Method for improving poor cloud and mist in laser-assisted sintering, photovoltaic cell and photovoltaic module
Through laser selective etching of the coiled silicon nitride film and the metal electrode elevation slurry that reduces the content of glass powder, combined with laser-assisted sintering and reverse bias, the problem of cloud and mist is solved and the photoelectric conversion efficiency of photovoltaic cells is improved .
Patent Information
- Application Number
- CN202411078627.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-07
- Publication Date
- 2024-11-22
AI Technical Summary
In the existing laser-assisted sintering technology, the reduction in the glass powder content of the metal electrode slurry leads to insufficient corrosion of the dielectric layer on the front edge of the battery cell, resulting in a small initial contact density, which is prone to excessively high carrier passage current, resulting in poor clouds and mist problems. , affecting the improvement of photoelectric conversion efficiency of photovoltaic cells.
The metal electrode elevation slurry with a pulse of 10-18-10-12s and a wavelength of 200-600nm is used to etch the coiled silicon nitride film to reduce the content of glass powder to form the emitter after sintering. Excellent ohmic contact, combined with laser-assisted sintering and reverse bias, ensures contact density and contact quality.
It effectively avoids the problem of bad clouds and mist, improves the photoelectric conversion efficiency of photovoltaic cells, ensures the passivation effect of the passivation and reduction film, and reduces the glass powder content of the metal electrode efficiency slurry, and improves the gain of photoelectric conversion efficiency.
Smart Images

Figure CN119008769A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of new energy technology, and in particular to a method for improving the cloudiness of laser-assisted sintering, a photovoltaic cell and a photovoltaic module. Background Art
[0002] At present, laser-assisted sintering technology has become one of the important means to improve the photoelectric conversion efficiency of TOPCON cells. In the prior art, as shown in publication number CN118398713A, the application method of laser-assisted sintering technology in photovoltaic cells such as TOPCON cells is as follows:
[0003] The metal electrode paste (such as silver paste) printed on the surface of the cell corrodes the dielectric layer (such as the passivation anti-reflection film) during the high-temperature sintering process to form a metal electrode (such as the front electrode), and the metal electrode and the silicon surface (such as the emitter) initially form a contact point; then, laser-assisted sintering technology is used to locally induce photogenerated carriers by scanning the front of the cell with a focused laser beam, and separate free carriers by applying a bias voltage to the cell, thereby causing a high current to pass through the contact point interface, causing the contact point to reach a high temperature locally and quickly perform secondary sintering to promote the diffusion of silver silicon at the contact point, so that the metal electrode forms a good ohmic contact with the silicon surface. In this way, the photoelectric conversion efficiency of photovoltaic cells such as TOPCON cells can be improved.
[0004] At present, further improvement or optimization of the related technologies of laser-assisted sintering metal electrode paste (such as silver paste) is becoming more and more important. The existing improvement directions are mainly focused on: reducing the glass powder content in the metal electrode paste to reduce the gate line resistance of the metal composite and metal electrode, so as to improve the open circuit voltage (Uoc) and fill factor (FF) of the photovoltaic cell, thereby achieving the purpose of further improving the photoelectric conversion efficiency of the photovoltaic cell.
[0005] However, the reduction of glass powder content in metal electrode slurry will inevitably bring about the following disadvantages: due to the problem of silicon nitride film plating at the edge of the front side of the cell, the edge area of the front side of the cell (the thickness of the passivation anti-reflection film in the edge area is usually 90-100nm) is 10-20nm thicker than the middle area of the front side of the cell (the thickness of the passivation anti-reflection film in the middle area is usually 80nm); therefore, during the first high-temperature sintering to form the initial contact points, due to the presence of the plating silicon nitride film, it is easy for the dielectric layer (such as the passivation anti-reflection film) at the edge of the front side of the cell to be insufficiently corroded, resulting in a low density of initial contact points formed at the edge of the front side of the cell; and further during laser-assisted sintering, it is easy for the current in the carrier passage path to be too high, resulting in overburning fog problems at the edge of the front side of the cell, thereby affecting the further improvement of the photoelectric conversion efficiency of the photovoltaic cell. Summary of the invention
[0006] The purpose of the present invention is to overcome the shortcomings of the prior art and provide a method for improving the cloudiness of laser-assisted sintering, a photovoltaic cell and a photovoltaic module.
[0007] Based on this, the present invention discloses a method for improving the cloudiness of laser-assisted sintering, comprising the following steps:
[0008] S1. Prepare a semi-finished cell; wherein the semi-finished cell comprises a silicon substrate and an emitter and a passivation anti-reflection film sequentially stacked on the surface of the silicon substrate, and the edge area of the surface of the passivation anti-reflection film has a silicon nitride film coated around it;
[0009] S2, the pulse is 10 -18 -10 -12 s, and selectively scanning the silicon nitride film with a laser having a wavelength of 200-600 nm to etch a local area of the silicon nitride film;
[0010] S3, printing a metal electrode efficiency-enhancing slurry in the local area; wherein the glass powder content of the metal electrode efficiency-enhancing slurry is 0.5-5%;
[0011] S4, sintering, so that the metal electrode efficiency enhancement slurry corrodes the passivation anti-reflection film during the sintering process to form a first electrode that makes preliminary contact with the emitter;
[0012] S5. Perform laser-assisted sintering on the sintered semi-finished battery cell to form an ohmic contact between the first electrode and the emitter.
[0013] Preferably, in step S2, the laser is a femtosecond ultraviolet laser, and the pulse of the femtosecond ultraviolet laser is 10 -15 s, power is 1-20W, frequency is 100-2000kHz, scanning speed is 10-100m / s, wavelength is 200-400nm.
[0014] Further preferably, the etching depth of the local area of the wrap-around silicon nitride film is 5-80 nm, and the etching width is 5-60 μm.
[0015] Preferably, in step S3, the metal electrode efficiency improvement slurry is a metal electrode efficiency improvement slurry with a small glass powder content, which comprises the following raw materials in percentage by mass: 0.5-3% glass powder, 87-92% silver powder, and 7-10% organic carrier.
[0016] Preferably, step S3 further comprises: a step of locally printing metal electrode paste on another surface of the semi-finished battery cell.
[0017] Further preferably, during the sintering process of step S4, the metal electrode slurry can also form a second electrode that is in ohmic contact with another surface of the semi-finished battery cell locally;
[0018] In step S4, the sintering temperature is 670-740°C.
[0019] Preferably, in step S5, the laser-assisted sintering is performed on the sintered battery cell semi-finished product by laser scanning combined with applying a reverse bias voltage; the laser power is 1-20W, and the reverse bias voltage is 11-17V.
[0020] Preferably, in step S1, the semi-finished cell product further comprises: a passivation contact structure and a second silicon nitride film stacked in sequence on the other surface of the silicon substrate; the passivation contact structure comprises a tunneling oxide layer and a doped polysilicon layer disposed on the tunneling oxide layer;
[0021] The passivation anti-reflection film includes an aluminum oxide film disposed on the surface of the emitter and a first silicon nitride film disposed on the surface of the aluminum oxide film.
[0022] The present invention also discloses a photovoltaic cell, which is manufactured by using the method for improving the poor cloudiness of laser-assisted sintering as described above in the present invention.
[0023] The present invention also discloses a photovoltaic assembly, which comprises the photovoltaic cell described above in the present invention.
[0024] Compared with the prior art, the present invention has at least the following beneficial effects:
[0025] The method for improving the cloudiness of laser-assisted sintering of the present invention comprises: (1) increasing the pulse to 10 -18 -10 -12 s, and the laser selective etching step with a wavelength of 200-600nm can remove the local area of the silicon nitride film coated around the edge, so as to ensure that the printed metal electrode efficiency-enhancing slurry with a low glass powder content can form a first electrode with sufficient contact points with the emitter after sintering and laser-assisted sintering, so that the first electrode and the emitter form an excellent ohmic contact, and effectively avoid the clouding problem on the edge of the photovoltaic cell surface caused by the metal electrode efficiency-enhancing slurry with a low glass powder content after laser-assisted sintering, which can greatly improve the photoelectric conversion efficiency of the photovoltaic cell. (2) Moreover, the use of a pulse of 10 -18 -10 -12s, and the laser with a wavelength of 200-600nm can control the etching depth of the coated silicon nitride film to the nanometer level. The peak power of the laser with the above specific pulse and wavelength is high and the absorption is strong, which has almost no effect on the etching bottom layer and will not cause damage to the passivation anti-reflection film and the silicon surface on the lower surface of the coated silicon nitride film, thereby ensuring the passivation effect of the passivation anti-reflection film. (3) At the same time, adding the step of selectively etching the local area of the coated silicon nitride film with the laser with the above specific pulse and wavelength can further reduce the glass powder content of the metal electrode efficiency enhancement slurry, which can not only ensure the improvement of clouding, but also fully tap the gain in photoelectric conversion efficiency brought by laser-assisted sintering with metal electrode efficiency enhancement slurry with less glass powder content. BRIEF DESCRIPTION OF THE DRAWINGS
[0026] Figure 1 This is a schematic diagram of the cross-sectional structure of the semi-finished battery cell in step 1 of this embodiment.
[0027] Figure 2 Schematic diagram of the cross-sectional structure of the semi-finished battery cell after processing in step 2 of this embodiment.
[0028] Figure 3 Schematic diagram of the cross-sectional structure of the semi-finished battery cell after processing in step 4 of this embodiment.
[0029] Figure 4 Schematic diagram of the cross-sectional structure of the semi-finished battery cell subjected to laser-assisted sintering in step 5 of this embodiment.
[0030] Figure 5 Schematic diagram of the cross-sectional structure of the photovoltaic cell after being processed in step 5 of this embodiment.
[0031] Figure 6 This is a picture of the cloud anomaly in the front edge area of an existing conventional photovoltaic cell after laser-assisted sintering.
[0032] Figure 7 This is a diagram showing the fog improvement effect on the front edge area of the photovoltaic cell after being processed in step 5 of this embodiment.
[0033] Explanation of the accompanying drawings: silicon substrate 1; P+ emitter 2; aluminum oxide film 3; front silicon nitride film 4; plated silicon nitride film 5; tunneling oxide layer 6; doped polysilicon layer 7; back silicon nitride film 8; back electrode 9; front electrode 10. DETAILED DESCRIPTION
[0034] In order to make the above-mentioned objects, features and advantages of the present invention more obvious and easy to understand, the present invention is further described in detail below with reference to the accompanying drawings and specific embodiments.
[0035] Example
[0036] A method for improving the cloudiness of laser-assisted sintering in this embodiment is shown in Figure 1 , comprising the following steps in sequence:
[0037] Step 1: Prepare the semi-finished battery cell. Figure 1 The semi-finished cell comprises: a silicon substrate 1, a passivation contact structure and a back silicon nitride film 8 are sequentially stacked on the back of the silicon substrate 1, an emitter and a passivation anti-reflection film are sequentially stacked on the front of the silicon substrate 1, and a silicon nitride film 5 is also coated around the edge area of the front of the passivation anti-reflection film.
[0038] In step 1, see Figure 1 The passivation contact structure includes a tunneling oxide layer 6 disposed on the back of the silicon substrate 1 and a doped polysilicon layer 7 disposed on the back of the tunneling oxide layer 6. The silicon substrate 1 is preferably an n-type silicon substrate, and correspondingly, the emitter is preferably a P+ emitter 2, and the doped polysilicon layer 7 is preferably an N+ polysilicon layer.
[0039] In step 1, see Figure 1 The front surface of the silicon substrate 1 is preferably a velvet surface with a pyramidal morphology, so the front surfaces of the emitter, the passivation anti-reflection film and the coated silicon nitride film 5 are also velvet surfaces with a pyramidal morphology. Preferably, the passivation anti-reflection film includes an aluminum oxide film 3 disposed on the front surface of the emitter and a front silicon nitride film 4 disposed on the front surface of the aluminum oxide film 3.
[0040] Step 2: Use a pulse of 10 -18 -10 -12 s, and a laser with a wavelength of 200-600nm is used to selectively scan the silicon nitride film 5 to etch a local area of the silicon nitride film 5 (the local area corresponds to the area where the metal electrode efficiency enhancement slurry is subsequently printed). The semi-finished battery cell processed in step 2 is as follows. Figure 2 shown.
[0041] In step 2, the laser preferably has a pulse of 10 -15 s femtosecond ultraviolet laser, the power of the femtosecond ultraviolet laser is 1-20W (such as 8W), the frequency is 100-2000kHz (such as 1000kHz), and the scanning speed is 10-100m / s (such as 30m / s).
[0042] The shorter the laser pulse, the more concentrated the energy; the femtosecond ultraviolet laser has better performance in etching the dimensional accuracy of the coated silicon nitride film 5 and controlling the damage of the passivation anti-reflection film, and better preservation of the pyramid morphology of the velvet surface. The wavelength of the femtosecond ultraviolet laser is preferably 200-400nm (such as 365nm). The lower wavelength leads to a decrease in the absorption depth of the material, which can better control the etching thickness of the coated silicon nitride film 5. In step 2, the etching depth of the local area of the coated silicon nitride film 5 is 5-80nm (such as 20nm) and the etching width is 5-60μm (such as 15μm).
[0043] The pulse width of the femtosecond ultraviolet laser is extremely short. Relying on its own extremely high peak power and strong absorption, it can instantly vaporize the etched material with almost no thermal effect. Selectively etching the local area of the silicon nitride film 5 coated around the front edge of the semi-finished cell (corresponding to the area where the metal electrode efficiency enhancement slurry is subsequently printed) with a femtosecond ultraviolet laser can effectively avoid the edge fog problem caused by the subsequent laser-assisted sintering of the metal electrode efficiency enhancement slurry with a low glass powder content, thereby maximizing the improvement of the photoelectric conversion efficiency of the photovoltaic cell.
[0044] Step 3, printing a metal electrode efficiency-enhancing slurry (such as an efficiency-enhancing silver paste with a low glass powder content) on the front side of the local area where the bypass-plated silicon nitride film 5 is etched away; the glass powder content in the metal electrode efficiency-enhancing slurry is low, and its glass powder content is only 0.5-5%; and printing a metal electrode slurry (such as a conventional silver paste) locally on the back side of the back silicon nitride film 8.
[0045] In step 3, the metal electrode efficiency improvement slurry is preferably a silver paste with a low glass powder content, which includes the following raw materials in mass percentage: 0.5-5% glass powder (preferably less than 3%, such as 2%), 87-92% (90%) silver powder, and 7-10% (8%) organic carrier.
[0046] Specifically, the metal electrode efficiency enhancement paste in step 3 is Hangzhou Zhengyin 5015 series silver paste. Preferably, the printing area of the metal electrode efficiency enhancement paste corresponds to the etched local area of the plated silicon nitride film 5.
[0047] Step 4, sintering, so that the metal electrode efficiency slurry corrodes the passivation anti-reflection film during the sintering process to form a front electrode 10 that makes preliminary contact with the emitter, and the metal electrode slurry corrodes the back silicon nitride film 8 during the sintering process to form a back electrode 9 that makes ohmic contact with the doped polysilicon layer 7. At this time, the front electrode 10 and the emitter are in preliminary contact through the contact points that are initially formed. The semi-finished cell after step 4 is as follows Figure 3 shown.
[0048] If the sintering temperature is too high, the metal electrode enhancement slurry will corrode the passivation anti-reflection film too much, which will affect the open circuit voltage of the photovoltaic cell (experiments have shown that appropriately lowering the temperature of the first sintering will help improve the open circuit voltage); and if the sintering temperature is too low, it will affect the formation of the contact point. Therefore, in step 4, the sintering temperature is preferably 670-740°C (such as 680°C).
[0049] When the metal electrode paste is a conventional silver paste, in step 4, the back electrode 9 and the doped polysilicon layer 7 are in ohmic contact through the contact of silver crystals. In practice, after the metal electrode paste on the back is sintered in step 4 (i.e., once sintered), the back electrode 9 and the doped polysilicon layer 7 can achieve excellent ohmic contact.
[0050] However, since there are no electron-reduced silver crystals on the front P+ emitter 2, the front metal electrode efficiency enhancement slurry cannot achieve excellent ohmic contact between the front electrode 10 and the P+ emitter 2 after sintering in step 4 (one sintering); therefore, the front side needs to be further combined with the laser-assisted sintering in the following step 5 to achieve excellent ohmic contact between the front electrode 10 and the P+ emitter 2.
[0051] Step 5: Use laser scanning and reverse bias (such as Figure 4 As shown), the sintered cell semi-finished product is subjected to laser-assisted sintering, so that the front electrode 10 and the emitter can achieve excellent ohmic contact by forming excellent silver-silicon contact, so as to improve the clouding problem of the front edge area caused by the low glass powder content of the metal electrode efficiency slurry during the laser-assisted sintering process. The photovoltaic cell after step 5 is as follows Figure 5 shown.
[0052] In step 5, if the reverse bias is too low, it will affect the silver silicon diffusion and ohmic contact performance. Experiments have found that when the reverse bias is too low, the contact resistance of the photovoltaic cell is high, which will greatly affect the fill factor. Therefore, in step 5, the reverse bias is preferably 11-17V (such as 12V) and the laser power is 1-20W (such as 10W).
[0053] Performance Testing
[0054] The photovoltaic cell of this embodiment and the metal electrode efficiency-enhancing slurry printed on the front thereof were tested for performance, as were the conventional photovoltaic cells and the conventional silver paste printed on the front thereof. Compared with the conventional photovoltaic cells (BL), the photovoltaic cell of this embodiment, in its preparation process, added the above-mentioned step 2 (i.e., selective etching of the silicon nitride film coated on the front by femtosecond ultraviolet laser), and the front thereof was printed with a metal electrode efficiency-enhancing slurry with a low glass powder content (such as Hangzhou Zhengyin 5015 series silver paste). The test results are shown in Table 1 below.
[0055] Table 1
[0056]
[0057] In Table 1, Eta is the photoelectric conversion efficiency; Uoc is the open circuit voltage; Isc is the short circuit current; FF is the fill factor; Rsh is the parallel resistance; Rs is the series resistance; Irev12 is the reverse bias voltage of 12V, which is used to characterize the leakage current of the photovoltaic cell; the wet weight refers to the wet weight of the metal electrode efficiency enhancement paste (or conventional silver paste) printed on the front of the semi-finished cell.
[0058] Combined with Table 1 and Figure 6-7 It can be seen that compared with the existing conventional photovoltaic cells, the photovoltaic cell prepared by the method of improving the laser-assisted sintering fog problem of this embodiment effectively improves the fog problem, and its series resistance and leakage current are smaller, and its open circuit voltage, short circuit current, fill factor and photoelectric conversion efficiency are further improved.
[0059] Although the preferred embodiments of the present invention have been described, those skilled in the art may make additional changes and modifications to these embodiments once they have learned the basic creative concept. Therefore, the appended claims are intended to be interpreted as including the preferred embodiments and all changes and modifications that fall within the scope of the embodiments of the present invention.
[0060] The technical solution provided by the present invention is introduced in detail above. Specific examples are used in this article to illustrate the principle and implementation mode of the present invention. The description of the above embodiments is only used to help understand the method of the present invention and its core idea. At the same time, for those skilled in the art, according to the idea of the present invention, there will be changes in the specific implementation mode and application scope. In summary, the content of this specification should not be understood as limiting the present invention.
Claims
1. A method for improving the cloudiness of laser-assisted sintering, characterized in that: The steps include: S1. Prepare a semi-finished cell; wherein the semi-finished cell comprises a silicon substrate and an emitter and a passivation anti-reflection film sequentially stacked on the surface of the silicon substrate, and the edge area of the surface of the passivation anti-reflection film has a silicon nitride film coated around it; S2, the pulse is 10 -18 -10 -12 s, and selectively scanning the silicon nitride film with a laser having a wavelength of 200-600 nm to etch a local area of the silicon nitride film; S3, printing a metal electrode efficiency-enhancing slurry in the local area; wherein the glass powder content of the metal electrode efficiency-enhancing slurry is 0.5-5%; S4, sintering, so that the metal electrode efficiency enhancement slurry corrodes the passivation anti-reflection film during the sintering process to form a first electrode that makes preliminary contact with the emitter; S5. Perform laser-assisted sintering on the sintered semi-finished battery cell to form an ohmic contact between the first electrode and the emitter.
2. The method for improving the cloudiness of laser-assisted sintering according to claim 1, characterized in that: In step S2, the laser is a femtosecond ultraviolet laser, and the pulse of the femtosecond ultraviolet laser is 10 -15 s, power is 1-20W, frequency is 100-2000kHz, scanning speed is 10-100m / s, wavelength is 200-400nm.
3. A method for improving the cloudiness of laser-assisted sintering according to claim 1 or 2, characterized in that: The etching depth of the local area of the coated silicon nitride film is 5-80nm, and the etching width is 5-60μm.
4. The method for improving the cloudiness of laser-assisted sintering according to claim 1, characterized in that: In step S3, the metal electrode efficiency improvement slurry is a metal electrode efficiency improvement slurry with a small glass powder content, which includes the following raw materials in percentage by mass: 0.5-3% glass powder, 87-92% silver powder, and 7-10% organic carrier.
5. The method for improving the cloudiness of laser-assisted sintering according to claim 1, characterized in that: Step S3 also includes: a step of locally printing metal electrode paste on another surface of the semi-finished battery cell.
6. The method for improving the cloudiness of laser-assisted sintering according to claim 5, characterized in that: During the sintering process of step S4, the metal electrode slurry can also form a second electrode that is in ohmic contact with another surface of the semi-finished battery cell; In step S4, the sintering temperature is 670-740°C.
7. The method for improving the cloudiness of laser-assisted sintering according to claim 1, characterized in that: In step S5, the laser-assisted sintering is performed on the sintered semi-finished battery cell by combining laser scanning with application of reverse bias voltage; the laser power is 1-20W, and the reverse bias voltage is 11-17V.
8. The method for improving the cloudiness of laser-assisted sintering according to claim 1, characterized in that: In step S1, the semi-finished cell product further includes: a passivation contact structure and a second silicon nitride film stacked in sequence on the other surface of the silicon substrate; the passivation contact structure includes a tunneling oxide layer and a doped polysilicon layer disposed on the tunneling oxide layer; The passivation anti-reflection film includes an aluminum oxide film disposed on the surface of the emitter and a first silicon nitride film disposed on the surface of the aluminum oxide film.
9. A photovoltaic cell, characterized in that: The laser assisted sintering device is prepared by using the method for improving the cloudiness of laser assisted sintering as described in any one of claims 1 to 8.
10. A photovoltaic module, characterized in that: It comprises the photovoltaic cell as claimed in claim 9.
Citation Information
Cited By
Preparation method of solar cell and solar cell
CN120583772A
Method for manufacturing a solar cell and solar cell
CN120583772B