Co-doped lithium-rich manganese-based material, positive plate, preparation method of positive plate and battery

By co-doping lithium-rich manganese-based materials, the problem of insufficient rate performance and cycle stability of the positive electrode material in the prior art is solved. By introducing alternative lithium ions and transition metal elements, a stable layered structure is formed, and the lithium ion battery is improved performance and lifespan.

CN119008929APending Publication Date: 2024-11-22中汽新能(天津)电池科技有限公司
View PDF 0 Cites 2 Cited by

Patent Information

Application Number
CN202411147388.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-21
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

The existing lithium-rich manganese-based positive electrode materials have shortcomings in rate performance and cycle stability, resulting in performance and life of lithium-ion batteries.

Method used

Co-doped lithium-manganese-rich material is used to adjust the crystal structure and electron conduction properties of the material by introducing metal elements and transition metal elements that replace lithium ions, as well as halogen elements, to form a more stable layered structure. The specific method includes preparing a lithium-rich manganese-based positive electrode material precursor, grinding and calcining, forming a co-doped material with a specific chemical formula, and combining it with a positive electrode conductive agent and a binder to form a positive electrode sheet.

Benefits of technology

Improve the rate performance and cycle stability of lithium-ion batteries, extend the battery life, and stabilize the layered structure of the material through synergistically acting multiple anion and cation doping, reducing the migration resistance of lithium ions and the migration of transition metals. , enhances the chemical stability of the material.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005002569120000061
    Figure BDA0005002569120000061
  • Figure BDA0005002569120000071
    Figure BDA0005002569120000071
Patent Text Reader

Abstract

The invention belongs to the field of batteries, and particularly relates to a co-doped lithium-rich manganese-based material, a positive plate, a preparation method of the positive plate and a battery. The chemical general formula of the co-doped lithium-rich manganese-based material is Li < a-x > M < x > Mn N < z > N < c > Co < d > O < 2-x-y > R < x > Q < y >, a < = 1.5, 0.4 < = blt; 0.9, 0 lt; c < = 0.4, 0 < = d < = 0.4, 0 < = x < = 0.15, 0 < = y < = 0.2, 0 < = z < = 0.2, and bgt; c, bgt; d; m is a metal element; n is a transition metal element; r and Q are independently halogen elements. According to the lithium-rich manganese-based material, co-doping of multiple anions and cations achieves a synergistic effect, so that the lithium-rich manganese-based material after co-doping of multiple anions and cations has better cycle stability.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the field of batteries, and in particular relates to a co-doped lithium-rich manganese-based material, a positive electrode sheet and a preparation method thereof, and a battery. Background Art

[0002] As the most commonly used green high-energy battery, lithium-ion batteries have become a wide choice for mobile phones, laptops and other portable devices due to their excellent high energy density, outstanding high specific capacity, no memory effect, and their environmentally friendly characteristics. With the increasing popularity of electric vehicles, higher requirements are placed on the performance of lithium-ion batteries, including cycle life, energy density and cost. The positive electrode material of lithium-ion batteries plays a vital role in its composition and has a profound impact on the performance, life and cost of lithium-ion batteries. Therefore, the design and synthesis of lithium-ion battery positive electrode materials with high capacity, excellent rate performance, long cycle life and economical and affordable has become a core direction of the development of lithium-ion battery technology. At present, the issue of improving the performance of lithium-ion battery positive electrode materials has received widespread attention.

[0003] Lithium-rich manganese-based cathode materials are a type of lithium-ion battery cathode material with broad application prospects due to their extremely high gram capacity (over 250mAh / g). However, lithium-rich manganese-based cathode materials have disadvantages such as poor rate performance and cycle stability. The modification of lithium-rich manganese-based materials is an important research field aimed at improving the performance and stability of lithium-ion battery cathode materials. This modification aims to overcome some of the problems of lithium-rich manganese-based materials, such as gas production, decreased rate performance, and insufficient cycle life. By introducing new elements or structural regulation, the electrochemical properties of lithium-rich manganese-based materials can be improved, and their capacity, rate performance, and cycle life can be increased. Researchers use different modification methods, such as surface coating and element doping, to adjust the crystal structure and electronic conductivity of lithium-rich manganese-based materials. The development of these modification methods is expected to promote the advancement of lithium-ion battery technology, improve its energy density and cycle life, and thus promote more sustainable and high-performance applications in electric vehicles and portable devices. Summary of the invention

[0004] The purpose of the present invention is to overcome the shortcomings of the prior art and provide a co-doped lithium-rich manganese-based material, a positive electrode sheet and a preparation method thereof, and a battery.

[0005] To achieve the above object, the technical solution adopted by the present invention is:

[0006] A co-doped lithium-rich manganese-based material with a general chemical formula of Li a-x M x Mn b N z Ni c Co d O2-x-y R x Q y , where 1 < a ≤ 1.5, 0.4 ≤ b < 0.9, 0 < c ≤ 0.4, 0 ≤ d ≤ 0.4, 0 ≤ x ≤ 0.15, 0 ≤ y ≤ 0.2, 0 ≤ z ≤ 0.2, and b > c, b > d; M is a metallic element; N is a transition metallic element; R and Q are independently halogen elements.

[0007] M is a metallic element substituting for Li; N is a metallic element substituting for transition metallic elements Mn, Ni, and Co.

[0008] M is one or more of the elements Na, K, Rb, and Cs, in a positive valence state in the compound, and its radius is greater than that of the lithium ion; N is one or more of Mg, Al, Sn, La, Cr, Zr, Y, Ca, Ti, Zn, and Fe.

[0009] M:Li = (0.0001 - 0.15):1, preferably (0.01 - 0.05):1; more preferably 0.01:1;

[0010] N:Mn = (0.0001 - 0.10):1, preferably (0.01 - 0.05):1; more preferably 0.01:1;

[0011] R:O = (0.0001 - 0.3):1, preferably (0.01 - 0.1):1; more preferably 0.01:1;

[0012] Q:O = (0.0001 - 0.3):1, preferably (0.01 - 0.1):1, more preferably (0.02 - 0.03):1.

[0013] The present invention further includes a method for preparing the co-doped lithium-rich manganese-based material as described above, comprising the following steps:

[0014] 1) Prepare a precursor of the lithium-rich manganese-based cathode material; the chemical general formula is (Mn b Ni c Co d )CO3,

[0015] (Mn b Ni c Co d )(OH)2 or (Mn b Ni c Co d )O2, where b > c, b > d;

[0016] 2) Mix the precursor powder, a lithium salt, a halogen compound MR of the metallic element M, and a halogen compound NQ of the metallic element N e(e is a natural number of the valence state of the composite molecule) The powders are mixed uniformly, ground, pre-calcined and calcined to obtain the anion- and cation-co-doped lithium-rich manganese-based positive electrode material.

[0017] Specifically, the lithium salt is one or more of lithium hydroxide, lithium nitrate, lithium carbonate, lithium oxalate, lithium acetate, lithium oxide, and lithium citrate;

[0018] The halogen compound powder containing the metal element M is one or more of NaF, KF, RbF, NaCl, KCl, or RbCl;

[0019] The halogen compound containing the metal element N is one or more of MgF2, AlF3, SnF4, LaF3, CrF3, ZrF4, YF3, CaF2, TiF4, ZnF2, FeF3, and VF3.

[0020] Specifically, the pre-calcination is to pre-calcine the powder prepared in the above step at a temperature of 300-600° C. for 3-8 hours; the calcination is to pre-calcine the powder prepared in the above step at a temperature of 600-1000° C. for 8-20 hours.

[0021] The present invention also includes a positive electrode sheet, comprising the co-doped lithium-rich manganese-based material, a positive electrode conductor and a positive electrode binder;

[0022] Preferably, the conductive agent is positive electrode carbon nanotubes; preferably, the positive electrode binder is PVDF;

[0023] Preferably, the mass ratio of the co-doped lithium-rich manganese-based material, the positive electrode conductor and the positive electrode binder is (90-98):(1-5):(1-5); preferably 96:2:2.

[0024] The present invention also includes a method for preparing the positive electrode sheet, comprising the following steps: fully stirring the co-doped lithium-rich manganese-based material, the positive electrode conductor, and the positive electrode binder in a solvent, coating them on aluminum foil, drying them, and cold pressing them to obtain the positive electrode sheet.

[0025] The present invention also includes a battery, comprising the positive electrode sheet, the negative electrode sheet, the separator and the electrolyte;

[0026] Preferably, the negative electrode sheet comprises a negative electrode active material, a negative electrode conductive agent and a negative electrode binder; preferably, the negative electrode active material is graphite; preferably, the negative electrode conductive agent is acetylene black; preferably, the negative electrode binder is a mixture of styrene-butadiene rubber and carboxymethyl cellulose; the mass ratio of the two is 1:1;

[0027] Preferably, the diaphragm is a polyethylene porous polymer film;

[0028] Preferably, the electrolyte comprises a lithium salt and an electrolyte solvent;

[0029] Preferably, the lithium salt is LiPF6; preferably, the concentration of the lithium salt is 1 to 1.5 mol / L, preferably 1.2 mol / L;

[0030] Preferably, the electrolyte solvent is a mixture of fluoroethylene carbonate: dimethyl carbonate: ethylene carbonate; preferably, the volume ratio of the three is 3:1:1.

[0031] Compared with the prior art, the present invention has the following beneficial effects:

[0032] The co-doped lithium-rich manganese-based material of the present application is doped by selecting anions and cations that are similar in physical and chemical properties. The metal element M that replaces Li can not only reduce the diffusion resistance of Li ions in the lattice by increasing the Li interlayer spacing, but also stabilize the layered structure of the positive electrode material, thereby showing higher rate performance and excellent cycle stability. This is because the cation M replaces part of the lithium in the lithium-rich material, and its atomic radius is larger than Li, and it does not participate in the migration, which leads to a low gram capacity of the material, and the doping of the cation M increases the lattice constant c of the material, and the migration barrier of lithium ions becomes smaller, which can reduce the polarization of the material, and can inhibit the migration of transition metal ions to the lithium layer to stabilize the structure.

[0033] At the same time, the anions are doped with halogen elements, especially F - F ion doping can replace OR (R = Ni, Co, Mn) bonds with stronger FR bonds, making the layered structure of the material more stable and improving the cycle stability of the material.

[0034] At the same time, the cation N can replace some transition metal elements such as Mn, Ni, and Co in the lithium-rich material. It can inhibit the migration and dissolution of transition metals, fix lattice oxygen, and make the crystal structure of lithium-rich manganese-based positive electrode materials more stable. This is because the doping of the replacement transition metal element N effectively stabilizes the layered structure of the lithium-rich material, which can slow down the continuous transformation of the material from the layered structure to the spinel structure during the cycle, reduce the attenuation of the voltage platform, and thus improve the cycle stability of the material. Moreover, since the negatively valenced R or Q element replaces the oxygen in the lithium-rich manganese-based positive electrode material, a bond with stronger bond energy is formed to replace the OR (R = Ni, Co, Mn) bond, making the structure of the lithium-rich manganese-based material more stable and improving the cycle stability of the material.

[0035] The co-doping of multiple anions and cations in the present application has a synergistic effect, so that the lithium-rich manganese-based material after co-doping of multiple anions and cations has better cycle stability. Moreover, the cations used to replace the lithium ions in the lithium-rich manganese-based material and the anions used to replace the oxygen ions in the lithium-rich manganese-based material in the present application are derived from the same compound. It can save raw materials, reduce the introduction of impurity elements, and replace the doping of Li elements, transition metal elements and O elements, which can better stabilize the layered structure of lithium-rich manganese-based materials. DETAILED DESCRIPTION

[0036] In order to enable those skilled in the art to better understand the technical solution of the present invention, the present invention is further described in detail below in conjunction with embodiments.

[0037] Example 1

[0038] Co-doped lithium-rich manganese-based materials, in which sodium replaces lithium and fluorine replaces oxygen, with the replacement ratio of sodium and fluorine being 1%. Aluminum replaces manganese and chlorine replaces oxygen, with the replacement ratios of aluminum and chlorine being 1% and 3% respectively.

[0039] The preparation process is as follows: weigh 92.6 g (1 mol) of (Mn 0.6 Ni 0.2 Co 0.2 )(OH)2 and 111g of Li2CO3, 0.420g of sodium fluoride and 1.334g of aluminum chloride were mixed and ground, and then heated to 450°C for pre-calcination for 5h and then heated to 900°C for calcination for 18h to obtain the anion-cation co-doped lithium-rich manganese-based material (chemical formula: Li 1.19 Na 0.01 Mn 0.59 Al 0.01 Ni 0.2 Co 0.2 O 1.96 Cl 0.03 F 0.01 ).

[0040] Embodiment 2:

[0041] Co-doped lithium-rich manganese-based materials, in which potassium replaces lithium and chlorine replaces oxygen, with the replacement ratio of potassium and chlorine being 1%. Zirconium replaces manganese and fluorine replaces oxygen, with the replacement ratios of zirconium and fluorine being 1% and 4% respectively.

[0042] The preparation process is as follows: weigh 92.6 g (1 mol) of (Mn 0.6 Ni 0.2 Co 0.2)(OH)2 and 111g of Li2CO3, 0.745g of potassium chloride and 1.672g of zirconium fluoride were mixed and ground, and then heated to 450°C for pre-calcination for 5h and then heated to 900°C for calcination for 18h to obtain the anion-cation co-doped lithium-rich manganese-based material (chemical formula: Li 1.19 K 0.01 Mn 0.59 Zr 0.01 Ni 0.2 Co 0.2 O 1.95 Cl 0.01 F 0.04 ).

[0043] Embodiment 3:

[0044] Co-doped lithium-rich manganese-based materials, in which sodium replaces lithium and chlorine replaces oxygen, with the replacement ratio of sodium and chlorine being 1%. Zirconium replaces manganese and fluorine replaces oxygen, with the replacement ratio of zirconium and fluorine being 1% and 3% respectively.

[0045] The preparation process is as follows: weigh 92.6 g (1 mol) of (Mn 0.6 Ni 0.2 Co 0.2 )(OH)2 and 111g of Li2CO3, 0.584g of sodium chloride and 1.672g of zirconium fluoride were mixed and ground, and then heated to 450°C for pre-calcination for 5h and then heated to 900°C for calcination for 16h to obtain the anion-cation co-doped lithium-rich manganese-based material (chemical formula: Li 1.19 Na 0.01 Mn 0.59 Zr 0.01 Ni 0.2 Co 0.2 O 1.96 Cl 0.01 F 0.04 ).

[0046] Embodiment 4:

[0047] Co-doped lithium-rich manganese-based materials, in which potassium replaces lithium and chlorine replaces oxygen, with the replacement ratio of potassium and chlorine being 1%. Lanthanum replaces manganese and chlorine replaces oxygen, with the replacement ratios of lanthanum and chlorine being 1% and 3% respectively.

[0048] The preparation process is as follows: weigh 92.6 g (1 mol) of (Mn 0.6 Ni 0.2 Co 0.2)(OH)2 and 111g of Li2CO3, 0.42g of potassium chloride and 2.453g of lanthanum chloride were mixed and ground, and then heated to 450°C for pre-calcination for 5h and then heated to 900°C for calcination for 18h to obtain the anion-cation co-doped lithium-rich manganese-based material (chemical formula: Li 1.19 K 0.01 Mn 0.59 La 0.01 Ni 0.2 Co 0. 2O 1.96 Cl 0.04 ).

[0049] Comparative Example 1:

[0050] A method for preparing anion-cation co-doped lithium-rich manganese-based positive electrode material, wherein sodium element is used to replace lithium element, chlorine element is used to replace oxygen element, and the replacement ratio of sodium element and chlorine element is 1%. The preparation process is as follows: weigh 92.6g (1 mol) of (Mn 0.6 Ni 0.2 Co 0.2 )(OH)2, 111g of Li2CO3 and 0.420g of sodium fluoride were mixed and ground, and then heated to 450°C for pre-calcination for 5h and then heated to 900°C for calcination for 18h to obtain the anion-cation co-doped lithium-rich manganese-based material (chemical formula: Li 1.19 Na 0.01 Mn 0.6 Ni 0.2 Co 0.2 O 1.96 F 0.01 ).

[0051] Comparative Example 2:

[0052] A method for preparing anion-cation co-doped lithium-rich manganese-based positive electrode material, wherein aluminum replaces manganese, chlorine replaces oxygen, and the replacement ratios of aluminum and chlorine are 1% and 3%, respectively. The preparation process is as follows: weigh 92.6g (1 mol) of (Mn 0.6 Ni 0.2 Co 0.2 )(OH)2, 111g of Li2CO3 and 0.840g of AlF3 were mixed and ground, and then heated to 450°C for pre-calcination for 5h and then heated to 850°C for calcination for 18h to obtain the anion-cation co-doped lithium-rich manganese-based material (chemical formula: Li 1.20 Mn 0.59 Al 0.01 Ni 0.2 Co 0.2 O 1.97 Cl 0.03 ).

[0053] Comparative Example 3:

[0054] A method for preparing a lithium-rich manganese-based positive electrode material, the preparation process is as follows: weigh 92.6g (1 mol) of (Mn 0.6 Ni 0.2 Co 0.2 )(OH)2 and 111g of Li2CO3 were mixed and ground, and then heated to 450°C for pre-calcination for 5h and then heated to 850°C for calcination for 18h to obtain the anion-cation co-doped lithium-rich manganese-based material (chemical formula: Li 1.2 Mn 0.6 Ni 0.2 Co 0.2 O2).

[0055] The lithium-rich manganese-based materials prepared in Examples 1-4 and Comparative Examples 1-3 were used to prepare lithium-ion batteries in the following manner, and the prepared lithium-ion batteries were tested to test their 0.1C discharge capacity mAh / g and cycle capacity retention rate.

[0056] Preparation of lithium-ion batteries:

[0057] Preparation of positive electrode sheet: The positive electrode active material, conductive agent carbon nanotubes, and binder polyvinylidene fluoride (PVDF) are fully stirred in N-methylpyrrolidone solvent at a mass ratio of 96:2:2, coated on aluminum foil, dried, and cold pressed to obtain a positive electrode sheet.

[0058] Preparation of negative electrode sheet: Active material artificial graphite, conductive agent acetylene black, styrene-butadiene rubber (SBR), and carboxymethyl cellulose (CMC) are fully stirred and mixed in deionized water in a mass ratio of 97:1:1:1, coated on copper foil, dried, and cold pressed to obtain a negative electrode sheet.

[0059] Separation membrane: Polyethylene (PE) porous polymer film is used as the separation membrane.

[0060] Preparation of electrolyte: Add a certain amount of LiPF6 into a solvent of fluoroethylene carbonate: dimethyl carbonate: ethylene carbonate in a volume ratio of 3:1:1 to make its concentration 1.2 mol / L.

[0061] The positive electrode sheet, separator, and negative electrode sheet are stacked in order, with the separator between the positive and negative electrodes to play a role of isolation, and then wound or stacked. The battery cell is placed in an outer package, and the electrolyte is injected and packaged.

[0062] Performance testing of lithium-ion batteries

[0063] Capacity test: Take 10 batteries from each of the examples and comparative examples, charge them to 4.6V at room temperature at a constant current of 0.1C, and then charge them at a constant voltage of 4.6V until the current is lower than 0.02C, so that they are in a fully charged state of 4.6V. Then discharge them to 2.0V at a constant current of 0.1C to obtain the discharge capacity, and calculate the discharge capacity in grams by the following formula:

[0064] Discharge gram capacity = discharge capacity / mass of lithium-rich manganese-based positive electrode material.

[0065] Cycle capacity retention rate test: Take one battery each from the embodiment and the comparative example, perform charge and discharge cycles on the lithium-ion battery through the following steps, and calculate the discharge capacity retention rate of the lithium-ion battery. In an environment of 45°C, charge and discharge at a constant current and constant voltage charge at a charging current of 0.2C until the upper limit voltage is 4.5V and the cutoff current is 0.02C; then leave it for 10 minutes; then perform constant current discharge at a discharge current of 0.2C until 2.0V. Cycle capacity retention rate test = (discharge capacity of the nth cycle / discharge capacity of the first cycle) × 100%.

[0066]

[0067]

[0068] It can be seen from the data in Table 1 that the first cycle coulombic efficiency of the lithium-rich manganese-based material after anion and cation co-doping is lower than that of the lithium-rich manganese-based material without multiple anion and cation co-doping, and the 0.1C discharge gram capacity is slightly reduced, but the cycle stability of the lithium-rich manganese-based material is improved. This may be because an appropriate amount of cation M replaces part of the lithium in the lithium-rich material. Since its atomic radius is larger than Li, it does not participate in the migration, resulting in a low gram capacity of the material. In addition, the doping of cation M increases the lattice constant c of the material, reduces the migration barrier of lithium ions, reduces the polarization of the material, and inhibits the migration of transition metal ions to the lithium layer to stabilize the structure. An appropriate amount of cation N can replace part of the transition metal elements such as Mn, Ni, and Co in the lithium-rich material. It can inhibit the migration and dissolution of transition metals, fix lattice oxygen, and make the crystal structure of the lithium-rich manganese-based positive electrode material more stable. At the same time, the negatively valenced R or Q element replaces the oxygen in the lithium-rich manganese-based positive electrode material to form a bond with stronger bond energy to replace the OR (R = Ni, Co, Mn) bond, making the structure of the lithium-rich manganese-based material more stable and improving the cycle stability of the material. The co-doping of multiple anions and cations has a synergistic effect, making the lithium-rich manganese-based materials co-doped with multiple anions and cations have better cycle stability.

[0069] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.

Claims

1. A co-doped lithium-rich manganese-based material, characterized in that: The chemical general formula is Li a-x M x Mn b N z Ni c Co d O 2-x-y R x Q y , where 1 < a ≤ 1.5, 0.4 ≤ b < 0.9, 0 < c ≤ 0.4, 0 ≤ d ≤ 0.4, 0 ≤ x ≤ 0.15, 0 ≤ y ≤ 0.2, 0 ≤ z ≤ 0.2, and b > c, b > d; M is a metal element; N is a transition metal element; R and Q are independently halogen elements.

2. The co-doped lithium-rich manganese-based material according to claim 1, characterized in that: M is a metal element replacing Li; N is a metal element replacing the transition metal elements Mn, Ni, and Co.

3. The co-doped lithium-rich manganese-based material according to claim 1, characterized in that: M is one or more of the elements Na, K, Rb, and Cs, is in a positive state in the compound, and its radius is larger than that of lithium ion; N is one or more of Mg, Al, Sn, La, Cr, Zr, Y, Ca, Ti, Zn, Fe, and V.

4. The co-doped lithium-rich manganese-based material according to claim 1, characterized in that: By molar ratio; M: Li = (0.0001 to 0.15): 1, preferably (0.01 to 0.05): 1; more preferably 0.01: 1; N:Mn=(0.0001-0.10):1, preferably (0.01-0.05):1; more preferably 0.01:1; R:O=(0.0001-0.3):1, preferably (0.01-0.1):1; more preferably 0.01:1; Q:O=(0.0001-0.3):1, preferably (0.01-0.1):1, more preferably (0.02-0.03):

1.

5. A method for preparing the co-doped lithium-rich manganese-based material according to any one of claims 1 to 4, characterized in that: The steps include: 1) Preparation of lithium-rich manganese-based cathode material precursor; the general chemical formula is (Mn b Ni c Co d )CO3, (Mn b Ni c Co d )(OH)2 or (Mn b Ni c Co d )O2, where b>c, b>d; 2) The precursor powder, lithium salt, halogen compound containing metal element M and halogen compound powder containing metal element N are uniformly mixed, and the anion-cation co-doped lithium-rich manganese-based positive electrode material is obtained after grinding, pre-calcination and calcination.

6. The preparation method according to claim 5, characterized in that: The lithium salt is one or more of lithium hydroxide, lithium nitrate, lithium carbonate, lithium oxalate, lithium acetate, lithium oxide, and lithium citrate; The halogen compound powder containing the metal element M is one or more of NaF, KF, RbF, NaCl, KCl, or RbCl; The halogen compound containing the metal element N is one or more of MgF2, AlF3, SnF4, LaF3, CrF3, ZrF4, YF3, CaF2, TiF4, ZnF2, FeF3, and VF3.

7. The preparation method according to claim 5, characterized in that: The pre-calcination is to pre-calcine the powder prepared in the above step at a temperature of 300-600° C. for 3-8 hours; the calcination is to pre-calcine the powder prepared in the above step at a temperature of 600-1000° C. for 8-20 hours.

8. A positive electrode sheet, characterized in that: Comprising the co-doped lithium-rich manganese-based material according to any one of claims 1 to 4, a positive electrode conductor and a positive electrode binder; Preferably, the conductive agent is positive electrode carbon nanotubes; preferably, the positive electrode binder is PVDF; Preferably, the mass ratio of the co-doped lithium-rich manganese-based material, the positive electrode conductor and the positive electrode binder is (90-98):(1-5):(1-5); preferably 96:2:

2.

9. A method for preparing the positive electrode sheet according to claim 8, characterized in that: The method comprises the following steps: fully and uniformly stirring the co-doped lithium-rich manganese-based material, the positive electrode conductive agent and the positive electrode binder in a solvent, coating the mixture on an aluminum foil, drying it and cold pressing it to obtain a positive electrode sheet.

10. A battery, characterized in that: The positive electrode sheet, the negative electrode sheet, the separator and the electrolyte according to claim 8; Preferably, the negative electrode sheet comprises a negative electrode active material, a negative electrode conductive agent and a negative electrode binder; preferably, the negative electrode active material is graphite; preferably, the negative electrode conductive agent is acetylene black; preferably, the negative electrode binder is a mixture of styrene-butadiene rubber and carboxymethyl cellulose; the mass ratio of the two is 1:1; Preferably, the diaphragm is a polyethylene porous polymer film; Preferably, the electrolyte comprises a lithium salt and an electrolyte solvent; Preferably, the lithium salt is LiPF6; preferably, the concentration of the lithium salt is 1 to 1.5 mol / L, preferably 1.2 mol / L; Preferably, the electrolyte solvent is a mixture of fluoroethylene carbonate: dimethyl carbonate: ethylene carbonate; preferably, the volume ratio of the three is 3:1:1.

Citation Information

Cited By

  • Lithium-rich manganese-based positive electrode material with combined action of surface heterojunction and bulk phase doping as well as preparation method and application of lithium-rich manganese-based positive electrode material

    CN120024944A

  • Positive electrode material, and preparation method therefor and use thereof

    WO2026153007A1