Composite porous carbon material as well as preparation method and application thereof

By using composite porous carbon materials in lithium-ion batteries, combining carbon layer and silicon graphene composite materials, the shortcomings of traditional lithium-ion battery anode materials in fast charging and discharge and structural stability are solved, and high energy density and rapid The compatibility of charge and discharge improves the overall performance of the battery.

CN119008901APending Publication Date: 2024-11-22合肥国轩新材料科技有限公司
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411113169.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-14
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

The negative electrode materials of traditional lithium-ion batteries are difficult to meet the requirements of fast charging and high energy density. The embedded reaction free energy of existing carbon materials during charging and discharging is large, the diffusion coefficient is low, and the conductivity is unstable, so it is impossible to take into account both fast charging and discharging and structure. stability.

Method used

Using composite porous carbon materials, by covering the carbon layer on the surface of the porous carbon material and evenly distributing the silicon @ graphene composite material inside, the silicon is covered by the graphene layer and there is a cavity between the graphene layer, and polyethylene is used. Imin forms hydrogen bonds with nanosilicon and graphene oxide electrostatic assembly, and after carbonization, a tightly bonded structure is formed to improve electron transport performance and structural stability.

Benefits of technology

It realizes fast and large-scale charging and discharging, maintains good structural stability and high capacity, solves the problem of incompatibility between fast charging and high energy density of lithium-ion batteries, and improves the charging and discharging cycle performance of the battery and the stability of the electrolyte.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119008901A_ABST
    Figure CN119008901A_ABST
Patent Text Reader

Abstract

The invention discloses a composite porous carbon material which is characterized in that the surface of the porous carbon material is coated with a carbon layer, and a silicon-graphene composite material is uniformly distributed in the porous carbon material; in the silicon and graphene composite material, silicon is coated with a graphene layer, and a cavity exists between the silicon and the graphene layer. The invention also discloses a preparation method of the composite porous carbon material, which comprises the following steps: uniformly mixing a polyethyleneimine aqueous solution with the pH value of 4-4.5 with nano silicon, reacting, and carrying out solid-liquid separation to obtain an intermediate 1; uniformly mixing the intermediate 1 with a graphene oxide dispersion liquid, carrying out electrostatic assembly, and carrying out solid-liquid separation to obtain an intermediate 2; uniformly mixing the intermediate 2, a coke source and a binder, granulating, and carbonizing to obtain an intermediate 3; and vapor-depositing a carbon layer on the surface of the intermediate 3 to obtain the composite porous carbon material. The invention also discloses an application of the composite porous carbon material in a negative electrode material. The lithium ion battery has both capacity and charge-discharge rate, and is stable in structure.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of lithium ion batteries, and in particular to a composite porous carbon material and a preparation method and application thereof. Background Art

[0002] As the main energy carrier in the new energy era, lithium-ion batteries have the advantages of high energy density, long cycle life, low self-discharge rate, and no memory effect. As a power source, they are mainly used in pure electric vehicles, plug-in electric vehicles, and other hybrid vehicles. They are also the main energy storage components of consumer electronic devices such as mobile phones and laptops. At the same time, traditional lithium-ion batteries also have the characteristics of slow charging speed, which brings inconvenience to the use of pure electric vehicles, mobile phones and other electronic appliances. In order to cope with this change, improving the charging speed of lithium-ion batteries, fast charging methods are becoming the focus of people's attention.

[0003] The main structure of a traditional lithium-ion battery includes: positive electrode, negative electrode, separator, and electrolyte. Among the factors that affect the performance of lithium-ion batteries, in addition to the positive electrode material, the negative electrode material is also important. Whether a negative electrode material with high performance, fast charging and fast discharging can be prepared directly determines the performance of the battery. In general, high-performance negative electrode materials should have the characteristics of small free energy changes in highly reversible embedding reactions during charging and discharging, high free diffusion coefficients of lithium ions in negative electrode materials, high electrical conductivity, and stable thermodynamic properties. At present, the research work on negative electrode materials is mainly focused on various carbon materials, but existing carbon materials are difficult to meet the growing requirements of high energy and high power density batteries. Therefore, providing a high-performance negative electrode material that can take into account fast charging and high energy density has become an important issue in the development of lithium batteries. Summary of the invention

[0004] Based on the technical problems existing in the background technology, the present invention proposes a composite porous carbon material and a preparation method and application thereof. The composite porous carbon material of the present invention achieves both capacity and charge and discharge rate and has good structural stability.

[0005] A composite porous carbon material, wherein a carbon layer is coated on the surface of the porous carbon material, and a silicon@graphene composite material is uniformly distributed inside the porous carbon material; wherein, in the silicon@graphene composite material, silicon is coated by the graphene layer, and a cavity exists between the silicon and the graphene layer.

[0006] Preferably, the graphene layer is tightly combined with the porous carbon material.

[0007] Preferably, the silicon in the silicon@graphene composite material is nano-silicon.

[0008] The present invention also proposes a method for preparing the above-mentioned composite porous carbon material, comprising the following steps: mixing a polyethyleneimine aqueous solution with a pH of 4-4.5 with nano-silicon, reacting, and performing solid-liquid separation to obtain an intermediate 1; mixing the intermediate 1 with a graphene oxide dispersion, electrostatically assembling, and performing solid-liquid separation to obtain an intermediate 2; mixing the intermediate 2, a coke source, and a binder to form particles, and carbonizing to obtain an intermediate 3; and vapor-depositing a carbon layer on the surface of the intermediate 3 to obtain a composite porous carbon material.

[0009] The present invention allows the secondary amine groups of polyethyleneimine to form hydrogen bonds with the hydroxyl groups on the surface of nano-silicon under acidic conditions and to carry a positive charge, so that the polyethyleneimine is coated on the surface of the nano-silicon to obtain an intermediate 1. The positive charge can make the intermediate 1 evenly dispersed to avoid agglomeration, and can be electrostatically assembled with negatively charged graphene oxide so that the graphene oxide layer is coated on the surface of the intermediate 1 to obtain an intermediate 2.

[0010] Intermediate 2 carries a negative charge to avoid agglomeration, so that it is evenly dispersed with the coke source and the binder, and the active groups in the graphene oxide layer (such as carboxyl, epoxy group, etc.) can react and graft with the groups in the binder (such as hydroxyl, etc.) to achieve firm fixation; then carbonization can obtain a porous structure, and polyethyleneimine can decompose to form a cavity between the nanosilicon and the graphene layer, and during carbonization, the graphene layer can be tightly combined with the porous carbon to provide support for the graphene layer to avoid the collapse of the graphene layer to obtain the specific structure of intermediate 3. On the one hand, the graphene layer and the porous carbon can serve as a protective shell, so that the nanosilicon can expand and contract freely without being easily broken, thereby improving the structural stability of the porous carbon material during the charge and discharge cycle, avoiding contact between the electrolyte and the nanosilicon, improving the stability of the SEI film, and increasing the capacity of the porous carbon. On the other hand, the graphene layer can improve the electronic transport performance of the porous carbon material to achieve Li + Rapid embedding and de-embedding enable fast and high-rate charge and discharge while maintaining good structural stability;

[0011] In addition, vapor deposition of a carbon layer on the surface of the intermediate 3 can reduce the specific surface area of ​​the porous carbon and improve the initial coulombic efficiency. The carbon layer can slow down its direct contact with the electrolyte, further improving the initial efficiency of the porous carbon, and can form a relatively stable structural framework, further improving the stability of the porous carbon structure. After the carbon layer is deposited, the voids inside the porous carbon are still retained, retaining a large number of lithium storage sites, further improving the capacity of the porous carbon. The coating of the carbon layer also improves the dispersion ability of the porous carbon.

[0012] The mass fraction of the polyethyleneimine aqueous solution can be 6-8wt%; and the pH of the polyethyleneimine aqueous solution is adjusted with hydrochloric acid.

[0013] Preferably, the coke source is at least one of needle coke and petroleum coke.

[0014] Preferably, the D50 of the focus source is 1-8 μm.

[0015] Preferably, the weight ratio of polyethyleneimine to nano-silicon is 6-8:1.

[0016] Preferably, the reaction is carried out at room temperature for 50-60 min.

[0017] Preferably, the graphene oxide dispersion is a graphene oxide aqueous dispersion with a mass fraction of 1-3 wt%.

[0018] The amount of the graphene oxide dispersion is not limited, as long as it can immerse the intermediate 1.

[0019] Preferably, the electrostatic assembly is performed at room temperature for 20-30 minutes.

[0020] Preferably, the binder is a phenolic resin.

[0021] Preferably, the weight ratio of the intermediate 2, the coke source and the binder is 30-50:45-65:5.

[0022] Preferably, the carbonization is carried out under the protection of an inert gas.

[0023] Preferably, the carbonization temperature is 1000-1200° C. and the time is 4-6 hours.

[0024] Preferably, the D50 of Intermediate 3 is 10-12 μm.

[0025] Preferably, the vapor deposition is chemical vapor deposition.

[0026] Preferably, the vapor deposition is performed under inert gas protection.

[0027] Preferably, the carbon source for vapor deposition is one or two of butyne, ethylene and propylene.

[0028] Preferably, the carbon source has an inflow rate of 850-1300 mL / min.

[0029] Preferably, the temperature of the vapor deposition is 700-900° C., and the time is 3-7 hours.

[0030] Preferably, the heating rate of vapor deposition is 8-25° C. / min; more preferably 10-18° C. / min.

[0031] The present invention selects appropriate vapor deposition temperature and time, so that the carbon layer has a good coating effect, avoiding the problems of excessive consumption and poor coating effect due to too high temperature, and too long reaction time and too low efficiency due to too low temperature.

[0032] The water mentioned above may be deionized water or the like.

[0033] The inert gas mentioned above may be nitrogen, argon or the like.

[0034] The present invention also proposes the application of the composite porous carbon material in negative electrode materials.

[0035] Preferably, the invention is used in negative electrode materials of lithium-ion batteries.

[0036] The specific structure of the composite porous carbon material of the present invention can satisfy the requirements of Li + Rapid embedding and de-embedding make fast and high-rate charging and discharging possible while having a higher capacity. It also has good structural stability and effectively solves the incompatibility problem between fast charging and high energy density required by power batteries and consumer-grade batteries. BRIEF DESCRIPTION OF THE DRAWINGS

[0037] Figure 1 This is an electron microscope image of the composite porous carbon material prepared in Example 3. DETAILED DESCRIPTION

[0038] The technical solution of the present invention is described in detail below through specific embodiments.

[0039] Example 1

[0040] A composite porous carbon material, wherein a carbon layer is coated on the surface of the porous carbon material, and a silicon@graphene composite material is uniformly distributed inside the porous carbon material; wherein, in the silicon@graphene composite material, silicon is coated by the graphene layer, and there is a cavity between the silicon and the graphene layer, the graphene layer is tightly combined with the porous carbon material, and the silicon in the silicon@graphene composite material is nano-silicon.

[0041] The method for preparing the composite porous carbon material comprises the following steps:

[0042] 6 g of polyethyleneimine was added to 100 g of deionized water, stirred to dissolve, and then adjusted to pH 4.5 with a dilute hydrochloric acid solution, and then 1 g of nano-silicon was added and mixed, reacted at room temperature for 50 min, centrifuged, washed with water, and dried at 40° C. to obtain intermediate 1; intermediate 1 was added to 100 ml of a 3 wt% graphene oxide aqueous dispersion, mixed, electrostatically assembled at room temperature for 20 min, centrifuged, aqueous solid, and dried at 40° C. to obtain intermediate 2;

[0043] The intermediate 2, petroleum coke with a D50 of 1-8 μm, and phenolic resin were mixed in a weight ratio of 30:65:5, granulated, heated to 1000°C for carbonization for 6 hours under nitrogen protection, crushed, sieved, washed with water, and dried to obtain the intermediate 3 with a D50 of 10-12 μm;

[0044] Nitrogen protection was introduced into the device containing the intermediate 3, butyne was introduced into the device at a flow rate of 850 mL / min, the temperature was raised to 700°C at a rate of 18°C / min for vapor deposition for 7 hours, a carbon layer was deposited on the surface of the intermediate 3, and a composite porous carbon material was obtained.

[0045] Example 2

[0046] A composite porous carbon material, wherein a carbon layer is coated on the surface of the porous carbon material, and a silicon@graphene composite material is uniformly distributed inside the porous carbon material; wherein, in the silicon@graphene composite material, silicon is coated by the graphene layer, and there is a cavity between the silicon and the graphene layer, the graphene layer is tightly combined with the porous carbon material, and the silicon in the silicon@graphene composite material is nano-silicon.

[0047] The method for preparing the composite porous carbon material comprises the following steps:

[0048] 8 g of polyethyleneimine was added to 100 g of deionized water, stirred to dissolve, and then adjusted to pH = 4 with a dilute hydrochloric acid aqueous solution, and then 1 g of nano-silicon was added and mixed, reacted at room temperature for 60 min, centrifuged, washed with water, and dried at 40°C to obtain intermediate 1; intermediate 1 was added to 100 ml of 1 wt% graphene oxide aqueous dispersion, mixed, electrostatically assembled at room temperature for 30 min, centrifuged, aqueous solid, and dried at 40°C to obtain intermediate 2;

[0049] The intermediate 2, needle coke with a D50 of 1-8 μm, and phenolic resin were mixed in a weight ratio of 50:45:5, granulated, heated to 1200° C. for carbonization for 4 h under nitrogen protection, crushed, sieved, washed with water, and dried to obtain the intermediate 3 with a D50 of 10-12 μm;

[0050] Nitrogen protection was introduced into the device containing the intermediate 3, ethylene was introduced into the device at a flow rate of 1300 mL / min, the temperature was raised to 900°C at a rate of 10°C / min for vapor deposition for 3 hours, a carbon layer was deposited on the surface of the intermediate 3, and a composite porous carbon material was obtained.

[0051] Example 3

[0052] A composite porous carbon material, wherein a carbon layer is coated on the surface of the porous carbon material, and a silicon@graphene composite material is uniformly distributed inside the porous carbon material; wherein, in the silicon@graphene composite material, silicon is coated by the graphene layer, and there is a cavity between the silicon and the graphene layer, the graphene layer is tightly combined with the porous carbon material, and the silicon in the silicon@graphene composite material is nano-silicon.

[0053] The method for preparing the composite porous carbon material comprises the following steps:

[0054] 7 g of polyethyleneimine was added to 100 g of deionized water, stirred to dissolve, and then adjusted to pH 4.2 with a dilute hydrochloric acid solution, and then 1 g of nano-silicon was added and mixed, reacted at room temperature for 60 min, centrifuged, washed with water, and dried at 40° C. to obtain intermediate 1; intermediate 1 was added to 100 ml of a 2 wt% graphene oxide aqueous dispersion, mixed, electrostatically assembled at room temperature for 30 min, centrifuged, aqueous solid, and dried at 40° C. to obtain intermediate 2;

[0055] The intermediate 2, needle coke with a D50 of 1-8 μm, and phenolic resin were mixed in a weight ratio of 40:55:5, granulated, heated to 1100° C. under nitrogen protection for carbonization for 5 h, crushed, sieved, washed with water, and dried to obtain the intermediate 3 with a D50 of 10-12 μm;

[0056] Nitrogen protection was introduced into the device containing the intermediate 3, ethylene was introduced into the device at a flow rate of 1000 mL / min, the temperature was raised to 850°C at a rate of 15°C / min for vapor deposition for 5 hours, a carbon layer was deposited on the surface of the intermediate 3, and a composite porous carbon material was obtained.

[0057] Figure 1 This is an electron microscope image of the composite porous carbon material prepared in Example 3.

[0058] Comparative Example 1

[0059] The preparation method of the composite porous carbon material comprises the following steps: replacing "intermediate 2" with "intermediate 1", and the rest is the same as Example 3.

[0060] Comparative Example 2

[0061] The preparation method of the composite porous carbon material comprises the following steps: without adding the intermediate 2, the weight ratio of the needle coke and the phenolic resin is 95:5, and the rest is the same as in Example 3.

[0062] Comparative Example 3

[0063] The composite porous carbon material is intermediate 3 of Example 3.

[0064] The materials prepared in Examples 1-3 and Comparative Examples 1-3 were used as negative electrode materials, and negative electrode slurries were prepared by mixing the negative electrode materials, conductive agent (Super-P), and binder PVDF in a weight ratio of 94:2:4, and coated on copper foil, and vacuum dried and rolled to prepare negative electrode sheets; the positive electrode used a metal lithium sheet, and the electrolyte used a 1 mol / L LiPF6 solution to assemble a CR2025 button cell. The battery performance was tested, and the results are shown in Table 1.

[0065] Table 1 Test results

[0066] Grouping 0.2C first discharge capacity (mAh / g) 5C cycle 1500 times capacity retention rate (%) Example 1 590 93.1 Example 2 563 92.6 Example 3 578 93.8 Comparative Example 1 437 75.2 Comparative Example 2 341 60.3 Comparative Example 3 420 70.5

[0067] It can be seen from Table 1 that the composite porous carbon material of the present invention has good capacity and charge and discharge rate.

[0068] The above description is only a preferred specific implementation manner of the present invention, but the protection scope of the present invention is not limited thereto. Any technician familiar with the technical field can make equivalent replacements or changes according to the technical scheme and inventive concept of the present invention within the technical scope disclosed by the present invention, which should be covered by the protection scope of the present invention.

Claims

1. A composite porous carbon material, characterized in that: A carbon layer is coated on the surface of the porous carbon material, and a silicon@graphene composite material is uniformly distributed inside the porous carbon material; wherein, in the silicon@graphene composite material, silicon is coated by the graphene layer, and a cavity exists between the silicon and the graphene layer.

2. The composite porous carbon material according to claim 1, characterized in that: The graphene layer is tightly combined with the porous carbon material; preferably, the silicon in the silicon@graphene composite material is nano-silicon.

3. A method for preparing the composite porous carbon material as claimed in claim 1 or 2, characterized in that: The method comprises the following steps: mixing a polyethyleneimine aqueous solution with a pH value of 4-4.5 with nano-silicon, reacting, and performing solid-liquid separation to obtain an intermediate 1; mixing the intermediate 1 with a graphene oxide dispersion, electrostatically assembling, and performing solid-liquid separation to obtain an intermediate 2; mixing the intermediate 2, a coke source, and a binder, granulating, and carbonizing to obtain an intermediate 3; and vapor-depositing a carbon layer on the surface of the intermediate 3 to obtain a composite porous carbon material.

4. The method for preparing the composite porous carbon material according to claim 3, characterized in that: The coke source is at least one of needle coke and petroleum coke; preferably, the D50 of the coke source is 1-8 μm.

5. The method for preparing the composite porous carbon material according to claim 3 or 4, characterized in that: The weight ratio of polyethyleneimine to nano-silicon is 6-8:1; preferably, the reaction is carried out at room temperature for 50-60 minutes; preferably, the graphene oxide dispersion is a graphene oxide aqueous dispersion with a mass fraction of 1-3wt%; preferably, the electrostatic assembly is carried out at room temperature for 20-30 minutes.

6. The method for preparing the composite porous carbon material according to any one of claims 3 to 5, characterized in that: The binder is a phenolic resin; preferably, the weight ratio of the intermediate 2, the coke source, and the binder is 30-50:45-65:

5.

7. The method for preparing the composite porous carbon material according to any one of claims 3 to 6, characterized in that: The carbonization is carried out under the protection of an inert gas; preferably, the carbonization temperature is 1000-1200° C., and the time is 4-6 h; preferably, the D50 of the intermediate 3 is 10-12 μm.

8. The method for preparing the composite porous carbon material according to any one of claims 3 to 7, characterized in that: The vapor deposition is chemical vapor deposition; preferably, the vapor deposition is carried out under the protection of an inert gas; preferably, the carbon source for the vapor deposition is one or two of butyne, ethylene, and propylene; preferably, the inlet flow rate of the carbon source is 850-1300 mL / min.

9. The method for preparing the composite porous carbon material according to any one of claims 3 to 8, characterized in that: The temperature of vapor deposition is 700-900° C., and the time is 3-7 hours; preferably, the heating rate of vapor deposition is 8-25° C. / min.

10. Use of the composite porous carbon material as claimed in claim 1 or 2 in negative electrode materials; preferably, use in negative electrode materials for lithium-ion batteries.