Processing method of light-transmitting cadmium telluride power generation glass
By using linear laser and diffraction optical components for light transmission processing in cadmium telluride power glass, the problems of low processing efficiency and poor electrical performance in the existing technology are solved, and high transparency, neat edges and improved electrical performance are achieved. Effect.
Patent Information
- Application Number
- CN202411076374.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-07
- Publication Date
- 2024-11-22
AI Technical Summary
In the light-transmitting processing of existing cadmium telluride power glass, there are problems such as low processing efficiency, poor brightness, many edge burrs, obvious splicing color difference and difficult to control thermal influence, resulting in poor electrical performance and appearance effects.
Linear laser is used for light transmission processing, combined with diffraction optical component shaping, select the appropriate laser power and frequency, and use specific red phosphor to encapsulate materials to improve the photoelectric conversion effect.
It improves processing rate and transparency, ensures neat edges, reduces the risk of short circuits, eliminates splicing color difference, improves electrical performance and appearance effects, and has uniform energy distribution and small thermal impact.
Smart Images

Figure CN119008767A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of cadmium telluride power generation glass, and in particular to a processing method of light-transmitting cadmium telluride power generation glass. Background Art
[0002] With the deterioration of the global environment and the increase in energy consumption, especially when building energy consumption accounts for a relatively large proportion, various countries have vigorously developed clean energy, among which the development of photovoltaic buildings has gradually become the main target, that is, to reduce building energy consumption and improve living comfort. In the current BIPV application, cadmium telluride power generation glass hollow applications are relatively widespread, but the translucent cadmium telluride power generation glass currently used is basically processed by laser circular spot splicing, so the main problems are insufficient head brightness and poor appearance consistency of the translucent chip.
[0003] The existing thin-film batteries, including cadmium telluride power generation glass, are basically processed by laser processing or acid etching. Solution etching is basically not used because of narrow process window, pollution and other problems. However, the laser method generally uses a circular spot and Gaussian light.
[0004] It can be seen that the existing technology has the following disadvantages: (1) Single spot superposition, low processing efficiency, affecting production capacity; (2) After etching, the transparency of the power generation glass is poor and the whole is yellow; (3) There are many burrs on the processing edge, which can easily cause short circuits and affect electrical performance; (4) After processing, the appearance is prone to obvious problems such as splicing color difference; (5) Due to the use of Gaussian light, the etching depth and thermal impact are difficult to control, affecting electrical performance. Summary of the invention
[0005] The purpose of the present invention is to solve at least one of the technical problems existing in the prior art and to provide a method for processing light-transmitting cadmium telluride power generation glass.
[0006] The technical solution of the present invention is as follows:
[0007] A method for processing light-transmitting cadmium telluride power generation glass comprises the following steps:
[0008] The substrate is sequentially plated with a light absorption layer, laser-scribed lines P1, filled with photoresist, laser-scribed lines P2, plated with a back electrode, laser-scribed lines P3, laser-cleaned edges P4, laser-transmitted P5, and packaged to obtain a cadmium telluride power generation glass;
[0009] Among them, the laser transparent P5 is processed by linear laser.
[0010] As a preferred solution of the present invention, the linear laser adopts a picosecond green laser with a wavelength of 532 nanometers.
[0011] As a preferred solution of the present invention, the laser light transmission P5 adopts a diffraction optical element DOE method to perform laser shaping to obtain a flat-top linear laser.
[0012] As a preferred solution of the present invention, in the laser light transmittance P5, the laser power is selected to be 100W and the frequency is selected to be 100-150KHz.
[0013] As a preferred embodiment of the present invention, in the laser light transmission P5, the linear laser length is ≥200 mm.
[0014] As a preferred solution of the present invention, in the laser light transmittance P5, the linear laser line width is 100um to 200um.
[0015] As a preferred embodiment of the present invention, in the laser light transmission P5, the processing speed of the linear laser is 1500 mm / s to 3000 mm / s.
[0016] As a preferred embodiment of the present invention, in the laser light-transmitting P5, the height of the linear laser processing is 250 mm to 400 mm.
[0017] As a preferred embodiment of the present invention, the encapsulation adopts EVA film, and its preparation method is as follows: 80-90 parts by weight of ethylene-vinyl acetate copolymer, 0.5-3 parts by weight of cross-linking agent, 3-6 parts by weight of red phosphor, 0.5-1 parts by weight of silane coupling agent, 0.5-3 parts by weight of filler, 0.5-1 parts by weight of surfactant and 0.5-2 parts by weight of light stabilizer are mixed and cross-linked to obtain the obtained product.
[0018] As a preferred embodiment of the present invention, the preparation method of the red phosphor is:
[0019] According to the molar ratio of lithium carbonate, yttrium oxide, germanium oxide and bismuth oxide of 1:0.995:2:0.005, the raw materials are respectively ground and mixed, dried and then put into an alumina crucible, sintered at 800-900°C in an air atmosphere for 1-5 hours in a high-temperature furnace, and cooled to room temperature with the furnace to obtain a precursor material. The mixed precursor is fully ground and mixed again, dried and put into an alumina crucible, put into a high-temperature furnace, sintered at 1100-1200°C in an air atmosphere for 4-8 hours, cooled to room temperature with the furnace, taken out and ground evenly to obtain.
[0020] The beneficial effects of the present invention are:
[0021] (1) The present invention uses a linear laser to perform light-transmitting processing on cadmium telluride power generation glass, and the processing speed is high.
[0022] (2) The present invention adopts linear laser processing, which has good processing effect, high brightness and is suitable for curtain wall applications.
[0023] (3) The present invention adopts linear laser processing, the processing edge is neat, there is no edge burst, etc., and the risk of short circuit is small.
[0024] (4) The present invention uses linear laser processing to achieve a good appearance effect without any color difference between light and dark splicing.
[0025] (5) The linear laser of the present invention is shaped into a flat-top light, which has uniform energy distribution, small thermal impact, and improved electrical performance.
[0026] (6) The linear laser used in the present invention has the advantages of high brightness, high contrast, and long life.
[0027] (7) The packaging film used in the present invention can absorb a wide band of ultraviolet light and infrared light when in use by adding specific red light phosphors, thereby improving its photoelectric conversion effect. BRIEF DESCRIPTION OF THE DRAWINGS
[0028] Figure 1 The figure is a process flow chart of the cadmium telluride power generation glass of the present invention. DETAILED DESCRIPTION
[0029] The embodiments of the present invention are described in detail below. The embodiments described below are exemplary and are only used to explain the present invention, and should not be construed as limiting the present invention. If no specific techniques or conditions are specified in the embodiments, the techniques or conditions described in the literature in this area or the product specifications are used. The reagents or instruments used that do not specify the manufacturer are all conventional products that can be obtained commercially.
[0030] In the following embodiments, the light absorption layer is a PN node layer composed of cadmium telluride and cadmium selenide, with thicknesses of 4um and 150nm respectively; the coating temperature is 700℃; the laser line P1 adopts ultraviolet nanosecond, the frequency is 200khz, the total power is 50W, and the overlap rate is controlled at about 50%. The photoresist filling wet film thickness is 20um, the baking temperature is 100℃, and the developer adopts hydrogen peroxide. The laser lines P2 and P3 adopt green light nanosecond, the total power is 20W, and the frequency is 100khz. The back electrode adopts metal molybdenum, the coating thickness is 20nm and 300nm respectively, and the square resistance is less than 1Ω / □; the laser edge cleaning adopts infrared nanosecond, the total power is 2000W, and the frequency is above 500khz.
[0031] Example 1
[0032] A method for processing light-transmitting cadmium telluride power generation glass comprises the following steps:
[0033] The substrate (glass substrate) is sequentially plated with a light absorption layer, laser lined P1, photoresist filled, laser lined P2, back electrode plated, laser lined P3, laser edge cleaning P4, laser light transmission P5 and packaged to obtain cadmium telluride power generation glass, refer to Figure 1 ;
[0034] Among them, the laser transparent P5 is processed by linear laser.
[0035] The linear laser uses a picosecond green laser with a wavelength of 532 nanometers.
[0036] Laser Transparent P5 uses diffractive optical element DOE to perform laser shaping to obtain flat-top linear laser.
[0037] In the laser light transmittance P5, the laser power is selected as 100W and the frequency is selected as 110KHz.
[0038] In laser transparent P5, the linear laser length is ≥200mm.
[0039] In the laser transparent P5, the linear laser line width is 189um.
[0040] In the laser transparent P5, the processing speed of the linear laser is 1500mm / s.
[0041] In the laser transparent P5, the height of the linear laser processing is 280mm.
[0042] Example 2
[0043] A method for processing light-transmitting cadmium telluride power generation glass comprises the following steps:
[0044] The substrate is sequentially plated with a light absorption layer, laser lined P1, photoresist filled, laser lined P2, back electrode plated, laser lined P3, laser edge cleaning P4, laser light transmission P5 and packaged to obtain cadmium telluride power generation glass, refer to Figure 1 ;
[0045] Among them, the laser transparent P5 is processed by linear laser.
[0046] The linear laser uses a picosecond green laser with a wavelength of 532 nanometers.
[0047] Laser Transparent P5 uses diffractive optical element DOE to perform laser shaping to obtain flat-top linear laser.
[0048] In the laser light transmittance P5, the laser power is selected as 100W and the frequency is selected as 110KHz.
[0049] In laser transparent P5, the linear laser length is ≥200mm.
[0050] In the laser transparent P5, the linear laser line width is 120um.
[0051] In the laser transparent P5, the processing speed of the linear laser is 1600mm / s.
[0052] In the laser transparent P5, the height of the linear laser processing is 250mm.
[0053] Example 3
[0054] A method for processing light-transmitting cadmium telluride power generation glass comprises the following steps:
[0055] The substrate is sequentially plated with a light absorption layer, laser lined P1, photoresist filled, laser lined P2, back electrode plated, laser lined P3, laser edge cleaning P4, laser light transmission P5 and packaged to obtain cadmium telluride power generation glass, refer to Figure 1 ;
[0056] Among them, the laser transparent P5 is processed by linear laser.
[0057] The linear laser uses a picosecond green laser with a wavelength of 532 nanometers.
[0058] Laser Transparent P5 uses diffractive optical element DOE to perform laser shaping to obtain flat-top linear laser.
[0059] In the laser light transmittance P5, the laser power is selected as 100W and the frequency is selected as 110KHz.
[0060] In laser transparent P5, the linear laser length is ≥200mm.
[0061] In the laser transparent P5, the linear laser line width is 160um.
[0062] In the laser transparent P5, the processing speed of the linear laser is 1900mm / s.
[0063] In the laser transparent P5, the height of the linear laser processing is 280mm.
[0064] Example 4
[0065] A method for processing light-transmitting cadmium telluride power generation glass comprises the following steps:
[0066] The substrate is sequentially plated with a light absorption layer, laser lined P1, photoresist filled, laser lined P2, back electrode plated, laser lined P3, laser edge cleaning P4, laser light transmission P5 and packaged to obtain cadmium telluride power generation glass, refer to Figure 1 ;
[0067] Among them, the laser transparent P5 is processed by linear laser.
[0068] The linear laser uses a picosecond green laser with a wavelength of 532 nanometers.
[0069] Laser Transparent P5 uses diffractive optical element DOE to perform laser shaping to obtain flat-top linear laser.
[0070] In the laser light transmittance P5, the laser power is selected as 100W and the frequency is selected as 110KHz.
[0071] In laser transparent P5, the linear laser length is ≥200mm.
[0072] In the laser transparent P5, the linear laser line width is 150um.
[0073] In the laser transparent P5, the processing speed of the linear laser is 2500mm / s.
[0074] In the laser transparent P5, the height of the linear laser processing is 300mm.
[0075] Example 5
[0076] A method for processing light-transmitting cadmium telluride power generation glass comprises the following steps:
[0077] The substrate is sequentially plated with a light absorption layer, laser lined P1, photoresist filled, laser lined P2, back electrode plated, laser lined P3, laser edge cleaning P4, laser light transmission P5 and packaged to obtain cadmium telluride power generation glass, refer to Figure 1 ;
[0078] Among them, the laser transparent P5 is processed by linear laser.
[0079] The linear laser uses a picosecond green laser with a wavelength of 532 nanometers.
[0080] Laser Transparent P5 uses diffractive optical element DOE to perform laser shaping to obtain flat-top linear laser.
[0081] In the laser light transmittance P5, the laser power is selected as 100W and the frequency is selected as 110KHz.
[0082] In laser transparent P5, the linear laser length is ≥200mm.
[0083] In the laser transparent P5, the linear laser line width is 200um.
[0084] In the laser transparent P5, the processing speed of the linear laser is 3000mm / s.
[0085] In the laser transparent P5, the height of the linear laser processing is 400mm.
[0086] Example 6
[0087] A method for processing light-transmitting cadmium telluride power generation glass comprises the following steps:
[0088] The substrate is sequentially plated with a light absorption layer, laser lined P1, photoresist filled, laser lined P2, back electrode plated, laser lined P3, laser edge cleaning P4, laser light transmission P5 and packaged to obtain cadmium telluride power generation glass, refer to Figure 1 ;
[0089] Among them, the laser transparent P5 is processed by linear laser.
[0090] The linear laser uses a picosecond green laser with a wavelength of 532 nanometers.
[0091] Laser Transparent P5 uses diffractive optical element DOE to perform laser shaping to obtain flat-top linear laser.
[0092] In the laser light transmittance P5, the laser power is selected as 100W and the frequency is selected as 120KHz.
[0093] In laser transparent P5, the linear laser length is ≥200mm.
[0094] In the laser transparent P5, the linear laser line width is 200um.
[0095] In the laser transparent P5, the processing speed of the linear laser is 3000mm / s.
[0096] In the laser transparent P5, the height of the linear laser processing is 400mm.
[0097] Example 7
[0098] A method for processing light-transmitting cadmium telluride power generation glass comprises the following steps:
[0099] The substrate is sequentially plated with a light absorption layer, laser lined P1, photoresist filled, laser lined P2, back electrode plated, laser lined P3, laser edge cleaning P4, laser light transmission P5 and packaged to obtain cadmium telluride power generation glass, refer to Figure 1 ;
[0100] Among them, the laser transparent P5 is processed by linear laser.
[0101] The linear laser uses a picosecond green laser with a wavelength of 532 nanometers.
[0102] Laser Transparent P5 uses diffractive optical element DOE to perform laser shaping to obtain flat-top linear laser.
[0103] In the laser light transmittance P5, the laser power is selected as 100W and the frequency is selected as 130KHz.
[0104] In laser transparent P5, the linear laser length is ≥200mm.
[0105] In the laser transparent P5, the linear laser line width is 200um.
[0106] In the laser transparent P5, the processing speed of the linear laser is 3000mm / s.
[0107] In the laser transparent P5, the height of the linear laser processing is 400mm.
[0108] Example 8
[0109] A method for processing light-transmitting cadmium telluride power generation glass comprises the following steps:
[0110] The substrate is sequentially plated with a light absorption layer, laser lined P1, photoresist filled, laser lined P2, back electrode plated, laser lined P3, laser edge cleaning P4, laser light transmission P5 and packaged to obtain cadmium telluride power generation glass, refer to Figure 1 ;
[0111] Among them, the laser transparent P5 is processed by linear laser.
[0112] The linear laser uses a picosecond green laser with a wavelength of 532 nanometers.
[0113] Laser Transparent P5 uses diffractive optical element DOE to perform laser shaping to obtain flat-top linear laser.
[0114] In the laser light transmittance P5, the laser power is selected as 100W and the frequency is selected as 140KHz.
[0115] In laser transparent P5, the linear laser length is ≥200mm.
[0116] In the laser transparent P5, the linear laser line width is 200um.
[0117] In the laser transparent P5, the processing speed of the linear laser is 3000mm / s.
[0118] In the laser transparent P5, the height of the linear laser processing is 400mm.
[0119] Example 9
[0120] A method for processing light-transmitting cadmium telluride power generation glass comprises the following steps:
[0121] The substrate is sequentially plated with a light absorption layer, laser lined P1, photoresist filled, laser lined P2, back electrode plated, laser lined P3, laser edge cleaning P4, laser light transmission P5 and packaged to obtain cadmium telluride power generation glass, refer to Figure 1 ;
[0122] Among them, the laser transparent P5 is processed by linear laser.
[0123] The linear laser uses a picosecond green laser with a wavelength of 532 nanometers.
[0124] Laser Transparent P5 uses diffractive optical element DOE to perform laser shaping to obtain flat-top linear laser.
[0125] In the laser light transmittance P5, the laser power is selected as 100W and the frequency is selected as 150KHz.
[0126] In laser transparent P5, the linear laser length is ≥200mm.
[0127] In the laser transparent P5, the linear laser line width is 200um.
[0128] In the laser transparent P5, the processing speed of the linear laser is 3000mm / s.
[0129] In the laser transparent P5, the height of the linear laser processing is 400mm.
[0130] Example 10
[0131] A method for processing light-transmitting cadmium telluride power generation glass comprises the following steps:
[0132] The substrate is sequentially plated with a light absorption layer, laser lined P1, photoresist filled, laser lined P2, back electrode plated, laser lined P3, laser edge cleaning P4, laser light transmission P5 and packaged to obtain cadmium telluride power generation glass, refer to Figure 1 ;
[0133] Among them, the laser transparent P5 is processed by linear laser.
[0134] The linear laser uses a picosecond green laser with a wavelength of 532 nanometers.
[0135] Laser Transparent P5 uses diffractive optical element DOE to perform laser shaping to obtain flat-top linear laser.
[0136] In the laser light transmittance P5, the laser power is selected as 100W and the frequency is selected as 110KHz.
[0137] In laser transparent P5, the linear laser length is ≥200mm.
[0138] In laser transparent P5, the linear laser line width is 100um.
[0139] In the laser transparent P5, the processing speed of the linear laser is 3000mm / s.
[0140] In the laser transparent P5, the height of the linear laser processing is 400mm.
[0141] Embodiment 11
[0142] A method for processing light-transmitting cadmium telluride power generation glass comprises the following steps:
[0143] The substrate is sequentially plated with a light absorption layer, laser lined P1, photoresist filled, laser lined P2, back electrode plated, laser lined P3, laser edge cleaning P4, laser light transmission P5 and packaged to obtain cadmium telluride power generation glass, refer to Figure 1 ;
[0144] Among them, the laser transparent P5 is processed by linear laser.
[0145] The linear laser uses a picosecond green laser with a wavelength of 532 nanometers.
[0146] Laser Transparent P5 uses diffractive optical element DOE to perform laser shaping to obtain flat-top linear laser.
[0147] In the laser light transmittance P5, the laser power is selected as 100W and the frequency is selected as 110KHz.
[0148] In laser transparent P5, the linear laser length is ≥200mm.
[0149] In the laser transparent P5, the linear laser line width is 150um.
[0150] In the laser transparent P5, the processing speed of the linear laser is 3000mm / s.
[0151] In the laser transparent P5, the height of the linear laser processing is 400mm.
[0152] Example 12
[0153] This embodiment is carried out on the basis of Embodiment 11. Specifically, EVA film is used for encapsulation, and its preparation method is as follows: 85 parts by weight of ethylene-vinyl acetate copolymer (VA content is 38%), 1 part by weight of cross-linking agent (2,5-dimethyl-2,5-di-tert-butyl peroxide hexane), 4 parts by weight of red phosphor, 0.7 parts by weight of silane coupling agent (vinyl triethoxysilane), 1.2 parts by weight of filler (whisker silicon carbide), 0.8 parts by weight of surfactant (a mixture of betaine and polysorbate in a ratio of 1:1 by mass) and 0.9 parts by weight of light stabilizer (2,4-dihydroxybenzophenone) are mixed and cross-linked to obtain the obtained product.
[0154] Preparation method of red phosphor:
[0155] According to the molar ratio of lithium carbonate, yttrium oxide, germanium oxide and bismuth oxide of 1:0.995:2:0.005, the raw materials are respectively ground, mixed and dried, and then put into an alumina crucible, sintered at 850°C for 3 hours in a high-temperature furnace in an air atmosphere, and cooled to room temperature with the furnace to obtain a precursor material. The mixed precursor is fully ground, mixed and dried again, and then put into an alumina crucible, put into a high-temperature furnace, sintered at 1180°C in an air atmosphere for 6 hours, cooled to room temperature with the furnace, taken out and ground evenly to obtain
[0156] Comparative Example 1
[0157] The difference from Example 1 is that a point laser is used (11 samples are taken and the following tests are carried out respectively).
[0158] Comparative Example 2
[0159] Different from Example 12, no red phosphor is added.
[0160] The above embodiments and comparative examples were subjected to performance tests, and the test results are shown in Tables 1 and 2.
[0161] Table 1 Performance test results of embodiments and comparative examples
[0162]
[0163] Table 2 Performance test results of embodiments and comparative examples
[0164] Light transmittance power VOC Isc FF Beat(s) Thermal impact(um) Etching method 20% 247.3 189.0 1.88 0.72 110 ≤3 Linear laser (Example 6) 20% 247.1 190.2 1.89 0.72 110 ≤3 Linear laser (Example 7) 20% 247.5 180.3 1.88 0.72 110 ≤3 Linear laser (Example 8) 20% 247.5 179.8 1.99 0.72 110 ≤3 Linear laser (Example 9) 20% 246.9 181.3 1.83 0.72 110 ≤3 Linear laser (Example 10) 20% 247.3 177.9 1.89 0.72 110 ≤3 Linear laser (Example 11) 20% 239.7 187.5 1.80 0.71 160 ±15 Point Laser 20% 238.6 188.4 1.82 0.71 160 ±15 Point Laser 20% 240.0 188.7 1.80 0.71 160 ±15 Point Laser 20% 239.4 188.3 1.77 0.71 160 ±15 Point Laser 20% 239.5 188.6 1.80 0.71 160 ±15 Point Laser
[0165] The above performance tests are conducted using an internationally accepted IV tester with a standard light intensity of 1000W / ㎡ and a temperature of 25±2℃), transmittance (the transmittance can be obtained by testing the ratio of the transparent area to the non-transparent area under a microscope); cycle time (the time from film input to film output); and thermal influence (tested under a microscope).
[0166] Tables 1 and 2 show that, under the condition of ensuring the same transmittance, the linear photolithography is obviously better than the point laser in terms of thermal impact, power performance and beat. That is, the performance of the embodiment is better than the comparative example, that is, the linear laser processing method is better than the point laser processing method. The linear laser is shaped into a flat top light, the energy distribution is uniform, the thermal impact is small, and the electrical performance is improved. Moreover, through linear laser processing, the appearance effect is good, and the embodiment does not have the problem of light and dark splicing color difference.
[0167] The performance of the EVA films of Example 12 and Comparative Example 2 were compared and tested, and the test results are shown in Table 3.
[0168] Table 3 Performance comparison results of Example 12 and Comparative Example 2 samples
[0169] Sample Photoelectric conversion rate Example 12 23.1 Comparative Example 2 20.1
[0170] It can be seen that the photoelectric conversion rate of Example 12 is better than that of Comparative Example 2, which may be mainly due to the addition of specific red light phosphors, which absorb a wide band of ultraviolet light and infrared light, thereby improving its photoelectric conversion effect.
[0171] The above-mentioned embodiments only express the preferred implementation modes of the present invention, and the description thereof is relatively specific and detailed, but it cannot be understood as limiting the scope of the present invention. It should be pointed out that, for ordinary technicians in this field, various other corresponding changes and deformations can be made according to the technical solutions and concepts described above, and all these changes and deformations should fall within the scope of protection of the claims of the present invention.
Claims
1. A method for processing light-transmitting cadmium telluride power generation glass, characterized in that: The following steps are involved: The substrate is sequentially plated with a light absorption layer, laser-scribed lines P1, filled with photoresist, laser-scribed lines P2, plated with a back electrode, laser-scribed lines P3, laser-cleaned edges P4, laser-transmitted P5, and packaged to obtain a cadmium telluride power generation glass; Among them, the laser transparent P5 is processed by linear laser.
2. The method for processing a light-transmitting cadmium telluride power generation glass according to claim 1, characterized in that: The linear laser uses a picosecond green laser with a wavelength of 532 nanometers.
3. The method for processing a light-transmitting cadmium telluride power generation glass according to claim 1, characterized in that: Laser Transparent P5 uses diffractive optical element DOE to perform laser shaping to obtain flat-top linear laser.
4. The method for processing a light-transmitting cadmium telluride power generation glass according to claim 1, characterized in that: In the laser transmittance P5, the laser power is selected as 100W and the frequency is selected as 100~150KHz.
5. The method for processing light-transmitting cadmium telluride power generation glass according to claim 1, characterized in that: In laser transparent P5, the linear laser length is ≥200mm.
6. The method for processing light-transmitting cadmium telluride power generation glass according to claim 1, characterized in that: In laser transparent P5, the linear laser line width is 100um~200um. The method for processing a light-transmitting cadmium telluride power generation glass according to claim 1 is characterized in that, in the laser light transmission P5, the processing speed of the linear laser is 1500 mm / s to 3000 mm / s.
7. The method for processing light-transmitting cadmium telluride power generation glass according to claim 1, characterized in that: In the laser transparent P5, the height of linear laser processing is 250mm~400mm.
8. The method for processing light-transmitting cadmium telluride power generation glass according to claim 1, characterized in that: The encapsulation adopts EVA film, and its preparation method is as follows: 80-90 weight parts of ethylene-vinyl acetate copolymer, 0.5-3 weight parts of cross-linking agent, 3-6 weight parts of red light phosphor, 0.5-1 weight part of silane coupling agent, 0.5-3 weight parts of filler, 0.5-1 weight part of surfactant and 0.5-2 weight parts of light stabilizer are mixed and cross-linked to produce the obtained film.
9. The method for processing light-transmitting cadmium telluride power generation glass according to claim 8, characterized in that: The preparation method of the red phosphor: According to the molar ratio of lithium carbonate, yttrium oxide, germanium oxide and bismuth oxide of 1:0.995:2:0.005, the raw materials are respectively ground and mixed, dried and then put into an alumina crucible, sintered at 800-900°C in an air atmosphere for 1-5 hours in a high-temperature furnace, and cooled to room temperature with the furnace to obtain a precursor material. The mixed precursor is fully ground and mixed again, dried and put into an alumina crucible, put into a high-temperature furnace, sintered at 1100-1200°C in an air atmosphere for 4-8 hours, cooled to room temperature with the furnace, taken out and ground evenly to obtain.