Composite material, composite sheet, and preparation method and application thereof

By using the tafl-shaped structure of LiVxAl1-xPO4F and LiAlPO4F in the oxide-type all-solid state battery of lithium-ion secondary batteries, the close combination of electrolyte and positive electrode is achieved, the interface contact problem is solved, and the battery's magnification and low temperature are improved. Performance, suitable for large-scale production.

CN119009063APending Publication Date: 2024-11-22LIONGO (CHANGZHOU) NEW ENERGY CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411102729.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-12
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

Due to the interface contact problem, the oxide-type all-solid state battery of lithium-ion secondary batteries has high internal resistance and limited lithium-ion transmission rate. The existing deposition technology is high cost and low production efficiency, and the porous structure manufacturing is complex, making it difficult to achieve large-scale Production and industrialization.

Method used

Using composite materials, including a positive electrode active material layer and a solid electrolyte layer formed in situ, the taflite-shaped structure of LiVxAl1-xPO4F and LiAlPO4F can achieve tight and solid atoms between the electrolyte and the positive electrode through hydrothermal reaction and high-temperature and high-pressure ion exchange reaction. Combining stages reduces interface impedance.

Benefits of technology

It significantly improves the rate performance and low temperature performance of all solid-state batteries, achieves low internal resistance and high capacity, and is simple in preparation process, which is suitable for large-scale production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004989926070000241
    Figure BDA0004989926070000241
  • Figure HDA0004989926160000011
    Figure HDA0004989926160000011
  • Figure HDA0004989926160000012
    Figure HDA0004989926160000012
Patent Text Reader

Abstract

The invention provides a composite material. The composite material comprises a positive electrode active material layer and a solid electrolyte layer formed on the surface of the positive electrode active material layer in situ, the positive electrode active material layer comprises LiV < x > Al < 1-x > PO < 4 > F, and the solid electrolyte layer comprises LiAl < 4 > O < 4 > F. The invention also provides a composite sheet comprising the composite material and an all-solid-state battery. In the composite material provided by the invention, the positive electrode active material and the solid electrolyte both belong to a taffeta-type structure, the electrolyte and the positive electrode are in tight and firm atomic-scale combination, the problem of interface contact between the electrolyte and the positive electrode is solved, meanwhile, the LiAlPO4F solid electrolyte has relatively high lithium affinity, and after lithium is molten on the electrolyte, the solid electrolyte can be separated from the positive electrode. The positive electrode-electrolyte-negative electrode compact structure is obtained, so that the prepared all-solid-state battery shows extremely low interface impedance and high rate capability, and also has the performance advantage which can still be normally exerted at low temperature.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of battery technology, and in particular to a composite material, a composite sheet, a preparation method thereof and applications thereof. Background Art

[0002] Lithium-ion secondary batteries have high energy density, low self-discharge rate and long life, but lithium-ion secondary batteries using liquid electrolytes also have prominent safety issues and capacity limitations. All-solid-state batteries are batteries that use solid electrodes and solid electrolytes. Their structure consists of a positive electrode layer with a current collector and a negative electrode layer sandwiched between a solid electrolyte layer. All-solid-state batteries have good safety performance and have been seen in recent years as batteries that can inherit the status of lithium-ion batteries.

[0003] Based on the raw materials of solid electrolytes, all-solid-state batteries can be classified into oxide-type all-solid-state batteries, polymer-type all-solid-state batteries and sulfide-type all-solid-state batteries. Oxide-type solid electrolytes are classified into crystalline solid electrolytes or amorphous solid electrolytes. The ionic conductivity of crystalline solid electrolytes is higher than that of amorphous solid electrolytes, so crystalline solid electrolytes have attracted widespread attention as solid electrolytes for next-generation batteries. The main problem with the application of oxide solid electrolytes in all-solid-state batteries is the interface contact. The low solid-solid interface contact between the solid electrolyte and the electrode leads to extremely large internal resistance, resulting in a reduction in lithium ion channels and stress accumulation, which limits the transmission rate of lithium ions.

[0004] In order to solve the point-to-point contact problem of the cathode / oxide solid electrolyte interface and increase the interface contact area, the prior art discloses a variety of methods, including the use of deposition techniques such as chemical vapor deposition, pulsed laser deposition (PLD), atomic layer deposition (ALD), magnetron sputtering, etc., to deposit an oxide solid electrolyte film on the cathode, or to deposit the cathode material on oxide solid electrolyte particles. These deposition techniques can greatly improve the interface contact problem, but the deposition technology requires expensive equipment and high energy consumption, and the production efficiency is extremely low. At the same time, the deposited material is also very easy to fall off during use. The prior art also discloses the use of porous and multilayer structures to solve the above problems, wherein the porous layer can be used as a high-load carrier for the cathode material and the lithium metal anode, which will greatly increase the contact area, but usually requires a complex manufacturing process, which may limit the repeatability and stability of large-scale production and industrialization of such a structure. The prior art also discloses a preparation method by modifying the traditional cathode, such as preparing a flexible cathode, etc., but the flexible cathode is still in point-to-point contact with the electrolyte. Summary of the invention

[0005] In view of this, the present invention provides a composite material, a composite sheet, a preparation method and an application thereof. In the composite material provided in the present application, the positive electrode and the electrolyte are tightly combined, which greatly reduces the interface resistance. When used in an all-solid-state battery, the rate performance and low-temperature performance of the all-solid-state battery can be improved.

[0006] The present application provides a composite material, comprising a positive electrode active material layer and a solid electrolyte layer formed in situ on the surface of the positive electrode active material layer;

[0007] The positive electrode active material layer includes a positive electrode active material represented by formula (I):

[0008] V x Al 1-x PO4F formula (I);

[0009] In formula (I), 0.8≤x≤0.9;

[0010] The solid electrolyte layer includes LiAlPO4F.

[0011] The composite material provided in the present application comprises a positive electrode active material layer and a solid electrolyte layer formed in situ on the surface of the positive electrode active material layer, wherein the positive electrode active material layer comprises a positive electrode active material represented by formula (I): LiV x Al 1-x PO4F formula (I); the solid electrolyte layer comprises LiAlPO4F; LiV x Al 1-x PO4F and LiAlPO4F both belong to the taffeta structure. According to the principle of like dissolves like, the electrolyte and the positive electrode are tightly and firmly bonded at the atomic level, which solves the problem of interface contact between the electrolyte and the positive electrode. At the same time, LiAlPO4F solid electrolyte has strong lithium affinity. By melting lithium on the electrolyte, a tight structure of positive electrode-electrolyte-negative electrode is obtained. The prepared all-solid-state battery exhibits extremely low interface impedance and high rate performance, and has the performance advantage of being able to function normally at low temperatures.

[0012] The composite material provided in the present application comprises a positive electrode active material layer, wherein the positive electrode active material layer comprises a positive electrode active material represented by formula (I):

[0013] V x Al 1-x PO4F formula (I);

[0014] In formula (I), 0.8≤x≤0.9.

[0015] Cathode active material LiV x Al 1-xPO4F has a taffeta structure, wherein x is 0.8, 0.83, 0.85, 0.88 or 0.9, or any value between 0.8 and 0.9. In some specific implementations, the positive electrode active material LiV x Al 1-x There is no special restriction on the source of PO4F, which can be purchased from the market or prepared by oneself. x Al 1-x When PO4F is prepared by itself, the present application has no special restrictions on its preparation method, and it can be prepared according to the following method:

[0016] V x Al 1-x PO4 and LiF are mixed evenly and then subjected to hydrothermal reaction, and LiV is obtained after drying. x Al 1-x PO4F.

[0017] This application is based on V x Al 1-x PO4 is the raw material, and this application has no special restrictions on its source. It can be purchased on the market or prepared by itself. x Al 1-x When PO4 is prepared by itself, the present application has no special restrictions on its preparation method, and it can be prepared according to the following method:

[0018] The vanadium source, aluminum source, phosphorus source and carbon source are mixed and heat treated to obtain V x Al 1-x PO4.

[0019] In some specific implementations, the vanadium source includes but is not limited to vanadium pentoxide. The aluminum source includes but is not limited to one or more of aluminum oxide, aluminum hydroxide and aluminum nitrate. When the aluminum source is selected from multiple of them, the present application has no special restrictions on the proportion of each specific substance. In some specific implementations, the phosphorus source includes but is not limited to one or more of diammonium hydrogen phosphate and ammonium dihydrogen phosphate. When the phosphorus source is selected from multiple of them, the present application has no special restrictions on the proportion of each specific substance. In some specific implementations, the carbon source includes but is not limited to one or more of carbon black, sucrose, glucose and citric acid. When the carbon source is selected from multiple of them, the present application has no special restrictions on the proportion of each specific substance. In some specific implementations, the molar ratio of the vanadium source, aluminum source, phosphorus source and carbon source is (0.45-0.4): (0.05-0.2): 1: (1.2-1.5), preferably (0.45-0.4): (0.1-0.15): 1: (1.2-1.5).

[0020] The present application first mixes a vanadium source, an aluminum source, a phosphorus source and a carbon source, and preferably grinds them to obtain a mixed slurry. In some specific implementations, the grinding includes but is not limited to a planetary mill or a stirred mill. Specifically, the present application disperses the vanadium source, the aluminum source, the phosphorus source and the carbon source in a solvent for grinding, and the grinding time is 1h to 3h, preferably 1.5h to 2.5h. In some specific implementations, the ratio of the solvent mass to the total mass of the vanadium source, the aluminum source, the phosphorus source and the carbon source is 2:1 to 5:1, preferably 2.5 to 4.5:1. In some specific implementations, the solvent includes but is not limited to one or more of deionized water, anhydrous ethanol, isopropanol and N-methylpyrrolidone, preferably deionized water. When the solvent is a plurality of them, the present application has no special restrictions on the specific proportion of each substance. In some specific implementations, the material of the grinding ball used in grinding is but is not limited to zirconia balls, aluminum oxide balls or agate balls, preferably zirconia balls. In some specific implementations, the diameter of the grinding ball is 0.6mm to 3mm, preferably 3mm. In some specific implementations, the grinding rotation speed is preferably 300 rpm to 500 rpm, preferably 350 rpm to 450 rpm.

[0021] After grinding, the obtained slurry is preferably dried. The present application has no particular restrictions on the temperature and time of the drying, and the slurry can be dried. In some specific embodiments, the drying is specifically drying, and the drying temperature is preferably 100°C to 120°C, and more preferably 105°C to 115°C.

[0022] After drying, the obtained slurry is heat treated to obtain V x Al 1-x PO4. In some specific implementations, the heat treatment is preferably carried out in an argon atmosphere, the temperature of the heat treatment is preferably 700°C to 800°C, and the time is preferably 4h to 6h. In some specific implementations, the heat treatment is carried out in a tube furnace.

[0023] In this application, V x Al 1-x PO4 and LiF are mixed evenly and then subjected to hydrothermal reaction, and LiV is obtained after drying. x Al 1- x In some specific implementations, the reaction medium of the hydrothermal reaction is water, preferably deionized water. x Al 1-x PO4 and LiF are preferably mixed uniformly in the reaction medium. In some specific implementations, V x Al 1-xThe molar ratio of PO4 to LiF is preferably 1:0.9 to 1.1, more preferably 1:1. In some specific implementations, the temperature of the hydrothermal reaction is 200°C to 300°C, and the time is preferably 36h to 48h. In some specific implementations, the hydrothermal reaction is carried out in a hydrothermal kettle.

[0024] After the reaction is completed, the obtained reaction product is preferably washed and dried. In some specific implementations, the obtained reaction product is preferably washed with deionized water. In some specific implementations, the drying temperature is preferably 200° C. to 300° C., and the drying time is preferably 30 min to 60 min.

[0025] In some specific implementations, the positive electrode active material layer is a positive electrode active material LiV x Al 1-x The dense structure formed by PO4F. In some specific implementations, the thickness of the positive electrode active material layer is 20 μm to 50 μm, preferably 25 μm to 45 μm.

[0026] The present application has no particular limitation on the method for preparing the positive electrode active material layer, and the positive electrode active material layer can be prepared according to the following method:

[0027] The positive electrode active material LiV x Al 1-x PO4F, a plasticizer and a binder are mixed to prepare a glue to obtain a glue solution;

[0028] The glue solution is coated on the surface of the release film, the release film is removed after drying, and the positive electrode active material layer is obtained after sintering.

[0029] In some specific implementations, the present application preferably uses the positive electrode active material LiV x Al 1-x PO4F is ground. In some specific implementations, the grinding includes but is not limited to a planetary mill or a stirring mill. Specifically, the positive electrode active material LiV x Al 1-x PO4F is dispersed in a solvent and ground for 10 to 40 minutes, preferably 20 to 40 minutes, and more preferably 15 to 35 minutes. In some specific implementations, the quality of the solvent is related to the positive electrode active material LiV x Al 1-xThe ratio of PO4F is 5 to 20:1, preferably 10 to 20:1, and more preferably 10 to 15:1. In some specific implementations, the solvent includes but is not limited to one or more of deionized water, anhydrous ethanol, isopropanol and N-methylpyrrolidone, preferably deionized water. When the solvent is more than one of them, the present application has no special restrictions on the specific proportions of each substance. In some specific implementations, the material of the grinding balls used in grinding includes but is not limited to zirconia balls, alumina balls or agate balls, preferably zirconia balls. In some specific implementations, the diameter of the grinding balls is 0.6 mm to 3 mm, preferably 3 mm. In some specific implementations, the grinding speed is preferably 300 rpm to 500 rpm, preferably 350 rpm to 450 rpm.

[0030] The ground positive electrode active material LiV x Al 1-x PO4F is mixed with a plasticizer and a binder to obtain a glue solution. In some specific implementations, the plasticizer includes but is not limited to dimethyl phthalate, diethyl phthalate, di-n-butyl phthalate, dioctyl phthalate, and butyl benzyl phthalate. Dimethyl phthalate is preferred. When the plasticizer is multiple, the present application has no special restrictions on the proportion of each substance therein. In some specific implementations, the binder includes but is not limited to polyvinyl alcohol, polyvinyl butyral, polyacrylic acid, and polyacrylonitrile, preferably polyvinyl alcohol. In some specific implementations, the positive electrode active material LiV x Al 1-x The mass ratio of PO4F, plasticizer and binder is preferably 5-20:1:1, preferably 10-15:1:1. In some specific implementations, the ground positive electrode active material LiV x Al 1-x PO4F is mixed with a plasticizer and a binder in water to prepare a glue, and more preferably in deionized water. In some specific implementations, the mixing is preferably performed using a homogenizer for 10 to 20 minutes.

[0031] After mixing, the obtained glue is preferably ground. In some specific implementations, the grinding speed is preferably 400rpm to 500rpm, and the time is preferably 20 to 40min. After grinding, the obtained glue is coated on a release film substrate, wherein the function of the release film substrate is to provide support for the glue to form a positive electrode active material layer. In some specific implementations, the base film includes but is not limited to a polyethylene release film, a polyethylene terephthalate release film or a polypropylene release film. In some specific implementations, the coating thickness of the glue is preferably 40μm to 60μm, preferably 45μm to 55μm.

[0032] The coated glue solution is dried, preferably at room temperature, and the drying time is preferably 10 hours to 20 hours. After drying, the release film substrate is removed, and the obtained sample is sintered to make the positive electrode active material LiV x Al 1- x PO4F forms a dense positive electrode active material layer. In some specific implementations, the sintering temperature is preferably 700-800° C., and the sintering time is preferably 6-8 hours.

[0033] The composite material provided in the present application also includes a solid electrolyte layer formed in situ on the surface of the positive electrode active material layer, and the solid electrolyte layer includes LiAlPO4F. LiAlPO4F and the positive electrode active material have the same taffeta structure. When formed in situ on the surface of the positive electrode active material layer, the interface resistance between the electrode and the solid electrolyte can be significantly reduced. In some specific implementations, the thickness of the solid electrolyte layer is 1 μm to 2 μm.

[0034] In some specific implementations, the solid electrolyte layer is formed of LiAlPO4F. The present application has no particular limitation on the preparation method thereof, and the solid electrolyte layer can be prepared according to the following method:

[0035] Aluminum salt is deposited on the surface of the positive electrode active material layer to undergo a replacement reaction, thereby generating LiAlPO4F in situ.

[0036] The present invention forms LiAlPO4F in situ by reacting aluminum salt with the surface of the positive electrode active material layer under high temperature and high pressure. In some specific implementations, the aluminum salt includes but is not limited to aluminum nitrate or aluminum chloride, for example, Al(NO3)3·9H2O or AlCl3. The aluminum salt powder is deposited on the surface of the positive electrode active material layer, and the mass ratio of the aluminum salt to the area of ​​the positive electrode active material layer is 1g to 2g: 200mm 2 ~400mm 2 , preferably 1g~2g: 250mm 2 ~350mm 2 In some specific implementations, the replacement reaction pressure is 1MPa to 3MPa, preferably 1.5MPa to 2.5MPa; the temperature is 80°C to 200°C, preferably 90°C to 190°C; the time is 1h to 2h, preferably 1.2h to 1.8h. In some specific implementations, the replacement reaction can be carried out in a high pressure furnace.

[0037] After the replacement reaction is completed, the obtained product is washed, preferably with deionized water for 3 to 6 times, and then dried to obtain LiV x Al1-x PO4F-LiAlPO4F composite sheet. In some specific implementations, the drying can be carried out in a tube furnace with an argon flow, and the drying temperature is preferably 80°C to 120°C, more preferably 100°C. In some specific implementations, the thickness of the solid electrolyte layer is preferably 1 μm to 2 μm, preferably 1.2 μm to 1.8 μm.

[0038] The present application forms a solid electrolyte layer including LiAlPO4F in situ on a positive electrode active material layer including a positive electrode active material represented by formula (I), which can achieve tight and strong atomic-level bonding, solve the problem of interfacial contact between the electrolyte and the positive electrode, and enable the prepared all-solid-state battery to exhibit extremely low interfacial impedance and high rate performance, while having the performance advantage of being able to function normally at low temperatures.

[0039] The present application also provides a composite sheet, comprising: a positive electrode current collector, a positive electrode conductive layer formed on the surface of the positive electrode current collector, and a composite material formed on the surface of the conductive layer;

[0040] The composite material comprises a positive electrode active material layer formed on the surface of the conductive layer and a solid electrolyte layer formed in situ on the surface of the positive electrode active material layer;

[0041] The positive electrode active material layer includes a positive electrode active material represented by formula (I):

[0042] V x Al 1-x PO4F formula (I);

[0043] In formula (I), 0.8≤x≤0.9;

[0044] The solid electrolyte layer includes LiAlPO4F.

[0045] The composite sheet provided in the present application includes a positive electrode current collector, which may be a metal foil, including but not limited to aluminum foil, nickel foil, stainless steel, etc., preferably aluminum foil.

[0046] A positive electrode conductive layer is formed on the surface of the positive electrode current collector, and the positive electrode conductive layer includes a conductive agent and an adhesive for bonding the positive electrode current collector and the composite material. In some specific implementations, the conductive agent includes but is not limited to carbon black, hard carbon, graphite, carbon nanotubes, graphene, silver powder, nickel powder, tin oxide, conductive titanium dioxide, etc., and can be one or more of them. When the conductive agent is a mixture of multiple specific substances, the present application does not make too many restrictions on the ratio between each specific substance. The adhesive includes but is not limited to polyvinylidene fluoride, polytetrafluoroethylene, polyacrylic acid, polyamide, lithium polyacrylate, methacrylate, sodium polymethylcellulose, aluminum dihydrogen phosphate, etc., and can be one or more of them. When the adhesive is a mixture of multiple specific substances, the present application does not make too many restrictions on the ratio between each specific substance. In some specific implementations, the mass ratio of the conductive agent and the adhesive is preferably 1 to 2:1 to 2, and more preferably 1:1.

[0047] The composite material described in the above technical solution is formed on the surface of the positive electrode conductive layer, and the positive electrode conductive layer is in contact with the positive electrode active material layer.

[0048] In some specific implementations, the composite sheet further includes a negative electrode active material layer formed on the surface of the solid electrolyte layer. In some specific implementations, the negative electrode active material layer is preferably a metal lithium sheet. The present application has no particular restrictions on the formation method of the negative electrode active material layer, and a method commonly used by those skilled in the art may be used.

[0049] In some specific implementations, the composite sheet also includes a negative electrode conductive layer formed on the negative electrode active material layer and a negative electrode current collector formed on the negative electrode conductive layer. In some specific implementations, the negative electrode conductive layer includes a conductive agent, a binder and a thickener. In some specific implementations, the mass ratio of the conductive agent, the binder and the thickener is 0.05-1:0.01-1:1-20, preferably 0.1-0.5:0.1-0.5:5-15. In some specific implementations, the conductive agent includes but is not limited to carbon black, hard carbon, graphite, carbon nanotubes, graphene, silver powder, nickel powder, tin oxide, conductive titanium dioxide, etc., and can be one or more of them. When the conductive agent is a mixture of multiple specific substances, this application does not make too many restrictions on the ratio between the specific substances. The binder includes but is not limited to styrene-butadiene rubber (SBR), polyacrylic acid (PAA), polyvinyl butyral (PVB), etc., and can be one or more thereof. When the binder is a mixture of multiple specific substances, the present application does not make too many restrictions on the ratio between the specific substances. The thickener includes but is not limited to sodium carboxymethyl cellulose (CMC), methyl cellulose (MC), ethyl cellulose (EC), hydroxyethyl cellulose (HEC), etc., and can be one or more thereof. When the thickener is a mixture of multiple specific substances, the present application does not make too many restrictions on the ratio between the specific substances.

[0050] In some specific implementations, the negative electrode current collector may be a metal foil, including but not limited to aluminum foil, nickel foil, stainless steel, etc. For example, the negative electrode current collector may be aluminum foil.

[0051] The present application has no special restrictions on the preparation method of the composite sheet, and the composite sheet can be prepared according to the following method:

[0052] forming a negative electrode active material layer on one side of the composite material solid electrolyte layer;

[0053] The positive electrode conductive layer slurry is coated on the surface of the positive electrode current collector, and the negative electrode conductive layer slurry is coated on the surface of the negative electrode current collector. One side of the positive electrode active material layer of the composite material is laminated with the positive electrode conductive layer slurry, and one side of the negative electrode active material layer is laminated with the negative electrode conductive layer slurry. After baking, a composite sheet is obtained.

[0054] The present application first forms a negative electrode active material layer on one side of the composite material solid electrolyte layer. The present application has no special restrictions on its formation method. For example, when the negative electrode active material layer is a metal lithium sheet, it can be prepared according to the following method:

[0055] The metal lithium sheet is laminated to one side of the composite material solid electrolyte layer and then heat treated to fuse the metal lithium sheet with the solid electrolyte layer.

[0056] In some specific implementations, the heat treatment is performed in an argon atmosphere, the temperature of the heat treatment is 60° C. to 100° C., preferably 80° C., and the time is 10 min to 20 min, preferably 12 min to 18 min.

[0057] The positive electrode conductive layer slurry is a slurry for forming the positive electrode conductive layer, as described above, including a conductive agent and a binder, which will not be described in detail in this application. In addition, the positive electrode conductive layer slurry also includes a solvent to form a slurry with the conductive agent and the binder. The present application has no special restrictions on the solvent and its amount, preferably N-methylpyrrolidone (NMP). Similarly, the negative electrode conductive layer slurry is a slurry for forming the negative electrode conductive layer, as described above, including a conductive agent, a binder and a thickener, which will not be described in detail in this application. In addition, the negative electrode conductive layer slurry also includes a solvent to form a slurry with the conductive agent, the binder and the thickener. The present application has no special restrictions on the solvent and its amount, preferably water.

[0058] In some specific implementations, the baking is performed in an argon atmosphere, the baking temperature is 80° C. to 120° C., preferably 100° C., and the baking time is 6 h to 8 h, preferably 6.5 h to 7.5 h. After the baking is completed, a composite sheet can be obtained.

[0059] The present application also provides an all-solid-state battery, comprising the composite material described in the above technical solution or the composite sheet described in the above technical solution.

[0060] The compact structure of positive electrode-electrolyte-negative electrode provided by the present application exhibits extremely low interface impedance and high rate performance, and has the performance advantage of being able to function normally at low temperatures. Experimental results show that the internal resistance of the all-solid-state battery provided by the present application is as low as 0.5mΩ or less, the fractional capacity is as high as 118mAh / g or more, the 1C charge and discharge capacity at -40°C is as high as 117Ah or more, and the capacity retention rate of 1C charge and discharge 200 times reaches more than 94%. BRIEF DESCRIPTION OF THE DRAWINGS

[0061] Figure 1 This is a scanning electron microscope image of a cross section of the composite sheet prepared in Example 1;

[0062] Figure 2 For the corresponding Figure 1 Energy dispersion spectrum of P element in the cross section;

[0063] Figure 3 For the corresponding Figure 1 Energy dispersion spectrum of Al element in the cross section;

[0064] Figure 4 For the corresponding Figure 1 Energy dispersion spectrum of the V element in the cross section. DETAILED DESCRIPTION

[0065] It should be understood that the expression "one or more of..." includes each of the items recited after the expression individually and in various different combinations of two or more of the recited items, unless otherwise understood from the context and usage. The expression "and / or" in combination with three or more recited items should be understood to have the same meaning, unless otherwise understood from the context.

[0066] The use of the terms "comprising", "having" or "containing", including their grammatical synonyms, should generally be understood as open and non-restrictive, for example not excluding other unrecited elements or steps, unless otherwise specifically stated or otherwise understood from the context.

[0067] It should be understood that the order of steps or the order in which certain actions are performed is not important as long as the present invention remains operable. In addition, two or more steps or actions may be performed simultaneously.

[0068] The use of any and all examples or exemplary language, such as "for example" or "including", herein is intended only to better illustrate the invention and does not limit the scope of the invention unless otherwise claimed. No language in this specification should be construed as indicating that any non-claimed element is essential to the practice of the invention.

[0069] In addition, the numerical ranges and parameters used to define the present invention are approximate values, and the relevant values ​​in the specific embodiments have been presented as accurately as possible. However, any numerical value inherently inevitably contains standard deviations due to individual test methods. Therefore, unless otherwise expressly stated, it should be understood that all ranges, quantities, values ​​and percentages used in this disclosure are modified by "about". Here, "about" generally means that the actual value is within plus or minus 10%, 5%, 1% or 0.5% of a specific value or range.

[0070] The present application provides a composite material, comprising a positive electrode active material layer and a solid electrolyte layer formed in situ on the surface of the positive electrode active material layer;

[0071] The positive electrode active material layer includes a positive electrode active material represented by formula (I):

[0072] V x Al 1-x PO4F formula (I);

[0073] In formula (I), 0.8≤x≤0.9;

[0074] The solid electrolyte layer includes LiAlPO4F.

[0075] The composite material provided in the present application comprises a positive electrode active material layer and a solid electrolyte layer formed in situ on the surface of the positive electrode active material layer, wherein the positive electrode active material layer comprises a positive electrode active material represented by formula (I): LiV x Al 1-x PO4F formula (I); the solid electrolyte layer comprises LiAlPO4F; LiV x Al 1-x PO4F and LiAlPO4F both belong to the taffeta structure. According to the principle of like dissolves like, the electrolyte and the positive electrode are tightly and firmly bonded at the atomic level, which solves the problem of interface contact between the electrolyte and the positive electrode. At the same time, LiAlPO4F solid electrolyte has strong lithium affinity. By melting lithium on the electrolyte, a tight structure of positive electrode-electrolyte-negative electrode is obtained. The prepared all-solid-state battery exhibits extremely low interface impedance and high rate performance, and has the performance advantage of being able to function normally at low temperatures.

[0076] The composite material, the composite sheet, the preparation method and the application thereof are further described below in conjunction with the embodiments.

[0077] Example 1

[0078] 1. V 0.9 Al 0.1 Preparation of PO4 intermediate:

[0079] Weigh 75.7 g of vanadium pentoxide, 4.7 g of aluminum oxide, 106.3 g of ammonium dihydrogen phosphate, and 13.3 g of carbon black, disperse the above powders in 400 g of deionized water by planetary ball milling or stirring milling, add 1000 g of zirconia balls with a diameter of 3 mm, and grind for 1 hour. After grinding, dry the above slurry at 100° C. to obtain a precursor mixture; heat the precursor mixture to 800° C. in an argon atmosphere in a tube furnace and keep it warm for 4 hours to obtain black V 0.9 Al 0.1 PO4 intermediate.

[0080] 2. LiV 0.9 Al 0.1 Preparation of PO4F:

[0081] Take 10g of the V prepared above 0.9 Al 0.1 PO4 and 1.8 g of LiF were premixed in deionized water and then transferred to the polytetrafluoroethylene liner of a hydrothermal autoclave. The hydrothermal autoclave was placed in an oven and heated to 250°C for 36 h. The sample was washed three times with deionized water and transferred to a tube furnace equipped with an argon flow and dried at 250°C for 30 min to obtain LiV 0.9 Al 0.1 PO4F powder.

[0082] 3. LiV 0.9 Al 0.1 Preparation of PO4F positive electrode sheet:

[0083] Take 10g of the LiV prepared above 0.9 Al 0.1 PO4F powder was put into a ball mill, 100g of deionized water and 200g of zirconium oxide balls were added, the ball mill speed was 400rpm, and the ball milling was carried out for 20min; 10g of deionized water was poured into a glue making cup, 1g of dimethyl phthalate and 1g of polyvinyl alcohol were added, and the glue was made by mixing with a homogenizer for 10min, and the prepared glue was added to the above ball mill, the speed was 500rpm, and the ball milling was continued for 40min; the slurry in the ball mill was coated on the polyethylene release film substrate with a coating thickness of 50μm, and the coating was dried at room temperature after the coating was completed, and the drying time was 10h; the dried film was cut into discs with a diameter of 20mm, and after peeling off the release film, it was transferred to a muffle furnace for sintering at a sintering temperature of 800℃ and a sintering time of 6h to obtain a dense LiV 0.9 Al 0.1 PO4F positive electrode sheet, the thickness of the positive electrode sheet is 43μm.

[0084] 4. LiV 0.9 Al 0.1 Preparation of PO4F-LiAlPO4F-Li composite sheet:

[0085] LiV 0.9 Al 0.1 1g of Al(NO3)3·9H2O metal salt powder was deposited on one side of the PO4F positive electrode sheet and kept at 80°C for 1h in a high pressure furnace at 2MPa pressure. It was washed with deionized water three times and dried at 100°C in a tube furnace with argon flow to obtain LiV 0.9 Al 0.1 PO4F-LiAlPO4F composite sheet.

[0086] See also Figure 1 , Figure 2 , Figure 3 and Figure 4 ,in, Figure 1 This is a scanning electron microscope image of the composite fragment prepared in Example 1. Figure 2 For the corresponding Figure 1 Energy dispersion spectrum of P element in the cross section, Figure 3 For the corresponding Figure 1 Energy dispersion spectrum of Al element in the cross section, Figure 4 For the corresponding Figure 1 Energy dispersion spectrum of V element in the cross section. Figure 1 to Figure 4It can be seen that the thickness of the LiAlPO4F layer in the composite sheet is 2 μm, the Al content in the upper region of about 2 μm is significantly increased, and no V element appears in this region, proving that the layer has been transformed into LiAlPO4F.

[0087] The metal lithium negative electrode sheet is stacked on the LiV 0.9 Al 0.1 One side of the LiAlPO4F of the PO4F-LiAlPO4F composite sheet was heated at 80°C for 10 min in an argon atmosphere to ensure full fusion of the metal lithium and the electrolyte, and LiV was obtained after cooling. 0.9 Al 0.1 PO4F-LiAlPO4F-Li composite sheet.

[0088] 5. Preparation of all-solid-state batteries:

[0089] 0.25 g of conductive carbon black and 0.25 g of polyvinylidene fluoride were added to 10 mL of NMP solution and stirred (at a speed of 400 rpm) for 8 h to prepare a positive electrode conductive agent slurry. The positive electrode conductive agent slurry was coated on an aluminum foil and a composite sheet of LiV 0.9 Al 0.1 One side of PO4F was laminated with conductive agent slurry, 0.25g conductive carbon black, 11g sodium carboxymethyl cellulose (1.5% solid content) and 0.25g styrene-butadiene rubber (solid content 40%) were mixed and stirred (speed of 400rpm) for 8h to prepare negative electrode conductive agent slurry, the negative electrode conductive agent slurry was coated on copper foil, and one side of the composite sheet was laminated with the negative electrode conductive agent slurry, and baked at 100°C for 8h in an argon atmosphere. The composite sheet prepared above was made into an all-solid-state lithium-ion battery, which was sealed into a CR2032 button battery with a battery shell.

[0090] 6. Electrochemical performance test:

[0091] The battery was tested according to GB / T 31484-2015 and GB / T 31486-2015 standards. The results are shown in Table 1. Table 1 shows the performance parameters of the batteries prepared in the embodiments of the present invention and the comparative examples.

[0092] Example 2

[0093] 1. V 0.8 Al 0.2 Preparation of PO4 intermediate:

[0094] Weigh 20.5g of vanadium pentoxide, 2.2g of aluminum hydroxide, 32.5g of ammonium dihydrogen phosphate, and 144.8g of sucrose, disperse the above powders in 600g of anhydrous ethanol by planetary ball milling or stirring milling, add 2000g of zirconia balls with a diameter of 0.6mm, grind for 3h, and after grinding, dry the above slurry at 120℃ to obtain a precursor mixture. Heat the precursor mixture to 700℃ in an argon atmosphere of a tube furnace and keep it warm for 6h to obtain black V 0.8 Al 0.2 PO4 intermediate.

[0095] 2. LiV 0.8 Al 0.2 Preparation of PO4F:

[0096] Take 10g of the V prepared above 0.8 Al 0.2 PO4 and 1.84 g of LiF were premixed in deionized water and then transferred to the polytetrafluoroethylene liner of a hydrothermal autoclave. The hydrothermal autoclave was placed in an oven and heated to 250°C for 48 h. The sample was washed 6 times with deionized water and transferred to a tube furnace equipped with an argon flow and dried at 250°C for 60 min to obtain LiV 0.8 Al 0.2 PO4F powder.

[0097] 3. LiV 0.8 Al 0.2 Preparation of PO4F positive electrode sheet:

[0098] Take 10g of the LiV prepared above 0.8 Al 0.2 PO4F powder was put into a ball mill, 200g of deionized water and 300g of zirconium oxide balls were added, the ball mill speed was 500rpm, and the ball milling was carried out for 40min; 10g of deionized water was poured into a glue making cup, 1g of diethyl phthalate and 1g of polyvinyl butyral were added, and the glue was made by mixing with a homogenizer for 20min, and the prepared glue was added to the above-mentioned ball mill, the speed was 400rpm, and the ball milling was continued for 20min; the slurry in the ball mill was coated on the polyethylene terephthalate release film substrate with a coating thickness of 50μm, and the coating was dried at room temperature after the coating was completed, and the drying time was 10h; the dried film was cut into discs with a diameter of 20mm, the release film was peeled off and transferred to a muffle furnace for sintering, the sintering temperature was 800℃, and the sintering time was 8h to obtain a dense positive electrode sheet with a thickness of 40μm.

[0099] 4. LiV 0.8 Al 0.2 Preparation of PO4F-LiAlPO4F-Li composite sheet:

[0100] LiV0.8 Al 0.2 2g of AlCl3 metal salt powder was deposited on one side of the PO4F positive electrode sheet and kept at 2MPa and 200℃ for 2h in a high pressure furnace. It was washed with deionized water 6 times and dried at 100℃ in a tube furnace with argon flow to obtain LiV 0.8 Al 0.2 PO4F-LiAlPO4F composite sheet, LiAlPO4F layer thickness is 1μm;

[0101] The metal lithium negative electrode sheet is stacked on the LiV 0.8 Al 0.2 The LiAlPO4F side of the PO4F-LiAlPO4F composite sheet was heated at 80°C for 20 min in an argon atmosphere to ensure full fusion of the metal lithium and the electrolyte. After cooling, LiV 0.8 Al 0.2 PO4F-LiAlPO4F-Li composite sheet.

[0102] 5. Preparation of all-solid-state batteries:

[0103] 0.25 g of conductive carbon black and 0.25 g of polyvinylidene fluoride were added to 10 mL of NMP solution and stirred (at a speed of 400 rpm) for 8 h to prepare a positive electrode conductive agent slurry. The positive electrode conductive agent slurry was coated on an aluminum foil and a composite sheet of LiV 0.8 Al 0.2 One side of PO4F is laminated with conductive agent slurry; 0.25g conductive carbon black, 11g methyl cellulose (1.5% solid content) and 0.25g polyacrylic acid (solid content 40%) are mixed and stirred (speed of 400rpm) for 8h to prepare negative electrode conductive agent slurry, which is coated on copper foil, and one side of the composite sheet Li is laminated with the negative electrode conductive agent slurry in an argon atmosphere and baked at 100℃ for 7h. The composite sheet prepared above is made into an all-solid-state lithium-ion battery and sealed into a CR2032 button battery with a battery shell.

[0104] 6. Electrochemical performance test:

[0105] The battery was tested according to GB / T 31484-2015 and GB / T 31486-2015 standards. The results are shown in Table 1. Table 1 shows the performance parameters of the batteries prepared in the embodiments of the present invention and the comparative examples.

[0106] Example 3

[0107] 1. V 0.85 Al 0.15 Preparation of PO4 intermediate:

[0108] Weigh 29.9g of vanadium pentoxide, 21.7g of aluminum nitrate, 51g of diammonium hydrogen phosphate, and 97.4g of glucose, and disperse the above powders in 1000g of deionized water by planetary ball milling or stirring milling, add 1500g of zirconia balls with a diameter of 1mm, and grind for 2h. After grinding, dry the above slurry at 110°C to obtain a precursor mixture. Heat the precursor mixture to a reaction temperature of 750°C in an argon atmosphere of a tube furnace and keep it warm for 5h to obtain black V 0.85 Al 0.15 PO4 intermediate.

[0109] 2. LiV 0.85 Al 0.15 Preparation of PO4F:

[0110] Take 10g of the V prepared above 0.85 Al 0.15 PO4 and 1.83 g of LiF were premixed in deionized water and then transferred to the polytetrafluoroethylene liner of a hydrothermal autoclave. The hydrothermal autoclave was placed in an oven and heated to 250°C for 40 h. The sample was washed with deionized water 5 times and transferred to a tube furnace equipped with an argon flow and dried at 250°C for 40 min to obtain LiV 0.85 Al 0.15 PO4F powder.

[0111] 3. LiV 0.85 Al 0.15 Preparation of PO4F positive electrode sheet:

[0112] Take 10g of the LiV prepared above 0.85 Al 0.15 PO4F powder was put into a ball mill, 150g of deionized water and 250g of zirconium oxide balls were added, the ball mill speed was 450rpm, and the ball milling was carried out for 30min; 10g of deionized water was poured into a glue making cup, 1g of di-n-butyl phthalate and 1g of polyacrylic acid were added, and the glue was made by mixing with a homogenizer for 15min, and the prepared glue was added to the above-mentioned ball mill, the speed was 450rpm, and the ball milling was continued for 30min; the slurry in the ball mill was coated on a polypropylene release film substrate with a coating thickness of 50μm, and dried at room temperature after coating, and the drying time was 11h; the dried film was cut into discs with a diameter of 20mm, and after peeling off the release film, it was transferred to a muffle furnace for sintering at a sintering temperature of 700℃ and a sintering time of 7h to obtain a dense positive electrode sheet with a thickness of 39μm.

[0113] 4. LiV 0.85 Al 0.15 Preparation of PO4F-LiAlPO4F-Li composite sheet:

[0114] LiV0.85 Al 0.15 1.5g of Al(NO3)3·9H2O metal salt powder was deposited on one side of the PO4F positive electrode sheet and kept at 80°C for 1h in a high pressure furnace at 2MPa pressure. It was washed with deionized water 4 times and dried at 100°C in a tube furnace with argon flow to obtain LiV 0.85 Al 0.15 PO4F-LiAlPO4F composite sheet, LiAlPO4F layer thickness is 1.5μm;

[0115] The metal lithium negative electrode sheet is stacked on the LiV 0.85 Al 0.15 The LiAlPO4F side of the PO4F-LiAlPO4F composite sheet was heated at 80°C for 20 min in an argon atmosphere to ensure full fusion of the metal lithium and the electrolyte. After cooling, LiV 0.85 Al 0.15 PO4F-LiAlPO4F-Li composite sheet.

[0116] 5. Preparation of all-solid-state batteries:

[0117] 0.25 g of conductive carbon black and 0.25 g of polyvinylidene fluoride were added to 10 mL of NMP solution and stirred (at a speed of 400 rpm) for 8 h to prepare a positive electrode conductive agent slurry. The positive electrode conductive agent slurry was coated on an aluminum foil and the LiV 0.85 Al 0.15 One side of PO4F is bonded with conductive agent slurry; 0.25g conductive carbon black, 11g ethyl cellulose (1.5% solid content) and 0.25g polyvinyl butyral (solid content 40%) are mixed and stirred (speed is 400rpm) for 8h to prepare negative electrode conductive agent slurry, and the negative electrode conductive agent slurry is coated on copper foil, and one side of Li of the composite sheet is bonded with the negative electrode conductive agent slurry, and baked at 100°C in an argon atmosphere for 6h.

[0118] The composite sheet prepared above is made into an all-solid-state lithium-ion battery, which is sealed in a battery shell to form a CR2032 button battery.

[0119] 6. Electrochemical performance test:

[0120] The battery was tested according to GB / T 31484-2015 and GB / T 31486-2015 standards. The results are shown in Table 1. Table 1 shows the performance parameters of the batteries prepared in the embodiments of the present invention and the comparative examples.

[0121] Example 4

[0122] 1. V 0.8 Al 0.2 Preparation of PO4 intermediate:

[0123] Weigh 34.2g of vanadium pentoxide, 4.5g of aluminum hydroxide, 50.9g of ammonium dihydrogen phosphate, and 110.4g of sucrose, disperse the above powders in 800g of deionized water by planetary ball milling or stirring milling, add 1700g of zirconia balls with a diameter of 2mm, grind for 1.5h, and after grinding, dry the above slurry at 110°C to obtain a precursor mixture. Heat the precursor mixture to a reaction temperature of 700°C in an argon atmosphere of a tube furnace and keep it warm for 5h to obtain black V 0.8 Al 0.2 PO4 intermediate.

[0124] 2. LiV 0.8 Al 0.2 Preparation of PO4F:

[0125] Take 10g of the V prepared above 0.8 Al 0.2 PO4 and 1.84 g of LiF were premixed in deionized water and then transferred to the polytetrafluoroethylene liner of a hydrothermal autoclave. The hydrothermal autoclave was placed in an oven and heated to 250°C for 42 h. The sample was washed 4 times with deionized water and transferred to a tube furnace equipped with an argon flow and dried at 250°C for 40 min to obtain LiV 0.8 Al 0.2 PO4F powder.

[0126] 3. LiV 0.8 Al 0.2 Preparation of PO4F positive electrode sheet:

[0127] Take 10g of the LiV prepared above 0.8 Al 0.2 PO4F powder was put into a ball mill, and 150g of deionized water and 300g of zirconium oxide balls were added. The ball mill speed was 450rpm and the ball milling was carried out for 25min. 10g of deionized water was poured into a glue making cup, and 1g of dioctyl phthalate and 1g of polyacrylonitrile were added. The glue was made by mixing with a homogenizer for 15min. The prepared glue was added to the above-mentioned ball mill, and the speed was 450rpm. The ball milling was continued for 30min. The slurry in the ball mill was coated on a polyethylene release film substrate with a coating thickness of 50μm. After coating, it was dried at room temperature for 12h. The dried film was cut into discs with a diameter of 20mm, and after peeling off the release film, it was transferred to a muffle furnace for sintering at a sintering temperature of 750℃ and a sintering time of 7h to obtain a dense positive electrode sheet with a thickness of 42μm.

[0128] 4. LiV 0.8 Al 0.2 Preparation of PO4F-LiAlPO4F-Li composite sheet:

[0129] LiV 0.8 Al 0.2 1.5g of AlCl3 metal salt powder was deposited on one side of the PO4F positive electrode sheet and kept at 2MPa and 200℃ for 1h in a high pressure furnace. It was washed with deionized water 4 times and dried at 100℃ in a tube furnace with argon flow to obtain LiV 0.8 Al 0.2 PO4F-LiAlPO4F composite sheet, LiAlPO4F layer thickness is 1μm;

[0130] The metal lithium negative electrode sheet is stacked on the LiV 0.8 Al 0.2 One side of the LiAlPO4F of the PO4F-LiAlPO4F composite sheet was heated at 80°C for 15 min in an argon atmosphere to ensure full fusion of the metal lithium and the electrolyte, and LiV was obtained after cooling. 0.8 Al 0.2 PO4F-LiAlPO4F-Li composite sheet.

[0131] 5. Preparation of all-solid-state batteries:

[0132] 0.25 g of conductive carbon black and 0.25 g of polyvinylidene fluoride were added to 10 mL of NMP solution and stirred (at a speed of 400 rpm) for 8 h to prepare a positive electrode conductive agent slurry. The positive electrode conductive agent slurry was coated on an aluminum foil and the LiV 0.8 Al 0.2 One side of PO4F is laminated with conductive agent slurry; 0.25g conductive carbon black, 11g hydroxyethyl cellulose (1.5% solid content) and 0.25g polyacrylic acid (solid content 40%) are mixed and stirred (speed of 400rpm) for 8h to prepare negative electrode conductive agent slurry, which is coated on copper foil, and one side of the composite sheet Li is laminated with the negative electrode conductive agent slurry, and baked at 100℃ for 7h in an argon atmosphere. The composite sheet prepared above is made into an all-solid-state lithium-ion battery, which is sealed into a CR2032 button battery with a battery shell.

[0133] 6. Electrochemical performance test:

[0134] The battery was tested according to GB / T 31484-2015 and GB / T 31486-2015 standards. The results are shown in Table 1. Table 1 shows the performance parameters of the batteries prepared in the embodiments of the present invention and the comparative examples.

[0135] Example 5

[0136] 1. V 0.9 Al 0.1 Preparation of PO4 intermediate:

[0137] Weigh 68.7g of vanadium pentoxide, 6.5g of aluminum oxide, 110.7g of ammonium dihydrogen phosphate, and 14.1g of carbon black, and disperse the above powders in 500g of deionized water by planetary ball milling or stirring milling, add 1200g of zirconia balls with a diameter of 0.8mm, and grind for 2.5h. After grinding, dry the above slurry at 115°C to obtain a precursor mixture. Heat the precursor mixture to a reaction temperature of 700°C in an argon atmosphere of a tube furnace and keep it warm for 6h to obtain black V 0.9 Al 0.1 PO4 intermediate.

[0138] 2. LiV 0.9 Al 0.1 Preparation of PO4F:

[0139] Take 10g of the V prepared above 0.9 Al 0.1 PO4 and 1.8 g of LiF were premixed in deionized water and then transferred to the polytetrafluoroethylene liner of a hydrothermal autoclave. The hydrothermal autoclave was placed in an oven and heated to 250°C for 46 h. The sample was washed 4 times with deionized water and transferred to a tube furnace equipped with an argon flow and dried at 250°C for 55 min to obtain LiV 0.9 Al 0.1 PO4F powder.

[0140] 3. LiV 0.9 Al 0.1 Preparation of PO4F positive electrode sheet:

[0141] Take 10g of the LiV prepared above 0.9 Al 0.1 PO4F powder was put into a ball mill, 100g of deionized water and 250g of zirconium oxide balls were added, the ball mill speed was 400rpm, and the ball milling was carried out for 40min; 10g of deionized water was poured into a glue making cup, 1g of butyl benzyl phthalate and 1g of polyvinyl alcohol were added, and the glue was made by mixing with a homogenizer for 10min, and the prepared glue was added to the above-mentioned ball mill, the speed was 500rpm, and the ball milling was continued for 25min; the slurry in the ball mill was coated on the polyethylene terephthalate release film substrate with a coating thickness of 50μm, and the coating was dried at room temperature after the coating was completed, and the drying time was 10h; the dried film was cut into discs with a diameter of 20mm, and after peeling off the release film, it was transferred to a muffle furnace for sintering at a sintering temperature of 800℃ and a sintering time of 7h to obtain a dense positive electrode sheet with a thickness of 40μm.

[0142] 4. LiV 0.9 Al 0.1 Preparation of PO4F-LiAlPO4F-Li composite sheet:

[0143] LiV0.9 Al 0.1 2g of AlCl3 metal salt powder was deposited on one side of the PO4F positive electrode sheet and kept at 2MPa and 200℃ for 2h in a high pressure furnace. It was washed with deionized water 4 times and dried at 100℃ in a tube furnace with argon flow to obtain LiV 0.9 Al 0.1 PO4F-LiAlPO4F composite sheet, LiAlPO4F layer thickness is 2μm;

[0144] The metal lithium negative electrode sheet is stacked on the LiV 0.9 Al 0.1 One side of the LiAlPO4F of the PO4F-LiAlPO4F composite sheet was heated at 80°C for 15 min in an argon atmosphere to ensure full fusion of the metal lithium and the electrolyte, and LiV was obtained after cooling. 0.9 Al 0.1 PO4F-LiAlPO4F-Li composite sheet.

[0145] 5. Preparation of all-solid-state batteries:

[0146] 0.25 g of conductive carbon black and 0.25 g of polyvinylidene fluoride were added to 10 mL of NMP solution and stirred (at a speed of 400 rpm) for 8 h to prepare a positive electrode conductive agent slurry. The positive electrode conductive agent slurry was coated on an aluminum foil and the LiV 0.9 Al 0.1 One side of PO4F is laminated with positive electrode conductive agent slurry; 0.25g conductive carbon black, 11g sodium carboxymethyl cellulose (1.5% solid content) and 0.25g styrene butadiene rubber (solid content 40%) are mixed and stirred (speed of 400rpm) for 8h to prepare negative electrode conductive agent slurry, which is coated on copper foil, and one side of the composite sheet is laminated with the negative electrode conductive agent slurry, and baked at 100℃ for 6h in an argon atmosphere. The composite sheet prepared above is made into an all-solid-state lithium-ion battery, which is sealed into a CR2032 button battery with a battery shell.

[0147] 6. Electrochemical performance test:

[0148] The battery was tested according to GB / T 31484-2015 and GB / T 31486-2015 standards. The results are shown in Table 1. Table 1 shows the performance parameters of the batteries prepared in the embodiments of the present invention and the comparative examples.

[0149] Comparative Example 1 In LiV 0.9 Al 0.1 LiAlPO4F solid electrolyte coated on PO4F positive electrode

[0150] 1. V 0.9 Al0.1 Preparation of PO4 intermediate:

[0151] Weigh 68.7g of vanadium pentoxide, 6.5g of aluminum oxide, 110.7g of ammonium dihydrogen phosphate, and 14.1g of carbon black, and disperse the above powders in 500g of deionized water by planetary ball milling or stirring milling, add 1200g of zirconia balls with a diameter of 0.8mm, and grind for 2.5h. After grinding, dry the above slurry at 115°C to obtain a precursor mixture. Heat the precursor mixture to a reaction temperature of 700°C in an argon atmosphere of a tube furnace and keep it warm for 6h to obtain black V 0.9 Al 0.1 PO4 intermediate.

[0152] 2. LiV 0.9 Al 0.1 PO4 F Preparation:

[0153] Take 10g of the V prepared above 0.9 Al 0.1 PO4 and 1.8 g of LiF were premixed in deionized water and then transferred to the polytetrafluoroethylene liner of a hydrothermal autoclave. The hydrothermal autoclave was placed in an oven and heated to 250°C for 46 h. The sample was washed 4 times with deionized water and transferred to a tube furnace equipped with an argon flow and dried at 250°C for 55 min to obtain LiV 0.9 Al 0.1 PO4F powder.

[0154] 3. LiV 0.9 Al 0.1 Preparation of PO4F positive electrode sheet:

[0155] Take 10g of the LiV prepared above 0.9 Al 0.1 PO4F powder was put into a ball mill, and 100g of deionized water and 250g of zirconium oxide balls were added. The ball mill speed was 400rpm and the ball milling time was 40min. 10g of deionized water was poured into a glue making cup, and 1g of plasticizer and 1g of polyvinyl alcohol were added. The glue was made by mixing with a homogenizer for 10min. The prepared glue was added to the above ball mill, and the speed was 500rpm. The ball milling was continued for 25min. The slurry in the ball mill was coated on the polyethylene release film substrate with a coating thickness of 50μm. After coating, it was dried at room temperature for 10h. The dried film was cut into discs with a diameter of 20mm, and after peeling off the release film, it was transferred to a muffle furnace for sintering at a sintering temperature of 800℃ and a sintering time of 7h to obtain a dense positive electrode sheet.

[0156] 4. LiV 0.9 Al 0.1Preparation of PO4F-LiAlPO4F-Li composite sheet:

[0157] LiOH, Al(NO3)3·9H2O, NH4H2PO4, and NH4F were weighed in a molar ratio of 1:1:1:1 to a total of 100 g, 500 g of deionized water was added, and the mixture was mixed at a speed of 500 rpm using a planetary ball mill for 1 hour to obtain a precursor slurry, which was dried in an oven at 100°C for 20 min and kept in a muffle furnace at 500°C for 6 hours to obtain LiAlPO4F powder; the powder was sand-milled to a particle size of 50 nm using a sand mill, and the slurry was coated on the surface of the positive electrode sheet using a screen printing process to a coating thickness of 20 μm, dried in an oven at 100°C for 20 min, and kept in a muffle furnace at 600°C for 6 hours to obtain LiV 0.9 Al 0.1 PO4F-LiAlPO4F composite sheet;

[0158] The metal lithium negative electrode sheet is stacked on the LiV 0.9 Al 0.1 One side of the LiAlPO4F of the PO4F-LiAlPO4F composite sheet was heated at 80°C for 15 min in an argon atmosphere to ensure full fusion of the metal lithium and the electrolyte, and LiV was obtained after cooling. 0.9 Al 0.1 PO4F-LiAlPO4F-Li composite sheet.

[0159] 5. Preparation of all-solid-state batteries:

[0160] 0.25 g of conductive carbon black and 0.25 g of polyvinylidene fluoride were added to 10 mL of NMP solution and stirred (at a speed of 400 rpm) for 8 h to prepare a positive electrode conductive agent slurry. The positive electrode conductive agent slurry was coated on an aluminum foil and the LiV 0.9 Al 0.1 One side of PO4F is laminated with conductive agent slurry; 0.25g conductive carbon black, 11g sodium carboxymethyl cellulose (1.5% solid content) and 0.25g styrene-butadiene rubber (solid content 40%) are mixed and stirred (speed of 400rpm) for 8h to prepare negative electrode conductive agent slurry, which is coated on copper foil, and one side of the composite sheet is laminated with the negative electrode conductive agent slurry, and baked at 100℃ for 6h in an argon atmosphere. The composite sheet prepared above is made into an all-solid-state lithium-ion battery, which is sealed into a CR2032 button battery with a battery shell.

[0161] 6. Electrochemical performance test:

[0162] The battery was tested according to GB / T 31484-2015 and GB / T 31486-2015 standards. The results are shown in Table 1. Table 1 shows the performance parameters of the batteries prepared in the embodiments of the present invention and the comparative examples.

[0163] Comparative Example 2: Design of porous layer of LiAlPO4F solid electrolyte sheet and coating of cathode slurry

[0164] 1. V 0.9 Al 0.1 Preparation of PO4 intermediate:

[0165] Weigh 68.7g of vanadium pentoxide, 6.5g of aluminum oxide, 110.7g of ammonium dihydrogen phosphate, and 14.1g of carbon black, and disperse the above powders in 500g of deionized water by planetary ball milling or stirring milling, add 1200g of zirconia balls with a diameter of 0.8mm, and grind for 2.5h. After grinding, dry the above slurry at 115°C to obtain a precursor mixture. Heat the precursor mixture to a reaction temperature of 700°C in an argon atmosphere of a tube furnace and keep it warm for 6h to obtain black V 0.9 Al 0.1 PO4 intermediate.

[0166] 2. LiV 0.9 Al 0.1 Preparation of PO4F:

[0167] Take 10g of the V prepared above 0.9 Al 0.1 PO4 and 1.8 g of LiF were premixed in deionized water and then transferred to the polytetrafluoroethylene liner of a hydrothermal autoclave. The hydrothermal autoclave was placed in an oven and heated to 250°C for 46 h. The sample was washed 4 times with deionized water and transferred to a tube furnace equipped with an argon flow and dried at 250°C for 55 min to obtain LiV 0.9 Al 0.1 PO4F powder.

[0168] 3. Preparation of LiAlPO4F single-sided porous sheet:

[0169] LiOH, Al(NO3)3·9H2O, NH4H2PO4, and NH4F were weighed in a molar ratio of 1:1:1:1 to a total of 100 g, and 500 g of deionized water was added. The mixture was mixed for 1 h using a planetary ball mill at a speed of 500 rpm to obtain a precursor slurry. The mixture was dried in an oven at 100°C for 20 min and kept in a muffle furnace at 500°C for 6 h to obtain LiAlPO4F powder. 0.1 g of the powder was taken and pre-pressed at a pressure of 5 MPa for 3 min using a tablet press. 0s, then, take 10g of the powder and disperse it in 50g of deionized water, add 0.1g of polyvinyl pyrrolidone, mix well and dry, take 0.1g of the mixed powder, use a tablet press to pre-press at a pressure of 5MPa for 30s, then stack the two pre-pressed thin sheets, use a tablet press to maintain the pressure at 20MPa for 1min to obtain a LiAlPO4F single-sided porous sheet precursor, place the sheet in a muffle furnace and keep it at 600℃ for 6h to obtain a LiAlPO4F single-sided porous sheet.

[0170] 4. Preparation of all-solid-state batteries:

[0171] 2g of LiV 0.9 Al 0.1 PO4F powder, 0.25g of conductive carbon black and 0.25g of polyvinylidene fluoride were added to 10mL of NMP solution and stirred (at a speed of 400rpm) for 8h to prepare a positive electrode slurry, which was coated on the porous side of the LiAlPO4F single-sided porous sheet, and aluminum foil was attached to the positive electrode slurry, and baked at 100°C for 6h in an argon atmosphere;

[0172] The metal lithium negative electrode sheet is stacked on the other side of LiAlPO4F, and heated at 80°C for 15 minutes in an argon atmosphere to ensure that the metal lithium and the electrolyte are fully integrated to form a composite sheet; 0.25g of conductive carbon black, 11g of sodium carboxymethyl cellulose (1.5% solid content) and 0.25g of styrene-butadiene rubber (solid content 40%) are mixed and stirred (speed of 400rpm) for 8h to prepare a negative electrode conductive agent slurry, which is coated on a copper foil, and one side of the composite sheet Li is bonded to the negative electrode conductive agent slurry, baked at 100°C for 6h in an argon atmosphere, and cooled to obtain a positive electrode-LiAlPO4F-negative electrode composite sheet. The composite sheet prepared above is made into an all-solid-state lithium-ion battery, which is sealed into a CR2032 button battery with a battery shell.

[0173] 5. Electrochemical performance test:

[0174] The battery was tested according to GB / T 31484-2015 and GB / T 31486-2015 standards. The results are shown in Table 1. Table 1 shows the performance parameters of the batteries prepared in the embodiments of the present invention and the comparative examples.

[0175] Comparative Example 3 LiAlPO4F solid electrolyte sheet coated with cathode slurry

[0176] 1. V 0.9 Al 0.1 Preparation of PO4 intermediate:

[0177] Weigh 68.7g of vanadium pentoxide, 6.5g of aluminum oxide, 110.7g of ammonium dihydrogen phosphate, and 14.1g of carbon black, and disperse the above powders in 500g of deionized water by planetary ball milling or stirring milling, add 1200g of zirconia balls with a diameter of 0.8mm, and grind for 2.5h. After grinding, dry the above slurry at 115°C to obtain a precursor. Heat the precursor mixture to a reaction temperature of 700°C in an argon atmosphere in a tube furnace and keep it warm for 6h to obtain black V 0.9 Al 0.1 PO4 intermediate.

[0178] 2. LiV 0.9 Al 0.1 Preparation of PO4F:

[0179] Take 10g of the V prepared above 0.9 Al 0.1 PO4 and 1.8 g of LiF were premixed in deionized water and then transferred to the polytetrafluoroethylene liner of a hydrothermal autoclave. The hydrothermal autoclave was placed in an oven and heated to 250°C for 46 h. The sample was washed 4 times with deionized water and transferred to a tube furnace equipped with an argon flow and dried at 250°C for 55 min to obtain LiV 0.9 Al 0.1 PO4F powder.

[0180] 3. Preparation of LiAlPO4F electrolyte sheet:

[0181] LiOH, Al(NO3)3·9H2O, NH4H2PO4 and NH4F were weighed in a molar ratio of 1:1:1:1, a total of 100 g were weighed, 500 g of deionized water was added, and the mixture was mixed for 1 hour at a rotation speed of 500 rpm using a planetary ball mill to obtain a precursor slurry. The slurry was dried in an oven at 100°C for 20 min, and then kept in a muffle furnace at 500°C for 6 h to obtain LiAlPO4F powder. 0.1 g of the powder was taken, and a tablet press was used to maintain the pressure at 20 MPa for 1 min to obtain a LiAlPO4F electrolyte sheet precursor. The sheet was placed in a muffle furnace and kept at 600°C for 6 h to obtain a LiAlPO4F electrolyte sheet.

[0182] 4. Preparation of all-solid-state batteries:

[0183] 2g of LiV 0.9 Al 0.1PO4F powder, 0.25g of conductive carbon black and 0.25g of polyvinylidene fluoride were added to 10mL of NMP solution and stirred (at a speed of 400rpm) for 8h to prepare a positive electrode slurry, which was coated on one side of a LiAlPO4F electrolyte sheet, and an aluminum foil was attached to the positive electrode slurry, and baked at 100°C for 6h in an argon atmosphere;

[0184] The metal lithium negative electrode sheet is stacked on the other side of LiAlPO4F, and heated at 80°C for 15 minutes in an argon atmosphere to ensure that the metal lithium and the electrolyte are fully integrated to form a composite sheet; 0.25g of conductive carbon black, 11g of sodium carboxymethyl cellulose (1.5% solid content) and 0.25g of styrene-butadiene rubber (solid content 40%) are mixed and stirred (speed of 400rpm) for 8h to prepare a negative electrode conductive agent slurry, which is coated on a copper foil, and one side of the composite sheet Li is bonded to the negative electrode conductive agent slurry, baked at 100°C for 6h in an argon atmosphere, and cooled to obtain a positive electrode-LiAlPO4F-negative electrode composite sheet. The composite sheet prepared above is made into an all-solid-state lithium-ion battery, which is sealed into a CR2032 button battery with a battery shell.

[0185] 5. Electrochemical performance test:

[0186] The battery was tested according to GB / T 31484-2015 and GB / T 31486-2015 standards. The results are shown in Table 1. Table 1 shows the performance parameters of the batteries prepared in the embodiments of the present invention and the comparative examples.

[0187] Comparative Example 4 LATP and LiV 0.9 Al 0.1 PO4F co-sintering to prepare cathode-solid electrolyte layer

[0188] 1. V 0.9 Al 0.1 Preparation of PO4 intermediate:

[0189] Weigh 68.7g of vanadium pentoxide, 6.5g of aluminum oxide, 110.7g of ammonium dihydrogen phosphate, and 14.1g of carbon black, disperse the above powders in 500g of deionized water by planetary ball milling or stirring milling, add 1200g of zirconia balls with a diameter of 0.8mm, grind for 2.5h, and after grinding, dry the above slurry at 115℃. Heat the precursor mixture to the reaction temperature of 700℃ in an argon atmosphere of a tube furnace and keep it warm for 6h to obtain black V 0.9 Al 0.1 PO4 intermediate.

[0190] 2. LiV 0.9 Al 0.1 Preparation of PO4F:

[0191] Take 10g of the V prepared above 0.9 Al 0.1 PO4 and 1.8 g of LiF were premixed in deionized water and then transferred to the polytetrafluoroethylene liner of a hydrothermal autoclave. The hydrothermal autoclave was placed in an oven and heated to 250°C for 46 h. The sample was washed 4 times with deionized water and transferred to a tube furnace equipped with an argon flow and dried at 250°C for 55 min to obtain LiV 0.9 Al 0.1 PO4F powder.

[0192] 3. Li 1.3 Al 0.3 Ti 1.7 (PO4)3-LiV 0.9 Al 0.1 Preparation of PO4F composite sheet:

[0193] Take commercially available Li 1.3 Al 0.3 Ti 1.7 0.1 g of (PO4)3 powder was pre-pressed for 30 s at a pressure of 5 MPa using a tablet press, and then LiV 0.9 Al 0.1 0.1 g of PO4F powder was pre-pressed for 30 seconds at a pressure of 5 MPa using a tablet press, and then two pre-pressed sheets were stacked and maintained at a pressure of 20 MPa for 1 minute using a tablet press to obtain Li 1.3 Al 0.3 Ti 1.7 (PO4)3-LiV 0.9 Al 0.1 PO4F composite sheet precursor, the sheet was placed in a muffle furnace at 600 ° C for 6 hours to obtain Li 1.3 Al 0.3 Ti 1.7 (PO4)3-LiV 0.9 Al 0.1 PO4F composite sheet.

[0194] 4. Preparation of all-solid-state batteries:

[0195] 0.25 g of conductive carbon black and 0.25 g of polyvinylidene fluoride were added to 10 mL of NMP solution and stirred (at a speed of 400 rpm) for 8 h to prepare a conductive agent slurry. The conductive agent slurry was coated on the LiV 0.9 Al 0.1 PO4F side, and laminate aluminum foil on the conductive agent slurry, and bake at 100℃ for 6h in argon atmosphere; stack the metal lithium negative electrode sheet on Li 1.3 Al 0.3 Ti 1.7On the other side of (PO4)3, heat at 80°C for 15 min in an argon atmosphere to ensure full fusion of metallic lithium and the electrolyte to form a composite sheet; 0.25 g of conductive carbon black, 11 g of sodium carboxymethyl cellulose (1.5% solid content) and 0.25 g of styrene-butadiene rubber (solid content 40%) are mixed and stirred (at a speed of 400 rpm) for 8 h to prepare a negative electrode conductive agent slurry, which is coated on a copper foil, and one side of the composite sheet Li is bonded to the negative electrode conductive agent slurry, and baked at 100°C for 6 h in an argon atmosphere, and the positive electrode-Li is obtained after cooling. 1.3 Al 0.3 Ti 1.7 (PO4)3-negative electrode composite sheet. The composite sheet prepared above is made into an all-solid-state lithium-ion battery, which is sealed in a battery shell to form a CR2032 button battery.

[0196] 5. Electrochemical performance test:

[0197] The battery was tested according to GB / T 31484-2015 and GB / T 31486-2015 standards. The results are shown in Table 1. Table 1 shows the performance parameters of the batteries prepared in the embodiments of the present invention and the comparative examples.

[0198] Comparative Example 5: Using LiV electrolyte 0.9 Al 0.1 PO4F positive electrode particles for Li batteries

[0199] 1. V 0.9 Al 0.1 Preparation of PO4 intermediate:

[0200] Weigh 68.7g of vanadium pentoxide, 6.5g of aluminum oxide, 110.7g of ammonium dihydrogen phosphate, and 14.1g of carbon black, and disperse the above powders in 500g of deionized water by planetary ball milling or stirring milling, add 1200g of zirconia balls with a diameter of 0.8mm, and grind for 2.5h. After grinding, dry the above slurry at 115°C to obtain a precursor mixture. Heat the precursor mixture to a reaction temperature of 700°C in an argon atmosphere of a tube furnace and keep it warm for 6h to obtain black V 0.9 Al 0.1 PO4 intermediate.

[0201] 2. LiV 0.9 Al 0.1 Preparation of PO4F:

[0202] Take 10g of the V prepared above 0.9 Al 0.1PO4 and 1.8 g of LiF were premixed in deionized water and then transferred to the polytetrafluoroethylene liner of a hydrothermal autoclave. The hydrothermal autoclave was placed in an oven and heated to 250°C for 46 h. The sample was washed 4 times with deionized water and transferred to a tube furnace equipped with an argon flow and dried at 250°C for 55 min to obtain LiV 0.9 Al 0.1 PO4F powder.

[0203] 3. LiV 0.9 Al 0.1 Preparation of PO4F cathode slurry:

[0204] 2g of LiV 0.9 Al 0.1 PO4F powder, 0.25 g of conductive carbon black and 0.25 g of polyvinylidene fluoride were added to 10 mL of NMP solution and stirred (at a speed of 400 rpm) for 8 h to prepare a positive electrode slurry.

[0205] 4. Preparation of batteries:

[0206] 1M LiPF6 was dissolved in a mixed solution of ethylene carbonate (EC) / dimethyl carbonate (DMC) / diethyl carbonate (EMC) (volume ratio of 1:1:1) as the electrolyte, and the cells were assembled in the order of copper foil-lithium sheet-electrolyte-diaphragm-electrolyte-positive electrode-aluminum foil, and sealed in a battery case to form a CR2032 button cell.

[0207] 5. Electrochemical performance test:

[0208] The battery was tested according to GB / T 31484-2015 and GB / T 31486-2015 standards. The results are shown in Table 1. Table 1 shows the performance parameters of the batteries prepared in the embodiments of the present invention and the comparative examples.

[0209] Comparative Example 6: Using LiV electrolyte 0.9 Al 0.1 PO4F positive electrode for Li battery

[0210] 1. V 0.9 Al 0.1 Preparation of PO4 intermediate:

[0211] Weigh 68.7 g of vanadium pentoxide, 6.5 g of aluminum oxide, 110.7 g of ammonium dihydrogen phosphate, and 14.1 g of carbon black, disperse the above powders in 500 g of deionized water by planetary ball milling or stirring milling, add 1200 g of zirconia balls with a diameter of 0.8 mm, and grind for 2.5 hours. After grinding, dry the above slurry at 115°C to obtain a precursor mixture; heat the precursor mixture to a reaction temperature of 700°C in an argon atmosphere of a tube furnace and keep it warm for 6 hours to obtain black V0.9 Al 0.1 PO4 intermediate.

[0212] 2. LiV 0.9 Al 0.1 Preparation of PO4F:

[0213] Take 10g of the V prepared above 0.9 Al 0.1 PO4 and 1.8 g of LiF were premixed in deionized water and then transferred to the polytetrafluoroethylene liner of a hydrothermal autoclave. The hydrothermal autoclave was placed in an oven and heated to 250°C for 46 h. The sample was washed 4 times with deionized water and transferred to a tube furnace equipped with an argon flow and dried at 250°C for 55 min to obtain LiV 0.9 Al 0.1 PO4F powder.

[0214] 3. LiV 0.9 Al 0.1 Preparation of PO4F positive electrode sheet:

[0215] Take 10g of the LiV prepared above 0.9 Al 0.1 PO4F powder was put into a ball mill, and 100g of deionized water and 250g of zirconium oxide balls were added. The ball mill speed was 400rpm and the ball milling time was 40min. 10g of deionized water was poured into a glue making cup, and 1g of plasticizer and 1g of polyvinyl alcohol were added. The glue was made by mixing with a homogenizer for 10min. The prepared glue was added to the above ball mill, and the speed was 500rpm. The ball milling was continued for 25min. The slurry in the ball mill was coated on the substrate with a coating thickness of 50μm. After coating, it was dried at room temperature for 10h. The dried film was cut into discs with a diameter of 20mm and transferred to a muffle furnace for sintering at a sintering temperature of 850℃ and a sintering time of 7h to obtain a dense positive electrode sheet.

[0216] 4. Preparation of batteries:

[0217] 1M LiPF6 was dissolved in a mixed solution of ethylene carbonate (EC) / dimethyl carbonate (DMC) / diethyl carbonate (EMC) (volume ratio of 1:1:1) as an electrolyte; 0.25g conductive carbon black and 0.25g polyvinylidene fluoride were added to 10mL NMP solution, stirred (rotation speed of 400rpm) for 8h to prepare a conductive agent slurry, and the conductive agent slurry was coated on aluminum foil; the battery was assembled in the order of copper foil-lithium sheet-electrolyte-diaphragm-electrolyte-positive electrode sheet-aluminum foil, and sealed with a battery case to form a CR2032 button battery.

[0218] 5. Electrochemical performance test:

[0219] The battery was tested according to GB / T 31484-2015 and GB / T 31486-2015 standards. The results are shown in Table 1. Table 1 shows the performance parameters of the batteries prepared in the embodiments of the present invention and the comparative examples.

[0220] Table 1 Performance parameters of batteries prepared in the embodiments of the present invention and comparative examples

[0221]

[0222] As shown in Table 1, Examples 1 to 5 are LiV x Al 1-x The LiAlPO4F electrolyte layer is in-situ generated on the PO4F positive electrode sheet. When used in all-solid-state batteries, a tight and strong atomic-level bond is formed between the electrolyte and the positive electrode, which solves the interface contact problem between the electrolyte and the positive electrode. The lithium ions released from the positive electrode can be quickly transferred through the electrolyte layer without the need for solvation and desolvation processes. The designed LiAlPO4F solid electrolyte has a very strong lithium affinity. The assembled battery exhibits excellent performance of low internal resistance, high capacity, low temperature resistance and strong cycle stability.

[0223] Comparative Example 1 is formed by coating the electrolyte slurry and then sintering. Due to the sintering stress, it is difficult to ensure the contact of the interface, resulting in poor performance; Comparative Example 2 increases the contact with the positive electrode by designing a porous solid electrolyte. The porous design can only increase the contact area to a certain extent and cannot solve the contact problem; Comparative Example 3 is a solid electrolyte sheet directly coated with a positive electrode slurry, and the effect is worse than that of Comparative Example 2; Comparative Example 4 is Li 1.3 Al 0.3 Ti 1.7 (PO4)3 and LiV 0.9 Al 0.1 The co-sintering of PO4F to prepare composite sheets will cause major problems in interface contact due to the difference in thermal expansion coefficient caused by composition and structure; Comparative Examples 5 to 6 are liquid batteries using electrolytes. Compared with all-solid-state batteries, the solvation and desolvation processes are added during the lithium ion transmission process. The flow of electrolyte is hindered at low temperatures, which impedes the performance.

[0224] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.

Claims

1. A composite material comprising a positive electrode active material layer and a solid electrolyte layer formed in situ on the surface of the positive electrode active material layer; The positive electrode active material layer includes a positive electrode active material represented by formula (I): V x Al 1-x PO4F formula (I); In formula (I), 0.8≤x≤0.9; The solid electrolyte layer includes LiAlPO4F.

2. The composite sheet according to claim 1, characterized in that: The thickness of the solid electrolyte layer is 1 μm to 2 μm.

3. A composite sheet comprising: A positive electrode current collector, a positive electrode conductive layer formed on a surface of the positive electrode current collector, and a composite material formed on a surface of the conductive layer; The composite material comprises a positive electrode active material layer formed on the surface of the conductive layer and a solid electrolyte layer formed in situ on the surface of the positive electrode active material layer; The positive electrode active material layer includes a positive electrode active material represented by formula (I): LiV x Al 1-x LiV x Al 1-x (PO4)F of formula (I); In formula (I), 0.8≤x≤0.9; The solid electrolyte layer includes LiAlPO4F.

4. The composite sheet according to claim 3, characterized in that: Also included is a negative electrode active material layer formed on the surface of the solid electrolyte layer.

5. The composite sheet according to claim 4, characterized in that: Also included is a negative electrode conductive layer formed on the negative electrode active material layer and a negative electrode current collector formed on the negative electrode conductive layer.

6. A method for preparing a composite material, comprising the following steps: Step a) forming a positive electrode active material layer on a release film with a positive electrode active material represented by formula (I): LiV x Al 1-x LiV x Al 1-x (PO4)F of formula (I); In formula (I), 0.8≤x≤0.9; Step b) depositing aluminum salt on the surface of the positive electrode active material layer to perform a replacement reaction to generate LiAlPO4F in situ to form a solid electrolyte layer, thereby obtaining a composite material.

7. The preparation method according to claim 6, characterized in that: The aluminum salt is selected from aluminum chloride or aluminum nitrate; The ratio of the mass of the aluminum salt to the area of ​​the positive electrode active material layer is 1 g to 2 g: 200 mm 2 ~400mm 2 .

8. The preparation method according to claim 7, characterized in that: The replacement reaction is carried out at a pressure of 1 MPa to 3 MPa, a temperature of 80° C. to 200° C., and a time of 1 h to 2 h.

9. The preparation method according to claim 8, characterized in that: The step a) is specifically as follows: The positive electrode active material, the plasticizer and the binder are mixed to obtain a glue solution, and the glue solution is coated on the positive base current collector and then dried and sintered; The sintering temperature is 700° C. to 800° C., and the sintering time is 6 h to 8 h.

10. An all-solid-state battery, comprising the composite material according to claim 1 or 2, or the composite sheet according to any one of claims 3 to 5, or a composite material prepared by the method according to any one of claims 6 to 9.