Porous cellulose-based lithium ion battery diaphragm as well as preparation method and application thereof

By preparing porous cellulose-based lithium-ion battery separators, the problems of low solubility and uneven distribution of lithium nitrate in lithium-ion batteries are solved, and the uniform distribution and sustained release of LiNO3 are achieved, which improves the circulation and rate performance of the battery and enhances the battery. stability and safety.

CN119009358AActive Publication Date: 2024-11-22SOUTH CHINA UNIV OF TECH

Patent Information

Application Number
CN202411301235.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-18
Publication Date
2024-11-22
Estimated Expiration
2044-09-18

AI Technical Summary

Technical Problem

The low solubility of lithium nitrate in lithium-ion batteries makes it difficult to maintain sufficient concentration in the electrolyte, limiting its function performance. The existing loading methods lead to uneven distribution of LiNO3, affecting the safety and stability of the battery.

Method used

Using the preparation method of porous cellulose-based lithium-ion battery separator, the preparation of bacterial cellulose suspension, grafted with chitosan treatment and lithium salt loading, a separator with a three-dimensional porous network structure is formed to promote the uniform distribution of lithium nitrate. and sustained release.

Benefits of technology

The uniform distribution and sustained release of LiNO3 in the electrolyte is achieved, which reduces the interfacial mass transfer impedance of lithium ions, improves the cycling and rate performance of the battery, and enhances the stability and safety of the battery.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119009358A_ABST
    Figure CN119009358A_ABST
Patent Text Reader

Abstract

The invention discloses a porous cellulose-based lithium ion battery diaphragm as well as a preparation method and application thereof. The preparation method of the battery diaphragm comprises the following steps: treating flaky bacterial cellulose with a NaOH solution to prepare a bacterial cellulose suspension, or further grafting chitosan to obtain a bacterial cellulose suspension grafted with chitosan; performing suction filtration to form a membrane, and soaking the membrane in ethanol to obtain the porous bacterial cellulose lithium ion battery diaphragm. And finally, soaking the porous cellulose in a lithium salt solution to obtain the lithium salt-loaded porous cellulose-based lithium ion battery diaphragm. The method provided by the invention can improve the deposition and stripping behaviors of lithium ions in the lithium ion battery, thereby improving the cycle and rate performance of the battery.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of battery separator materials, and particularly relates to a porous cellulose-based lithium-ion battery separator and a preparation method and application thereof. Background Art

[0002] Electrolyte additives play a vital role in lithium-ion batteries. They can significantly improve the overall performance of the battery, extend the battery life, increase the battery energy density, and enhance the battery safety. Among them, lithium nitrate LiNO3 is an important additive. It can play a variety of functions in the electrolyte, such as stabilizing the solid electrolyte interface (SEI) layer, reducing the occurrence of side reactions, and inhibiting the instability of the battery during the charge and discharge process, thereby improving the battery's cycle life and rate performance.

[0003] During the charge and discharge process of the battery, LiNO3 can preferentially decompose to form a high-quality SEI layer. The SEI layer is the interface layer between the battery electrode and the electrolyte, and plays a key role in the battery's cycle performance and safety. LiNO3 can promote the formation of Li3N, an inorganic component of the SEI layer. This interface layer is more stable and has better conductivity than the SEI layer of traditional organic substances, thereby reducing side reactions during battery cycles. The higher mechanical strength can also inhibit the growth and penetration of lithium dendrites and extend the battery's service life. Secondly, the stable SEI formed by LiNO3 can also inhibit the side reactions of the battery at high voltage and reduce unnecessary side reactions between the electrolyte and the electrode materials. On the positive electrode side, the CEI formed can inhibit the loss of active materials, reduce the generation of unstable byproducts, and ultimately effectively improve the stability and safety of the battery.

[0004] Although LiNO3 can effectively improve the performance of lithium-ion batteries, it faces great challenges in practical applications. The main problem is its low solubility in ester electrolytes, which makes it difficult for LiNO3 to maintain a sufficient concentration in the electrolyte, which directly limits its function in lithium-ion batteries. In order to solve this problem, it is usually necessary to increase the amount of lithium nitrate added, but the insoluble LiNO3 crystals suspended in the electrolyte will not only increase the mass transfer resistance of the solution, but also may adhere to the electrode surface to hinder the redox process of lithium ions, resulting in an increase in interfacial impedance.

[0005] In order to overcome the problem of low solubility of LiNO3 in ester electrolytes, some researchers have tried to use a sandwich structure to load lithium nitrate between two PP membranes (Reference 1: S. Stuckenberg; M. Bela; C. T. Lechtenfeld; M. Mense; V. Kupers; T. T. Ingber; M. Winter; M. C. Stan. Influence of LiNO(3) on the Lithium Metal Deposition Behavior in Carbonate-Based Liquid Electrolytes and on the Electrochemical Performance in Zero-Excess Lithium Metal Batteries. Small 2024, 20(6), e2305203. DOI: 10.1002 / smll.202305203. Reference 2: Y. Liu; X. Qin; D. Zhou; H. Xia; S. Zhang; G. Chen; F. Kang; B. Li. A biscuit-like separator enabling high performance lithium batteries by continuous and protected releasing of NO3-in carbonate electrolyte.Energy Storage Materials 2020, 24, 229-236.DOI:10.1016 / j.ensm.2019.08.016.). However, this method has a significant drawback, that is, the distribution of LiNO3 crystals in the sandwich layer is often uneven, and the shapes and sizes vary, which leads to uneven deposition of lithium ions. This uneven deposition can cause local short circuits and thermal runaway of the battery, seriously affecting the safety and stability of the battery.Some studies have also loaded LiNO3 into glass fiber membranes, but the glass fiber membranes are too thick and have large pores, which can easily form large crystals to block the pores. At the same time, the glass fiber membranes cannot promote the sustained release of LiNO3, which is not conducive to its reduction on the negative electrode surface (Q. Shi; Y. Zhong; M. Wu; H. Wang; H. Wang. High-capacity rechargeable batteries based on deeply cyclable lithium metal anodes. Proc Natl Acad Sci US A2018, 115 (22), 5676-5680. DOI: 10.1073 / pnas.1803634115.).

[0006] Therefore, it is necessary to find a suitable way to load LiNO3 so that it can be fixed in the electrolyte and evenly distributed. At the same time, the diaphragm can also promote the dissolution and slow release of lithium nitrate, ultimately achieving improved battery performance. Summary of the invention

[0007] The primary purpose of the present invention is to overcome the shortcomings and deficiencies of the prior art and provide a method for preparing a porous cellulose-based lithium-ion battery separator.

[0008] Another object of the present invention is to provide a porous cellulose-based lithium-ion battery separator prepared by the method.

[0009] Another object of the present invention is to provide an application of the porous cellulose-based lithium-ion battery separator.

[0010] The purpose of the present invention is achieved through the following technical solutions:

[0011] A method for preparing a porous cellulose-based lithium-ion battery separator comprises the following steps:

[0012] (1) Preparation of bacterial cellulose suspension

[0013] Cut the flake bacterial cellulose into small pieces, wash with water, and then completely boil in NaOH solution for 1 to 1.5 hours to clean the residual medium and impurities; then rinse with water, add CH3COOH solution to neutralize, and then wash with water until neutral, and finally use a homogenizer to fiberize it into slurry to obtain a bacterial cellulose suspension;

[0014] (2) Suspension of bacterial cellulose grafted with chitosan

[0015] Adding NaIO4 to the bacterial cellulose suspension obtained in step (1), deoxygenating with nitrogen, stirring and reacting under the conditions of light shielding and 50±2°C, adding ethylene glycol to terminate the reaction after the reaction is completed, and obtaining an oxidized bacterial cellulose solution; adding chitosan powder to a CH3COOH solution, stirring and dissolving at 60-70°C to form a transparent chitosan solution; then adding the oxidized bacterial cellulose solution to the chitosan solution, stirring and reacting at 50-60°C, centrifuging and washing after the reaction is completed, and obtaining a bacterial cellulose suspension grafted with chitosan;

[0016] (3) Preparation of porous bacterial cellulose lithium-ion battery separator

[0017] The bacterial cellulose suspension obtained in step (1) and / or the bacterial cellulose suspension grafted with chitosan obtained in step (2) is diluted with water and then filtered to form a membrane to obtain a wet porous cellulose-based membrane; then the membrane is immersed in pure ethanol so that the water in the porous cellulose-based membrane is completely replaced by ethanol, and finally dried at 75-100° C. to obtain a porous bacterial cellulose lithium-ion battery membrane;

[0018] (4) Battery separator loaded with lithium salt

[0019] Add lithium salt to ethanol, stir and dissolve to prepare a lithium salt solution with a mass concentration of 0.5-2.5%; then immerse the porous bacterial cellulose lithium ion battery separator obtained in step (3) in the lithium salt solution, take it out after immersion, and dry it at 90-120° C. to obtain a porous cellulose-based lithium ion battery separator loaded with lithium salt; wherein the lithium salt is at least one of lithium nitrate, lithium tetrafluoroborate and lithium perchlorate.

[0020] In step (1), cutting into small pieces means cutting the bacterial cellulose flakes into pieces of (2-5)*(2-5) cm in size; preferably, cutting the bacterial cellulose flakes into pieces of 3*3 cm in size.

[0021] The concentration of the NaOH solution in step (1) is 0.05-0.2 mol / L, preferably 0.1 mol / L.

[0022] The concentration of the CH3COOH solution in step (1) is 0.3±0.1% by volume.

[0023] The homogenizer described in step (1) is a high-speed homogenizer, and its rotation speed is 25000-30000rpm.

[0024] The concentration of the bacterial cellulose suspension in step (1) is 0.4-0.5% by mass.

[0025] The amount of NaIO4 added in step (2) is calculated based on its final concentration in the reaction system of 0.1 to 0.2 mol / L; preferably, it is calculated based on its final concentration in the reaction system of 0.15 mol / L.

[0026] In step (2), the stirring reaction conditions under the conditions of shading and 50±2° C. are: a rotation speed of 300 to 500 rpm / min and a stirring reaction time of 2 to 2.5 h.

[0027] The amount of ethylene glycol used in step (2) accounts for 5-6% of the volume of the reaction system.

[0028] The concentration of the chitosan solution in step (2) is 0.02-0.03 g / ml, preferably 0.02 g / ml.

[0029] The chitosan described in step (2) is medium viscosity chitosan, and its viscosity is 200-400 mPa.s.

[0030] The concentration of the CH3COOH solution in step (2) is 2-3% by volume, preferably 2% by volume.

[0031] The stirring and dissolving time in step (2) is 1 to 2 hours.

[0032] In step (2), the stirring reaction time at 50-60° C. is 2-3 h.

[0033] The number of centrifugal washings in step (2) is 4 to 6 times.

[0034] The concentration of the bacterial cellulose suspension grafted with chitosan in step (2) is 0.4-0.5% by mass.

[0035] The dilution described in step (3) is dilution by adding water 10 to 20 times.

[0036] The soaking time in step (3) is 3 to 4 hours.

[0037] The drying in step (3) is performed by using a drum dryer for 5 to 10 minutes.

[0038] The thickness of the porous bacterial cellulose lithium-ion battery separator described in step (3) is 0.8±0.1 cm.

[0039] The lithium salt described in step (4) is preferably lithium nitrate.

[0040] The stirring time in step (4) is 1 to 2 hours, preferably 1 hour.

[0041] The soaking time in step (4) is 1 to 2 hours, preferably 2 hours.

[0042] The drying temperature in step (4) is preferably 110° C., and the product is dried in a vacuum drying oven until there is no significant change in quality.

[0043] A porous cellulose-based lithium-ion battery separator is prepared by any of the methods described above.

[0044] The porous cellulose-based lithium-ion battery separator has a three-dimensional porous network structure, a porosity of 20% to 80% (preferably 31 to 65%), and a separator thickness of 14 μm to 100 μm (preferably 16 to 32 μm).

[0045] Application of the porous cellulose-based lithium-ion battery separator in lithium-ion batteries.

[0046] A lithium ion battery comprises a positive electrode, a negative electrode, the above-mentioned porous cellulose-based lithium ion battery separator and an electrolyte.

[0047] The positive electrode, electrolyte and negative electrode are conventional positive electrode, electrolyte and negative electrode in the art, and can be assembled into button cells or soft-pack batteries using existing conventional battery devices.

[0048] The positive electrode is composed of an active material capable of embedding and extracting lithium ions, a conductive agent, a binder and a current collector; wherein,

[0049] The active material includes but is not limited to at least one of lithium cobalt oxide, nickel-cobalt-manganese ternary material, nickel-cobalt-aluminum ternary material, lithium iron phosphate and lithium manganese oxide; preferably lithium iron phosphate;

[0050] The conductive agent includes but is not limited to at least one of acetylene black, carbon black, graphite and carbon fiber; preferably acetylene black;

[0051] The binder includes but is not limited to at least one of polyvinylidene fluoride and polyacrylic acid; preferably polyvinylidene fluoride;

[0052] The current collector is aluminum foil.

[0053] The preparation method of the positive electrode is as follows: a slurry of 80wt% lithium iron phosphate, 10wt% acetylene black and 10wt% polyvinylidene fluoride is coated on an aluminum foil, then dried in an oven at 60±5°C, and then cut into positive electrode sheets.

[0054] The drying time is 5 to 8 hours, preferably 6 hours.

[0055] The size of the positive electrode sheet can be cut according to actual needs. For example, when assembled into a button battery R2032, the radius of the positive electrode sheet is 0.6 cm.

[0056] The negative electrode can be made of conventional negative electrode materials in the art, such as metallic lithium (sheet), or composed of an active material capable of embedding and extracting lithium ions, a conductive agent, a binder, and a current collector.

[0057] The negative electrode active material includes but is not limited to one or more of graphite, silicon-based materials and lithium titanate;

[0058] The conductive agent includes but is not limited to acetylene black, carbon black, graphite and carbon fiber; preferably acetylene black;

[0059] The binder includes but is not limited to carboxymethyl cellulose and styrene-butadiene rubber;

[0060] The current collector is copper foil.

[0061] The electrolyte plays a role in conducting lithium ions in lithium-ion batteries and is usually composed of lithium salts and solvents; wherein,

[0062] The lithium salt includes but is not limited to one or more of lithium hexafluorophosphate (LiPF6), lithium bis(trifluoromethylsulfonyl imide) and lithium fluorosulfonyl imide; preferably lithium hexafluorophosphate;

[0063] The solvent is an ester solvent, including but not limited to one or more of ethylene carbonate (EC), dimethyl carbonate (DMC), ethyl methyl carbonate (EMC) and propylene carbonate (PC); preferably, ethylene carbonate (EC), ethyl methyl carbonate (EMC) and dimethyl carbonate (DMC) are mixed in a mass ratio of 1:1:1.

[0064] The concentration of lithium salt in the electrolyte is 0.5-2 mol / L, preferably 1 mol / L.

[0065] In the present invention, LiNO3 loaded in the porous cellulose-based diaphragm can be gradually released in the ester electrolyte to form a stable solid electrolyte layer SEI on the surface of the negative electrode, thereby reducing the occurrence of side reactions between the electrolyte and the electrode surface, thereby reducing the interfacial mass transfer impedance of lithium ions, improving the deposition / stripping process of lithium ions, and improving the cycle and rate performance of the battery.

[0066] Compared with the prior art, the present invention has the following advantages and effects:

[0067] 1. The present invention provides a method for preparing a porous cellulose-based lithium-ion battery separator capable of sustained-release lithium nitrate. The porous cellulose-based lithium-ion battery separator can load LiNO3 and affect the sustained-release of lithium nitrate, the transfer of lithium ions and the formation process of SEI through the characteristic functional groups on different cellulose bases, thereby effectively improving the various performances of the battery.

[0068] 2. In order to solve the disadvantage of uneven loading of traditional LiNO3, the present invention realizes the uniform distribution of LiNO3 in the porous cellulose-based battery separator through the interaction between the characteristic functional groups on different celluloses and LiNO3, thereby reducing the agglomeration of crystals and the influence of polarization.

[0069] 3. In view of the defect of low porosity of conventional cellulose-based diaphragms, the present invention modifies and grafts cellulose to prepare a cellulose-based battery diaphragm with high porosity. While achieving LiNO3 coating, it increases the absorption of electrolyte, thereby promoting the rapid conduction of lithium ions.

[0070] 4. The sustained release of LiNO3 by the porous cellulose-based diaphragm prepared in the present invention keeps the concentration of LiNO3 in the electrolyte in a saturated state, thereby further affecting the reaction process at the electrode / electrolyte interface, promoting the formation of inorganic components in SEI, improving the deposition / stripping behavior of lithium ions, and ultimately improving the cycle and rate performance of the battery.

[0071] 5. The present invention prepares porous cellulose-based battery separators using three different cellulose raw materials (bacterial cellulose, bacterial cellulose grafted with chitosan, and TEMPO oxidized cellulose), and finds that nanoscale cellulose raw materials can form separators with higher strength and more uniform pore size distribution.

[0072] 6. In the present invention, a porous cellulose-based lithium-ion battery separator is used to load LiNO3, and the solvent ethanol is used to dissolve LiNO3. It is found that when water is used as the solvent for LiNO3, the porosity and liquid absorption rate of the obtained bacterial cellulose separator will decrease; the LiNO3 concentration is 0.5% to 2.5%. If the concentration is too low, the load amount in the separator will be too small, and LiNO3, as a sacrificial additive, will be difficult to maintain its effect for a long time; if the load amount is too large, the pores of the separator will be blocked, resulting in increased battery polarization and affecting the transfer of lithium ions.

[0073] 7. The present invention immerses the porous cellulose membrane in a LiNO3 solution, and adopts a heating in-situ recrystallization loading method to compound LiNO3 in the porous cellulose-based lithium-ion battery separator, wherein the immersion time is 1 to 2 hours, and the heating temperature during drying after taking out is 90 to 120°C. If the heating temperature is too low, the solvent cannot be completely removed, thereby inducing side reactions and reducing battery performance. BRIEF DESCRIPTION OF THE DRAWINGS

[0074] Figure 1 This is the SEM image of the porous bacterial cellulose membrane without LiNO3 loading in Example 1.

[0075] Figure 2 This is the SEM image of the porous bacterial cellulose membrane grafted with chitosan without LiNO3 loading in Example 6.

[0076] Figure 3 This is the SEM image of the oxidized bacterial cellulose membrane in Comparative Example 6 with a LiNO3 loading of 0.5%.

[0077] Figure 4 This is the SEM image of the bacterial cellulose membrane grafted with chitosan in Example 8 with a LiNO3 loading of 1.5%.

[0078] Figure 5 This is the SEM image of the bacterial cellulose membrane grafted with chitosan in Comparative Example 2 with a LiNO3 loading of 3%. DETAILED DESCRIPTION

[0079] The present invention is further described in detail below in conjunction with examples, but the embodiments of the present invention are not limited thereto. Unless otherwise specified, the reagents, methods and equipment used in the present invention are conventional reagents, methods and equipment in the art. The test methods for which specific experimental conditions are not specified in the following examples are usually in accordance with conventional experimental conditions. Unless otherwise specified, the reagents and raw materials used in the present invention can be obtained commercially.

[0080] In the present invention, unless otherwise specified, all percentages (%) are mass percentages (wt %).

[0081] The sheet-like bacterial cellulose involved in the embodiments of the present invention was purchased from Hainan Yide Food Co., Ltd. (obtained by fermenting the commercial bacterial cellulose fermentation strain, Acetobacter xylinum, for 5 to 7 days, and the film thickness was 3 to 20 mm).

[0082] Example 1

[0083] 1. Preparation of porous cellulose-based lithium-ion battery separator using bacterial cellulose as raw material

[0084] (1) Preparation of bacterial cellulose suspension: Cut the flake bacterial cellulose into small pieces of 3*3 cm, wash with water and completely boil in excess 0.1M NaOH solution for 1-1.5h to clean the residual medium and impurities. After washing with distilled water several times, neutralize with 0.3±0.1% (v / v) CH3COOH solution, and finally wash the bacterial cellulose with distilled water until the pH value reaches neutral (pH=7±0.5); then use a high-speed homogenizer to fiberize the wet small pieces of bacterial cellulose (about 30-35g) into slurry at a speed of 25000-30000rpm to obtain a bacterial cellulose suspension with a concentration of 0.4-0.5wt%.

[0085] (2) Preparation of porous bacterial cellulose lithium-ion battery separator: A porous bacterial cellulose lithium-ion battery separator is prepared by vacuum filtration, and a three-dimensional porous network is formed by staggered stacking of cellulose fibers. 6 to 7 g of the bacterial cellulose suspension obtained in step (1) is diluted with water to 80 to 100 g, and then poured into a sand core funnel for filtration to form a membrane. Subsequently, the wet porous cellulose-based separator is placed in excess pure ethanol for 3 to 4 hours so that the water in the porous cellulose-based separator is completely replaced by ethanol. The wet porous cellulose-based separator is then dried at 75 to 100°C with a drum dryer for 5 to 10 minutes to obtain the desired porous bacterial cellulose lithium-ion battery separator, and the radius of the membrane is 0.8 cm.

[0086] (3) Battery diaphragm loaded with lithium nitrate: 0.18 g of LiNO3 was dissolved in 10 g of pure ethanol and stirred for 1 h until the solution was clear. The porous bacterial cellulose lithium ion battery diaphragm prepared in step (2) was immersed in the solution for 2 h. The solution was then taken out and placed on a glass plate. The solution was dried in a vacuum drying oven at 110°C until there was no significant change in mass, thereby obtaining a porous bacterial cellulose lithium ion battery diaphragm loaded with lithium nitrate.

[0087] 2. Assemble button batteries

[0088] The positive electrode is selected by coating a slurry of 80wt% lithium iron phosphate, 10wt% acetylene black and 10wt% polyvinylidene fluoride on aluminum foil, then drying in an oven at 60°C for 6h, and then cutting into a positive electrode sheet with a radius of 0.6cm and a gram capacity of 150mAh / g; the electrolyte is 60μL of 1M LiPF6-EC / DMC / EMC (in an argon atmosphere, ethylene carbonate (EC), ethyl methyl carbonate (EMC) and dimethyl carbonate (DMC) are first mixed in a mass ratio of 1:1:1, and then lithium salt lithium hexafluorophosphate (LiPF6) is added to dissolve and mix evenly to prepare a 1M LiPF6 solution); the negative electrode is a metal lithium sheet with a radius of 0.75cm and a thickness of 0.5mm. The diaphragm dried in step (3) is assembled with the positive electrode sheet, the negative electrode and the electrolyte into a button battery R2032, and the entire assembly process is carried out in a glove box filled with argon.

[0089] Example 2

[0090] 1. Preparation of porous bacterial cellulose lithium-ion battery separator loaded with lithium nitrate

[0091] (1) Preparation of bacterial cellulose suspension: The method is the same as Example 1.

[0092] (2) Preparation of porous bacterial cellulose lithium-ion battery separator: The method is the same as that in Example 1.

[0093] (3) Battery diaphragm loaded with lithium nitrate: 0.36 g LiNO3 was dissolved in 10 g pure ethanol and stirred for 1 h until the solution was clear. The porous bacterial cellulose lithium ion battery diaphragm prepared in step (2) was immersed in the solution for 2 h. The solution was then taken out and placed on a glass plate. The solution was dried in a vacuum drying oven at 110°C until there was no significant change in mass. Thus, a porous bacterial cellulose lithium ion battery diaphragm loaded with lithium nitrate was obtained.

[0094] 2. Assemble button batteries

[0095] Assemble button cells in the same manner as in Example 1.

[0096] Example 3

[0097] 1. Preparation of porous bacterial cellulose lithium-ion battery separator loaded with lithium nitrate

[0098] (1) Preparation of bacterial cellulose suspension: The method is the same as Example 1.

[0099] (2) Preparation of porous bacterial cellulose lithium-ion battery separator: The method is the same as that in Example 1.

[0100] (3) Battery diaphragm loaded with lithium nitrate: 0.54 g LiNO3 was dissolved in 10 g pure ethanol and stirred for 1 h until the solution was clear. The porous bacterial cellulose lithium ion battery diaphragm prepared in step (2) was immersed in the solution for 2 h. The solution was then taken out and placed on a glass plate. The solution was dried in a vacuum drying oven at 110°C until there was no significant change in mass, thereby obtaining a porous bacterial cellulose lithium ion battery diaphragm loaded with lithium nitrate.

[0101] 2. Assemble button batteries

[0102] Assemble button cells in the same manner as in Example 1.

[0103] Example 4

[0104] 1. Preparation of porous bacterial cellulose lithium-ion battery separator loaded with lithium nitrate

[0105] (1) Preparation of bacterial cellulose suspension: The method is the same as Example 1.

[0106] (2) Preparation of porous bacterial cellulose lithium-ion battery separator: The method is the same as that in Example 1.

[0107] (3) Battery diaphragm loaded with lithium nitrate: 0.72 g of LiNO3 was dissolved in 10 g of pure ethanol and stirred for 1 h until the solution was clear. The porous bacterial cellulose lithium ion battery diaphragm prepared in step (2) was immersed in the solution for 2 h. The solution was then taken out and placed on a glass plate. The solution was dried in a vacuum drying oven at 110°C until there was no significant change in mass, thereby obtaining a porous bacterial cellulose lithium ion battery diaphragm loaded with lithium nitrate.

[0108] 2. Assemble button batteries

[0109] Assemble button cells in the same manner as in Example 1.

[0110] Example 5

[0111] 1. Preparation of porous bacterial cellulose lithium-ion battery separator loaded with lithium nitrate

[0112] (1) Preparation of bacterial cellulose suspension: The method is the same as Example 1.

[0113] (2) Preparation of porous bacterial cellulose lithium-ion battery separator: The method is the same as that in Example 1.

[0114] (3) Battery diaphragm loaded with lithium nitrate: 0.9 g LiNO3 was dissolved in 10 g pure ethanol and stirred for 1 h until the solution was clear. The porous bacterial cellulose lithium ion battery diaphragm prepared in step (2) was immersed in the solution for 2 h. The porous bacterial cellulose lithium ion battery diaphragm was then taken out and placed on a glass plate. The porous bacterial cellulose lithium ion battery diaphragm was dried in a vacuum drying oven at 110°C until there was no significant change in mass, thereby obtaining a porous bacterial cellulose lithium ion battery diaphragm loaded with lithium nitrate.

[0115] 2. Assemble button batteries

[0116] Assemble button cells in the same manner as in Example 1.

[0117] Example 6

[0118] 1. Preparation of porous cellulose-based lithium-ion battery separator using bacterial cellulose grafted with chitosan as raw material

[0119] (1) Preparation of bacterial cellulose suspension: The method is the same as Example 1.

[0120] (2) Suspension of bacterial cellulose grafted with chitosan: 100 mL of the bacterial cellulose suspension prepared in step (1) was placed in a conical flask, and NaIO4 was added to a final concentration of 0.15 mol·L -1After deoxygenation with nitrogen, the mixture was stirred at 300-500 rpm / min for 2-2.5 h under the conditions of light shielding and 50±2°C to obtain oxidized bacterial cellulose, and then 5-6 mL of ethylene glycol was added to terminate the reaction. 10 g of chitosan powder was dispersed in 500 ml of 2% (v / v) CH3COOH solution and stirred at 60-70°C for 1-2 h to form a transparent chitosan solution. The oxidized bacterial cellulose solution is added to the chitosan solution, stirred continuously at 50-60°C for 2-3 hours, and then washed 4-6 times by a centrifuge to obtain a modified bacterial cellulose suspension grafted with chitosan at a concentration of 0.4-0.5wt%; wherein the viscosity of the chitosan is a medium viscosity of 200-400mPa.s (purchased from MacLean Reagent Company) (Note: when the viscosity is 200mPa.s, the molecular weight of chitosan is usually around 100,000 to 200,000; when the viscosity is 400mPa.s, the molecular weight of chitosan is usually around 200,000 to 400,000).

[0121] (3) Preparation of porous bacterial cellulose lithium-ion battery separator: A bacterial cellulose lithium-ion battery separator grafted with chitosan is prepared by vacuum filtration, and a three-dimensional porous network is formed by staggered stacking of cellulose fibers. 6 to 7 g of the bacterial cellulose suspension grafted with chitosan obtained in step (1) is diluted with water to 80 to 100 g, and then poured into a sand core funnel for filtration to form a membrane. Subsequently, the wet separator is placed in excess pure ethanol for 3 to 4 hours so that the water in the separator is completely replaced by ethanol. The separator is then dried at 75 to 100°C in a drum dryer for 5 to 10 minutes to obtain the desired porous bacterial cellulose lithium-ion battery separator grafted with chitosan, and the radius of the membrane is 0.8 cm.

[0122] (4) Battery diaphragm loaded with lithium nitrate: 0.18 g of LiNO3 was dissolved in 10 g of pure ethanol and stirred for 1 h until the solution was clear. The porous bacterial cellulose lithium ion battery diaphragm grafted with chitosan prepared in step (3) was immersed in the solution for 2 h. The solution was then taken out and placed on a glass plate. The solution was dried in a vacuum drying oven at 110°C until there was no significant change in mass. Thus, a bacterial cellulose lithium ion battery diaphragm grafted with chitosan loaded with lithium nitrate was obtained.

[0123] 2. Assemble button batteries

[0124] Assemble button cells in the same manner as in Example 1.

[0125] Example 7

[0126] 1. Preparation of porous bacterial cellulose lithium-ion battery separator grafted with chitosan

[0127] (1) Preparation of bacterial cellulose suspension: The method is the same as Example 6.

[0128] (2) Suspension of bacterial cellulose grafted with chitosan: The method is the same as that of Example 6.

[0129] (3) Preparation of porous bacterial cellulose lithium-ion battery separator: The method is the same as Example 6.

[0130] (4) Battery diaphragm loaded with lithium nitrate: 0.36 g of LiNO3 was dissolved in 10 g of pure ethanol and stirred for 1 h until the solution was clear. The porous bacterial cellulose lithium ion battery diaphragm grafted with chitosan prepared in step (3) was immersed in the solution for 2 h. The solution was then taken out and placed on a glass plate. The solution was dried in a vacuum drying oven at 110°C until there was no significant change in mass. Thus, a bacterial cellulose lithium ion battery diaphragm grafted with chitosan loaded with lithium nitrate was obtained.

[0131] 2. Assemble button batteries

[0132] Assemble button cells in the same manner as in Example 1.

[0133] Example 8

[0134] 1. Preparation of porous bacterial cellulose lithium-ion battery separator grafted with chitosan

[0135] (1) Preparation of bacterial cellulose suspension: The method is the same as Example 6.

[0136] (2) Suspension of bacterial cellulose grafted with chitosan: The method is the same as that of Example 6.

[0137] (3) Preparation of porous bacterial cellulose lithium-ion battery separator: The method is the same as Example 6.

[0138] (4) Battery diaphragm loaded with lithium nitrate: 0.54 g LiNO3 was dissolved in 10 g pure ethanol and stirred for 1 h until the solution was clear. The porous bacterial cellulose lithium ion battery diaphragm grafted with chitosan prepared in step (3) was immersed in the solution for 2 h. The solution was then taken out and placed on a glass plate. The solution was dried in a vacuum drying oven at 110°C until there was no significant change in mass. Thus, a bacterial cellulose lithium ion battery diaphragm grafted with chitosan loaded with lithium nitrate was obtained.

[0139] 2. Assemble button batteries

[0140] Assemble button cells in the same manner as in Example 1.

[0141] Example 9

[0142] 1. Preparation of porous bacterial cellulose lithium-ion battery separator grafted with chitosan

[0143] (1) Preparation of bacterial cellulose suspension: The method is the same as Example 6.

[0144] (2) Suspension of bacterial cellulose grafted with chitosan: The method is the same as that of Example 6.

[0145] (3) Preparation of porous bacterial cellulose lithium-ion battery separator: The method is the same as Example 6.

[0146] (4) Battery diaphragm loaded with lithium nitrate: 0.72 g of LiNO3 was dissolved in 10 g of pure ethanol and stirred for 1 h until the solution was clear. The porous bacterial cellulose lithium ion battery diaphragm grafted with chitosan prepared in step (3) was immersed in the solution for 2 h. The solution was then taken out and placed on a glass plate. The solution was dried in a vacuum drying oven at 110°C until there was no significant change in mass. Thus, a bacterial cellulose lithium ion battery diaphragm grafted with chitosan loaded with lithium nitrate was obtained.

[0147] 2. Assemble button batteries

[0148] Assemble button cells in the same manner as in Example 1.

[0149] Example 10

[0150] 1. Preparation of porous bacterial cellulose lithium-ion battery separator grafted with chitosan

[0151] (1) Preparation of bacterial cellulose suspension: The method is the same as Example 6.

[0152] (2) Suspension of bacterial cellulose grafted with chitosan: The method is the same as that of Example 6.

[0153] (3) Preparation of porous bacterial cellulose lithium-ion battery separator: The method is the same as Example 6.

[0154] (4) Battery diaphragm loaded with lithium nitrate: 0.9 g of LiNO3 was dissolved in 10 g of pure ethanol and stirred for 1 h until the solution was clear. The porous bacterial cellulose lithium ion battery diaphragm grafted with chitosan prepared in step (3) was immersed in the solution for 2 h. The solution was then taken out and placed on a glass plate. The solution was dried in a vacuum drying oven at 110°C until there was no significant change in mass. Thus, a bacterial cellulose lithium ion battery diaphragm grafted with chitosan loaded with lithium nitrate was obtained.

[0155] 2. Assemble button batteries

[0156] Assemble button cells in the same manner as in Example 1.

[0157] Comparative Example 1

[0158] 1. Preparation of porous bacterial cellulose lithium-ion battery separator loaded with lithium nitrate

[0159] (1) Preparation of bacterial cellulose suspension: The method is the same as Example 1.

[0160] (2) Preparation of porous bacterial cellulose lithium-ion battery separator: The method is the same as that in Example 1.

[0161] (3) Battery diaphragm loaded with lithium nitrate: 1.08 g of LiNO3 was dissolved in 10 g of pure ethanol and stirred for 1 h until the solution was clear. The porous bacterial cellulose lithium ion battery diaphragm prepared in step (2) was immersed in the solution for 2 h. The porous bacterial cellulose lithium ion battery diaphragm was then taken out and placed on a glass plate. The porous bacterial cellulose lithium ion battery diaphragm was dried in a vacuum drying oven at 110°C until there was no significant change in mass, thereby obtaining a porous bacterial cellulose lithium ion battery diaphragm loaded with lithium nitrate.

[0162] 2. Assemble button batteries

[0163] Assemble button cells in the same manner as in Example 1.

[0164] Comparative Example 2

[0165] 1. Preparation of porous bacterial cellulose lithium-ion battery separator grafted with chitosan

[0166] (1) Preparation of bacterial cellulose suspension: The method is the same as Example 6.

[0167] (2) Suspension of bacterial cellulose grafted with chitosan: The method is the same as that of Example 6.

[0168] (3) Preparation of porous bacterial cellulose lithium-ion battery separator: The method is the same as Example 6.

[0169] (4) Battery diaphragm loaded with lithium nitrate: 1.08 g of LiNO3 was dissolved in 10 g of pure ethanol and stirred for 1 h until the solution was clear. The porous bacterial cellulose lithium ion battery diaphragm grafted with chitosan prepared in step (3) was immersed in the solution for 2 h. The solution was then taken out and placed on a glass plate. The solution was dried in a vacuum drying oven at 110°C until there was no significant change in mass. Thus, a bacterial cellulose lithium ion battery diaphragm grafted with chitosan loaded with lithium nitrate was obtained.

[0170] 2. Assemble button batteries

[0171] Assemble button cells in the same manner as in Example 1.

[0172] Comparative Example 3

[0173] 1. Preparation of porous bacterial cellulose lithium-ion battery separator loaded with lithium nitrate

[0174] (1) Preparation of bacterial cellulose suspension: The method is the same as Example 1.

[0175] (2) Preparation of porous bacterial cellulose lithium-ion battery separator: The method is the same as that in Example 1.

[0176] (3) Battery diaphragm loaded with lithium nitrate: 0.18 g of LiNO3 was dissolved in 10 g of deionized water, and the solution was stirred for 1 h until it became clear. The porous bacterial cellulose lithium-ion battery diaphragm prepared in step (2) was immersed in the solution for 2 h, and then taken out and placed on a glass plate. The solution was dried in a vacuum drying oven at 110°C until there was no significant change in mass, thereby obtaining a porous bacterial cellulose lithium-ion battery diaphragm loaded with lithium nitrate.

[0177] 2. Assemble button batteries

[0178] Assemble button cells in the same manner as in Example 1.

[0179] Comparative Example 4

[0180] 1. Preparation of lithium-ion battery separator

[0181] Dissolve 0.18 g of LiNO3 in 10 g of pure ethanol and stir for 1 hour until the solution is clear. Soak a commercial polypropylene PP lithium-ion battery separator (purchased from Cluder Co., Ltd., with a film thickness of 14 to 18 μm) in it for 2 hours, then take it out and place it on a glass plate. Dry it in a vacuum drying oven at 110°C until there is no obvious change in quality to obtain a lithium-ion battery separator.

[0182] 2. Assemble button batteries

[0183] Assemble button cells in the same manner as in Example 1.

[0184] Comparative Example 5

[0185] 1. Preparation of porous bacterial cellulose lithium-ion battery separator loaded with lithium nitrate

[0186] (1) Preparation of bacterial cellulose suspension: The method is the same as Example 1.

[0187] (2) Preparation of porous bacterial cellulose lithium-ion battery separator: The method is the same as that in Example 1.

[0188] (3) Loading lithium nitrate on battery diaphragm: the method is the same as that in Example 1.

[0189] 2. Preparation of electrolyte

[0190] In an argon atmosphere, ethylene carbonate (EC), ethyl methyl carbonate (EMC) and dimethyl carbonate (DMC) were first mixed in a mass ratio of 1:1:1, and then lithium salt lithium hexafluorophosphate (LiPF6) was added to dissolve and mix well to obtain an electrolyte with a lithium salt concentration of 1 M. LiNO3 was added to the above electrolyte at a weight ratio of 0.5%.

[0191] 3. Assemble button batteries

[0192] Assemble button cells in the same manner as in Example 1.

[0193] Comparative Example 6

[0194] 1. Porous oxidized bacterial cellulose lithium-ion battery separator loaded with lithium nitrate

[0195] (1) Preparation of bacterial cellulose suspension: The method is the same as Example 1.

[0196] (2) Preparation of oxidized bacterial cellulose: 100 mL of the bacterial cellulose suspension prepared in step (1) was placed in a conical flask and NaIO4 was added at a concentration of 0.15 mol·L -1 After deoxygenation with nitrogen, the mixture was stirred at 300-500 rpm / min for 2-2.5 h under the conditions of light shielding and 50±2°C to obtain oxidized bacterial cellulose. Finally, 5-6 mL of ethylene glycol was added to terminate the reaction.

[0197] (3) Preparation of porous oxidized bacterial cellulose lithium-ion battery separator: The oxidized bacterial cellulose lithium-ion battery separator is prepared by vacuum filtration, and a three-dimensional porous network is formed by staggered stacking of cellulose fibers. 6 to 7 g of the oxidized bacterial cellulose suspension prepared in step (2) is diluted with water to 80 to 100 g, and then poured into a sand core funnel for filtration to form a membrane. Subsequently, the wet membrane is placed in ethanol for 3 to 4 hours so that the water in the membrane is completely replaced by ethanol. The membrane is then dried at 75 to 100°C in a drum dryer for 5 to 10 minutes to obtain the desired porous oxidized bacterial cellulose lithium-ion battery separator, and the radius of the membrane is 0.8 cm.

[0198] (4) Battery diaphragm loaded with lithium nitrate: 0.18 g of LiNO3 was dissolved in 10 g of pure ethanol and stirred for 1 h until the solution was clear. The porous oxidized bacterial cellulose lithium ion battery diaphragm prepared in step (3) was immersed in the solution for 2 h. The solution was then taken out and placed on a glass plate. The solution was dried in a vacuum drying oven at 110°C until there was no significant change in mass. Thus, a porous oxidized bacterial cellulose lithium ion battery diaphragm loaded with lithium nitrate was obtained.

[0199] 2. Assemble button batteries

[0200] Assemble button cells in the same manner as in Example 1.

[0201] Effect Example

[0202] 1. Scanning electron microscopy observation

[0203] The scanning electron microscope (SEM) observation results of the porous bacterial cellulose lithium ion battery separator (not loaded with LiNO3) prepared in step (2) of Example 1 and the porous bacterial cellulose lithium ion battery separator (not loaded with LiNO3) grafted with chitosan prepared in step (3) of Example 6 are as follows: Figure 1 and Figure 2 As shown in Figure 2, it can be seen that the pores of the bacterial cellulose membrane grafted with chitosan are more abundant, so it can absorb more electrolyte and promote the migration of lithium ions.

[0204] The SEM image of the porous oxidized bacterial cellulose lithium ion battery separator (LiNO3 loading is 0.5%) prepared in step (4) of Comparative Example 6 is as follows: Figure 3 As shown, Figure 1 By comparison, it can be seen that the pore size of the oxidized bacterial cellulose is significantly reduced, showing a denser surface.

[0205] The SEM images of the bacterial cellulose lithium ion battery separators of chitosan grafted with lithium nitrate prepared in step (4) of Example 8 and Comparative Example 2 (the loading amounts of LiNO3 are 1.5% and 3%, respectively) are as follows: Figure 4 and Figure 5 As shown. It can be seen that too high a concentration of LiNO3 will block the pores of the bacterial cellulose membrane, thereby increasing the difficulty of lithium ion conduction and making it easier to produce polarization in the battery.

[0206] 2. Performance Testing

[0207] The porous cellulose-based lithium-ion battery separators prepared in Examples 1 to 10 and the lithium-ion battery separators in Comparative Examples 1 to 6 were measured and compared in terms of thickness, porosity and liquid absorption, and the cycle performance and coulomb efficiency were tested. The experiment was repeated three times. The specific test method is as follows:

[0208] ①Porosity test method: Soak the diaphragm in n-butanol for 1 hour to fully infiltrate it, and then calculate the porosity according to the formula:

[0209]

[0210] Where W b and W c are the wet weight and dry weight of the membrane, respectively, b and ρ c are the densities of n-butanol and the membrane, respectively.

[0211] ②Test method for liquid absorption rate: weigh the mass of the diaphragm before and after absorbing the electrolyte, and divide the mass after absorption by the mass before absorption.

[0212] ③Test methods for cycle performance and coulomb efficiency:

[0213] At 25°C, the assembled button battery is charged to 3.8V at a constant current of 0.2C. At this time, the button battery is fully charged, and the charging capacity of the first cycle is recorded as the initial charging capacity; after the button battery is left to stand for 2 minutes, it is discharged at a constant current of 0.5C to a discharge cut-off voltage of 2.5V. This is a cyclic charge and discharge process, and the discharge capacity of the first cycle is recorded as the initial discharge capacity. The button battery is subjected to a cyclic charge and discharge test according to the above method, and the discharge capacity after each cycle is recorded until the discharge capacity of the button battery decays to 80% of the discharge capacity of the first cycle. The number of cycles at this time is used to characterize the cycle performance of the button battery. The higher the number of cycles, the better the cycle performance of the button battery. Coulomb efficiency is the ratio of discharge capacity to charging capacity.

[0214] The results are shown in Table 1 below.

[0215] Table 1

[0216]

[0217]

[0218] Note: In the table, LiNO3 concentration (%) is the mass ratio concentration of LiNO3 in the membrane, that is, the mass of lithium nitrate loaded in the membrane divided by the mass of the membrane.

[0219] Result analysis:

[0220] It can be seen from Examples 1 to 4 and Comparative Example 3 that loading LiNO3 in the porous bacterial cellulose membrane can effectively improve the cycle performance of the battery. This is because LiNO3 can be slowly released in the electrolyte and always remain in a saturated state, so that it can preferentially decompose on the surface of the negative electrode to form a stable SEI mainly composed of inorganic components, which promotes the deposition / stripping behavior of lithium ions and reduces the side reactions between the electrolyte and the electrode.

[0221] It can be seen from Examples 1 to 5 and Examples 6 to 10 that the porosity and liquid absorption rate of the bacterial cellulose membrane grafted with chitosan are improved, so it can store more electrolyte, and further promote the conduction of lithium ions, thereby improving the cycle efficiency of the battery. In addition, it can be seen that when the concentration of LiNO3 is 1.5%, the porosity and liquid absorption rate of the membrane decrease by a small margin, and the SEI formed is the most stable, and the battery cycle is the highest. This shows that too low a concentration of LiNO3 is not enough to maintain the formation of a stable SEI layer, while too high a concentration of LiNO3 will block the pores of the porous membrane and reduce the conduction of lithium ions. However, when the concentration of LiNO3 continues to increase to 3% (Comparative Examples 1 and 2), excess lithium nitrate will block the pores because lithium nitrate itself is insoluble in the electrolyte, thereby reducing the cycle performance of the battery.

[0222] It can be seen from Example 1 and Comparative Example 3 that in Comparative Example 1, water is used as the solvent for LiNO3, and the porosity and liquid absorption rate of the bacterial cellulose membrane obtained will decrease. This is because the polarity of water is stronger than that of ethanol, and the spacing between cellulose chains will be reduced during the drying process, thereby forming a denser structure, which will lead to reduced absorption of the electrolyte and increase the transmission impedance of lithium ions.

[0223] It can be seen from Examples 1 and 6 and Comparative Examples 3 and 4 that the porous structure can effectively load LiNO3 and play a role in sustained release, while the commercial PP membrane has only a single layer of pores and cannot load LiNO3 therein by physical coating, indicating that the porous cellulose-based membrane can serve as an effective sustained-release carrier for insoluble additives.

[0224] It can be seen from Example 1 and Comparative Example 5 that when LiNO3 is directly added to the electrolyte, LiNO3 cannot be completely dissolved and can only exist in the electrolyte in the form of crystals, which leads to aggregation on the electrode surface to cause polarization, inhibit the conduction of lithium ions and thus reduce the cycle performance of the battery.

[0225] It can be seen from Examples 1, 6 and Comparative 6 that only oxidizing bacterial cellulose without grafting chitosan will cause a certain degree of damage to the degree of polymerization of cellulose, reducing the size of cellulose to form a denser diaphragm, which will reduce the absorption of electrolyte and increase the mass transfer impedance of lithium ions, ultimately reducing the cycle performance.

[0226] The above embodiments are preferred implementation modes of the present invention, but the implementation modes of the present invention are not limited to the above embodiments. Any other changes, modifications, substitutions, combinations, and simplifications that do not deviate from the spirit and principles of the present invention should be equivalent replacement methods and are included in the protection scope of the present invention.

Claims

1. A method for preparing a porous cellulose-based lithium-ion battery separator, characterized in that: The steps include: (1) Preparation of bacterial cellulose suspension Cut the flake bacterial cellulose into small pieces, wash with water, and then completely boil in NaOH solution for 1 to 1.5 hours to clean the residual medium and impurities; then rinse with water, add CH3COOH solution to neutralize, and then wash with water until neutral, and finally use a homogenizer to fiberize it into slurry to obtain a bacterial cellulose suspension; (2) Suspension of bacterial cellulose grafted with chitosan Adding NaIO4 to the bacterial cellulose suspension obtained in step (1), deoxygenating with nitrogen, stirring and reacting under the conditions of light shielding and 50±2°C, adding ethylene glycol to terminate the reaction after the reaction is completed, and obtaining an oxidized bacterial cellulose solution; adding chitosan powder to a CH3COOH solution, stirring and dissolving at 60-70°C to form a transparent chitosan solution; then adding the oxidized bacterial cellulose solution to the chitosan solution, stirring and reacting at 50-60°C, centrifuging and washing after the reaction is completed, and obtaining a bacterial cellulose suspension grafted with chitosan; (3) Preparation of porous bacterial cellulose lithium-ion battery separator The bacterial cellulose suspension obtained in step (1) and / or the bacterial cellulose suspension grafted with chitosan obtained in step (2) is diluted with water and then filtered to form a membrane to obtain a wet porous cellulose-based membrane; then the membrane is immersed in pure ethanol so that the water in the porous cellulose-based membrane is completely replaced by ethanol, and finally dried at 75-100° C. to obtain a porous bacterial cellulose lithium-ion battery membrane; (4) Battery separator loaded with lithium salt Add lithium salt to ethanol, stir and dissolve to prepare a lithium salt solution with a mass concentration of 0.5-2.5%; then immerse the porous bacterial cellulose lithium ion battery separator obtained in step (3) in the lithium salt solution, take it out after immersion, and dry it at 90-120° C. to obtain a porous cellulose-based lithium ion battery separator loaded with lithium salt; wherein the lithium salt is at least one of lithium nitrate, lithium tetrafluoroborate and lithium perchlorate.

2. The method according to claim 1, characterized in that: The concentration of the bacterial cellulose suspension in step (1) is 0.4-0.5% by mass; The concentration of the bacterial cellulose suspension grafted with chitosan in step (2) is 0.4-0.5% by mass.

3. The method according to claim 1, characterized in that: The concentration of the chitosan solution in step (2) is 0.02-0.03 g / ml; The chitosan described in step (2) is medium viscosity chitosan, and its viscosity is 200-400 mPa.s.

4. The method according to claim 1, characterized in that: The concentration of the NaOH solution in step (1) is 0.05-0.2 mol / L; The amount of NaIO4 added in step (2) is calculated based on the final concentration of NaIO4 in the reaction system being 0.1 to 0.2 mol / L; The amount of ethylene glycol used in step (2) accounts for 5-6% of the volume of the reaction system; The dilution described in step (3) is dilution by adding water 10 to 20 times.

5. The method according to claim 1, characterized in that: The homogenizer described in step (1) is a high-speed homogenizer, and its rotation speed is 25000~30000rpm; In step (2), the stirring reaction conditions under the conditions of shading and 50±2° C. are: a rotation speed of 300 to 500 rpm / min, and a stirring reaction time of 2 to 2.5 h; The stirring and dissolving time in step (2) is 1 to 2 hours; In step (2), the stirring reaction time at 50-60° C. is 2-3 h; The number of centrifugal washings in step (2) is 4 to 6 times; The soaking time in step (3) is 3 to 4 hours; The drying in step (3) is performed by using a drum dryer for 5 to 10 minutes; The stirring time in step (4) is 1 to 2 hours; The soaking time in step (4) is 1 to 2 hours.

6. A porous cellulose-based lithium-ion battery separator, characterized in that: It is prepared by the method according to any one of claims 1 to 5.

7. Use of the porous cellulose-based lithium-ion battery separator according to claim 6 in lithium-ion batteries.

8. A lithium ion battery, characterized in that: The invention comprises a positive electrode, a negative electrode, the porous cellulose-based lithium-ion battery separator as claimed in claim 6 and an electrolyte.

9. The lithium-ion battery according to claim 8, characterized in that: The positive electrode is composed of an active material capable of embedding and extracting lithium ions, a conductive agent, a binder and a current collector; wherein, The active material comprises at least one of lithium cobalt oxide, nickel-cobalt-manganese ternary material, nickel-cobalt-aluminum ternary material, lithium iron phosphate and lithium manganese oxide; The conductive agent includes at least one of acetylene black, carbon black, graphite and carbon fiber; The binder includes at least one of polyvinylidene fluoride and polyacrylic acid; The current collector is aluminum foil.

10. The lithium-ion battery according to claim 8, characterized in that: The electrolyte is composed of lithium salt and solvent; wherein, The lithium salt includes one or more of lithium hexafluorophosphate, lithium bis(trifluoromethylsulfonyl)imide and lithium fluorosulfonyl imide; The solvent includes one or more of ethylene carbonate, dimethyl carbonate, ethyl methyl carbonate and propylene carbonate; The concentration of lithium salt in the electrolyte is 0.5-2 mol / L.

Citation Information

Patent Citations

  • Functional lithium ion battery diaphragm and preparation method thereof

    CN107369799A

  • Composite diaphragm with slow release function as well as preparation method and application of composite diaphragm

    CN114927828A

  • Method for preparing UIO-66-NH2 cross-linked bacterial cellulose lithium ion battery diaphragm

    CN116315424A

  • Cellulose-based separators comprising flame retardant, and uses thereof in electrochemistry

    US20220109214A1

Cited By

  • Cellulose diaphragm, preparation method thereof and lithium battery

    CN121097341A

  • Cellulose-based separator, method for preparing the same, and lithium battery

    CN121097341B

  • Quick-charge gel-state polymer electrolyte, preparation thereof and lithium ion battery

    CN121237998A

  • A fast-charging type gel polymer electrolyte, preparation thereof and lithium ion battery

    CN121237998B