrous ethanol, acetone and other organic solvents, wherein the mass ratio of the matrix material to anhydrous ethanol and acetone is (2-5):3:(1-3).
[0040] Step 2, 3D printing slurry preparation;
[0041] In a preferred but non-limiting embodiment of the present invention, step 2 specifically comprises:
[0042] Step 2.1, Fe2O3, ZnO, NiO, CuO, SiO2, B2O3, and Co2O3 are mixed with pure water in a set ratio to obtain a mixture A, and the mixture A is ball-milled;
[0043] In a preferred but non-limiting embodiment of the present invention, the set ratio is 21.3-24.7% Fe2O3, 15.3-18.7% ZnO, 5.6-8.3% NiO, 5.2-6.7% CuO, 1.5-3.0% SiO2, 0.5-1.2% B2O3, 0.5-0.8% Co2O3 and the balance pure water.
[0044] Furthermore, the ball milling speed is 320-400 r / min, and the time is 2.5-4 hours.
[0045] Step 2.2, calcining the ball-milled mixed material A at a high temperature and ball-milling it again to obtain a mixed material B;
[0046] In a preferred but non-limiting embodiment of the present invention, the ball milling process is carried out at a rotation speed of 380 to 450 r / min for 4 to 5 hours.
[0047] Step 2.3, mixing the mixture B with polydimethylsiloxane to obtain a 3D printing slurry.
[0048] In a preferred but non-limiting embodiment of the present invention, the mass fraction of the mixture B is 35-65%.
[0049] Step 3, 3D printing to obtain a flexible composite film for high-frequency current measurement;
[0050] In a preferred but non-limiting embodiment of the present invention, step 3 specifically includes: transferring to the printer slurry barrel, and spreading the base material on the 3D printer workbench, controlling the 3D printer to print and form a rectangular shape on the surface of the base material, and then sintering at high temperature, and finally rolling to obtain a flexible composite film prepared by 3D printing for high-frequency current measurement.
[0051] In a preferred but non-limiting embodiment of the present invention, the 3D printing speed is 15 to 25 mm / s, the nozzle diameter of the 3D printer is 0.2 to 1.5 mm, and the thickness of the 3D printed composite film is 3 to 8 mm;
[0052] It is worth noting that because printing is performed on the surface of the base material, the size of the base material must be larger than the printed shape, but its shape size does not affect the performance of the flexible film.
[0053] More preferably, the sintering temperature is 900-950° C., and the sintering time is 15-20 hours.
[0054] The present invention also provides a flexible composite film for high-frequency current measurement, which is prepared by the above-mentioned method for preparing a flexible composite film for high-frequency current measurement. The flexible composite film includes: a substrate layer and a high-frequency current sensing material layer, and the substrate layer plays a supporting role for the composite film.
[0055] Example 1
[0056] This embodiment provides a flexible composite film for high-frequency current measurement and a preparation method thereof, the steps are as follows:
[0057] Step 1: Put the silica nano aerogel felt with a pore size of 25nm and a porosity of 90% into an organic solvent formed by a mixture of anhydrous ethanol and acetone for cleaning, wherein the mass ratio of the base material to anhydrous ethanol and acetone is 2:3:1, and the immersion cleaning time is 2 hours; after cleaning, put it into an oven, heat it to 60°C, and dry it for 2 hours.
[0058] Step 2: Preparation of 3D printing slurry: ① According to the molar fraction, 21.5% Fe2O3, 15.8% ZnO, 5.9% NiO, 5.5% CuO, 1.5% SiO2, 0.8% B2O3, 0.5% Co2O3 and 48.5% pure water were mixed to obtain mixture A, and then the mixture A was ball-milled, wherein the ball-milling speed was 350r / min and the ball-milling time was 3 hours. ② The ball-milled mixture A was calcined at 1050℃ for 8 hours, and ball-milled again, the ball-milling speed was 400r / min, and the ball-milling time was 5 hours, to obtain mixture B. ③ Mix mixture B with polydimethylsiloxane, wherein the mass fraction of mixture B was 52%, to obtain 3D printing slurry.
[0059] Step 3: Transfer the obtained 3D printing slurry to the printer slurry barrel, and spread the base material on the 3D printer workbench, wherein the base material is 200 mm wide and 500 mm long. Control the 3D printer to print on the surface of the base material in a rectangular shape of 220 mm long and 100 mm wide. The 3D printing speed is 20 mm / s, the 3D printer nozzle diameter is 0.5 mm, and the 3D printed composite film thickness is 5 mm. Then, the printed sample is sintered at a sintering temperature of 920°C and a sintering time of 15 hours. After sintering, it is crushed by rolling to obtain a 3D printed flexible composite film for high-frequency current measurement.
[0060] Example 2
[0061] This embodiment provides a flexible composite film for high-frequency current measurement and a preparation method thereof, the steps are as follows:
[0062] Step 1: Put the silica nano aerogel felt with a pore size of 30nm and a porosity of 92% into an organic solvent formed by a mixture of anhydrous ethanol and acetone for cleaning, wherein the mass ratio of the base material to anhydrous ethanol and acetone is 4:3:2, and the immersion cleaning time is 3 hours; after cleaning, put it into an oven, heat it to 60°C, and dry it for 2 hours.
[0063] Step 2: Preparation of 3D printing slurry: ① According to the molar fraction, 22.7% Fe2O3, 16.4% ZnO, 7.3% NiO, 5.3% CuO, 2.1% SiO2, 0.7% B2O3, 0.6% Co2O3 and 44.9% pure water were mixed to obtain mixture A, and then the mixture A was ball-milled, wherein the ball-milling speed was 320r / min and the ball-milling time was 4 hours. ② The ball-milled mixture A was calcined at 1080℃ for 7 hours, and ball-milled again, the ball-milling speed was 450r / min, and the ball-milling time was 4 hours, to obtain mixture B. ③ Mix mixture B with polydimethylsiloxane, wherein the mass fraction of mixture B was 45%, to obtain 3D printing slurry.
[0064] Step 3: Transfer the obtained 3D printing slurry to the printer slurry barrel, and spread the base material on the 3D printer workbench, wherein the base material is 200 mm wide and 500 mm long. Control the 3D printer to print on the surface of the base material in a rectangular shape of 250 mm long and 80 mm wide. The 3D printing speed is 15 mm / s, the 3D printer nozzle diameter is 0.3 mm, and the 3D printed composite film thickness is 3.6 mm. Then, the printed sample is sintered at a sintering temperature of 900°C and a sintering time of 20 hours. After sintering, it is crushed by rolling to obtain a 3D printed flexible composite film for high-frequency current measurement.
[0065] Example 3
[0066] This embodiment provides a flexible composite film for high-frequency current measurement and a preparation method thereof, the steps are as follows:
[0067] Step 1: Put the silica nano aerogel felt with a pore size of 45nm and a porosity of 85% into an organic solvent formed by a mixture of anhydrous ethanol and acetone for cleaning, wherein the mass ratio of the base material to anhydrous ethanol and acetone is 5:3:1, and the immersion cleaning time is 2 hours; after cleaning, put it into an oven, heat it to 60°C, and dry it for 2 hours.
[0068] Step 2: Preparation of 3D printing slurry: ① According to the molar fraction, 24.7% Fe2O3, 15.5% ZnO, 6.5% NiO, 5.8% CuO, 2.5% SiO2, 1.0% B2O3, 0.7% Co2O3 and 43.3% pure water were mixed to obtain mixture A, and then the mixture A was ball-milled, wherein the ball-milling speed was 400r / min and the ball-milling time was 3 hours. ② The ball-milled mixture A was calcined at 1000℃ for 8 hours, and ball-milled again, the ball-milling speed was 420r / min, and the ball-milling time was 4 hours, to obtain mixture B. ③ Mix mixture B with polydimethylsiloxane, wherein the mass fraction of mixture B was 55%, to obtain 3D printing slurry.
[0069] Step 3: Transfer the obtained 3D printing slurry to the printer slurry barrel, and spread the base material on the 3D printer workbench, wherein the base material is 200 mm wide and 500 mm long. Control the 3D printer to print on the surface of the base material in a rectangular shape of 200 mm long and 150 mm wide. The 3D printing speed is 18 mm / s, the 3D printer nozzle diameter is 0.4 mm, and the 3D printed composite film thickness is 4 mm. Then, the printed sample is sintered at a sintering temperature of 930°C and a sintering time of 16 hours. After sintering, it is crushed by rolling to obtain a 3D printed flexible composite film for high-frequency current measurement.
[0070] Example 4
[0071] This embodiment provides a flexible composite film for high-frequency current measurement and a preparation method thereof, the steps are as follows:
[0072] Step 1: Put the silica nano aerogel felt with a pore size of 35nm and a porosity of 95% into an organic solvent formed by a mixture of anhydrous ethanol and acetone for cleaning, wherein the mass ratio of the base material to anhydrous ethanol and acetone is 5:3:3, and the immersion cleaning time is 3 hours; after cleaning, put it into an oven, heat it to 60°C, and dry it for 2 hours.
[0073] Step 2: Preparation of 3D printing slurry: ① According to the molar fraction, 22.5% Fe2O3, 17.2% ZnO, 5.8% NiO, 6.3% CuO, 2.8% SiO2, 0.8% B2O3, 0.8% Co2O3 and 43.8% pure water were mixed to obtain mixture A, and then the mixture A was ball-milled, wherein the ball-milling speed was 360r / min and the ball-milling time was 2.5 hours. ② The ball-milled mixture A was calcined at 1080℃ for 8 hours, and ball-milled again, the ball-milling speed was 380r / min, and the ball-milling time was 4.5 hours, to obtain mixture B. ③ Mix mixture B with polydimethylsiloxane, wherein the mass fraction of mixture B was 62%, to obtain 3D printing slurry.
[0074] Step 3: Transfer the obtained 3D printing slurry to the printer slurry barrel, and spread the base material on the 3D printer workbench, wherein the base material is 200 mm wide and 500 mm long. Control the 3D printer to print on the surface of the base material in a rectangular shape of 300 mm long and 250 mm wide. The 3D printing speed is 22 mm / s, the 3D printer nozzle diameter is 1.2 mm, and the 3D printed composite film thickness is 4.8 mm. Then, the printed sample is sintered at a sintering temperature of 950°C and a sintering time of 17 hours. After sintering, it is crushed by rolling to obtain a 3D printed flexible composite film for high-frequency current measurement.
[0075] like Figure 4 As shown, the flexible composite films for high-frequency current measurement of Examples 1-4 were obtained through testing, and their initial magnetic permeabilities are as follows Figure 1 As shown, the quality factor is Figure 2 As shown, the transmission impedance value is Figure 3 It can be seen that the initial magnetic permeabilities of the four prepared embodiments are all greater than 100, and the quality factors are greater than 50, indicating that the four embodiments have good soft magnetic properties; the four transmission impedance values are all greater than 8mV / mA, meeting the use requirements.
[0076] The beneficial effect of the present invention is that, compared with the prior art,
[0077] (1) The present invention uses silicon dioxide nano-aerogel felt as a flexible base material, adopts an optimal raw material ratio and processing technology, and uses 3D printing technology to print and shape the configured 3D printing slurry on the surface of the base material, and then heats it at high temperature to prepare a high-permeability flexible magnetic core material with controllable structure and size, thereby obtaining a flexible composite film prepared by 3D printing for high-frequency current measurement;
[0078] (2) The composite film of the present invention has good flexibility and soft magnetic properties. According to actual tests, the initial magnetic permeability of the flexible composite film of the present invention is greater than 100, the quality factor is greater than 50, and the transmission impedance value is greater than 8mV / mA. At the same time, it has the characteristics of small magnetic core thickness, small volume and light weight, which can meet the needs of high-frequency current measurement of grounding current of power equipment such as transformers and cables.
[0079] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention rather than to limit it. Although the present invention has been described in detail with reference to the above embodiments, ordinary technicians in the relevant field should understand that the specific implementation methods of the present invention can still be modified or replaced by equivalents, and any modifications or equivalent replacements that do not depart from the spirit and scope of the present invention should be covered within the scope of protection of the claims of the present invention.
Claims
1. A method for preparing a flexible composite film for high-frequency current measurement, characterized in that: The following steps are involved: Step 1, pretreatment of the flexible substrate material: using silica nano-aerogel felt as the substrate material, washing it with an organic solvent of a set proportion, and obtaining a substrate material with a clean surface after drying; Step 2, preparation of 3D printing slurry: mixing materials in a set ratio to obtain a mixture A, calcining and ball-milling the mixture A to obtain a mixture B, and mixing the mixture B with polydimethylsiloxane to obtain a 3D printing slurry; Step 3, 3D printing to obtain a flexible composite film: The 3D printing slurry obtained in step 2 is 3D printed on the surface of the base material obtained in step 1 to obtain a flexible composite film for high-frequency current measurement after processing.
2. The method for preparing a flexible composite film for high-frequency current measurement according to claim 1, characterized in that: In step 1, the base material is a silicon dioxide nano-aerogel felt with a pore size range of 20-50 nm and a porosity of 85% to 95%.
3. The method for preparing a flexible composite film for high-frequency current measurement according to claim 1, characterized in that: In step 1, the organic solvent includes anhydrous ethanol and acetone, wherein the mass ratio of the matrix material to anhydrous ethanol and acetone is (2-5):3:(1-3).
4. The method for preparing a flexible composite film for high-frequency current measurement according to claim 1, characterized in that: Step 2 specifically includes: Step 2.1, Fe2O3, ZnO, NiO, CuO, SiO2, B2O3, and Co2O3 are mixed with pure water in a set ratio to obtain a mixture A, and the mixture A is ball-milled; Step 2.2, calcining the ball-milled mixed material A within a set temperature range and ball-milling again to obtain mixed material B; Step 2.3, mixing the mixture B with polydimethylsiloxane to obtain a 3D printing slurry.
5. The method for preparing a flexible composite film for high-frequency current measurement according to claim 4, characterized in that: In step 2.1, the set ratio is 21.3-24.7% Fe2O3, 15.3-18.7% ZnO, 5.6-8.3% NiO, 5.2-6.7% CuO, 1.5-3.0% SiO2, 0.5-1.2% B2O3, 0.5-0.8% Co2O3 and the balance is pure water.
6. The method for preparing a flexible composite film for high-frequency current measurement according to claim 4, characterized in that: The ball milling process in step 2.1 is carried out at a rotation speed of 320 to 400 r / min for 2.5 to 4 hours, and the ball milling process in step 2.2 is carried out at a rotation speed of 380 to 450 r / min for 4 to 5 hours.
7. The method for preparing a flexible composite film for high-frequency current measurement according to claim 4, characterized in that: In step 2.3, the mass fraction of the mixture B is 35-65%.
8. The method for preparing a flexible composite film for high-frequency current measurement according to claim 1, characterized in that: Step 3 specifically includes: transferring the 3D printing slurry into the printer slurry cylinder, and spreading the base material on the 3D printer workbench, controlling the 3D printer to print and form a rectangular shape on the surface of the base material, and then sintering at a set sintering temperature, and finally rolling to obtain a 3D printed flexible composite film for high-frequency current measurement.
9. The method for preparing a flexible composite film for high-frequency current measurement according to claim 8, characterized in that: The 3D printing speed is 15 to 25 mm / s, the nozzle diameter of the 3D printer is 0.2 to 1.5 mm, and the thickness of the 3D printed composite film is 3 to 8 mm; the sintering temperature is 900 to 950° C., and the sintering time is 15 to 20 hours.
10. A flexible composite film for high-frequency current measurement, prepared by the method for preparing a flexible composite film for high-frequency current measurement according to any one of claims 1 to 9, characterized in that: The flexible composite film comprises: a substrate layer and a high-frequency current sensing material layer, and the substrate layer plays a supporting role for the composite film.
Citation Information
Patent Citations
Magnetic core of printed circuit board transformer prepared by flexible magnetic material