Conductive dispersion for capacitor as well as preparation method and application of conductive dispersion

By using technical means such as organic solvents and emulsifiers in capacitors, conductive dispersions are prepared so that they can penetrate into the pores of the dielectric layer, and the problem of poor permeability of benzodifurandione derivatives in capacitors is solved. The capacity of the capacitor is improved and the equivalent series resistance is reduced, which improves the overall performance of the capacitor.

CN119008246APending Publication Date: 2024-11-22SHENZHEN CAPCHEM TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310551097.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-05-16
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

The existing conjugated polymer based on benzodifurandione and its derivatives is difficult to penetrate sufficiently in the capacitor, resulting in the problems of low capacitor capacity and high equivalent series resistance.

Method used

The high-conductive polymer is dissolved with organic solvent to form liquid A, and homogenize it in an aqueous solution containing an emulsifier and a dispersion stabilizer, and add polyether and polyhydroxy compound additives to prepare conductive D50 with a particle size of 100 nm or less. The dispersion allows it to completely penetrate and penetrate into the pores of the dielectric layer, forming a highly conductive polymer film layer, reducing the equivalent series resistance of the capacitor.

Benefits of technology

It significantly improves the capacity and comprehensive performance of the capacitor, reduces the equivalent series resistance, and improves the reliability and high-frequency performance of the capacitor.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119008246A_ABST
    Figure CN119008246A_ABST
Patent Text Reader

Abstract

In order to solve the problem that the capacity and equivalent series resistance of a capacitor are affected due to the fact that an existing conjugated polymer based on benzodifuran diketone and derivatives thereof is difficult to apply to the capacitor, the invention provides a preparation method of a conductive dispersion for the capacitor. Comprising the following operation steps: providing a solution A, wherein the solution A is a solution obtained by dissolving a high-conductivity polymer in an organic solvent; providing a solution B, wherein the solution B is an aqueous solution added with an emulsifier and a dispersion stabilizer; under a stirring condition, adding the solution A into the solution B; and adding an auxiliary agent into the primary dispersion, and then carrying out homogenization treatment to obtain the conductive dispersion for the capacitor with the D50 particle size of 100nm and below. Meanwhile, the invention also discloses the conductive dispersion for the capacitor prepared by the preparation method and application. The prepared conductive dispersion for the capacitor has the characteristics of small and uniform particle size, can completely infiltrate and permeate into pores of a dielectric layer, and effectively improves various electrochemical properties of the electrolytic capacitor.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of solid electrolytic capacitor materials, and specifically relates to a conductive dispersion for capacitors and a preparation method and application thereof. Background Art

[0002] As one of the three major passive components, capacitors play an irreplaceable role in the electrical and electronic industry and electrical equipment. With the development of the industry, in addition to the long-term reliability required of capacitors, more and higher requirements are also put forward for capacitors. For example, electrical equipment that operates at high frequencies, such as servers and computer hosts, requires capacitors to have small size and lower ESR (equivalent series resistance); fast charging plugs require higher voltage resistance and stable charging and discharging performance; base stations and outdoor electrical equipment require electrolytic capacitors to have stable and reliable performance under extreme high and low temperatures; large-capacity capacitors with both energy storage and current supplement functions have requirements for losses. In the past 20 years, conductive polymer-based electrolytic capacitors have made outstanding progress in high-frequency equivalent series resistance. At the same time, the application end mentioned above also puts forward new requirements for the performance of electrolytic capacitors. As the actual cathode material of electrolytic capacitors, the intrinsic conductivity and processing technology of conductive polymers are the core factors that determine the performance of electrolytic capacitors.

[0003] The conductivity of the conductive polymer, the mutual bonding between the conductive polymer and the components of the capacitor, and the filling of the conductive polymer in the capacitor have an important impact on the performance and reliability of the capacitor. There is a conjugated polymer based on benzodifurandione and its derivatives, which has the characteristics of high conductivity. However, when the emulsion prepared by this polymer is used for the element impregnation operation of the capacitor, it is difficult to fully penetrate into the interior of the capacitor element or the film-forming performance is poor, thereby affecting the capacity of the capacitor, and the equivalent series resistance of the obtained capacitor is relatively high. Summary of the invention

[0004] In view of the problem that existing conjugated polymers based on benzodifurandione and its derivatives are difficult to apply to capacitors, which affects the capacitor capacity and equivalent series resistance, the present invention provides a conductive dispersion for capacitors and a preparation method and application thereof.

[0005] The technical solution adopted by the present invention to solve the above technical problems is as follows:

[0006] In one aspect, the present invention provides a method for preparing a conductive dispersion for a capacitor, comprising the following steps:

[0007] Provide liquid A: Liquid A is a solution obtained by dissolving a highly conductive polymer in an organic solvent, wherein the highly conductive polymer includes a polymer obtained by polymerizing a compound represented by structural formula 1 and / or structural formula 2:

[0008]

[0009] wherein R is independently selected from a hydrogen atom, a C1-C18 alkyl group, a C1-C18 alkylene group, a C1-C18 alkyl derivative or a C1-C18 alkylene derivative;

[0010] Provide liquid B: liquid B is an aqueous solution with an emulsifier and a dispersion stabilizer added;

[0011] Under stirring conditions, add liquid A to liquid B to form a primary dispersion;

[0012] Adding an auxiliary agent to the primary dispersion, the auxiliary agent includes one or more of polyether and polyhydroxy compound, and then performing homogenization to obtain a conductive dispersion for capacitors with a D50 particle size of 100nm or less.

[0013] Optionally, the organic solvent includes one or more of dimethyl sulfoxide, dimethylformamide, tetrahydrofuran and pyridine.

[0014] Optionally, the mass concentration of the highly conductive polymer in the liquid A is 1% to 3%.

[0015] Optionally, the emulsifier includes one or more of dodecyl sulfonic acid, dodecylbenzene sulfonic acid, polystyrene sulfonic acid, N,N-dimethyl-n-octylamine, methyl-terminated polyoxyethylene ether 200-3000, ethylene glycol propylene glycol copolymer 200-2000, and polyoxyethylene fatty alcohol ether;

[0016] The dispersion stabilizer includes one or more of polyethylene glycol 200-4000, hydroxymethyl cellulose, cetyl alcohol, beeswax, decapolyglycerol myristate and glucitol.

[0017] Optionally, the mass concentration of the emulsifier in the liquid B is 0.01% to 5%, and the mass concentration of the dispersion stabilizer in the liquid B is 1% to 15%.

[0018] Optionally, the mixing mass ratio of the liquid A and the liquid B is (1-9):(9-1).

[0019] Optionally, the method of adding liquid A to liquid B is dropwise addition, and liquid A is added dropwise to liquid B at a stirring speed of 500 to 7000 rpm, and dispersed for 10 min to 10 h.

[0020] Optionally, the additive is added in an amount of 0.5% to 20% by mass;

[0021] The polyether includes one or more of polyoxyethylene ether with a molecular weight of 200 to 10,000, methyl-terminated polyoxyethylene ether with a molecular weight of 200 to 3,000, polypropylene glycol ether with a molecular weight of 200 to 10,000, ethylene glycol propylene glycol copolyether with a molecular weight of 200 to 2,000, and polytetrahydrofuran with a molecular weight of 200 to 2,000;

[0022] The polyhydroxy compound includes one or more of ethylene glycol, diethylene glycol, triethylene glycol, mannitol, glycerol, polyoxyethylene glycerol, xylitol, sorbitol, erythritol, arbutin, glucose, pentaerythritol, polyvinyl alcohol and dipentaerythritol.

[0023] In another aspect, the present invention provides a conductive dispersion for capacitors, which is prepared by the above-mentioned preparation method.

[0024] In another aspect, the present invention provides the use of the conductive dispersion for capacitors prepared by the preparation method as described above in the impregnation operation of electrolytic capacitors.

[0025] According to the preparation method of the conductive dispersion for capacitors provided by the present invention, an n-type doped highly conductive polymer of benzodifurandione and its derivatives is used. The inventors have found through experiments that the reason why such highly conductive polymers are poorly used in electrolytic capacitors is that it is difficult to achieve both film-forming properties on the surface of the dielectric layer and penetration properties into the pores of the dielectric layer. To solve this problem, the preparation method provided by the present invention first uses an organic solvent to dissolve the highly conductive polymer to form a liquid A, and adds the liquid A to an aqueous solution (liquid B) containing an emulsifier and a dispersion stabilizer in a dispersed state. After adding an auxiliary agent of a polyether and / or a polyhydroxy compound, a nano-scale conductive dispersion with a D50 particle size reduced to 100 nm or less can be obtained. The conductive dispersion can completely infiltrate and penetrate into the pores of the dielectric layer. After the drying process, the highly conductive polymer film layer forms an interface contact with the dielectric layer, thereby improving the capacity extraction rate; the conductive polymer forms a film between the pores of the dielectric layer, and the conductive polymer fills and conducts between the dielectric layer and the negative electrode, and with the help of the high conductivity of the polymer, the equivalent series resistance of the capacitor is significantly reduced. BRIEF DESCRIPTION OF THE DRAWINGS

[0026] Figure 1 is a cross-sectional view of the dielectric layer of the capacitor after impregnation provided by the present invention;

[0027] Figure 2 It is an enlarged cross-sectional view of the dielectric layer of the capacitor after impregnation provided by the present invention;

[0028] Figure 3 This is an electron microscope image of the surface of the dielectric layer of the capacitor after impregnation provided by the present invention. DETAILED DESCRIPTION

[0029] In order to make the technical problems, technical solutions and beneficial effects solved by the present invention more clearly understood, the present invention is further described in detail below in conjunction with the accompanying drawings and embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention.

[0030] An embodiment of the present invention provides a method for preparing a conductive dispersion for a capacitor, comprising the following steps:

[0031] Provide liquid A: Liquid A is a solution obtained by dissolving a highly conductive polymer in an organic solvent, wherein the highly conductive polymer includes a polymer obtained by polymerizing a compound represented by structural formula 1 and / or structural formula 2:

[0032]

[0033] wherein R is independently selected from a hydrogen atom, a C1-C18 alkyl group, a C1-C18 alkylene group, a C1-C18 alkyl derivative or a C1-C18 alkylene derivative;

[0034] Provide liquid B: liquid B is an aqueous solution with an emulsifier and a dispersion stabilizer added;

[0035] Under stirring conditions, add liquid A to liquid B to form a primary dispersion;

[0036] Adding an auxiliary agent to the primary dispersion, the auxiliary agent includes one or more of polyether and polyhydroxy compound, and then performing homogenization to obtain a conductive dispersion for capacitors with a D50 particle size of 100nm or less.

[0037] In the description of the present invention, the term "alkylene" refers to unsaturated hydrocarbon groups such as alkenyl and alkynyl. The term "alkyl derivative" refers to single or multiple hydrogens on the alkyl group replaced by other groups, and the term "alkylene derivative" refers to single or multiple hydrogens on the alkyl group replaced by other groups, and the other groups can be halogens, halogenated hydrocarbons, oxygen-containing groups, nitrogen-containing groups, etc.

[0038] The inventors have found through experiments that the reason why the n-type doped highly conductive polymer of benzodifurandione and its derivatives is poorly used in electrolytic capacitors is that it is difficult to achieve both film-forming performance on the surface of the dielectric layer and penetration performance into the pores of the dielectric layer. To solve this problem, the preparation method provided by the present invention first uses an organic solvent to dissolve the highly conductive polymer to form a liquid A, and then adds the liquid A to an aqueous solution (liquid B) containing an emulsifier and a dispersion stabilizer in a dispersed state. After adding an auxiliary agent such as a polyether and / or a polyhydroxy compound, a nano-scale conductive dispersion with a D50 particle size reduced to 100nm or less can be obtained. The conductive dispersion can completely infiltrate and penetrate into the pores of the dielectric layer. After the drying process, the highly conductive polymer film layer forms an interface contact with the dielectric layer, thereby improving the capacity extraction rate; the conductive polymer forms a film between the pores of the dielectric layer, and the conductive polymer fills and conducts between the dielectric layer and the negative electrode, and the equivalent series resistance of the capacitor is significantly reduced by virtue of the high conductivity of the polymer.

[0039] In some embodiments, the particle size of the highly conductive polymer particles of the primary dispersion is less than 1000 nm.

[0040] In some embodiments, the organic solvent is selected from organic polar solvents.

[0041] In some embodiments, the organic solvent includes one or more of dimethyl sulfoxide, dimethylformamide, tetrahydrofuran, and pyridine.

[0042] The above organic polar solvents can, on the one hand, fully dissolve and disperse the highly conductive polymer; on the other hand, the organic polar solvents also have a certain water solubility, which is conducive to dispersing the highly conductive polymer in the final aqueous solution.

[0043] In some embodiments, the mass concentration of the highly conductive polymer in the liquid A is 1% to 3%.

[0044] In a specific embodiment, the mass concentration of the highly conductive polymer in the liquid A may be 1%, 1.2%, 1.4%, 1.7%, 1.9%, 2%, 2.2%, 2.5%, 2.8% or 3%.

[0045] When the mass concentration of the highly conductive polymer in the A liquid is too low, the concentration of the highly conductive polymer in the formed conductive dispersion is insufficient, making it difficult to completely wet the capacitor elements; when the mass concentration of the highly conductive polymer in the A liquid is too high, the highly conductive polymer is prone to agglomeration during the dispersion stage, resulting in excessively large particle size in the conductive dispersion, which is in turn not conducive to the penetration of the highly conductive polymer in the dielectric layer.

[0046] In some embodiments, the emulsifier includes one or more of dodecyl sulfonic acid, dodecylbenzene sulfonic acid, polystyrene sulfonic acid, N,N-dimethyl-n-octylamine, methyl-terminated polyoxyethylene ether 200-3000, ethylene glycol propylene glycol copolymer 200-2000, and polyoxyethylene fatty alcohol ether;

[0047] The dispersion stabilizer includes one or more of polyethylene glycol 200-4000, hydroxymethyl cellulose, cetyl alcohol, beeswax, decapolyglycerol myristate and glucitol.

[0048] In some embodiments, the mass concentration of the emulsifier in the liquid B is 0.01% to 5%, and the mass concentration of the dispersion stabilizer in the liquid B is 1% to 15%.

[0049] In a specific embodiment, the mass concentration of the emulsifier in the B liquid can be 0.01%, 0.03%, 0.05%, 0.1%, 0.12%, 0.15%, 0.3%, 0.5%, 0.8%, 0.9%, 1.0%, 1.2%, 1.4%, 1.5%, 1.8%, 2%, 2.2%, 2.5%, 2.8%, 3.0%, 3.2%, 3.5%, 3.8%, 4.0%, 4.2%, 4.5%, 4.8% or 5.0%.

[0050] The emulsifier is used to fully disperse the highly conductive polymer in the aqueous solution. When the mass concentration of the emulsifier in the B liquid is too low, it is difficult to fully disperse the highly conductive polymer in the aqueous solution, and the problem of sedimentation and stratification of the highly conductive polymer is likely to occur; when the mass concentration of the emulsifier in the B liquid is too high, too much emulsifier remains in the conductive dispersion, affecting the film-forming performance of the conductive dispersion in the capacitor element impregnation process.

[0051] The mass concentration of the dispersion stabilizer in the B solution can be 1%, 2%, 3%, 4%, 5%, 6%, 7%, 8%, 9%, 10%, 11%, 12%, 13%, 14% or 15%.

[0052] The dispersion stabilizer is used to control the particle size of the highly conductive polymer in the conductive dispersion. When the mass concentration of the dispersion stabilizer in the B solution is too low, the particle size of the highly conductive polymer particles in the conductive dispersion formed is relatively large, affecting the impregnation effect; when the mass concentration of the dispersion stabilizer in the B solution is too high, it is also not conducive to improving the film-forming effect of the conductive dispersion.

[0053] In some embodiments, the mixing mass ratio of the A liquid and the B liquid is (1-9): (9-1).

[0054] In a preferred embodiment, the mixing mass ratio of the liquid A to the liquid B is (3-7):(7-3).

[0055] In a more preferred embodiment, the mixing mass ratio of the liquid A and the liquid B is (4-6):(6-4).

[0056] In some embodiments, solution A is added to solution B by dropwise addition at a dispersion speed of 500 to 7000 rpm, and the dispersion is carried out for 10 min to 10 h.

[0057] The dropping operation under high-speed dispersion state is beneficial to fully disperse the highly conductive polymer in liquid A in liquid B through high concentration gradient difference and dynamic action, which is beneficial to reduce the particle size of polymer particles in the obtained primary dispersion.

[0058] In some embodiments, the additive is added in an amount of 0.5% to 20% by mass;

[0059] The polyether includes one or more of polyoxyethylene ether with a molecular weight of 200 to 10,000, methyl-terminated polyoxyethylene ether with a molecular weight of 200 to 3,000, polypropylene glycol ether with a molecular weight of 200 to 10,000, ethylene glycol propylene glycol copolyether with a molecular weight of 200 to 2,000, and polytetrahydrofuran with a molecular weight of 200 to 2,000;

[0060] The polyhydroxy compound includes one or more of ethylene glycol, diethylene glycol, triethylene glycol, mannitol, glycerol, polyoxyethylene glycerol, xylitol, sorbitol, erythritol, arbutin, glucose, pentaerythritol, polyvinyl alcohol and dipentaerythritol. Another embodiment of the present invention provides a conductive dispersion for capacitors, which is prepared by the above preparation method.

[0061] In some embodiments, the conductive dispersion for capacitors includes the following components:

[0062] Highly conductive polymer, organic solvent, emulsifier, dispersion stabilizer, additive and water;

[0063] Wherein, the auxiliary agent includes one or more of polyether and polyhydroxy compound;

[0064] The highly conductive polymer includes a polymer obtained by polymerizing the compound represented by Structural Formula 1 and / or Structural Formula 2;

[0065] The D50 particle size of the highly conductive polymer particles in the conductive dispersion is 100 nm or less.

[0066] In some embodiments, the conductive dispersion for capacitors includes the following components by weight:

[0067] 1 to 3 parts of highly conductive polymer, 97 to 99 parts of organic solvent, 0.01 to 5 parts of emulsifier, 1 to 15 parts of dispersion stabilizer, 0.5 to 20 parts of auxiliary agent and 50 to 98.49 parts of water.

[0068] In some embodiments, the organic solvent includes one or more of dimethyl sulfoxide, dimethylformamide, tetrahydrofuran, and pyridine.

[0069] In some embodiments, the emulsifier includes one or more of dodecyl sulfonic acid, dodecylbenzene sulfonic acid, polystyrene sulfonic acid, N,N-dimethyloctylamine, methyl-terminated polyoxyethylene ether 200-3000, ethylene glycol propylene glycol copolymer 200-2000, and polyoxyethylene fatty alcohol ether.

[0070] In some embodiments, the dispersion stabilizer includes one or more of polyethylene glycol 200-4000, hydroxymethyl cellulose, cetyl alcohol, beeswax, decaglycerol myristate and glucitol.

[0071] The polyether includes one or more of polyoxyethylene ether with a molecular weight of 200 to 10,000, methyl-terminated polyoxyethylene ether with a molecular weight of 200 to 3,000, polypropylene glycol ether with a molecular weight of 200 to 10,000, ethylene glycol propylene glycol copolyether with a molecular weight of 200 to 2,000, and polytetrahydrofuran with a molecular weight of 200 to 2,000;

[0072] The polyhydroxy compound includes one or more of ethylene glycol, diethylene glycol, triethylene glycol, mannitol, glycerol, polyoxyethylene glycerol, xylitol, sorbitol, erythritol, arbutin, glucose, pentaerythritol, polyvinyl alcohol and dipentaerythritol.

[0073] Another embodiment of the present invention provides the use of the conductive dispersion for capacitors prepared by the preparation method described above in the impregnation operation of electrolytic capacitors.

[0074] The conductive dispersion is processed by solvents to disperse n-type doped conductive polymers of benzodifurandione and its derivatives in water to form a nano-scale dispersion with a D50 particle size of 100nm or less, which is deposited and filled in the pores and film layers of electrolytic capacitor elements by negative pressure impregnation, significantly reducing ESR and capacity extraction, and improving the overall performance of the capacitor. By regulating the conductive polymer nano-scale dispersion, the polymer material can be controlled to form a uniform conductive film on the surface of the capacitor dielectric layer, and a highly conductive film channel can be formed between the pores of the dielectric film.

[0075] like Figure 1 to Figure 3 As shown, it is a microscopic morphology of the capacitor element after being impregnated with the conductive dispersion provided by the present invention. Figure 1 to Figure 3It can be seen that the conductive dispersion provided by the present invention can fully penetrate into the micropores of the dielectric layer of the capacitor element and form a uniform conductive film layer on the dielectric layer of the capacitor element. The present invention is further described below through examples.

[0076] Example 1

[0077] This example is used to illustrate the conductive dispersion for capacitors and the preparation method thereof disclosed in the present invention, and includes the following steps:

[0078] Step (1): dissolving poly(3,7-dihydrobenzo[1,2-b:4,5-b']difuran-2,6-dione) in dimethyl sulfoxide to prepare a solution A with a mass concentration of 2%;

[0079] Step (2): adding 1% by mass concentration of N,N-dimethyl-n-octylamine and 8% by mass concentration of decaglycerol myristate to the aqueous solution to obtain liquid B; slowly adding 100 g of liquid A prepared in step (1) to 100 g of liquid B at a dispersion speed of 3000 rpm, and dispersing for 30 minutes to form a primary dispersion. At this time, the particle size distribution is measured by dynamic light scattering and recorded in Table 1;

[0080] Step (3): Add 8% by mass concentration of polytetrahydrofuran and 4% by mass concentration of arbutin to the primary dispersion prepared in step (2), stir for 8 hours, and homogenize under high pressure to obtain a conductive dispersion for capacitors. The particle size distribution is measured by dynamic light scattering and recorded in Table 1;

[0081] Step (4): The capacitor element is impregnated into the conductive dispersion for the capacitor obtained in step (3) by negative pressure impregnation, and is immersed at a pressure of -95KPa to +100KPa for 1 to 40 minutes. The poly(benzodifurandione) forms a film on the dielectric layer and fills the space between the dielectric layer and the negative electrode. The film is taken out and dried at a temperature of 100°C for 30 minutes. The above impregnation operation is repeated 3 times, and the capacitor is dried and assembled to obtain the capacitor.

[0082] Example 2

[0083] This example is used to illustrate the conductive dispersion for capacitors and the preparation method thereof disclosed in the present invention, and includes most of the operation steps in Example 1, except that:

[0084] Step (1): dissolving poly (1,5-dibutyl-5,7-dihydro-1H,3H-pyrrolo[2,3-f]indole-2,6-dione) in dimethyl sulfoxide to prepare a solution A with a mass concentration of 2%;

[0085] In step (2), 1% by mass concentration of polystyrene sulfonic acid and 8% by mass concentration of polyethylene glycol 1000 are added to the aqueous solution to obtain liquid B; 100 g of liquid A prepared in step (1) is slowly added dropwise to 100 g of liquid B at a dispersion speed of 3000 rpm, and dispersed for 30 minutes to form a primary dispersion. At this time, the particle size distribution is measured by dynamic light scattering and recorded in Table 1.

[0086] Example 3

[0087] This example is used to illustrate the conductive dispersion for capacitors and the preparation method thereof disclosed in the present invention, and includes most of the operation steps in Example 1, except that:

[0088] In step (2), 1% by mass concentration of polystyrene sulfonic acid and 8% by mass concentration of decaglycerol myristate are added to the aqueous solution to obtain liquid B; 100 g of liquid A prepared in step (1) is slowly added dropwise to 100 g of liquid B at a dispersion speed of 3000 rpm, and dispersed for 30 minutes to form a primary dispersion. At this time, the particle size distribution is measured by dynamic light scattering and recorded in Table 1.

[0089] Example 4

[0090] This example is used to illustrate the conductive dispersion for capacitors and the preparation method thereof disclosed in the present invention, and includes most of the operation steps in Example 1, except that:

[0091] In step (2), 1% by mass concentration of methyl-terminated polyoxyethylene ether 800 and 8% by mass concentration of decaglycerol myristate are added to the aqueous solution to obtain liquid B; 100 g of liquid A prepared in step (1) is slowly added dropwise to 100 g of liquid B at a dispersion speed of 3000 rpm, and dispersed for 30 minutes to form a primary dispersion. At this time, the particle size distribution is measured by dynamic light scattering and recorded in Table 1.

[0092] Example 5

[0093] This example is used to illustrate the conductive dispersion for capacitors and the preparation method thereof disclosed in the present invention, and includes most of the operation steps in Example 1, except that:

[0094] In step (2), 1% by mass concentration of polystyrene sulfonic acid and 12% by mass concentration of polyglycerol myristate are added to the aqueous solution to obtain liquid B; 100 g of liquid A prepared in step (1) is slowly added dropwise to 100 g of liquid B at a dispersion speed of 3000 rpm, and dispersed for 30 minutes to form a primary dispersion. At this time, the particle size distribution is measured by dynamic light scattering and recorded in Table 1.

[0095] Example 6

[0096] This example is used to illustrate the conductive dispersion for capacitors and the preparation method thereof disclosed in the present invention, and includes most of the operation steps in Example 1, except that:

[0097] In step (2), 1% by mass concentration of polystyrene sulfonic acid and 4% by mass concentration of decaglycerol myristate are added to the aqueous solution to obtain liquid B; 100 g of liquid A prepared in step (1) is slowly added dropwise to 100 g of liquid B at a dispersion speed of 3000 rpm, and dispersed for 30 minutes to form a primary dispersion. At this time, the particle size distribution is measured by dynamic light scattering and recorded in Table 1.

[0098] Example 7

[0099] This example is used to illustrate the conductive dispersion for capacitors and the preparation method thereof disclosed in the present invention, and includes most of the operation steps in Example 1, except that:

[0100] Step (2): Add 1% by mass concentration of N,N-dimethyloctylamine and 8% by mass concentration of decaglycerol myristate to the aqueous solution to obtain liquid B; slowly dropwise add 20 g of liquid A prepared in step (1) to 180 g of liquid B at a dispersion speed of 3000 rpm, and disperse for 30 minutes to form a primary dispersion. At this time, the particle size distribution is determined by dynamic light scattering and recorded in Table 1.

[0101] Example 8

[0102] This example is used to illustrate the conductive dispersion for capacitors and the preparation method thereof disclosed in the present invention, and includes most of the operation steps in Example 1, except that:

[0103] Step (2): Add 1% by mass concentration of N,N-dimethyloctylamine and 8% by mass concentration of decaglycerol myristate to the aqueous solution to obtain liquid B; slowly drop 180g of the liquid A prepared in step (1) into 20g of the liquid B at a dispersion speed of 3000 rpm, and disperse for 30 minutes to form a primary dispersion. At this time, the particle size distribution is determined by dynamic light scattering and recorded in Table 1.

[0104] Example 9

[0105] This example is used to illustrate the conductive dispersion for capacitors and the preparation method thereof disclosed in the present invention, and includes most of the operation steps in Example 2, except that:

[0106] Step (2): Add 1% by mass concentration of N,N-dimethyloctylamine and 8% by mass concentration of decaglycerol myristate to the aqueous solution to obtain liquid B; slowly dropwise add 120 g of liquid A prepared in step (1) to 80 g of liquid B at a dispersion speed of 3000 rpm, and disperse for 30 minutes to form a primary dispersion. At this time, the particle size distribution is determined by dynamic light scattering and recorded in Table 1.

[0107] Example 10

[0108] This example is used to illustrate the conductive dispersion for capacitors and the preparation method thereof disclosed in the present invention, and includes most of the operation steps in Example 2, except that:

[0109] Step (2): Add 1% by mass concentration of N,N-dimethyloctylamine and 8% by mass concentration of decaglycerol myristate to the aqueous solution to obtain liquid B; slowly dropwise add 80g of the liquid A prepared in step (1) to 120g of the liquid B at a dispersion speed of 3000 rpm, and disperse for 30 minutes to form a primary dispersion. At this time, the particle size distribution is determined by dynamic light scattering and recorded in Table 1.

[0110] Comparative Example 1

[0111] This comparative example is used to compare and illustrate the conductive dispersion for capacitors and the preparation method thereof disclosed in the present invention, and includes most of the operation steps in Example 1, except that:

[0112] In step (2): 100 g of solution A prepared in step (1) was slowly added dropwise to 100 g of water at a dispersion speed of 3000 rpm and dispersed for 30 min to form a primary dispersion. At this time, the particle size distribution was determined by dynamic light scattering and recorded in Table 1.

[0113] Comparative Example 2

[0114] This comparative example is used to compare and illustrate the conductive dispersion for capacitors and the preparation method thereof disclosed in the present invention, and includes most of the operation steps in Example 1, except that:

[0115] In step (2), 1% mass concentration of N,N-dimethyloctylamine was added to the aqueous solution to obtain liquid B; 100 g of liquid A prepared in step (1) was slowly added dropwise to 100 g of liquid B at a dispersion speed of 3000 rpm, and dispersed for 30 min to form a primary dispersion. At this time, the particle size distribution was determined by dynamic light scattering and recorded in Table 1.

[0116] Comparative Example 3

[0117] This comparative example is used to compare and illustrate the conductive dispersion for capacitors and the preparation method thereof disclosed in the present invention, and includes most of the operation steps in Example 1, except that:

[0118] In step (2), 8% mass concentration of decaglycerol myristate is added to the aqueous solution to obtain liquid B; 100 g of liquid A prepared in step (1) is slowly added dropwise to 100 g of liquid B at a dispersion speed of 3000 rpm, and dispersed for 30 min to form a primary dispersion. At this time, the particle size distribution is measured by dynamic light scattering and recorded in Table 1.

[0119] Comparative Example 4

[0120] This comparative example is used to compare and illustrate the conductive dispersion for capacitors and the preparation method thereof disclosed in the present invention, and includes most of the operation steps in Example 1, except that:

[0121] Do not perform step (3);

[0122] The primary dispersion obtained in step (2) is directly used for the impregnation operation in step (4).

[0123] Performance Testing

[0124] The electrolytic capacitors prepared above were subjected to the following performance tests:

[0125] Test conditions: 25±1℃, 60±5% air humidity;

[0126] Test equipment and methods: Digital bridge test at 120Hz, test the capacitance and DF value of the capacitor; at 100KHz, test the ESR of the capacitor;

[0127] Surge capacity attenuation test method: constant DC power supply, relay without protection resistor; capacitor rated voltage, charge for 1s, discharge for 1s, perform 10,000 charge and discharge cycles, and detect surge capacity attenuation rate after 10,000 charge and discharge cycles;

[0128] Low temperature capacity decay test method: Place the capacitor in a -40℃ low temperature box, keep warm for 4 hours, and test the parameters.

[0129] The test results obtained are entered in Table 1.

[0130] Table 1

[0131]

[0132] From the test results in Table 1, it can be seen that the conductive dispersion prepared by the preparation method provided by the present invention has a significantly lower particle size, reduces ESR and improves capacity extraction, and improves the overall performance of the capacitor. By regulating the conductive polymer nano-scale dispersion, the polymer material can be controlled to form a uniform conductive film on the surface of the capacitor dielectric layer, thereby improving the various properties of the electrolytic capacitor.

[0133] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions and improvements made within the spirit and principles of the present invention should be included in the protection scope of the present invention.

Claims

1. A method for preparing a conductive dispersion for a capacitor, characterized in that: The steps include: Provide liquid A: Liquid A is a solution obtained by dissolving a highly conductive polymer in an organic solvent, wherein the highly conductive polymer includes a polymer obtained by polymerizing a compound represented by structural formula 1 and / or structural formula 2: wherein R is independently selected from a hydrogen atom, a C1-C18 alkyl group, a C1-C18 alkylene group, a C1-C18 alkyl derivative or a C1-C18 alkylene derivative; Provide liquid B: liquid B is an aqueous solution with an emulsifier and a dispersion stabilizer added; Under stirring conditions, add liquid A to liquid B to form a primary dispersion; Adding an auxiliary agent to the primary dispersion, the auxiliary agent includes one or more of polyether and polyhydroxy compound, and then performing homogenization to obtain a conductive dispersion for capacitors with a D50 particle size of 100nm or less.

2. The method for preparing a conductive dispersion for a capacitor according to claim 1, characterized in that: The organic solvent includes one or more of dimethyl sulfoxide, dimethylformamide, tetrahydrofuran and pyridine.

3. The method for preparing a conductive dispersion for a capacitor according to claim 1, characterized in that: The mass concentration of the highly conductive polymer in the A solution is 1% to 3%.

4. The method for preparing a conductive dispersion for a capacitor according to claim 1, characterized in that: The emulsifier includes one or more of dodecyl sulfonic acid, dodecylbenzene sulfonic acid, polystyrene sulfonic acid, N,N-dimethyl n-octylamine, methyl-terminated polyoxyethylene ether 200-3000, ethylene glycol propylene glycol copolymer 200-2000, and polyoxyethylene fatty alcohol ether; The dispersion stabilizer includes one or more of polyethylene glycol 200-4000, hydroxymethyl cellulose, cetyl alcohol, beeswax, decapolyglycerol myristate and glucitol.

5. The method for preparing a conductive dispersion for capacitors according to claim 1 or 4, characterized in that: The mass concentration of the emulsifier in the B liquid is 0.01% to 5%, and the mass concentration of the dispersion stabilizer in the B liquid is 1% to 15%.

6. The method for preparing a conductive dispersion for a capacitor according to claim 1, characterized in that: The mixing mass ratio of the A liquid and the B liquid is (1-9):(9-1).

7. The method for preparing a conductive dispersion for a capacitor according to claim 1, characterized in that: Liquid A is added to liquid B by dropwise addition. At a stirring speed of 500 to 7000 rpm, liquid A is added dropwise to liquid B and dispersed for 10 minutes to 10 hours.

8. The method for preparing a conductive dispersion for a capacitor according to claim 1, characterized in that: The added mass of the auxiliary agent is 0.5% to 20%; The polyether includes one or more of polyoxyethylene ether with a molecular weight of 200 to 10,000, methyl-terminated polyoxyethylene ether with a molecular weight of 200 to 3,000, polypropylene glycol ether with a molecular weight of 200 to 10,000, ethylene glycol propylene glycol copolyether with a molecular weight of 200 to 2,000, and polytetrahydrofuran with a molecular weight of 200 to 2,000; The polyhydroxy compound includes one or more of ethylene glycol, diethylene glycol, triethylene glycol, mannitol, glycerol, polyoxyethylene glycerol, xylitol, sorbitol, erythritol, arbutin, glucose, pentaerythritol, polyvinyl alcohol and dipentaerythritol.

9. A conductive dispersion for capacitors, characterized in that: The compound is prepared by the preparation method according to any one of claims 1 to 8.

10. Use of the conductive dispersion for capacitors prepared by the preparation method according to any one of claims 1 to 8 in the impregnation operation of electrolytic capacitors.