Method and device for processing oxide semiconductor film through thermal pulse
Through the thermal pulse annealing technology of hydrogen-oxygen generator, the problem of oxygen vacancy regulation in oxide semiconductors is solved, and the efficient performance optimization of the oxide semiconductor thin film is achieved, and the stability and response speed of the material are improved.
Patent Information
- Application Number
- CN202411233933.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-04
- Publication Date
- 2024-11-22
AI Technical Summary
When regulating defects such as oxygen vacancies in oxide semiconductors, the problem of thermal stress, phase change, long annealing time, difficult plasma treatment to penetrate deep into the material and introduce new defects, and it is difficult to accurately control the oxygen vacancies distribution to optimize material performance. .
Using the thermal pulse annealing method based on the hydrogen-oxygen generator, the oxide semiconductor film is placed on a metal substrate for multiple thermal pulse annealing. By controlling the temperature, time and frequency, the oxygen vacancy distribution is accurately regulated, avoiding thermal damage and improving material stability. sex.
Accurate control of oxygen vacancies in oxide semiconductor thin films is achieved, the electrical and optical properties of the material are improved, defect concentration is reduced, thermal stability and mechanical strength of the material are improved, and time and energy are saved.
Smart Images

Figure CN119008473A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the field of semiconductor technology, and in particular to a method and device for thermal pulse processing of an oxide semiconductor film. Background Art
[0002] At present, the research on oxide semiconductors is still in its infancy. Detectors based on oxide semiconductors are subject to problems such as poor material stability, high defect density, large leakage current, and obvious persistent photoconductivity effect. Similar to other oxide semiconductors, intrinsic defects related to oxygen vacancies are one of the core factors that affect and determine the performance of materials and their optoelectronic devices. Oxygen vacancies, as a common point defect, will significantly change the conductivity and electron mobility of the material, thereby affecting the overall performance of the device. For example, in photoconductive Ga2O3 photodetectors, defect-related photoconductivity gain and persistent photoconductivity increase the responsivity and response recovery time, respectively, resulting in a mutually restrictive and contradictory relationship between responsivity and response recovery speed. Therefore, "rational regulation" of defects such as oxygen vacancies in oxide semiconductors is a difficult problem that needs to be solved urgently.
[0003] In the prior art, defects such as oxygen vacancies are usually regulated by high-temperature annealing and oxygen plasma treatment. Although it has advantages such as simple operation, simple process, and clear mechanism to a certain extent, it still has many shortcomings. For example, annealing at a higher temperature will cause thermal stress in the material or induce undesirable phase changes. The annealing process usually takes a long time to achieve the desired effect. Plasma treatment mainly acts on the surface of the material and is difficult to penetrate into the interior of the material. New surface defects or damage will also be introduced during the plasma treatment process. Therefore, there is an urgent need for a device and method that can accurately control oxygen vacancies and other defects to optimize the performance of oxide semiconductor materials. Summary of the invention
[0004] The object of the present invention is to provide a method and device for thermal pulse processing of oxide semiconductor films that can accurately control the distribution and concentration of oxygen vacancies inside a sample without damaging the sample.
[0005] On the one hand, the present invention provides a method for thermal pulse treatment of an oxide semiconductor film, the method is based on thermal pulse annealing of a hydrogen-oxygen generator, a sample to be treated is placed on a metal substrate in an open environment, and a treated sample is obtained after N thermal pulse annealings, and 9≤N≤15, the temperature of the thermal pulse annealing is 800~1000°C, the duration of the thermal pulse annealing treatment is 0.5~1s, and the frequency of the thermal pulse annealing is 0.5~1 Hz; The sample to be processed is an oxide semiconductor film to be processed, the oxygen vacancy concentration in the sample to be processed is n1, and the oxygen vacancies are evenly distributed, n1<38%; The treated sample is an oxide semiconductor film that has been annealed. The oxygen vacancy concentration of the surface film of the treated sample is n2, and the thickness of the surface film is d, and it satisfies 40%≤n2≤55%, d<10nm. When the oxygen vacancy concentration of the surface film of the treated sample is 40%≤n2≤55%, the detector has good photoelectric performance, the photocurrent can reach 27.8μA, and the detector response time is only 60μs.
[0006] Furthermore, the grain size of the surface of the sample to be processed in the method of the present invention is 0.48-0.52 nm; the grain size of the surface film is 9-13.6 nm.
[0007] Furthermore, the oxygen vacancy concentration n2 of the surface film of the sample after treatment by the method of the present invention satisfies: n2=k*3N+n1; and 0.3≤k≤0.4.
[0008] Furthermore, the thickness of the sample to be processed in the method of the present invention ranges from 80 to 110 nm.
[0009] Furthermore, in the method of the present invention, after placing the sample to be processed on a metal substrate in an open environment and before starting the thermal pulse annealing, first check whether the power supply of the oxyhydrogen generator is normal, and select the corresponding nozzle according to the size of the sample to be processed; then check the relay to ensure that the start valve is open when the relay is at a high level and the valve is closed when the relay is at a low level; finally, set the torch handle to the normally open state.
[0010] Furthermore, the thermal pulse annealing method of the present invention specifically includes: firstly, opening the pneumatic valve and the relay, controlling the pneumatic valve and the arc ignition module through the relay so that the flamethrower emits a pulse flame, performing thermal pulse annealing on the sample to be processed placed on the metal substrate, and closing the relay after reaching the specified duration; completing the entire thermal pulse annealing process according to the set thermal pulse annealing temperature, duration, frequency and number of times.
[0011] On the other hand, the present invention provides a device for thermal pulse treatment of oxide semiconductor films. The device is based on any of the above-mentioned methods for thermal pulse treatment of oxide semiconductor films. The device includes a oxyhydrogen generator, a flamethrower connected to the oxyhydrogen generator through a pipeline, and an iron frame. A relay is also provided on the pipeline, and a pneumatic valve is also provided on the pipeline between the oxyhydrogen generator and the relay; an arc ignition module is also provided at the flamethrower, and a metal substrate with adjustable height is also provided on the iron frame.
[0012] Furthermore, an anti-flashback valve is provided on the pipeline of the device of the present invention between the hydrogen and oxygen generator and the pneumatic valve.
[0013] Furthermore, the flamethrower of the device of the present invention comprises a nozzle and a handle.
[0014] Furthermore, the hydrogen-oxygen generator of the device of the present invention can produce hydrogen and oxygen in a ratio of 2:1, and can be used immediately after being turned on and produced on demand. The hydrogen-oxygen generator is equipped with sodium hydroxide with a concentration higher than 99.5%.
[0015] The method of the present invention can produce thermal activation effect and thermal stress effect, wherein the thermal activation effect is that at high temperature, the atoms in the material obtain more energy and can overcome the bond energy, thereby causing oxygen atoms to escape from the lattice position to form oxygen vacancies. The rapid heating characteristics of thermal pulse treatment exacerbate this effect. The rapid heating and cooling process will generate thermal stress inside the material. These stresses will destroy the integrity of the lattice, promote the migration and escape of oxygen atoms, and increase the formation of oxygen vacancies.
[0016] In addition, the heat pulse treatment not only affects the concentration of oxygen vacancies, but also has a significant impact on the recrystallization and other defects on the sample surface. The specific effects are as follows: Defect repair: Thermal pulse treatment can cause some defects in the crystal lattice, such as dislocations and grain boundaries, to be repaired through a recrystallization process at high temperatures. This repair process helps to improve the crystal quality of the material, reduce the defect concentration, and thus improve the electrical and optical properties of the material.
[0017] Improvement of material stability: The recrystallization process can improve the thermal and mechanical stability of the material. By eliminating or reducing defects such as grain boundaries and dislocations, the material's resistance to thermal shock and mechanical strength in subsequent use will be improved.
[0018] Improvement of surface morphology: Thermal pulse treatment can also improve the surface morphology of the sample, making the surface smoother and flatter. This is especially important for some applications that require high surface quality (such as optical devices and electronic devices).
[0019] Compared with the prior art, the present invention has the following beneficial technical effects: The method and device for thermal pulse processing of oxide semiconductor films described in the present invention, wherein the method can firstly accurately control the oxygen vacancy concentration, and by using a relay to control the pneumatic valve and the arc ignition module, the processing time and frequency can be accurately controlled, thereby accurately controlling the concentration of oxygen vacancies, avoiding the problem of being unable to accurately control in traditional processing methods.
[0020] Secondly, by placing the sample on an aluminum alloy metal substrate and keeping the substrate temperature below 100°C, potential thermal damage to the film substrate through "heat pulses" is effectively avoided, improving the safety and stability of the treatment. At the same time, the heat pulse treatment technology can achieve rapid surface annealing at nearly 1000°C, which is more efficient than traditional high-temperature atmosphere annealing, saving time and energy.
[0021] Furthermore, the use of a multi-pulse annealing strategy can ensure complete crystallization of the film, improving the treatment effect and stability.
[0022] Finally, the method and device of the present invention are not only carried out in an open environment, but the thermal pulse treatment technology is carried out in an open environment, the substrate temperature exceeds 800°C, but the temperature is kept below 100°C at a depth of 200 nm, which helps to maintain stable operation of the equipment. Moreover, the selected flamethrower has different aperture sizes to meet the requirements of flame range for samples of different sizes. BRIEF DESCRIPTION OF THE DRAWINGS
[0023] Figure 1 It is a schematic structural diagram of the device for thermal pulse processing of oxide semiconductor thin film according to the present invention; Figure 2 This is a performance test diagram of sample 3# in Example 3 of the present invention; Figure 3 This is a performance test diagram of the sample to be processed according to the present invention.
[0024] Among them: 1. Hydrogen and oxygen generator, 2. Pipeline, 3. Flame spray gun, 4. Iron frame, 5. Relay, 6. Pneumatic valve, 7. Arc ignition module, 8. Anti-backfire valve, 9. Metal substrate. DETAILED DESCRIPTION
[0025] In order to have a clearer understanding of the technical features, purposes and effects of the present invention, the specific implementation methods of the present invention are now described in detail with reference to the accompanying drawings. The described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention. If the specific conditions are not specified in the specific implementation methods, they shall be carried out according to the conventional conditions or the conditions recommended by the manufacturer.
[0026] When the following description refers to the drawings, unless otherwise indicated, the same numbers in different drawings represent the same or similar elements. The embodiments described in the following exemplary embodiments do not represent all embodiments consistent with the present disclosure. Instead, they are merely examples of methods and devices consistent with some aspects of the present disclosure as detailed in the appended claims. The terms used in the present disclosure are only for the purpose of describing specific embodiments and are not intended to limit the present disclosure.
[0027] The present invention is further described in detail below in conjunction with specific embodiments. Specific implementation method one:
[0028] A method for thermal pulse treatment of an oxide semiconductor film, the method is thermal pulse annealing based on a hydrogen-oxygen generator, placing a sample to be treated on a metal substrate in an open environment, performing N thermal pulse annealings to obtain a treated sample, and 9≤N≤15, the temperature of the thermal pulse annealing is 800~1000°C, the duration of the thermal pulse annealing treatment is 0.5~1s, and the frequency of the thermal pulse annealing is 0.5~1 Hz; The sample to be processed is an oxide semiconductor film to be processed, the oxygen vacancy concentration in the sample to be processed is n1, and the oxygen vacancies are evenly distributed, n1<38%; The treated sample is an oxide semiconductor film that has been annealed. The oxygen vacancy concentration of the surface film of the treated sample is n2, the thickness of the surface film is d, and satisfies 40%≤n2≤55%, d<10nm.
[0029] In some other embodiments, the grain size of the surface of the sample to be processed is 0.48-0.52 nm; the grain size of the surface film is 9-13.6 nm.
[0030] In some other embodiments, the oxygen vacancy concentration n2 of the surface film of the treated sample satisfies: n2=k*3N+n1; and 0.3≤k≤0.4.
[0031] In some other embodiments, the thickness of the sample to be processed ranges from 80 to 110 nm.
[0032] In some other embodiments, after placing the sample to be processed on a metal substrate in an open environment and before starting the thermal pulse annealing, first check whether the power supply of the hydrogen-oxygen generator is normal, and select the corresponding nozzle according to the size of the sample to be processed; then check the relay to ensure that the start valve is opened when the relay is at a high level and the valve is closed when the relay is at a low level; finally, set the torch handle to the normally open state.
[0033] In some other embodiments, the thermal pulse annealing specifically includes: first opening the pneumatic valve and the relay, controlling the pneumatic valve and the arc ignition module through the relay so that the flamethrower emits a pulse flame, performing thermal pulse annealing on the sample to be processed placed on the metal substrate, and closing the relay after reaching a specified duration; completing the entire thermal pulse annealing process according to the set thermal pulse annealing temperature, duration, frequency and number of times. Specific implementation method 2:
[0034] A device for thermal pulse processing of oxide semiconductor thin films, such as Figure 1As shown, the device is based on the method for thermal pulse processing of oxide semiconductor film described in any of the above items, and the device includes a hydrogen and oxygen generator 1, a flamethrower 3 connected to the hydrogen and oxygen generator 1 through a pipeline 2, and an iron frame 4. A relay 5 is also provided on the pipeline 2, and a pneumatic valve 6 is also provided on the pipeline 2 between the hydrogen and oxygen generator 1 and the relay 5; an arc ignition module 7 is also provided at the flamethrower, and a metal substrate 9 with adjustable height is also provided on the iron frame 4.
[0035] In some other embodiments, an anti-flashback valve 8 is further provided on the pipeline 2 between the oxyhydrogen generator 1 and the pneumatic valve 6 .
[0036] In some other embodiments, the flamethrower 3 includes a nozzle and a handle.
[0037] In some other embodiments, the hydrogen-oxygen generator 1 can produce hydrogen and oxygen in a ratio of 2:1, and can be used immediately upon startup and produced on demand. The hydrogen-oxygen generator 1 is equipped with sodium hydroxide having a concentration higher than 99.5%. Embodiment 1:
[0038] The present invention provides a method for thermal pulse processing of an oxide semiconductor film.
[0039] Specifically, the device for thermal pulse treatment of oxide semiconductor thin film in the second specific embodiment is adopted. In this embodiment 1, an anti-flashback valve 8 is also provided on the pipeline 2 between the hydrogen and oxygen generator 1 and the pneumatic valve 6. The flamethrower 3 includes a nozzle and a grip. The hydrogen and oxygen generator 1 can produce hydrogen and oxygen in a ratio of 2:1, and can be used immediately after startup and produced on demand. The hydrogen and oxygen generator 1 is equipped with sodium hydroxide with a concentration higher than 99.5%.
[0040] In this embodiment 1, the hydrogen-oxygen generator 1 and the anti-flashback valve 8 are from Henan Hanhao Technology Co., Ltd., model HG2200B; the relay 5 is risym, model: 4-way 6V, supporting high and low level trigger relays; the pneumatic valve 6 is manufactured by Lubos, 3V210-08-DC12V; the flamethrower 3 is manufactured by Hunan Walker Energy Technology Co., Ltd., model: 1.8 mm; the arc ignition module 7 is manufactured by zava, model: 1000KV high-voltage module. The pipeline 2 uses a PVC pressure-resistant and corrosion-resistant air pipe with an outer diameter of 6 and an inner diameter of 4. The anti-flashback valve 8 is a flashback valve for water welding machines, which can effectively resist accidental flashback during operation and flashback caused by the hydrogen-oxygen mixture pressure being as low as zero after the operation; the pneumatic valve 6 is a one-inlet and one-outlet DC 12V electromagnetic pneumatic valve; the external relay 5 is a 4-way 5V relay; the arc ignition module 7 can generate a high-energy arc, generate a high-temperature arc between the two poles by rapid discharge, and is placed in front of the flamethrower 3; the nozzle of the flamethrower 3 is connected to the pipe 2, and the nozzle has different aperture parameters, and common nozzle sizes are 0.5mm, 1mm, and 1.5mm.
[0041] In this embodiment 1, the metal substrate 9 is an aluminum alloy substrate with a thickness of 1 cm and a size of 10×10 cm; the iron stand 4 used is 40 cm high and is used to fix various parts to avoid experimental errors. The thickness of the sample to be processed is 90 nm of amorphous gallium oxide. The sample to be processed is an oxide semiconductor film to be processed, and the oxygen vacancy concentration in the sample to be processed is n1, and the oxygen vacancies are uniformly distributed, n1<38%.
[0042] The method is based on the thermal pulse annealing of the hydrogen and oxygen generator. The sample to be processed is placed on the metal substrate in an open environment. After the sample to be processed is placed on the metal substrate in the open environment and before the thermal pulse annealing is started, firstly check whether the power supply of the hydrogen and oxygen generator is normal, and select the corresponding nozzle according to the size of the sample to be processed; then check the relay to ensure that the start valve is opened when the relay is at a high level and the valve is closed when the relay is at a low level; finally, set the torch handle to a normally open state.
[0043] Then, N times of heat pulse annealing are performed to obtain a treated sample, and 9≤N≤15, the temperature of the heat pulse annealing is 800-1000° C., the duration of the heat pulse annealing treatment is 0.5-1 s, and the frequency of the heat pulse annealing is 0.5-1 Hz; The thermal pulse annealing specifically includes: firstly, opening the pneumatic valve and the relay, controlling the pneumatic valve and the arc ignition module through the relay so that the flamethrower emits a pulse flame, performing thermal pulse annealing on the sample to be processed placed on the metal substrate, and closing the relay after reaching the specified duration; completing the entire thermal pulse annealing process according to the set thermal pulse annealing temperature, duration, frequency and number of times.
[0044] In this embodiment 1, N is 9, the treated sample is sample 1#, sample 1# is an oxide semiconductor film that has completed annealing, the oxygen vacancy concentration of the surface film of sample 1# is n2, and the thickness of the surface film is d, see Table 1 for details. Embodiment 2:
[0045] The only difference between Example 2 and Example 1 is that N is 12 and the treated sample is sample #2. Embodiment 3:
[0046] The difference between Example 3 and Example 1 is that N is 15, the treated sample is sample 3#, and the test results are as follows: Figure 2 The test results of the samples to be processed are shown in Figure 3 shown.
[0047] Comparative Example 1: The difference between this comparative example 1 and example 1 is that N is 18 and the treated sample is sample 4#.
[0048] Comparative Example 2: The only difference between Comparative Example 2 and Example 1 is that the duration of the thermal pulse annealing treatment is too long, which is 1.5 seconds, and the sample after the treatment is sample 5#.
[0049] Comparative Example 3: The only difference between Comparative Example 3 and Example 1 is that the frequency of the thermal pulse annealing is too fast, specifically 1.5 Hz, and the treated sample is sample 6#.
[0050] Comparative Example 4: The difference between this comparative example 4 and example 1 is that N is 3 and the treated sample is sample #7.
[0051] Comparative Example 5: The difference between this comparative example 5 and example 1 is that N is 6 and the treated sample is sample #8.
[0052] Table 1 Test results of Examples 1 to 3 and Comparative Examples 1 to 5:
[0053] The present invention is described by the above specific embodiments, and those skilled in the art should understand that various changes and equivalent substitutions can be made to the present invention without departing from the scope of the present invention. The parts not described in detail in the present specification are well-known technologies to those skilled in the art. In addition, various modifications can be made to the present invention for specific situations or specific circumstances without departing from the scope of this new use. Therefore, the present invention is not limited to the disclosed specific embodiments, but should include all implementation methods falling within the scope of the claims of the present invention.
Claims
1. A method for thermal pulse treatment of an oxide semiconductor film, It is characterized in that The method is based on thermal pulse annealing of a hydrogen-oxygen generator, wherein a sample to be processed is placed on a metal substrate in an open environment, and N thermal pulse annealings are performed to obtain a processed sample, and 9≤N≤15, wherein the temperature of the thermal pulse annealing is 800-1000°C, the duration of the thermal pulse annealing is 0.5-1s, and the frequency of the thermal pulse annealing is 0.5-1 Hz; The sample to be processed is an oxide semiconductor film to be processed, the oxygen vacancy concentration in the sample to be processed is n1, and the oxygen vacancies are evenly distributed, n1<38%; The treated sample is an oxide semiconductor film that has been annealed. The oxygen vacancy concentration of the surface film of the treated sample is n2, the thickness of the surface film is d, and satisfies 40%≤n2≤55%, d<10nm.
2. The method according to claim 1, It is characterized in that The grain size of the surface of the sample to be processed is 0.48-0.52 nm; the grain size of the surface film is 9-13.6 nm.
3. The method according to claim 2, It is characterized in that The oxygen vacancy concentration n2 of the surface film of the sample after the treatment satisfies: n2=k*3N+n1; and 0.3≤k≤0.
4.
4. The method according to claim 3, It is characterized in that The thickness of the sample to be processed ranges from 80 to 110 nm.
5. The method according to claim 4, It is characterized in that After placing the sample to be processed on a metal substrate in an open environment and before starting thermal pulse annealing, first check whether the power supply of the oxyhydrogen generator is normal, and select the corresponding nozzle according to the size of the sample to be processed; then check the relay to ensure that the start valve is open when the relay is at a high level and the valve is closed when the relay is at a low level; finally, set the torch handle to the normally open state.
6. The method according to claim 5, It is characterized in that The thermal pulse annealing specifically includes: firstly, opening the pneumatic valve and the relay, controlling the pneumatic valve and the arc ignition module through the relay so that the flamethrower emits a pulse flame, performing thermal pulse annealing on the sample to be processed placed on the metal substrate, and closing the relay after reaching the specified duration; completing the entire thermal pulse annealing process according to the set thermal pulse annealing temperature, duration, frequency and number of times.
7. A device for thermal pulse treatment of oxide semiconductor thin films, It is characterized in that The device is based on the method for thermal pulse treatment of an oxide semiconductor film according to any one of claims 1 to 6, and comprises an oxyhydrogen generator (1), a flamethrower (3) connected to the oxyhydrogen generator (1) through a pipeline (2), and an iron frame (4); a relay (5) is also provided on the pipeline (2); a pneumatic valve (6) is also provided on the pipeline (2) between the oxyhydrogen generator (1) and the relay (5); an arc ignition module (7) is also provided at the flamethrower, and a metal substrate (9) capable of adjusting the height is also provided on the iron frame (4).
8. The device according to claim 7, It is characterized in that An anti-flashback valve (8) is also provided on the pipeline (2) between the oxyhydrogen generator (1) and the pneumatic valve (6).
9. The device according to claim 8, It is characterized in that The flamethrower (3) comprises a nozzle and a handle.
10. The device according to claim 9, It is characterized in that The hydrogen-oxygen generator (1) is capable of generating hydrogen and oxygen in a ratio of 2:1 and is ready for use upon startup and produces on demand. The hydrogen-oxygen generator (1) is provided with sodium hydroxide having a concentration higher than 99.5%.