Method for removing hard masks based on MOS (Metal Oxide Semiconductor) grids with different heights
Through dry etching technology and photoresist protection, the MOS gate hard mask layers of different heights are removed, which solves the damage problem in the prior art and improves the electrical performance and reliability of the device.
Patent Information
- Application Number
- CN202411079299.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-07
- Publication Date
- 2024-11-22
AI Technical Summary
The prior art can easily cause damage to the sidewall and surface when removing MOS gate hard mask layers at different heights, affecting the electrical performance of the device.
The organic flat layer is back-etched multiple times by using dry etching technology, gradually revealing and removing hard mask layers of different heights, and a photoresist is used to protect the gate sidewall and surface during the removal process to reduce damage.
It effectively avoids damage to the gate side wall and surface with large height difference, and improves the electrical performance and reliability of the device.
Smart Images

Figure CN119012681A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of semiconductor manufacturing, and in particular relates to a method for removing hard masks of MOS gates with different heights. Background Art
[0002] Display driver chip (DDIC) is an integrated circuit chip that controls the switch and display mode of liquid crystal panels and OLED panels. The static random access memory (SRAM) embedded in the chip is a very important module in the entire chip. With the improvement of display panel resolution and data transmission speed, the requirements for driver chips are also increasing. The smaller the size of the transistor, the faster the transmission speed and the lower the power consumption, and the higher the demand for SRAM with smaller unit size. Therefore, it is necessary to continue to develop more advanced high-voltage process platforms in the existing technology, covering 150nm, 90nm, 55nm, 40nm, 28nm and other technology nodes to provide more competitive SRAM.
[0003] In high-voltage platform applications, each transistor is designed for a different operating voltage. For a given operating voltage of a MOS device, the drain current is inversely proportional to the thickness of the gate oxide layer, so MOS devices with different gate oxide thickness characteristics can be formed to meet various requirements in a complex circuit. Generally, transistors operating at high voltages require thicker gate oxide layers, and transistors operating at low voltages require thinner gate oxide layers. Based on the above, the hard mask layer on top of the gate in the MOS structure is usually at different heights, so the process of removing the top hard mask layer also has a greater impact on the electrical performance of the device.
[0004] However, in the traditional removal of the hard mask layer, a wet method is usually used to solve the problem of removing the hard mask on the top of the gates of different heights, but it is easy to cause damage to the sidewalls and surfaces of the gates of different heights (silicon damage), especially the gates with large height differences, which affects the electrical performance of the MOS device. Therefore, how to optimize the removal method based on the hard mask of MOS gates of different heights to protect the sidewalls and surfaces from damage has become an important technical problem that needs to be urgently solved by technical personnel in this field. Summary of the invention
[0005] In view of the above-mentioned shortcomings of the prior art, the purpose of the present invention is to provide a method for removing MOS gate hard masks based on different heights, so as to solve the problem of damage to the sidewalls and surfaces of MOS devices of different heights in the prior art, thereby affecting the electrical performance of the device.
[0006] To achieve the above object, the present invention provides a method for removing MOS gate hard mask layers at different heights, comprising the following steps:
[0007] S1, providing a semiconductor substrate, the semiconductor substrate comprising a semiconductor substrate, a first gate, a second gate, a first hard mask layer and a second hard mask layer located on the semiconductor substrate; wherein the first gate comprises a first gate oxide layer, a first control gate and a first gate sidewall covering the first control gate stacked from bottom to top; the second gate comprises a second gate oxide layer, a second control gate and a second gate sidewall covering the second control gate stacked from bottom to top; the first hard mask layer is located on the first control gate and covers a top surface of the first control gate, the second hard mask layer is located on the second control gate and covers a top surface of the second control gate; and the first gate oxide layer and the second gate oxide layer have a thickness difference, so that the covered first hard mask layer is higher than the second hard mask layer;
[0008] S2, forming an organic planarization layer covering the first gate, the second gate, the first hard mask and the second hard mask on the semiconductor substrate;
[0009] S3, performing a first back etching on the organic planar layer by dry etching to completely expose the first hard mask layer;
[0010] S4, removing the first hard mask layer;
[0011] S5, performing a second back etching on the organic planar layer by dry etching to completely expose the second hard mask layer;
[0012] S6, forming a photoresist covering the first gate on the organic planar layer;
[0013] S7, removing the second hard mask layer;
[0014] S8, removing the organic planarization layer and the photoresist.
[0015] Optionally, the thickness difference has a value range of greater than 20 nm.
[0016] Optionally, the thickness difference has a value range of less than 20 nm, and steps S3 to S8 are replaced by the following steps:
[0017] S3': etching back the organic planar layer by dry etching to completely expose the first hard mask layer and the second hard mask layer;
[0018] S4': removing the first hard mask layer and the second hard mask layer;
[0019] S5': removing the organic planarization layer.
[0020] Optionally, the first gate oxide layer comprises SiO 2 layer, TaO5 layer, TiO 2 Layer, HfO 2 layer, ZrO 2 The second gate oxide layer comprises SiO 2 layer, TaO 5 layer, TiO 2 Layer, HfO 2 layer, ZrO 2 One or a combination of layers.
[0021] Optionally, the first hard mask layer includes a TiN layer, a SiN x Layer, SiO x The second hard mask layer includes a TiN layer, a SiN x Layer, SiO x One or a combination of layers.
[0022] Optionally, the organic planar layer includes one or a combination of a perfluoroalkoxy resin layer and a carbon-containing photosensitive resin layer.
[0023] Optionally, the removal method based on MOS gate hard masks of different heights is applicable to process nodes including 28nm, 40nm, 55nm, 90nm or 150nm.
[0024] Optionally, the first control gate includes one of a polysilicon control gate and an Al control gate, and the second control gate includes one of a polysilicon control gate and an Al control gate.
[0025] Optionally, the semiconductor substrate includes one or a combination of a P-type substrate and an N-type substrate.
[0026] The present invention also provides another method for removing MOS gate hard mask layers of different heights, comprising the following steps:
[0027] S1, providing a semiconductor substrate, wherein the semiconductor substrate comprises a semiconductor substrate, and at least three gates located on the semiconductor substrate, wherein the gate comprises a gate oxide layer, a control gate, and a gate sidewall covering the control gate stacked from bottom to top, wherein a hard mask layer is formed on the control gate, and the gate oxide layers of at least the three gates have different heights, so that the hard mask layers covering at least the three gates have different heights;
[0028] S2, forming an organic planarization layer covering all the gates on the semiconductor substrate;
[0029] S31, taking the hard mask layer with the highest current height as the target hard mask layer, and making the hard mask layer with a height difference of less than 20 nm from the target hard mask layer as the first hard mask layer to be removed;
[0030] S32, etching back the organic planar layer by dry etching to completely expose the target hard mask layer and the first hard mask layer to be removed, and removing the target hard mask layer and the first hard mask layer to be removed;
[0031] S33, repeat step S31;
[0032] S34, etching back the organic planar layer by dry etching to completely expose the target hard mask layer and the first hard mask layer to be removed, forming a photoresist covering the gate of the removed hard mask layer on the organic planar layer, and removing the target hard mask layer and all the first hard mask layers to be removed;
[0033] S35, repeating the above steps S33 and S34 until all the hard mask layers covering the gates are removed;
[0034] S4, removing the remaining organic planar layer and the photoresist.
[0035] As described above, the present invention is based on a method for removing hard masks of MOS gates of different heights. First, an organic flat layer is filled on a semiconductor substrate, and then the organic flat layer is first etched back by dry etching to expose the first hard mask layer. After removing the first hard mask layer, the organic flat layer is second etched back to expose the second hard mask layer, and then the surface of the first gate is covered with a photoresist. After removing the second hard mask layer, the remaining organic flat layer and the photoresist are removed to complete the removal of the hard mask layer. When there are 3 or more transistors with gates of different heights, transistors of different heights can be grouped and combined, so as to finally complete the removal of hard mask layers with different gate heights by performing multiple steps of etching back the organic flat layer, removing the hard mask layer, and covering the photoresist on the gate from which the hard mask layer has been removed. In this process, the sidewall and surface of the gate can be protected by the organic flat layer and the photoresist, thereby slowing down the damage to the sidewall and surface of the gate and improving the electrical performance and reliability of the device. BRIEF DESCRIPTION OF THE DRAWINGS
[0036] Figure 1 It is a schematic diagram of the process flow of removing MOS gate hard masks of different heights according to the present invention.
[0037] Figure 2 It is a schematic diagram of the structure before removing the hard mask on the top of the gate in Example 1 of the present invention.
[0038] Figure 3 It is a schematic diagram of the structure after filling the organic planarization layer in Example 1 of the present invention.
[0039] Figure 4 It is a schematic diagram of the structure after the first etching of the organic planarization layer in Example 1 of the present invention.
[0040] Figure 5 It is a schematic diagram of the structure after removing the first hard mask layer in Example 1 of the present invention.
[0041] Figure 6 It is a schematic diagram of the structure after the second etching of the organic planarization layer in Example 1 of the present invention.
[0042] Figure 7 It is a schematic diagram of the structure after forming a photoresist covering the first gate in Embodiment 1 of the present invention.
[0043] Figure 8 It is a schematic diagram of the structure after removing the second hard mask in Example 1 of the present invention.
[0044] Fig. 9 It is a schematic diagram of the structure after removing the organic planarization layer and the photoresist in Example 1 of the present invention.
[0045] Fig.10 It is a schematic diagram of the structure before removing the hard mask on the top of the gate in Example 3 of the present invention.
[0046] Fig.11 It is a schematic diagram of the structure after filling the organic planarization layer in Example 3 of the present invention.
[0047] Fig.12 It is a schematic diagram of the structure after the first etching of the organic planarization layer in Example 3 of the present invention.
[0048] Fig.13 It is a schematic diagram of the structure after removing the first hard mask in Example 3 of the present invention.
[0049] Fig.14 It is a schematic diagram of the structure after the second etching of the organic planarization layer in Example 3 of the present invention.
[0050] Fig.15 It is a schematic diagram of the structure after forming a photoresist covering the first gate in Example 3 of the present invention.
[0051] Fig.16 It is a schematic diagram of the structure after removing the second hard mask layer and the third hard mask layer in Example 3 of the present invention.
[0052] Fig.17 It is a schematic diagram of the structure after removing the organic planarization layer and the photoresist in Example 3 of the present invention.
[0053] Description of Reference Numerals
[0054] 101 Semiconductor Substrate
[0055] 102 First Gate
[0056] 103 Second Gate
[0057] 104 First gate oxide layer
[0058] 105 Second gate oxide layer
[0059] 106 Organic planar layer
[0060] 107 first hard mask layer
[0061] 108 second hard mask layer
[0062] 109 First control grid
[0063] 110 Second control grid
[0064] 111 First drain
[0065] 112 Second Source
[0066] 113 Second drain
[0067] 114 Photoresist
[0068] 115 first gate sidewall
[0069] 116 Second gate sidewall
[0070] 117 First Source
[0071] 118 Third gate oxide layer
[0072] 119 Third gate side wall
[0073] 120 third hard mask layer
[0074] 121 Third Gate
[0075] 122 Third drain
[0076] 123 Shallow Trench Isolation
[0077] 124 Third control grid
[0078] 125 Third Source DETAILED DESCRIPTION
[0079] The following describes the embodiments of the present invention through specific examples, and those skilled in the art can easily understand other advantages and effects of the present invention from the contents disclosed in this specification. The present invention can also be implemented or applied through other different specific embodiments, and the details in this specification can also be modified or changed in various ways based on different viewpoints and applications without departing from the spirit of the present invention.
[0080] For example, when describing the embodiments of the present invention in detail, for the sake of convenience, the cross-sectional view showing the device structure will not be partially enlarged according to the general scale, and the schematic view is only an example, which should not limit the scope of protection of the present invention. In addition, in actual production, the three-dimensional space dimensions of length, width and depth should be included.
[0081] For ease of description, spatial relational terms such as “under”, “below”, “below”, “below”, “over”, etc. may be used herein to describe the relationship of one element or feature shown in the drawings to other elements or features. It will be understood that these spatial relational terms are intended to include other orientations of the device in use or operation in addition to the orientation depicted in the drawings, and may include embodiments in which the first and second features are formed in direct contact, and may also include embodiments in which additional features are formed between the first and second features, so that the first and second features may not be in direct contact. In addition, when a layer is referred to as being “between” two layers, it may be the only layer between the two layers, or one or more intervening layers may also be present.
[0082] It should be noted that the illustrations provided in this embodiment are only used to illustrate the basic concept of the present invention in a schematic manner, and therefore the illustrations only show components related to the present invention rather than being drawn according to the number, shape and size of components in actual implementation. In actual implementation, the type, quantity and proportion of each component may be changed arbitrarily, and the component layout may also be more complicated.
[0083] Embodiment 1:
[0084] See also Figures 1 to 9 This embodiment provides a MOS gate hard mask removal method based on a first gate oxide layer and a second gate oxide layer having a thickness difference of D, and the thickness difference D is ≥ 20nm, which can effectively avoid damage to the gate sidewall and surface with a large height difference caused by removing the hard mask layer.
[0085] The following combination Figure 2 to Figure 9 , further introduces the method for removing the hard mask layer, including:
[0086] First, see Figure 1 and Figure 2, perform step S1-1, provide a semiconductor substrate, the semiconductor substrate includes a semiconductor substrate 101, a first gate 102 and a second gate 103 located on the semiconductor substrate 101, a first hard mask layer 107 and a second hard mask layer 108; wherein the first gate 102 includes a first gate oxide layer 104, a first control gate 109, and a first gate sidewall 115 covering the first control gate 109 stacked from bottom to top; the second gate 103 includes a second gate oxide layer 105, a first control gate 109, and a first gate sidewall 115 covering the first control gate 109 stacked from bottom to top A second control gate 110, and a second gate sidewall 116 covering the second control gate 110; the first hard mask layer 107 is located on the first control gate 109 and covers the top surface of the first control gate 109, the second hard mask layer 108 is located on the second control gate 110 and covers the top surface of the second control gate 110; and the first gate oxide layer 104 and the second gate oxide layer 105 have a thickness difference D, so that the covered first hard mask layer 107 is higher than the second hard mask layer 108.
[0087] Specifically, the semiconductor substrate 101 may include crystalline semiconductor material silicon, but may also include one or more other semiconductor materials, such as germanium, silicon-germanium alloy, compound semiconductor (e.g., GaAs, AlAs, InAs, GaN, AlN, etc.) or alloys thereof, oxide semiconductor (e.g., ZnO, SnO 2 、TiO 2 , Ga 2 O 3 etc.) or a combination thereof, and the semiconductor material may be doped or undoped.
[0088] In this embodiment, the value range of the thickness difference D is D≥20nm, such as D is 20nm, 50nm, 100nm, 200nm, etc. In this embodiment, the thickness difference D is preferably 85nm, wherein the thickness of the first gate oxide layer 104 is 105nm, and the thickness of the second gate oxide layer 105 is 20nm, but the selection of the thickness of the first gate oxide layer 104, the second gate oxide layer 105 and the thickness difference D therebetween can be selected according to specific needs and are not overly limited here.
[0089] Optionally, the first gate oxide layer 104 may include SiO 2 layer, TaO 5 layer, TiO 2 Layer, HfO 2 layer, ZrO 2 The second gate oxide layer 105 may include SiO 2 layer, TaO 5 layer, TiO 2Layer, HfO 2 layer, ZrO 2 In this embodiment, preferably, the first gate oxide layer 104 is SiO 2 layer, the second gate oxide layer 105 is SiO 2 However, the selection of specific types of the first gate oxide layer 104 and the second gate oxide layer 105 is not limited thereto.
[0090] Optionally, the first hard mask layer 107 may include a TiN layer, a SiN x Layer, SiO x The second hard mask layer 108 may include a TiN layer, a SiN x Layer, SiO x Preferably, the first hard mask layer 107 is SiN x layer, the second hard mask layer 108 is SiN x However, the specific types of the first hard mask layer 107 and the second hard mask layer 108 are not limited thereto.
[0091] Optionally, the first control gate 109 may include a polysilicon control gate or an Al control gate, and the second control gate 110 may include a polysilicon control gate or an Al control gate. In this embodiment, the first control gate 109 and the second control gate 110 are both made of the more commonly used polysilicon material, but the type of the control gate is not limited to this.
[0092] Optionally, the semiconductor substrate 101 may include a P-type substrate or an N-type substrate, or a combination thereof, and the semiconductor substrate 101 may be provided with an isolation structure therein as required. For example, the isolation structure may be Figure 2 The shallow trench isolation 123 in the embodiment is not excessively restricted here. Figure 2 It can be understood that the semiconductor substrate 101 also has a first source 117, a first drain 111, a second source 112, and a second drain 113. In this embodiment, preferably, the semiconductor substrate 101 is a combination of a P-type and an N-type substrate.
[0093] Next, see Figure 1 and Figure 3 , perform step S1 - 2 to form an organic planarization layer 106 on the semiconductor substrate 101 to cover the first gate 102 , the second gate 103 , the first hard mask layer 107 and the second hard mask layer 108 .
[0094] Among them, since the organic planar layer material is relatively x and SiN x, has a higher selectivity, is easier to remove, has good fluidity, is easy to solidify and shape, and can achieve good filling of the groove. Therefore, in this embodiment, the organic planar layer 106 is preferably used as a filling material layer. Further, the organic planar layer 106 may include one or a combination of a perfluoroalkoxy resin layer or a carbon-containing photosensitive resin layer. Carbon-containing polymers have aromatic groups and thus have excellent high temperature resistance. They are not easy to produce volatiles at high temperatures, which avoids the contamination of the resulting structure and ensures the production yield of the semiconductor structure. Therefore, in this embodiment, the organic planar layer 106 is preferably a carbon-containing photosensitive resin, but the specific type of the organic planar layer 106 is not limited thereto.
[0095] Next, see Figure 1 and Figure 4 , executing step S1 - 3 , performing a first back etching on the organic planarization layer 106 by dry etching to completely expose the first hard mask layer 107 .
[0096] Specifically, the organic planarization layer 106 is etched back to be flush with the lower surface of the first hard mask layer 107 , thereby exposing the first hard mask layer 107 .
[0097] Next, see Figure 1 and Figure 5 , perform step S1-4 to remove the first hard mask layer 107.
[0098] The method for removing the first hard mask layer 107 may be dry etching, and the etching selectivity ratio of the etching gas to the hard mask layer and the organic planar layer is preferably greater than or equal to 20:1, such as 20:1, 30:1, 40:1, etc., wherein the etching gas may include CF 4 , C 4 F 6 , C 4 F 8 , CHF 3 , CH 3 F, Cl 2 , CCl 4 wait.
[0099] Next, see Figure 1 and Figure 6 , executing step S1 - 5 , performing a second back etching on the organic planarization layer 106 by dry etching to completely expose the second hard mask layer 108 .
[0100] Specifically, the organic planarization layer 106 is etched back to be flush with the lower surface of the second hard mask layer 108 , thereby exposing the second hard mask layer 108 .
[0101] The organic planar layer 106 is etched using a dry etching process, which helps to precisely control the height and ensure good process control. Meanwhile, dry etching has a high selectivity and does not cause significant damage to the gate.
[0102] Next, see Figure 1 and Figure 7 , perform step S1-6 to form a photoresist 114 covering the first gate 102 on the organic planar layer 106. In the present embodiment, the photoresist 114 is used to protect the first gate 102 from which the first hard mask layer 107 has been removed. The material of the photoresist 114 is not excessively limited.
[0103] Next, see Figure 1 and Figure 8 , perform step S1-7 to remove the second hard mask layer 108.
[0104] The method for removing the second hard mask layer 108 may be dry etching, and the etching selectivity ratio of the etching gas to the hard mask layer and the organic planar layer is preferably greater than or equal to 20:1, such as 20:1, 30:1, 40:1, etc., wherein the etching gas may include CF 4 , C 4 F 6 , C 4 F 8 , CHF 3 , CH 3 F, Cl 2 , CCl 4 wait.
[0105] Next, see Figure 1 and Fig. 9 , perform step S1 - 8 to remove the organic planarization layer 106 and the photoresist 114 .
[0106] The removal method based on MOS gate hard masks of different heights in this embodiment is applicable to process nodes such as 28nm, 40nm, 55nm, 150nm, etc. In this embodiment, the preferred process node is 40nm.
[0107] In this embodiment, the thickness difference D is selected and set based on the etching selectivity of the dry etching gas to the material. When the thickness difference D between the first gate oxide layer 104 and the second gate oxide layer 105 is ≥ 20 nm, in the process of removing the hard mask, the organic planar layer 106 is used for covering, and the organic planar layer 106 is first etched back so that the organic planar layer 106 is flush with the lower surface of the first hard mask layer 107, so that the first hard mask layer 107 is exposed. After removing the first hard mask layer 107, the organic planar layer 106 is second etched back so that the organic planar layer 106 is flush with the lower surface of the second hard mask layer 108, so that the second hard mask layer 108 is exposed, and then the photoresist 114 is covered on the surface of the first gate 102. After removing the second hard mask layer 108, the remaining organic planar layer 106 and the photoresist 114 are removed. During the dry etching process, based on the etching selectivity ratio of the dry etching gas for the hard mask layer material and the sidewall protection material, this process can prevent the exposed sidewalls and surfaces within the thickness range D from top to bottom of the first gate 102 from being exposed to the etching atmosphere, thereby eliminating damage to the gate sidewalls and surface and protecting the electrical performance of the device.
[0108] Embodiment 2:
[0109] This embodiment provides a method for removing hard mask layers of MOS gates of different heights, wherein this embodiment is different from Embodiment 1 in that the thickness difference between the first gate oxide layer and the second gate oxide layer in this embodiment is d, and d<20nm. The method for removing the hard mask layer is further introduced as follows, specifically including:
[0110] First, step S2-1 is performed to provide a semiconductor substrate. This step is the same as step S1-1 in Example 1, except that the first gate oxide layer and the second gate oxide layer have a thickness difference d, and the value range of the thickness difference d is d<20nm. The materials of the semiconductor substrate and the gate are the same as those in Example 1 and will not be repeated here.
[0111] Next, step S2-2 is performed to form an organic planarization layer 106 on the semiconductor substrate to cover the first gate 102, the second gate 103, the first hard mask layer 107 and the second hard mask layer 108. This step is the same as step S1-2 in embodiment 1, and the material of the organic planarization layer is the same as that in embodiment 1, which will not be described again.
[0112] Next, step S2 - 3 is performed to etch back the organic planar layer using dry etching to completely expose all the hard mask layers.
[0113] Next, step S2 - 4 is performed to remove the first hard mask layer 107 and the second hard mask layer 108 .
[0114] Finally, step S2-5 is performed to remove the remaining organic planar layer.
[0115] In this embodiment, since the value range of the thickness difference d is relatively small d<20nm, such as d is 5, 10, 15, etc., in the process of removing the hard mask layer, the first hard mask layer and the second hard mask layer can be removed at the same time based on a one-step etching and one-step removal method, so that the hard mask can be removed conveniently without causing damage to the side wall and surface of the gate.
[0116] The above-mentioned Embodiment 1 and Embodiment 2 provide the case where there are two gates, and the gate oxide layers in the two gates have thickness differences of D and d.
[0117] The following describes the case where the thickness differences are D and d at the same time in combination with Example 3.
[0118] Embodiment 3:
[0119] This embodiment provides a method for removing a hard mask layer of a MOS gate with different heights, wherein this embodiment is different from Embodiment 1 mainly in that: this embodiment includes three gates, and the gate oxide layers of the three gates have different heights, wherein the first gate oxide layer and the second gate oxide layer have a thickness difference D≥20nm, and the second gate oxide layer and the third gate oxide layer have a thickness difference d<20nm. At this time, the following steps can be performed:
[0120] First, see Fig.10, performing step S3-1, providing a semiconductor substrate, the semiconductor substrate comprising a semiconductor substrate 101, a first gate 102, a second gate 103 and a third gate 121, a first hard mask layer 107, a second hard mask layer 108 and a third hard mask layer 120 located on the semiconductor substrate 101; wherein the first gate 102 comprises a first gate oxide layer 104, a first control gate 109 stacked from bottom to top, and a first gate sidewall 115 covering the first control gate 109; the second gate 103 comprises a second gate oxide layer 105, a second control gate 110 stacked from bottom to top, and a second gate sidewall 116 covering the second control gate 110; the third gate 121 comprises a third gate oxide layer 118 and a third control gate 124 stacked from bottom to top, and a third gate sidewall 119 covering the third control gate 124; the first hard mask layer 107 is located on the first control gate 109 and covers the top surface of the first control gate 109, the second hard mask layer 108 is located on the second control gate 110 and covers the top surface of the second control gate 110; the third hard mask layer 120 is located on the third control gate 124 and covers the top surface of the third control gate 124; and the first gate oxide layer 104 and the second gate oxide layer 105 have a thickness difference D, and the second gate oxide layer 105 and the third gate oxide layer 118 have a thickness difference d, so that the covered first hard mask layer 107 is higher than the second hard mask layer 108, and the covered second hard mask layer 108 is higher than the third hard mask layer 120.
[0121] Specifically, the material of the semiconductor substrate 101 may be the same as that of Embodiment 1, which will not be described in detail herein. Preferably, in this embodiment, semiconductor material silicon is used as the material of the semiconductor substrate 101 .
[0122] In this embodiment, the height difference D between the first hard mask layer and the second hard mask layer is greater than 20nm, the height difference d between the second hard mask layer and the third hard mask layer is less than 20nm, the thickness difference D is greater than or equal to 20nm, such as D can be 20nm, 50nm, 100nm, 200nm, etc., and in this embodiment, the thickness difference D is preferably 80nm; the thickness difference d is less than 20nm, such as d can be 18nm, 15nm, 10nm, 5nm, etc., and in this embodiment, the thickness difference d is preferably 18nm. Therefore, in this embodiment, the height difference between the first hard mask layer 107 and the third mask layer 120 is 98nm. Among them, the thicknesses of the first gate oxide 104, the second gate oxide 105, and the third gate oxide 118 can be 100nm, 20nm, and 2nm, respectively. However, the selection of the thicknesses of the first gate oxide layer 104, the second gate oxide layer 105, and the third gate oxide 118 and the thickness difference D and the thickness difference d can be selected according to specific needs and are not overly limited here.
[0123] Optionally, the semiconductor substrate 101 includes a P-type substrate or an N-type substrate, or a combination thereof, and the semiconductor substrate 101 may be provided with an isolation structure therein as required. The isolation structure may be Fig.10 The shallow trench isolation 123 in the embodiment is not excessively restricted here. Fig.10 It can be understood that the semiconductor substrate 101 also includes a first source 117, a first drain 111, a second source 112, a second drain 113, a third source 125, and a third drain 122. In this embodiment, preferably, the semiconductor substrate 101 is a combination of a P-type substrate and an N-type substrate.
[0124] The materials of the control gate, the gate oxide layer and the hard mask layer are the same as those in Example 1 and will not be described in detail here.
[0125] Next, see Fig.11 , perform step S3 - 2 to form an organic planarization layer 106 covering all the gates and corresponding to all the hard mask layers on the semiconductor substrate 101 . The material of the organic planarization layer 106 is the same as that of Embodiment 1 and will not be described again.
[0126] Next, step S3 - 31 is performed, wherein the hard mask layer with the highest current height is used as the target hard mask layer, and the hard mask layer with a height difference of less than 20 nm from the target hard mask layer is used as the first hard mask layer to be removed.
[0127] In this embodiment, the highest hard mask layer is the first hard mask layer 107. Since the height differences between the second hard mask layer 108 and the third hard mask layer 120 and the first hard mask layer 107 are 80 nm and 98 nm respectively, in this embodiment, the first hard mask layer 107 is the target hard mask layer 107. Since there is no hard mask layer with a height difference of less than 20 nm with the first hard mask layer 107, there is no first hard mask layer to be removed.
[0128] Next, execute step S3-32, see Fig.12 The organic planar layer 106 is etched back by dry etching to completely expose the first hard mask layer 107 as the target hard mask layer, and the first hard mask layer 107 as the target hard mask layer is removed. Fig.13 , removing the first hard mask layer 107 serving as a target mask layer.
[0129] Next, step S3-33 is executed. This step is the same as S3-31. The hard mask layer with the highest current height is used as the target mask layer, and the hard mask layer with a height difference of less than 20 nm from the target hard mask layer is used as the first hard mask layer to be removed.
[0130] In this embodiment, since the first hard mask layer 107 has been removed, the hard mask layer with the highest current height is the second hard mask layer 108. Therefore, the second hard mask layer 108 is used as the target mask layer. Since the height difference between the third hard mask layer 120 and the second hard mask layer 108 is <20nm, the third hard mask layer 120 is the first hard mask layer to be removed.
[0131] Next, execute step S3-34, see Fig.14 , the organic planar layer 106 is etched back by dry etching to completely expose the second hard mask layer 108 currently serving as the target hard mask layer and the third hard mask layer 120 currently serving as the first hard mask layer to be removed. Fig.15 , a photoresist 114 is formed on the organic planar layer 106 to cover the first gate 102 from which the hard mask layer has been removed. Fig.16 , the second hard mask layer 108 currently serving as the target hard mask layer and the third hard mask layer 120 currently serving as the first hard mask layer to be removed are removed.
[0132] In this embodiment, the photoresist 114 is used to protect the first gate 102 from which the first hard mask layer 107 has been removed, and the material of the photoresist 114 is not excessively limited. At the same time, in this embodiment, the method for removing the hard mask layer can be dry etching, and the etching selectivity ratio of the etching gas to the hard mask layer and the organic planar layer is preferably greater than or equal to 20:1, such as 20:1, 30:1, 40:1, etc., wherein the etching gas may include CF 4 , C 4 F 6 , C 4 F 8 , CHF 3 , CH 3 F, Cl 2 , CCl 4 wait.
[0133] By now, the hard mask layers of all gates have been removed.
[0134] Next, see Fig.17 , perform step S3 - 4 to remove the organic planarization layer 106 and the photoresist 114 .
[0135] In this embodiment, the thickness difference value is selected and set based on the etching selectivity of the dry etching gas to the material. When the thickness difference D between the first gate oxide layer 104 and the second gate oxide layer 105 is ≥20 nm, in the process of removing the hard mask, the organic planar layer 106 is used for covering, and the organic planar layer 106 is first etched back so that the organic planar layer 106 is flush with the lower surface of the first hard mask layer 107, so that the first hard mask layer 107 is exposed. After removing the first hard mask layer 107, the organic planar layer 106 is second etched back so that the organic planar layer 106 is flush with the lower surface of the third hard mask layer 120, so that the second hard mask layer 108 and the third hard mask layer 120 are exposed, and then the photoresist 114 is covered on the surface of the first gate 102. After removing the second hard mask layer 108 and the third hard mask layer 120, the remaining organic planar layer 106 and the photoresist 114 are removed. During the dry etching process, based on the etching selectivity of the dry etching gas for the hard mask layer material and the sidewall protection material, this process can prevent the exposed sidewalls and surfaces within the thickness range D from top to bottom of the first gate 102 from being exposed to the etching atmosphere, thereby eliminating the damage to the gate sidewalls and surfaces and protecting the electrical performance of the device. When the thickness difference d between the second gate oxide layer 105 and the third gate oxide layer 118 is less than 20nm, in the process of removing the hard mask, the organic flat layer 106 is used for covering, and one back etching is used to remove the second hard mask layer 108 and the third hard mask layer 120 at the same time. This process can not only save process steps and costs, but also the damage to the exposed sidewalls and surfaces within the range d from top to bottom of the second gate 103 is almost invisible.
[0136] Of course, in another embodiment, there may be 4 or more gates, wherein the gate oxide layers of at least three of the gates have different heights, so that the hard mask layers covering at least three of the gates have different heights, that is, the thickness difference includes the cases of all being D, all being d, and having both D and d. In this case, the following steps may be performed:
[0137] S1, providing a semiconductor substrate, wherein the semiconductor substrate comprises a semiconductor substrate, and at least three gates located on the semiconductor substrate, wherein the gates comprise a gate oxide layer, a control gate, and a gate sidewall covering the control gate stacked from bottom to top, wherein the control gate is covered with a hard mask layer, and the gate oxide layers of at least three of the gates have different heights, so that the hard mask layers covering at least three of the gates have different heights;
[0138] S2, forming an organic planarization layer covering all the gates on the semiconductor substrate;
[0139] S31, taking the hard mask layer with the highest current height as the target hard mask layer, and making the hard mask layer with a height difference of less than 20 nm from the target hard mask layer as the first hard mask layer to be removed;
[0140] S32, etching back the organic planar layer by dry etching to completely expose the target hard mask layer and the first hard mask layer to be removed, and removing the target hard mask layer and the first hard mask layer to be removed;
[0141] S33, repeat step S31;
[0142] S34, etching back the organic planar layer by dry etching to completely expose the target hard mask layer and the first hard mask layer to be removed, forming a photoresist covering the gate of the removed hard mask layer on the organic planar layer, and removing the target hard mask layer and all the first hard mask layers to be removed;
[0143] S35, repeating the above steps S33 and S34 until all the hard mask layers covering the gates are removed;
[0144] S4, removing the remaining organic planar layer and the photoresist.
[0145] In summary, the present invention is based on a method for removing hard masks of MOS gates of different heights. First, an organic flat layer is filled on a semiconductor substrate, and then the organic flat layer is first etched back by dry etching to expose the first hard mask layer. After removing the first hard mask layer, the organic flat layer is second etched back to expose the second hard mask layer, and then the surface of the first gate is covered with photoresist. After removing the second hard mask layer, the remaining organic flat layer and photoresist are removed to complete the removal of the hard mask layer. When there are 3 or more gate transistors of different heights, transistors of different heights can be grouped and combined, so that the removal of hard mask layers with different gate heights is finally completed by performing multi-step etching back of the organic flat layer, removing the hard mask layer, and covering the photoresist on the gate whose hard mask layer has been removed. In this process, the sidewall and surface of the gate can be protected by the organic flat layer and the photoresist, thereby slowing down the damage to the sidewall and surface and improving the electrical performance and reliability of the device. Therefore, the present invention effectively overcomes various shortcomings in the prior art and has a high industrial utilization value.
[0146] The above embodiments are merely illustrative of the principles and effects of the present invention, and are not intended to limit the present invention. Anyone familiar with the art may modify or alter the above embodiments without departing from the spirit and scope of the present invention. Therefore, all equivalent modifications or alterations made by a person of ordinary skill in the art without departing from the spirit and technical concept disclosed by the present invention shall still be covered by the claims of the present invention.
Claims
1. A method for removing MOS gate hard masks based on different heights, Features: The following steps are involved: S1, providing a semiconductor substrate, the semiconductor substrate comprising a semiconductor substrate, a first gate, a second gate, a first hard mask layer and a second hard mask layer located on the semiconductor substrate; wherein the first gate comprises a first gate oxide layer, a first control gate and a first gate sidewall covering the first control gate stacked from bottom to top; the second gate comprises a second gate oxide layer, a second control gate and a second gate sidewall covering the second control gate stacked from bottom to top; the first hard mask layer is located on the first control gate and covers a top surface of the first control gate, the second hard mask layer is located on the second control gate and covers a top surface of the second control gate; and the first gate oxide layer and the second gate oxide layer have a thickness difference, so that the covered first hard mask layer is higher than the second hard mask layer; S2, forming an organic planarization layer covering the first gate, the second gate, the first hard mask and the second hard mask on the semiconductor substrate; S3, performing a first back etching on the organic planar layer by dry etching to completely expose the first hard mask layer; S4, removing the first hard mask layer; S5, performing a second back etching on the organic planar layer by dry etching to completely expose the second hard mask layer; S6, forming a photoresist covering the first gate on the organic planar layer; S7, removing the second hard mask layer; S8, removing the organic planarization layer and the photoresist.
2. The method for removing MOS gate hard masks of different heights according to claim 1, Features: The thickness difference has a value range of more than 20 nm.
3. The method for removing MOS gate hard masks of different heights according to claim 1, Features: The thickness difference has a value range of less than 20 nm, and steps S3 to S8 are replaced by the following steps: S3': etching back the organic planar layer by dry etching to completely expose the first hard mask layer and the second hard mask layer; S4': removing the first hard mask layer and the second hard mask layer; S5': removing the organic planarization layer.
4. The method for removing MOS gate hard masks based on different heights according to claim 1, Features: The first gate oxide layer includes SiO 2 layer, TaO 5 layer, TiO 2 Layer, HfO 2 layer, ZrO 2 The second gate oxide layer comprises SiO 2 layer, TaO 5 layer, TiO 2 Layer, HfO 2 layer, ZrO 2 One or a combination of layers.
5. The method for removing MOS gate hard masks based on different heights according to claim 1, Features: The first hard mask layer includes a TiN layer, a SiN x Layer, SiO x The second hard mask layer includes a TiN layer, a SiN x Layer, SiO x One or a combination of layers.
6. The method for removing MOS gate hard masks based on different heights according to claim 1, Features: The organic planar layer includes one or a combination of a perfluoroalkoxy resin layer and a carbon-containing photosensitive resin layer.
7. The method for removing MOS gate hard masks based on different heights according to claim 1, Features: The method is applicable to process nodes including 28nm, 40nm, 55nm, 90nm or 150nm.
8. The method for removing MOS gate hard masks based on different heights according to claim 1, Features: The first control gate includes one of a polysilicon control gate and an Al control gate, and the second control gate includes one of a polysilicon control gate and an Al control gate.
9. The method for removing MOS gate hard masks based on different heights according to claim 1, Features: The semiconductor substrate includes one or a combination of a P-type substrate and an N-type substrate.
10. A method for removing MOS gate hard masks based on different heights, Features: The following steps are involved: S1, providing a semiconductor substrate, wherein the semiconductor substrate comprises a semiconductor substrate, and at least three gates located on the semiconductor substrate, wherein the gates comprise a gate oxide layer, a control gate, and a gate sidewall covering the control gate stacked from bottom to top, wherein the control gate is covered with a hard mask layer, and the gate oxide layers of at least three of the gates have different heights, so that the hard mask layers covering at least three of the gates have different heights; S2, forming an organic planarization layer covering all the gates on the semiconductor substrate; S31, taking the hard mask layer with the highest current height as the target hard mask layer, and making the hard mask layer with a height difference of less than 20 nm from the target hard mask layer as the first hard mask layer to be removed; S32, etching back the organic planar layer by dry etching to completely expose the target hard mask layer and the first hard mask layer to be removed, and removing the target hard mask layer and the first hard mask layer to be removed; S33, repeat step S31; S34, etching back the organic planar layer by dry etching to completely expose the target hard mask layer and the first hard mask layer to be removed, forming a photoresist covering the gate of the removed hard mask layer on the organic planar layer, and removing the target hard mask layer and all the first hard mask layers to be removed; S35, repeating the above steps S33 and S34 until all the hard mask layers covering the gates are removed; S4, removing the remaining organic planar layer and the photoresist.