Gel-resisting and sodium-supplementing layered oxide sodium battery positive electrode slurry and preparation method thereof
By using platinum acid or ethylenediaminetetraacetic acid as an acid mixer in the sodium ion battery positive electrode slurry, neutralizing the alkalinity of the layered oxide surface and decomposing it to provide sodium supplementation during charging, the sodium ion battery positive electrode slurry is solved. The problem of gelation and inability to decompose sodium oxalate improves battery capacity and cycling performance.
Patent Information
- Application Number
- CN202411119755.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-15
- Publication Date
- 2024-11-22
AI Technical Summary
The positive electrode slurry of existing sodium ion battery is easily gelled during the preparation process, and sodium oxalate cannot decompose at a charging voltage of 4.0V, resulting in a decrease in the capacity of sodium ion battery and the impact of the circulation performance.
A positive electrode slurry containing layered oxides, conductive agents, adhesives, acid mixing agents and organic solvents is used. The acid mixing agent is plaster acid or ethylenediaminetetraacetic acid, which can dissolve in organic solvents and decompose the sodium salt. The voltage is not more than 4V, neutralizes the alkalinity of the layered oxide surface, avoids gelation, and decomposes during charging to provide sodium supplementation.
The gelation of the positive electrode slurry is effectively avoided, the coating performance and battery capacity are improved, the circulation performance and first charging efficiency are enhanced, and the sodium ion loss caused by the O'3 phase transition is reduced.
Smart Images

Figure CN119008952A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of sodium ion batteries, and in particular to an anti-gel and sodium-supplementing layered oxide sodium battery positive electrode slurry and a preparation method thereof. Background Art
[0002] Compared with lithium, sodium has similar physical and chemical properties. In addition, sodium is abundant, cheap, safe, and has excellent low-temperature discharge capability. Therefore, sodium-ion batteries are considered to be the most promising alternative to lithium-ion batteries. Layered oxides have high energy density as positive electrode materials for sodium-ion batteries and have broad application prospects.
[0003] In the prior art, the surface alkalinity of the layered oxide material used to prepare the positive electrode slurry is relatively high and it is easy to react with water to form sodium hydroxide, which makes the positive electrode slurry alkaline. Fluorine-containing adhesives (such as PVDF) will undergo a defluorination reaction under alkaline conditions, which will cause the positive electrode slurry to gel and become uncoatable. At the same time, when the moisture in the ambient air enters the positive electrode slurry during the homogenization process, it will also react with the layered oxide to form sodium hydroxide, making the positive electrode slurry alkaline and exacerbating the gelation.
[0004] The prior art generally adopts an anti-gel method of adding oxalic acid to the positive electrode slurry to neutralize the alkalinity of the slurry. However, sodium oxalate generated after the neutralization of oxalic acid and alkali can only be decomposed at 4.11V, but the layered oxide in the sodium ion battery may form an irreversible O'3 phase at 4.0V. This phase change is usually caused by the high oxidation state of the transition metal ions of the layered oxide and the deintercalation of sodium ions. The oxidation state of the transition metal increases, causing the oxygen atom structure in the material to change and form an O'3 phase. This structural transformation may destroy the layered structure of the material, obstructing the diffusion path of sodium ions, and thus affecting the battery's cycle performance and capacity retention. Because sodium oxalate cannot decompose and play a role in sodium supplementation under the upper limit voltage of 4.0V for sodium ion batteries with layered oxides, the number of sodium ions is reduced and the battery capacity decreases.
[0005] Therefore, it is necessary to propose an improvement plan for the existing technology. Summary of the invention
[0006] 1. Technical issues to be resolved
[0007] In view of the above-mentioned shortcomings and deficiencies of the prior art, the present invention provides a gel-resistant and sodium-supplementing layered oxide sodium battery positive electrode slurry and a preparation method thereof, which solves the technical problems of gelation of the sodium battery positive electrode slurry and the inability of sodium oxalate to decompose and supplement sodium at the first charging voltage in the prior art.
[0008] (II) Technical solution
[0009] In order to achieve the above object, the main technical solutions adopted by the present invention include:
[0010] In a first aspect, the present invention provides a gel-resistant and sodium-supplemented layered oxide sodium battery positive electrode slurry, comprising a layered oxide, a conductive agent, an adhesive, an acid regulator and an organic solvent, wherein the acid regulator is an acid that can be dissolved in an organic solvent and whose sodium salt has a decomposition voltage of no more than 4V.
[0011] According to a preferred embodiment of the present invention, the acid regulator is at least one selected from squaric acid and ethylenediaminetetraacetic acid.
[0012] According to a preferred embodiment of the present invention, the layered oxide sodium battery positive electrode slurry comprises, by weight: 92-97 parts of layered oxide, 0.5-3.5 parts of conductive agent, 1-3 parts of adhesive, 0.2-1.5 parts of acid regulator, and 50-70 parts of organic solvent; wherein the total weight of layered oxide, conductive agent, adhesive and acid regulator is 100 parts.
[0013] According to a preferred embodiment of the present invention, in order to avoid excessive addition of the acid regulator, which causes the excessive acid regulator to react with the electrolyte and consume the electrolyte, the amount of the acid regulator added is determined according to the pH of the layered oxide, as follows:
[0014] When the pH is less than 12.6, the amount of the acidifier is 0.2-0.4 parts (including the end point);
[0015] When the pH is less than 12.8 and greater than or equal to 12.6, the amount of the acidifier is 0.4-0.6 parts (including the upper limit end point);
[0016] When the pH is less than 13.0 and greater than or equal to 12.8, the amount of the acidifier is 0.7-1.0 parts (including the end points);
[0017] When the pH is less than 13.2 and greater than or equal to 13.0, the amount of the acidifier is 1.0-1.3 parts (including the upper limit);
[0018] When the pH is greater than or equal to 13.2, the amount of the acid regulator is 1.3-1.5 parts (including the upper limit endpoint).
[0019] According to a preferred embodiment of the present invention, the conductive agent is at least one selected from conductive carbon black, Ketjen black, conductive graphite, carbon nanotubes and graphene.
[0020] According to a preferred embodiment of the present invention, the adhesive is a fluorine-containing polymer adhesive, preferably polyvinylidene fluoride selected from at least one of polyvinylidene fluoride (PVDF), polytetrafluoroethylene (PTFE), fluorinated polyacrylate (FPA), fluorinated polyether (FPE), fluorinated polyurethane (FPU) and fluorinated polyvinyl pyrrolidone (FPVP).
[0021] According to a preferred embodiment of the present invention, the organic solvent is at least one of N-methylpyrrolidone (NMP) and dimethylformamide (DMF).
[0022] According to a preferred embodiment of the present invention, the layered oxide is Na x MO y , M is one or more metal elements, x, y satisfy the charge balance between the elements in the chemical formula. M is a metal element, including one or more of nickel, manganese, magnesium, copper, iron, cobalt, vanadium, titanium, chromium, zinc, etc.; x, y satisfy the charge balance; preferably, 0.5<x<1.5; y≥1; the charge balance between the elements in the chemical formula is satisfied. In addition, the layered oxide can also be a multi-component composite layered oxide Na x [Fe,Mn]O2 or Na x [Fe,Ni,Mn]O2 or layered oxides with special structures Na x Ni x Mn 1-x O2、Na x Ni 0.5 Mn 0.5 At least one of O2 and Na3NiFeMnO6.
[0023] In a second aspect, the present invention provides a method for preparing a slurry of a layered oxide positive electrode slurry that resists gelation and replenishes sodium, comprising the following steps:
[0024] S1: mixing the adhesive and the acid conditioning agent, adding a part of the total amount of the organic solvent and stirring, and obtaining a glue solution after stirring;
[0025] S2: After adding the conductive agent to the glue solution and stirring, slurry 1 is obtained;
[0026] S3: adding the layered oxide and the remaining organic solvent to the slurry 1, and stirring to obtain the slurry 2;
[0027] S4: After adjusting slurry 2 to 2000-6000 mPa*s, filter through a sieve to obtain positive electrode slurry.
[0028] According to a preferred embodiment of the present invention, a double planetary mixer is used for stirring. In S1, 75-85% of the total amount of organic solvent is added, and the stirring is carried out for 90-120 minutes at a revolution speed of 15-25 rpm and a rotation speed of 1800-2500 rpm; in S2, the stirring is carried out for 10-15 minutes at a revolution speed of 5-8 rpm and a rotation speed of 400-600 rpm; after the slurry is scraped, the stirring is carried out for 90-120 minutes at a revolution speed of 20-30 rpm and a rotation speed of 2300-2700 rpm; in S3, the stirring is carried out for 12-17 minutes at a revolution speed of 5-8 rpm and a rotation speed of 400-600 rpm; after the slurry is scraped, the stirring is carried out for 90-120 minutes at a revolution speed of 20-30 rpm and a rotation speed of 2300-2700 rpm. In S4, the positive electrode slurry is filtered with a 150-mesh screen to obtain the positive electrode slurry.
[0029] In a third aspect, the present invention provides a sodium battery positive electrode plate, which is prepared by coating the above-mentioned layered oxide sodium battery positive electrode slurry on the surface of the positive electrode collector and then baking it.
[0030] (III) Beneficial effects
[0031] The beneficial effects of the present invention are:
[0032] The present invention discloses a positive electrode slurry for a layered oxide sodium battery with anti-gel and sodium supplementation. Since the acid regulator used in the positive electrode slurry can neutralize the residual alkali on the surface of the layered oxide, the alkalinity of the positive electrode slurry can be weakened, the gelation of the positive electrode slurry of the fluorine-containing adhesive (such as PVDF) can be avoided, and the coating performance of the slurry can be improved. The decomposition voltage of the sodium salt formed by the reaction of the acid regulator with the residual alkali on the surface of the layered oxide does not exceed 4V (does not exceed the O'3 phase transition voltage of the layered oxide positive electrode material), so the sodium salt can be decomposed before reaching the O'3 phase transition voltage of the layered oxide positive electrode material. The Na + It can be used as a sodium supplement to replenish the sodium lost in the positive electrode material during the first charging process, thereby improving the first efficiency and then the capacity, compensating for the negative impact of the O'3 phase transition of the layered oxide positive electrode material on the battery cycle performance and capacity retention ability and the problem of battery capacity reduction caused by partial sodium loss.
[0033] Preferably, the acid regulator is squaric acid or ethylenediaminetetraacetic acid, and the acid regulator neutralizes with the residual alkali on the surface of the layered oxide to form sodium squarate (decomposition voltage is 3.6V) or EDTA-4Na (decomposition voltage is 3.79V); when the sodium battery is charged to 3.6-3.8V for the first time, sodium squarate or EDTA-4Na will decompose to form Na + , CO2, etc., Na +The sodium lost in the positive electrode material during the first charge can be replenished to improve the first efficiency and battery capacity of the sodium battery; the CO2, CO and other gases generated after the first charge can be discharged after cutting off the cell airbag (cutting off the cell airbag is a necessary step in the preparation process of the soft-pack battery) without affecting the battery performance. The present invention further selects the appropriate amount of acid regulator based on the pH of the layered oxide to avoid excessive acid regulator consuming the electrolyte. BRIEF DESCRIPTION OF THE DRAWINGS
[0034] Figure 1 1 is a discharge curve diagram of the sodium battery prepared with the positive electrode slurry of Example 1 and Comparative Example 1. DETAILED DESCRIPTION
[0035] In order to better explain the present invention and facilitate understanding, the present invention is described in detail below through specific implementation modes in conjunction with the accompanying drawings.
[0036] The present invention proposes a layered oxide sodium battery positive electrode slurry that resists gelation and sodium supplementation, comprising a layered oxide, a conductive agent, an adhesive, an acid regulator and an organic solvent, wherein the acid regulator is an acid or a combination of acids that can be dissolved in an organic solvent and whose sodium salt has a decomposition voltage of no more than 4V. In the prior art, the preparation process of the layered oxide and the characteristic that it cannot be washed with water will cause some difficult-to-remove residues (excessive sodium carbonate) to adhere to the surface of the layered oxide, which will cause the surface of the layered oxide to be more alkaline. In the subsequent pulping and stirring process, the layered oxide will also react with moisture in the air to produce sodium hydroxide. In order to prevent the fluorine-containing adhesive from gelling due to being in an alkaline environment during the pulping process of the positive electrode slurry, the present invention first disperses the acid regulator in an organic solvent to form an acidic environment, and then adds the layered oxide to the pulping process. The alkali will be immediately neutralized by the acid regulator to generate a sodium salt (avoiding defluorination of the fluorine-containing adhesive when encountering alkali). This part of sodium salt decomposes to produce sodium ions during the first charge. Sodium ions are added to the positive electrode material to play the role of sodium supplement, which improves the battery capacity. Carbon dioxide, carbon monoxide and other gases produced by the decomposition of sodium salt can be discharged by cutting the battery cell airbag during the production of soft-pack batteries, which does not affect the battery performance. The first charging voltage of sodium batteries is generally 4V. Excessive voltage will cause irreversible adverse reactions in the battery and reduce the number of battery cycles.
[0037] Preferably, the layered oxide sodium battery positive electrode slurry comprises, by weight: 92-97 parts of layered oxide, 0.5-3.5 parts of conductive agent, 1-3 parts of adhesive, 0.2-1.5 parts of acid regulator, and 50-70 parts of organic solvent; the total weight of layered oxide, conductive agent, adhesive, and acid regulator is 100. In order to avoid excessive acid regulator reacting with the electrolyte, resulting in the consumption of the electrolyte, preferably, the present invention adjusts the amount of acid regulator added according to the pH value (alkalinity) of the layered oxide, and the corresponding relationship between the number of acid regulators added and the pH value of the layered oxide is as follows:
[0038] When the pH is less than 12.6, the amount of the acidifier is 0.2-0.4 parts (including the end point);
[0039] When the pH is less than 12.8 and greater than or equal to 12.6, the amount of the acidifier is 0.4-0.6 parts (including the upper limit end point);
[0040] When the pH is less than 13.0 and greater than or equal to 12.8, the amount of the acidifier is 0.7-1.0 parts (including the end points);
[0041] When the pH is less than 13.2 and greater than or equal to 13.0, the amount of the acidifier is 1.0-1.3 parts (including the upper limit);
[0042] When the pH is greater than or equal to 13.2, the amount of the acid regulator is 1.3-1.5 parts (including the upper limit endpoint).
[0043] Preferably, the acid regulator can be at least one of squaric acid and ethylenediaminetetraacetic acid (EDTA), wherein squaric acid reacts with a base to generate sodium squarate, and the decomposition voltage of sodium squarate is 3.6V; ethylenediaminetetraacetic acid reacts with a base to generate sodium ethylenediaminetetraacetate (EDTA-4Na), and the decomposition voltage of sodium ethylenediaminetetraacetate is 3.79V.
[0044] Preferably, the conductive agent can be at least one of the conductive agents commonly used in battery manufacturing, such as conductive carbon black, Ketjen black, conductive graphite, carbon nanotubes, and graphene.
[0045] Preferably, the adhesive is a fluorine-containing polymer adhesive, preferably polyvinylidene fluoride selected from at least one of polyvinylidene fluoride (PVDF), polytetrafluoroethylene (PTFE), fluorinated polyacrylate (FPA), fluorinated polyether (FPE), fluorinated polyurethane (FPU) and fluorinated polyvinyl pyrrolidone (FPVP).
[0046] Preferably, the organic solvent may be N-methylpyrrolidone (NMP) or dimethylformamide (DMF).
[0047] Preferably, the layered oxide may be Na x MO y , M is a metal element, including one or more of nickel, manganese, magnesium, copper, iron, cobalt, vanadium, titanium, chromium, zinc, etc.; x, y satisfy charge balance; preferably, 0.5<x<1.5; y≥1; the charge balance between the elements in the chemical formula is satisfied. Specifically, the layered oxide can be NaFeO2 (sodium iron oxide), NaCoO2, NaNiO2 (sodium nickel oxide), NaMnO2 (sodium manganese oxide), NaCrO2 (sodium chromium oxide), NaTiO2 (sodium titanium oxide), Na xFePO4 (sodium iron phosphate), etc. In addition, the layered oxide can also be a multi-component composite layered oxide Na x [Fe,Mn]O2 or Na x [Fe,Ni,Mn]O2 or layered oxides with special structures Na x Ni x Mn 1-x O2 and Na x Ni 0.5 Mn 0.5 O2 or Na3NiFeMnO6.
[0048] The present invention also provides a method for preparing a slurry of a layered oxide positive electrode slurry that resists gelation and replenishes sodium, comprising the following steps:
[0049] S1: Mix the adhesive and the acid adjuster evenly under dry conditions, add 75-85% of the organic solvent, and stir them using a double planetary mixer. After the adhesive, the acid adjuster and the organic solvent are fully stirred, a glue solution is obtained. At this time, the glue solution is acidic and can directly neutralize the alkali introduced by the layered oxide in the subsequent stage. The stirring parameters are: revolution 15-25rmp, dispersion 1800-2500rmp, and time 90-120min.
[0050] S2: After adding the conductive agent to the glue, perform preliminary stirring, and then perform scraping. After scraping, stir again to obtain slurry 1; wherein the preliminary stirring parameters are: revolution 5-8rmp, dispersion 400-600rmp, and time 10-15min; after scraping, the parameters for stirring again are: revolution 20-30rmp, dispersion 2300-2700rmp, and time 90-120min.
[0051] S3: Add layered oxide and remaining organic solvent to slurry 1, perform preliminary stirring, perform scraping after preliminary stirring, and stir again after scraping to obtain slurry 2; wherein the preliminary stirring parameters are: revolution 5-8rmp, dispersion 400-600rmp, and time 12-17min; after scraping, the parameters for stirring again are revolution 20-30rmp, dispersion 2300-2700rmp, and time 90-120min.
[0052] S4: Test the viscosity of slurry 2, first determine the viscosity of slurry 2 when it is discharged, then let it stand for 8 hours to determine whether the slurry viscosity is within the range of 2000-6000mPa*s, and filter it if it is qualified to obtain positive electrode slurry; wherein, the filter pore size is 150 mesh; otherwise, use a small amount of organic solvent to adjust the slurry viscosity to within the range of 2000-6000mPa*s, and then use a 150-mesh sieve to filter it for use.
[0053] The present invention also provides a sodium battery positive electrode plate, which is prepared by coating the layered oxide sodium battery positive electrode slurry on the surface of the positive electrode collector and then baking it.
[0054] In order to better understand the above technical solution, exemplary embodiments of the present invention will be described in more detail below with reference to the accompanying drawings. Although exemplary embodiments of the present invention are shown in the accompanying drawings, it should be understood that the present invention can be implemented in various forms and should not be limited by the embodiments described herein. On the contrary, these embodiments are provided to enable a clearer and more thorough understanding of the present invention and to fully convey the scope of the present invention to those skilled in the art.
[0055] Example 1
[0056] This embodiment provides a positive electrode slurry, and its formula is: 94.7 parts of layered oxide Na3NiFeMnO6, pH 12.9; 2.5 parts of carbon nanotubes, 2 parts of polyvinylidene fluoride, 0.8 parts of squaric acid, and 60 parts of NMP.
[0057] The method for preparing the positive electrode slurry comprises the following steps:
[0058] S1: Mix polyvinylidene fluoride and squaric acid evenly under dry conditions, add 48 parts of NMP into the mixture, and stir. After the polyvinylidene fluoride, squaric acid and NMP are fully stirred, a glue solution is obtained. The stirring parameters are: revolution 25 rpm, dispersion 2500 rpm, and time 120 min.
[0059] S2: After adding carbon nanotubes to the glue, perform preliminary stirring, and then perform scraping. After scraping, stir to obtain slurry 1, wherein the preliminary stirring parameters are: revolution 7 rpm, dispersion 500 rpm, and time 10 min; the stirring parameters after scraping are: revolution 25 rpm, dispersion 2500 rpm, and time 100 min.
[0060] S3: Add layered oxide Na3NiFeMnO6 and 12 parts of NMP to slurry 1, carry out preliminary stirring, scrape the slurry after the preliminary stirring, and stir to obtain slurry 2 after scraping; wherein the preliminary stirring parameters are: revolution 7rmp, dispersion 500rmp, time is 15min; the stirring parameters after scraping are: 25rmp, dispersion 2500rmp, time is 100min.
[0061] S4: Testing the viscosity of slurry 2. After standing, the viscosity of the slurry is between 2000 and 6000 mPa*s. Filter with a 150-mesh sieve to obtain a positive electrode slurry.
[0062] Example 2
[0063] This embodiment provides a positive electrode slurry, the formula of which is: including 94.3 parts of layered oxide Na3NiFeMnO6, pH 13.1; 2.5 parts of carbon nanotubes, 2 parts of polytetrafluoroethylene, 1.2 parts of EDTA, and 60 parts of NMP. The preparation method is as shown in Example 1 to prepare the positive electrode slurry.
[0064] Example 3
[0065] The present embodiment provides a positive electrode slurry, the formula of which includes: 95.1 parts of layered oxide Na3NiFeMnO6, pH 12.4; 2.5 parts of Ketjen black, 2 parts of polyvinylidene fluoride, 0.4 parts of squaric acid, and 60 parts of NMP.
[0066] The method for preparing the positive electrode slurry comprises the following steps:
[0067] S1: Mix polyvinylidene fluoride and squaric acid evenly under dry conditions, add 45 parts of NMP into the mixture, and stir. After the polyvinylidene fluoride, squaric acid and NMP are fully stirred, a glue solution is obtained. The stirring parameters are: revolution 20 rpm, dispersion 2500 rpm, and time 120 min.
[0068] S2: After adding carbon nanotubes to the glue, perform preliminary stirring, and then perform scraping. After scraping, stir to obtain slurry 1, wherein the preliminary stirring parameters are: revolution 7 rpm, dispersion 500 rpm, and time 10 min; the stirring parameters after scraping are: revolution 25 rpm, dispersion 2500 rpm, and time 100 min.
[0069] S3: Add layered oxide Na3NiFeMnO6 and 15 parts of NMP to slurry 1, perform preliminary stirring, perform scraping after preliminary stirring, and stir after scraping to obtain slurry 2; wherein the preliminary stirring parameters are: revolution 7 rpm, dispersion 500 rpm, and time 15 min; the stirring parameters after scraping are revolution 25 rpm, dispersion 2500 rpm, and time 100 min.
[0070] S4: Testing the viscosity of slurry 2. After standing, the viscosity of the slurry is between 2000 and 6000 mPa*s. The slurry is filtered through a 150-mesh sieve to obtain a positive electrode slurry.
[0071] Example 4
[0072] This embodiment provides a positive electrode slurry, the formula of which includes: 92 parts of layered oxide Na3NiFeZnO6, pH 13.4; 3.5 parts of conductive carbon black, 1 part of polyvinylidene fluoride, 2 parts of polytetrafluoroethylene, 1.0 part of squaric acid, 0.5 part of EDTA, 50 parts of NMP. The preparation method is as shown in Example 3 to prepare the positive electrode slurry.
[0073] Example 5
[0074] This embodiment provides a positive electrode slurry and a preparation method and application thereof:
[0075] The positive electrode slurry formula includes: 97 parts of layered oxide Na3NiFeZnO6, pH 12.4; 1.1 parts of graphene, 0.7 parts of conductive graphite, 1 part of polyvinylidene fluoride, 0.2 parts of squaric acid, and 70 parts of NMP.
[0076] The method for preparing the positive electrode slurry comprises the following steps:
[0077] S1: Mix polyvinylidene fluoride and squaric acid evenly under dry conditions, add 56 parts of NMP into the mixture, and stir. After the polyvinylidene fluoride, squaric acid and NMP are fully stirred, a glue solution is obtained. The stirring parameters are: revolution 15 rpm, dispersion 1800 rpm, and time 120 min.
[0078] S2: After adding graphene and conductive graphite to the glue, preliminary stirring is carried out, and then scraping is carried out. After scraping, stirring is continued to obtain slurry 1, wherein the preliminary stirring parameters are: revolution 5rmp, dispersion 400rmp, and time 10min; the stirring parameters after scraping are: revolution 20rmp, dispersion 2300rmp, and time 120min.
[0079] S3: Add layered oxide Na3NiFeZnO6 and 14 parts of NMP to slurry 1, perform preliminary stirring, perform scraping after preliminary stirring, and continue stirring after scraping to obtain slurry 2; wherein the preliminary stirring parameters are: revolution 5 rpm, dispersion 400 rpm, and time 15 min; the stirring parameters after scraping are revolution 20 rpm, dispersion 2300 rpm, and time 120 min.
[0080] S4: Test the viscosity of slurry 2. After standing, the viscosity of the slurry is between 2000 and 6000 mPa*s. Then filter through a 150 mesh to obtain a positive electrode slurry.
[0081] Example 6
[0082] This embodiment provides a positive electrode slurry and a preparation method and application thereof:
[0083] The positive electrode slurry formula includes: 97 parts of layered oxide NaFeO2, pH 13.0; 0.5 parts of graphene, 1.5 parts of polyvinylidene fluoride, 1 part of squaric acid, and 60 parts of NMP. The preparation method is as shown in Example 5 to prepare the positive electrode slurry.
[0084] Comparative Example 1
[0085] This comparative example provides a positive electrode slurry, which is different from Example 1 in that the positive electrode slurry formula is: 94.7 parts of layered oxide Na3NiFeMnO6, pH 12.9; 2.5 parts of carbon nanotubes, 2.1 parts of polyvinylidene fluoride, 0.2 parts of squaric acid, and 60 parts of NMP. The preparation method of the positive electrode slurry is as shown in Example 1.
[0086] Comparative Example 2
[0087] This comparative example provides a positive electrode slurry and its preparation method and application. The difference from Example 1 is that the positive electrode slurry formula is 94.7 parts of layered oxide Na3NiFeMnO6, pH is 12.9; 2.5 parts of carbon nanotubes, 2 parts of polyvinylidene fluoride, 1.2 parts of squaric acid, and 60 parts of NMP. The preparation method of the positive electrode slurry is shown in Example 1.
[0088] Comparative Example 3
[0089] This comparative example provides a positive electrode slurry and its preparation method and application. The difference from Example 1 is that the positive electrode slurry formula is 94.7 parts of layered oxide Na3NiFeMnO6, pH is 12.9; 2.5 parts of carbon nanotubes, 2 parts of polyvinylidene fluoride, 0.4 parts of oxalic acid, and 60 parts of NMP. The preparation method of the positive electrode slurry is shown in Example 1.
[0090] Comparative Example 4
[0091] This comparative example provides a positive electrode slurry and its preparation method and application. The difference from Example 1 is that the positive electrode slurry formula is 94.7 parts of layered oxide Na3NiFeMnO6, pH 12.9; 2.5 parts of carbon nanotubes, 2 parts of polyvinylidene fluoride, and 60 parts of NMP. The preparation method of the positive electrode slurry is shown in Example 1.
[0092] The positive electrode slurry of Examples 1-6 and Comparative Examples 1-4 was used to prepare the positive electrode of the sodium battery and the battery was assembled as follows: the positive electrode slurry was coated on the aluminum foil, and the positive electrode sheet was obtained after drying, rolling, slitting and welding the pole ear; the negative electrode used hard carbon as the active material, mixed with the conductive agent and the adhesive, and then coated on the aluminum foil, and the negative electrode sheet was also obtained after drying, rolling, slitting and welding the pole ear; the negative electrode sheet, the positive electrode sheet and the separator were prepared into a winding core by winding, and then the winding core was assembled into a 0455129 type soft package battery after shelling, top and side sealing, baking, liquid injection and sealing. After the pre-chemical and capacity division process, the airbag was cut off and the secondary sealing was performed.
[0093] The electrochemical performance test of the above assembled battery is carried out as follows:
[0094] In the pre-charge process, the battery is charged to 4.0V at a current rate of 0.05C, and then charged at a constant voltage with a cut-off of 0.05C. After being left for 10 minutes, the battery is discharged at a current rate of 1C in the capacity division process, and the cut-off voltage is 2.0V.
[0095] The test data are shown in Table 1 below, where the discharge curves of the sodium batteries prepared using the positive electrode slurries of Example 1 and Comparative Example 4 are as follows: Figure 1 shown.
[0096] Table 1: Electrochemical performance of various sodium-ion batteries
[0097]
[0098]
[0099] As can be seen from the above table, after the battery positive electrode slurry of each embodiment of the present invention and comparative example 3 was left standing for 8 hours, the slurry viscosity only increased slightly compared with the discharge viscosity, but the slurry viscosity after standing was still within the range of 2000-6000mPa*s, which did not affect the normal coating of the positive electrode slurry on the current collector and the preparation quality of the positive electrode of the sodium battery. However, the viscosity of the positive electrode slurry in comparative examples 1 and 4 increased significantly after standing for 8 hours, exceeding the viscosity range required for slurry coating, especially in comparative example 4, due to the lack of an acid conditioning agent, the slurry was significantly gelled after standing, and the gelled positive electrode slurry was difficult to be smoothly coated on the current collector. Although an acid regulator is added to the positive electrode slurry in Comparative Example 1, the amount of the acid regulator added is still less than the strong alkalinity of the layered oxide, resulting in gelation during the coating process of the positive electrode slurry. This is mainly because the acid regulator is not enough to neutralize the alkalinity of the layered oxide and the environmental moisture enters the positive electrode slurry during the coating process, which aggravates the gelation of the slurry. This also leads to the sodium battery prepared by the positive electrode slurry of Comparative Examples 1 and 4. The first discharge efficiency, gram capacity, cycle retention rate and other aspects are significantly deteriorated. The amount of acid regulator used in Comparative Example 2 is high, which will consume part of the electrolyte and have a certain negative impact on the performance of the battery. Comparative Example 3 uses oxalic acid as an acid regulator to prepare the positive electrode slurry. Although it can prevent the slurry from gelling and ensure the good coating performance of the slurry, sodium oxalate cannot act as a sodium supplement during the first charging process, so its battery performance is poorer than that of Examples 1-5 of the present invention.
[0100] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or replace some or all of the technical features therein with equivalents. However, these modifications or replacements do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of the present invention.
Claims
1. A gel-resistant and sodium-supplementing layered oxide sodium battery positive electrode slurry, characterized in that: The invention comprises layered oxide, conductive agent, adhesive, acid regulator and organic solvent, wherein the acid regulator is an acid which can be dissolved in the organic solvent and the decomposition voltage of the sodium salt of which does not exceed 4V.
2. The layered oxide sodium battery positive electrode slurry according to claim 1, characterized in that: The acid regulator is at least one selected from squaric acid and ethylenediaminetetraacetic acid.
3. The layered oxide sodium battery positive electrode slurry according to claim 1, characterized in that: The layered oxide sodium battery positive electrode slurry comprises, by weight: 92-97 parts of layered oxide, 0.5-3.5 parts of conductive agent, 1-3 parts of adhesive, 0.2-1.5 parts of acid regulator, and 50-70 parts of organic solvent; wherein the total weight of the layered oxide, conductive agent, adhesive and acid regulator is 100 parts.
4. The layered oxide sodium battery positive electrode slurry according to claim 1, characterized in that: The amount of acid regulator added is determined according to the pH of the layered oxide, as follows: When the pH is less than 12.6, the amount of acidifier is 0.2-0.4 parts; When the pH is less than 12.8 and greater than or equal to 12.6, the amount of acidifier is 0.4-0.6 parts; When the pH is less than 13.0 and greater than or equal to 12.8, the amount of acidifier is 0.7-1.0 parts; When the pH is less than 13.2 and greater than or equal to 13.0, the amount of acidifier is 1.0-1.3 parts; When the pH is greater than or equal to 13.2, the amount of the acidifier is 1.3-1.5 parts.
5. The layered oxide sodium battery positive electrode slurry according to claim 1, characterized in that: The conductive agent is at least one selected from conductive carbon black, Ketjen black, conductive graphite, carbon nanotubes and graphene.
6. The layered oxide sodium battery positive electrode slurry according to claim 1, characterized in that: The adhesive is a fluorine-containing polymer adhesive, specifically polyvinylidene fluoride selected from at least one of polyvinylidene fluoride (PVDF), polytetrafluoroethylene (PTFE), fluorinated polyacrylate (FPA), fluorinated polyether (FPE), fluorinated polyurethane (FPU) and fluorinated polyvinyl pyrrolidone (FPVP).
7. The layered oxide sodium battery positive electrode slurry according to claim 1, characterized in that: The organic solvent is at least one of N-methylpyrrolidone (NMP) and dimethylformamide (DMF).
8. The layered oxide sodium battery positive electrode slurry according to claim 1, characterized in that: The layered oxide is selected from NaFeO2, NaCoO2, NaNiO2, NaMnO2, NaCrO2, NaTiO2, Na x FePO4、Na x [Fe,Mn]O2、Na x [Fe,Ni,Mn]O2,Na x Ni x Mn 1-x O2、Na x Ni 0.5 Mn 0.5 At least one of O2 and Na3NiFeMnO6.
9. A method for preparing a slurry of a layered oxide positive electrode slurry that resists gelation and replenishes sodium, characterized in that: It includes the following steps: S1: mixing the adhesive and the acid conditioning agent, adding a part of the total amount of the organic solvent and stirring, and obtaining a glue solution after stirring; S2: After adding the conductive agent to the glue solution and stirring, slurry 1 is obtained; S3: adding the layered oxide and the remaining organic solvent to the slurry 1, and stirring to obtain the slurry 2; S4: After adjusting slurry 2 to 2000-6000 mPa*s, filter through a sieve to obtain positive electrode slurry.
10. A sodium battery positive electrode sheet, which is prepared by coating the layered oxide sodium battery positive electrode slurry according to any one of claims 1 to 9 on the surface of a positive electrode collector and then baking.