Method for preparing doped nanocrystalline silicon thin film of silicon-based heterojunction solar cell by hot filament CVD (chemical vapor deposition)

By pre-depositing a barrier layer on the silicon wafer substrate using hot wire CVD technology in silicon-based heterojunction solar cells, the intrinsic hydrogenated amorphous silicon film is solved, and the damage problem during the preparation of doped nanocrystalline silicon thin film is improved. Battery's life span and conversion efficiency.

CN119008783APending Publication Date: 2024-11-22NANCHANG UNIV GONGQINGCHENG OPTICAL HYDROGEN STORAGE TECH RES INST
View PDF 0 Cites 2 Cited by

Patent Information

Application Number
CN202411119100.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-15
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

Hot wire CVD technology can easily destroy the passivation effect of the intrinsic hydrogenated amorphous silicon film when preparing doped nanocrystalline silicon films, affecting the performance of silicon-based heterojunction solar cells.

Method used

The intrinsic hydrogenated amorphous silicon film is pre-deposited on the silicon wafer substrate, and a barrier layer is prepared using hot wire CVD, and then a doped nanocrystalline silicon thin film is deposited on the barrier layer to protect the intrinsic hydrogenated amorphous silicon film from being damaged.

Benefits of technology

It effectively prevents the damage of the intrinsic hydrogenated amorphous silicon film by doped nanocrystalline silicon film, significantly improves the oligono life and photoelectric conversion efficiency of silicon-based heterojunction solar cells, and increases the conversion efficiency by 1.2% abs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119008783A_ABST
    Figure CN119008783A_ABST
Patent Text Reader

Abstract

The invention provides a method for preparing a doped nanocrystalline silicon film of a silicon-based heterojunction solar cell by hot filament CVD (chemical vapor deposition), which comprises the following steps of: preparing a barrier layer on an intrinsic hydrogenated amorphous silicon film of a silicon wafer substrate by using the hot filament CVD; preparing a doped nanocrystalline silicon thin film on the barrier layer by using hot filament CVD (Chemical Vapor Deposition); the added barrier layer can protect the intrinsic hydrogenated amorphous silicon film, and can effectively reduce the reduction of passivation performance caused by direct deposition of the doped nanocrystalline silicon film on the intrinsic hydrogenated amorphous silicon film. The photoelectric conversion efficiency of the solar cell is maximally improved by 1.2% abs compared with that of a solar cell which is prepared by directly depositing a doped nanocrystalline silicon film on an intrinsic hydrogenated amorphous silicon film without adding a barrier layer.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of solar cells, and in particular to a method for preparing a doped nanocrystalline silicon film of a silicon-based heterojunction solar cell by hot-wire CVD. Background Art

[0002] A key technological breakthrough in silicon-based heterojunction (SHJ) solar cells in recent years is the application of doped nanocrystalline silicon films. Replacing the n-type or p-type doped hydrogenated amorphous silicon film in the cell structure with the corresponding doped nanocrystalline silicon film can greatly improve the conductivity of the film, and doping oxygen, carbon, nitrogen and other elements in the replaced doped nanocrystalline silicon film can further reduce its parasitic absorption of light, thereby obtaining silicon-based heterojunction solar cells with higher conversion efficiency.

[0003] However, the plasma enhanced chemical vapor deposition (PECVD) equipment used to prepare various types of doped nanocrystalline silicon films is expensive, accounting for a high proportion of the total investment in silicon-based heterojunction production line equipment, which has hindered the industrial development of such high-efficiency solar cells.

[0004] At present, the use of lower-cost hot-wire CVD technology instead of PECVD technology to prepare doped nanocrystalline silicon thin films is an effective way to solve this problem. Compared with PECVD technology, hot-wire CVD technology has the advantages of low equipment cost, high coating rate, low gas consumption, easy large-area coating and large equipment capacity, but there are still the following obstacles in the preparation of doped nanocrystalline silicon thin films: after the hot-wire CVD deposition and growth of the doped nanocrystalline silicon thin film layer, the intrinsic hydrogenated amorphous silicon passivation film between it and the silicon wafer substrate will always be destroyed, thus affecting the passivation effect.

[0005] Therefore, a new solution needs to be developed to enable the hot-filament CVD technology to be applied to the manufacture of new high-efficiency silicon-based heterojunction solar cells optimized with doped nanocrystalline silicon films. Summary of the invention

[0006] The present invention aims to provide a method for preparing a doped nanocrystalline silicon film for a silicon-based heterojunction solar cell by hot wire CVD. The hot wire CVD technology is used to deposit a barrier layer on an intrinsic hydrogenated amorphous silicon film, and then a doped nanocrystalline silicon film is deposited on the barrier layer. The problem that the passivation of the intrinsic hydrogenated amorphous silicon film is destroyed during the preparation of the doped nanocrystalline silicon film by hot wire CVD is solved, and the intrinsic hydrogenated amorphous silicon film is protected from being destroyed during the preparation of the doped nanocrystalline silicon film.

[0007] In a first aspect, the present invention provides a method for preparing a doped nanocrystalline silicon thin film for a silicon-based heterojunction solar cell by hot-wire CVD, comprising the following steps:

[0008] Pre-depositing an intrinsic hydrogenated amorphous silicon film on a silicon wafer substrate;

[0009] On the intrinsic hydrogenated amorphous silicon film, a barrier layer is prepared by hot wire CVD;

[0010] On the barrier layer, a doped nanocrystalline silicon film is prepared by hot wire CVD to obtain the doped nanocrystalline silicon film for the silicon-based heterojunction solar cell;

[0011] The doped nanocrystalline silicon film includes at least one layer of doped single-layer nanocrystalline silicon film;

[0012] The doping type of the doped single-layer nanocrystalline silicon film includes any one of an n-type doped single-layer nanocrystalline silicon film and a p-type doped single-layer nanocrystalline silicon film.

[0013] Optionally, the silicon wafer substrate includes any one of an n-type polished silicon wafer and an n-type textured silicon wafer.

[0014] Optionally, when preparing the doped multilayer nanocrystalline silicon film, it can be prepared by adjusting at least one of the following conditions: gas ratio, gas flow rate, gas type, hot wire temperature, and gas pressure.

[0015] Optionally, the parameters for preparing the barrier layer using hot wire CVD are: hot wire temperature 1600-2200° C., silane flow rate 2-1000 sccm, hydrogen flow rate 2-3000 sccm, gas pressure 0.3-5 Pa, and deposition time 5-100 s.

[0016] Optionally, when preparing the doped nanocrystalline silicon film, a dopant may be introduced during the preparation of the doped single-layer nanocrystalline silicon film, thereby changing the doping type of the doped single-layer nanocrystalline silicon film, comprising the following steps:

[0017] When preparing the n-type doped single-layer nanocrystalline silicon film, any one of 0.01-1000 sccm of phosphine and 0.01-1000 sccm of a mixture of phosphine and hydrogen is introduced;

[0018] When preparing the p-type doped single-layer nanocrystalline silicon film, any one of 0.01-1000 sccm of diborane and 0.01-1000 sccm of a mixture of diborane and hydrogen is introduced.

[0019] Optionally, when preparing the barrier layer, a dopant may also be introduced, wherein the dopant is related to the doping type of the prepared doped nanocrystalline silicon film, and the steps include:

[0020] When the doped nanocrystalline silicon film is prepared to be n-type, when preparing the barrier layer, any one of 0.01-1000 sccm of phosphine and 0.01-1000 sccm of a mixture of phosphine and hydrogen is introduced;

[0021] When the doped nanocrystalline silicon film is prepared to be p-type, any one of 0.01-1000 sccm of diborane and 0.01-1000 sccm of a mixture of diborane and hydrogen is introduced during the preparation of the barrier layer.

[0022] Optionally, the parameters for preparing the doped single-layer nanocrystalline silicon film using hot wire CVD are: hot wire temperature 1600-2200° C., silane flow rate 2-10000 sccm, hydrogen flow rate 50-300000 sccm, gas pressure 0.3-200 Pa, and deposition time 50-500 s.

[0023] Optionally, when preparing the barrier layer and the doped single-layer nanocrystalline silicon film, other gases may be introduced to reduce the parasitic absorption of light by the doped nanocrystalline silicon film.

[0024] Optionally, the flow rate of the other gas is 0.1-1000 sccm.

[0025] Optionally, the other gases include at least one of carbon dioxide, nitrous oxide, ammonia, methane, acetylene, ethylene, and monomethylsilane.

[0026] Optionally, the barrier layer has a thickness of 0.1-5 nm.

[0027] Optionally, the thickness of the doped nanocrystalline silicon film is 3-50 nm.

[0028] In a second aspect, the present invention provides a silicon-based heterojunction solar cell doped nanocrystalline silicon film produced by hot-wire CVD.

[0029] The beneficial effects of the present invention include:

[0030] (1) The preparation method provided by the present invention uses hot wire CVD technology to prepare the barrier layer and then prepare the doped nanocrystalline silicon film. The operation is simple, no other equipment is required, and the final structure is simple;

[0031] (2) The preparation method provided by the present invention uses a barrier layer prepared by hot wire CVD technology to effectively prevent the doped nanocrystalline silicon film prepared by hot wire CVD from damaging the intrinsic hydrogenated amorphous silicon film. The addition of the barrier layer significantly improves the minority carrier lifetime of the silicon-based heterojunction cell after the deposition of the doped nanocrystalline silicon film. After the addition of the barrier layer, the intrinsic hydrogenated amorphous silicon film is protected. The photoelectric conversion efficiency of the silicon-based heterojunction solar cell prepared in this way is increased by up to 1.2% compared with that without the barrier layer. abs . BRIEF DESCRIPTION OF THE DRAWINGS

[0032] Figure 1 A schematic diagram of the structure of preparing a doped nanocrystalline silicon film after depositing a barrier layer;

[0033] Figure 2 The minority carrier lifetime test results before and after hot wire CVD deposition of n-type oxygen-doped nanocrystalline silicon thin film (with barrier layer) on the n-type textured silicon wafer coated with intrinsic hydrogenated amorphous silicon film on both sides in Example 1;

[0034] Figure 3 The minority carrier lifetime results before and after hot wire CVD deposition of n-type amorphous silicon film on an n-type textured silicon wafer coated with intrinsic hydrogenated amorphous silicon film on both sides in Comparative Example 1;

[0035] Figure 4 The minority carrier lifetime results before and after hot wire CVD deposition of n-type oxygen-doped nanocrystalline silicon thin film (without barrier layer) on an n-type textured silicon wafer coated with intrinsic hydrogenated amorphous silicon film on both sides in Comparative Example 2;

[0036] Figure 5 The IV test results of the silicon-based heterojunction solar cells prepared in the examples and comparative examples are shown. DETAILED DESCRIPTION

[0037] The present invention will be further described through the following embodiments in conjunction with the accompanying drawings.

[0038] In a first aspect, an embodiment of the present invention provides a method for preparing a doped nanocrystalline silicon thin film for a silicon-based heterojunction solar cell by hot-wire CVD, such as Figure 1 The structure shown comprises the following steps:

[0039] Pre-depositing an intrinsic hydrogenated amorphous silicon film on a silicon wafer substrate;

[0040] On the intrinsic hydrogenated amorphous silicon film, a barrier layer is prepared by hot wire CVD;

[0041] On the barrier layer, a doped nanocrystalline silicon film is prepared by hot wire CVD to obtain the doped nanocrystalline silicon film for the silicon-based heterojunction solar cell;

[0042] The doped nanocrystalline silicon film includes at least one layer of doped single-layer nanocrystalline silicon film;

[0043] The doped nanocrystalline silicon film includes any one of an n-type doped single-layer nanocrystalline silicon film and a p-type doped single-layer nanocrystalline silicon film.

[0044] In some embodiments, the silicon wafer substrate includes any one of an n-type polished silicon wafer and an n-type textured silicon wafer.

[0045] In some embodiments, when preparing a multi-layer doped single-layer nanocrystalline silicon film, it can be prepared by adjusting any one of the conditions of gas ratio, gas flow, gas type, hot wire temperature, and gas pressure.

[0046] In some embodiments, the parameters for preparing the barrier layer using hot wire CVD are: hot wire temperature 1600-2200° C., silane flow rate 2-1000 sccm, hydrogen flow rate 2-3000 sccm, gas pressure 0.3-5 Pa, and deposition time 5-100 s.

[0047] In some embodiments, when preparing the doped nanocrystalline silicon film, the doping type of the doped single-layer nanocrystalline silicon film can be changed by changing the gas introduced when preparing the doped single-layer nanocrystalline silicon film, including the following steps:

[0048] When preparing the n-type doped single-layer nanocrystalline silicon film, any one of 0.01-1000 sccm of phosphine and 0.01-1000 sccm of a mixture of phosphine and hydrogen is introduced;

[0049] When preparing the p-type doped single-layer nanocrystalline silicon film, any one of 0.01-1000 sccm of diborane and 0.01-1000 sccm of a mixture of diborane and hydrogen is introduced.

[0050] In some embodiments, when preparing the barrier layer, a dopant may also be introduced, and the dopant is related to the doping type of the prepared doped nanocrystalline silicon film, including the following steps:

[0051] When the doped nanocrystalline silicon film is prepared to be n-type, when preparing the barrier layer, any one of 0.01-1000 sccm of phosphine and 0.01-1000 sccm of a mixture of phosphine and hydrogen is introduced;

[0052] When the doped nanocrystalline silicon film is prepared to be p-type, any one of 0.01-1000 sccm of diborane and 0.01-1000 sccm of a mixture of diborane and hydrogen is introduced during the preparation of the barrier layer.

[0053] In some embodiments, the parameters for preparing the doped nanocrystalline silicon film using hot wire CVD are: hot wire temperature 1600-2200° C., silane flow rate 2-10000 sccm, hydrogen flow rate 50-300000 sccm, gas pressure 0.3-200 Pa, and deposition time 50-500 s.

[0054] In some embodiments, when preparing the barrier layer and the doped single-layer nanocrystalline silicon film, other gases may be introduced to reduce the parasitic absorption of light by the doped nanocrystalline silicon film.

[0055] Specifically, the flow rate of the other gas is 0.1-1000 sccm.

[0056] In some embodiments, the other gas includes at least one of carbon dioxide, nitrous oxide, ammonia, methane, acetylene, ethylene, and monomethylsilane.

[0057] In some embodiments, the barrier layer has a thickness of 0.1-5 nm.

[0058] In some embodiments, the thickness of the doped nanocrystalline silicon film is 3-50 nm.

[0059] In a second aspect, the present invention provides an embodiment of a silicon-based heterojunction solar cell doped nanocrystalline silicon film produced by hot-wire CVD.

[0060] Example 1

[0061] Embodiment 1 of the present invention provides a method for preparing a doped nanocrystalline silicon thin film for a silicon-based heterojunction solar cell by hot-wire CVD, comprising the following steps:

[0062] S0, using hot wire CVD to deposit an intrinsic hydrogenated amorphous silicon film on both sides of an M2 size n-type textured silicon wafer;

[0063] The process parameters of hot-filament CVD for depositing the intrinsic hydrogenated amorphous silicon film are: 1Pa gas pressure, 1800°C hot-filament temperature, 20sccm silane, 8sccm hydrogen, and the deposited intrinsic hydrogenated amorphous silicon film has a thickness of 8nm;

[0064] S1, depositing a barrier layer on an M2-sized n-type textured silicon wafer with an intrinsic hydrogenated amorphous silicon film deposited on both sides using a hot wire CVD device;

[0065] The process parameters of hot-filament CVD for depositing the barrier layer are: 1Pa pressure, 1800°C hot-filament temperature, 20 sccm silane, 15 sccm hydrogen, 20 sccm of a mixture of phosphine and hydrogen (2% phosphine); the barrier layer thickness is 5 nm;

[0066] S2. After the barrier layer is deposited, a hot wire CVD device is used to deposit an n-type oxygen-doped nanocrystalline silicon thin film layer;

[0067] The process parameters of hot-filament CVD are: 4Pa gas pressure, 1850°C hot-filament temperature, 20sccm silane, 700sccm hydrogen, 20sccm phosphine and hydrogen mixture (2% phosphine), 16sccm carbon dioxide; the thickness of the n-type nanocrystalline silicon film layer is 20nm; silicon-based heterojunction solar cells (with barrier layer) are produced in this way.

[0068] Comparative Example 1

[0069] Comparative Example 1 of the present invention provides a method for preparing a doped amorphous thin film of a silicon-based heterojunction solar cell by hot wire CVD, which is different from Example 1 in that an n-type amorphous silicon film is deposited on an n-type textured silicon wafer with an intrinsic hydrogenated amorphous silicon film deposited on both sides, comprising the following steps:

[0070] Directly depositing an n-type amorphous silicon film on an M2-sized n-type textured silicon wafer with intrinsic hydrogenated amorphous silicon films deposited on both sides by using a hot wire CVD device;

[0071] The process parameters of hot-filament CVD are: 1Pa gas pressure, 1850°C hot-filament temperature, 20sccm silane, 20sccm hydrogen, 20sccm phosphine and hydrogen mixture (2% phosphine); the thickness of the n-type amorphous silicon film is 7nm; silicon-based heterojunction solar cells are produced in this way.

[0072] Comparative Example 2

[0073] Comparative Example 2 of the present invention provides a method for preparing a silicon-based heterojunction solar cell doped nanocrystalline silicon film by hot filament CVD. The difference from Example 1 is that step S1 is not performed, and an n-type oxygen-doped nanocrystalline silicon thin film layer is directly deposited on the intrinsic hydrogenated amorphous silicon film, and other conditions and steps remain consistent, thereby preparing a silicon-based heterojunction solar cell (without a barrier layer).

[0074] Performance Verification

[0075] 1. Verification of passivation effect

[0076] The passivation effect of silicon-based heterojunction solar cells is evaluated by minority carrier lifetime. The higher the minority carrier lifetime, the better the passivation effect. The minority carrier lifetime of silicon-based heterojunction solar cells is measured by Sinton WCT120 tester. The results are as follows: Figure 2-4 As shown;

[0077] The minority carrier lifetime results before and after hot wire CVD deposition of n-type oxygen-doped nanocrystalline silicon film (with barrier layer) on n-type textured silicon wafer coated with intrinsic hydrogenated amorphous silicon film on both sides in Example 1 are as follows: Figure 2 As shown;

[0078] The minority carrier lifetime results before and after hot wire CVD deposition of n-type amorphous silicon film on an n-type textured silicon wafer coated with intrinsic hydrogenated amorphous silicon film on both sides in Comparative Example 1 are as follows: Figure 3 As shown;

[0079] The minority carrier lifetime results before and after hot wire CVD deposition of n-type oxygen-doped nanocrystalline silicon film (without barrier layer) on n-type textured silicon wafer coated with intrinsic hydrogenated amorphous silicon film on both sides in Comparative Example 2 are as follows: Figure 4 shown.

[0080] See also Figures 2 to 4In comparative example 1, the minority carrier lifetime is significantly improved after depositing the n-type amorphous silicon film. In comparative example 2, the n-type oxygen-doped nanocrystalline silicon film is directly deposited without depositing a barrier layer, and the minority carrier lifetime is significantly reduced, indicating that the preparation of oxygen-doped nanocrystalline silicon film by hot-wire CVD will destroy the passivation and affect the passivation effect; in Example 1, the barrier layer is inserted before depositing the n-type oxygen-doped nanocrystalline silicon film, and the minority carrier lifetime can be significantly improved; therefore, the use of hot-wire CVD to deposit a barrier layer first provided by the present invention can effectively solve the destructive effect of hot-wire CVD on passivation when preparing oxygen-doped nanocrystalline silicon film, and the silicon-based heterojunction solar cell designed in this way is expected to achieve higher conversion efficiency than the conventional silicon-based heterojunction solar cell made of n-type amorphous silicon film.

[0081] 2. Performance evaluation of silicon-based heterojunction solar cells

[0082] The silicon-based heterojunction solar cells prepared in the examples and comparative examples were subjected to IV tests using a VISION VS-6825A tester. The n-type oxygen-doped nanocrystalline silicon thin film layer with a barrier layer in Example 1, the n-type amorphous silicon film layer in Comparative Example 1, and the n-type oxygen-doped nanocrystalline silicon thin film layer without a barrier layer in Comparative Example 2 were used as the front window layer. The measurement results are shown in FIG. Figure 5 shown.

[0083] See also Figure 5 In Comparative Example 2, hot wire CVD was used to prepare an oxygen-doped nanocrystalline silicon film. However, in the absence of a barrier layer, a higher conversion efficiency could not be obtained compared with the conventional n-type amorphous silicon film in Comparative Example 1. The open circuit voltage and fill factor were significantly lower, which was consistent with the phenomenon of passivation being destroyed. After a barrier layer was added in Example 1, the oxygen-doped nanocrystalline silicon film was prepared by hot wire CVD. The open circuit voltage and fill factor were significantly improved, and 1.25% could be achieved compared with the absence of a barrier layer. abs The conversion efficiency was improved, and an average conversion efficiency of 24.55% was obtained.

[0084] Although the embodiments of the present invention are described in detail above, it is obvious to those skilled in the art that various modifications and variations can be made to these embodiments. However, it should be understood that such modifications and variations are within the scope and spirit of the present invention as described in the claims. Moreover, the present invention described herein may have other embodiments and may be implemented or realized in a variety of ways.

Claims

1. A method for preparing doped nanocrystalline silicon thin films for silicon-based heterojunction solar cells by hot wire CVD, characterized in that: The following steps are involved: Pre-depositing an intrinsic hydrogenated amorphous silicon film on a silicon wafer substrate; On the intrinsic hydrogenated amorphous silicon film, a barrier layer is prepared by hot wire CVD; On the barrier layer, a nanocrystalline silicon film is prepared by hot wire CVD to obtain the doped nanocrystalline silicon film; The doped nanocrystalline silicon film includes at least one layer of doped single-layer nanocrystalline silicon film; The doping type of the doped single-layer nanocrystalline silicon film includes any one of an n-type doped single-layer nanocrystalline silicon film and a p-type doped single-layer nanocrystalline silicon film.

2. The method according to claim 1, characterized in that: The parameters for preparing the barrier layer using hot wire CVD are: hot wire temperature 1600-2200° C., silane flow rate 2-1000 sccm, hydrogen flow rate 2-3000 sccm, gas pressure 0.3-5 Pa, and deposition time 5-100 s.

3. The method according to claim 1, characterized in that When preparing the doped single-layer nanocrystalline silicon film, a dopant may be introduced, comprising the following steps: When preparing the n-type doped single-layer nanocrystalline silicon film, any one of 0.01-1000 sccm of phosphine and 0.01-1000 sccm of a mixture of phosphine and hydrogen is introduced; When preparing the p-type doped single-layer nanocrystalline silicon film, any one of 0.01-1000 sccm of diborane and 0.01-1000 sccm of a mixture of diborane and hydrogen is introduced.

4. The method according to claim 1, characterized in that: The parameters for preparing the doped single-layer nanocrystalline silicon film using hot wire CVD are: hot wire temperature 1600-2200° C., silane flow rate 2-10000 sccm, hydrogen flow rate 50-300000 sccm, gas pressure 0.3-200 Pa, and deposition time 50-500 s.

5. The method according to claim 1, characterized in that When preparing the barrier layer and the doped single-layer nanocrystalline silicon film, other gases may be introduced; The flow rate of the other gases is 0.1-1000 sccm; The other gases include at least one of carbon dioxide, methane, nitrous oxide, acetylene, ethylene, and monomethylsilane.

6. The method according to claim 1, characterized in that The thickness of the barrier layer is 0.1-5 nm.

7. The method according to claim 1, characterized in that The thickness of the doped nanocrystalline silicon film is 3-50 nm.

8. A silicon-based heterojunction solar cell doped nanocrystalline silicon film prepared by the method according to any one of claims 1 to 7.

Citation Information

Cited By

  • Method and equipment for preparing oxygen-doped microcrystalline silicon film

    CN120111987A

  • Method and equipment for preparing oxygen-doped microcrystalline silicon thin film

    CN120111987B