Photoelectric device, preparation method thereof and display device

By using carbon nanocage-inorganic semiconductor particle composite as the electron transport layer, the problem of easy oxidation of ligands on the surface of inorganic semiconductor particles is solved, the life and luminous efficiency of optoelectronic devices are improved, and more stable electron transport performance is achieved.

CN119012741APending Publication Date: 2024-11-22TCL TECHNOLOGY GROUP CORPORATION
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310555761.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-05-16
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

The existing optoelectronic devices have a short lifespan, which is mainly due to the easy oxidation and poor stability of the surface ligands of inorganic semiconductor particles, resulting in poor electron transport performance.

Method used

Carbon nanocage-inorganic semiconductor particle composite material is used as the electron transport layer material. Inorganic semiconductor particles are isolated through the carbon nanocage to avoid agglomeration, and surface ligands are removed through ultrasonic mixing and calcination to improve the stability and conductivity of the material.

Benefits of technology

It significantly improves the life and luminous efficiency of optoelectronic devices, enhances the stability and conductivity of the electron transport layer, and extends the service life of the device.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119012741A_ABST
    Figure CN119012741A_ABST
Patent Text Reader

Abstract

The invention discloses a photoelectric device and a preparation method thereof and a display device.The photoelectric device comprises a first electrode, an electron transport layer and a second electrode which are stacked, and the material of the electron transport layer comprises a carbon nanocage-inorganic semiconductor particle composite material; the carbon nanocage-inorganic semiconductor particle composite material includes a carbon nanocage and at least one inorganic semiconductor particle filled in the carbon nanocage. The material of the electron transport layer comprises the carbon nanocage-inorganic semiconductor particle composite material, the inorganic semiconductor particles are filled in the carbon nanocage, and the carbon nanocage can isolate the inorganic semiconductor particles, so that agglomeration caused by aggregation of a large number of inorganic semiconductor particles is avoided, and the electron transport layer has good electron transport performance. The carbon nanocage can play a role in isolating and protecting the inorganic semiconductor particles and prevent the inorganic semiconductor particles from being eroded by water and oxygen, so that the stability of the inorganic semiconductor particles is improved, the stability of the electron transport layer is further improved, and the service life of the photoelectric device is prolonged.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the technical field of optoelectronic devices, and in particular to an optoelectronic device, a method for preparing the optoelectronic device, and a display device including the optoelectronic device. Background Art

[0002] Currently, the widely used optoelectronic devices are organic optoelectronic devices (OLED) and quantum dot optoelectronic devices (QLED). OLED has become the mainstream technology in the field of display technology due to its excellent display performance such as self-luminescence, simple structure, ultra-thinness, fast response speed, wide viewing angle, low power consumption, and flexible display. QLED has the advantages of saturated color of emitted light, adjustable wavelength, low start-up voltage, good solution processability, easy fine control of quantum dots, and high photoluminescence and electroluminescence quantum yield. In recent years, it has become a strong competitor to OLED.

[0003] The structure of traditional OLED and QLED devices generally includes an anode, a hole injection layer, a hole transport layer, a light-emitting layer, an electron transport layer, an electron injection layer and a cathode. Under the action of the electric field, the holes generated by the anode of the optoelectronic device and the electrons generated by the cathode move and are injected into the hole transport layer and the electron transport layer respectively, and finally migrate to the light-emitting layer. When the two meet in the light-emitting layer, energy excitons are generated, thereby exciting the light-emitting molecules and finally producing visible light.

[0004] The lifespan of existing optoelectronic devices is relatively short and needs to be further improved. Summary of the invention

[0005] In view of this, the present application provides a photoelectric device, aiming to improve the problem of short life of existing photoelectric devices.

[0006] An embodiment of the present application is implemented as follows: a photoelectric device includes a stacked first electrode, an electron transport layer, and a second electrode, wherein the material of the electron transport layer includes a carbon nanocage-inorganic semiconductor particle composite material, and the carbon nanocage-inorganic semiconductor particle composite material includes a carbon nanocage and at least one inorganic semiconductor particle filled in the carbon nanocage.

[0007] Optionally, in some embodiments of the present application, in the carbon nanocage-inorganic semiconductor particle composite material, the mass ratio of the carbon nanocage to the inorganic semiconductor particle is 1:(2-4); and / or

[0008] The average particle size of the carbon nano cage is 30 to 50 nm; and / or

[0009] The average particle size of the inorganic semiconductor particles is 7 to 12 nm; and / or

[0010] The carbon nano cage has a plurality of nanopores, and the pore diameter of the nanopores is 4-16 nm.

[0011] Optionally, in some embodiments of the present application, each carbon nanocage is filled with 1 to 3 inorganic semiconductor particles.

[0012] Optionally, in some embodiments of the present application, the carbon nanocage comprises a graphene carbon nanocage; and / or

[0013] The inorganic semiconductor particles include one or more of undoped metal oxides, doped metal oxides, ceramic semiconductor materials, IIB-VIA semiconductor materials, IIIA-VA semiconductor materials, and IB-IIIA-VIA semiconductor materials. The undoped metal oxides include ZnO, TiO 2 SnO 2 、ZrO 2 、 2 O 5 One or more of the doped metal oxides; the metal oxides in the doped metal oxides include ZnO, TiO 2 SnO 2 、ZrO 2 、 2 O 5 、Al 2 O 3 The doping elements in the doped metal oxide include one or more of Al, Mg, Li, Mn, Y, La, Cu, Ni, Zr, Ce, In, and Ga. The ceramic semiconductor material includes barium titanate. The IIB-VIA semiconductor material includes one or more of ZnS, ZnSe, and CdS. The IIIA-VA semiconductor material includes one or more of InP and GaP. The IB-IIIA-VIA semiconductor material includes one or more of CuInS and CuGaS.

[0014] Optionally, in some embodiments of the present application, the optoelectronic device further includes a light-emitting layer, and the light-emitting layer is located between the first electrode and the electron transport layer or between the second electrode and the electron transport layer.

[0015] Optionally, in some embodiments of the present application, the first electrode and the second electrode independently include a doped metal oxide electrode, a composite electrode, a graphene electrode, a carbon nanotube electrode, a metal element electrode or an alloy electrode, and the material of the doped metal oxide electrode includes one or more of indium-doped tin oxide, fluorine-doped tin oxide, antimony-doped tin oxide, aluminum-doped zinc oxide, gallium-doped zinc oxide, indium-doped zinc oxide, magnesium-doped zinc oxide, aluminum-doped magnesium oxide, and cadmium-doped zinc oxide, and the composite electrode includes AZO / Ag / AZO, AZO / Al / AZO, ITO / Ag / ITO, ITO / Al / ITO, ZnO / Ag / ZnO, ZnO / Al / ZnO, TiO 2 / Ag / TiO 2 、TiO 2 / Al / TiO 2 , ZnS / Ag / ZnS, ZnS / Al / ZnS, Ca / Al, LiF / Ca, LiF / Al, BaF 2 / Al、CsF / Al、CaCO 3 / Al or BaF 2 / Ca / Al, the material of the metal single substance electrode includes one or more of Ag, Ni, Pt, Au, Ir, Cu, Mo, Al, Ca, Mg and Ba, and the alloy electrode includes Au:Mg alloy electrode or Ag:Mg alloy electrode; and / or

[0016] The material of the light-emitting layer includes one or more of an organic light-emitting material and a quantum dot light-emitting material, and the organic light-emitting material includes one or more of 4,4'-bis(N-carbazole)-1,1'-biphenyl:tri[2-(p-tolyl)pyridine iridium(III), 4,4',4"-tri(carbazole-9-yl)triphenylamine:tri[2-(p-tolyl)pyridine iridium, diaromatic anthracene derivatives, distilbene aromatic derivatives, pyrene derivatives, fluorene derivatives, TBPe fluorescent materials, TTPX fluorescent materials, TBRb fluorescent materials, DBP fluorescent materials, delayed fluorescent materials, TTA materials, thermally activated delayed materials, polymers containing covalent bonds of BN, hybrid localized charge transfer excited state materials, exciplex light-emitting materials, polyacetylene and its derivatives, polyparaphenylene and its derivatives, polythiophene and its derivatives, polyfluorene and its derivatives;The quantum dot luminescent material includes one or more of a single structure quantum dot, a core-shell structure quantum dot and a perovskite semiconductor material. The material of the single structure quantum dot, the core material of the core-shell structure quantum dot and the shell material of the core-shell structure quantum dot are independently selected from one or more of group II-VI compounds, group IV-VI compounds, group III-V compounds and group I-III-VI compounds. The group II-VI compounds include CdS, CdSe, CdTe, ZnS, ZnSe, ZnTe, ZnO, HgS, HgSe, HgTe, CdSeS, CdSe Te, CdSTe, ZnSeS, ZnSeTe, ZnSTe, HgSeS, HgSeTe, HgSTe, CdZnS, CdZnSe, CdZnTe, CdHgS, CdHgSe, CdHgTe, HgZnS, HgZnSe, HgZnTe, CdZnSeS, CdZnSeTe, CdZnSTe, CdHgSeS, CdHgSeTe, CdHgSTe, HgZnSeS, HgZnSeTe and HgZnSTe, the IV-VI group compound includes SnS, S The III-V group compounds include one or more of GaN, GaP, GaAs, GaSb, AlN, AlP, AlAs, AlSb, InN, InP, InAs, InSb, GaNP, GaNAs, GaNSb, GaPAs, GaP One or more of Sb, AlNP, AlNAs, AlNSb, AlPAs, AlPSb, InNP, InNAs, InNSb, InPAs, InPSb, GaAlNP, GaAlNAs, GaAlNSb, GaAlPAs, GaAlPSb, GaInNP, GaInNAs, GaInNSb, GaInPAs, GaInPSb, InAlNP, InAlNAs, InAlNSb, InAlPAs and InAlPSb, and the Group I-III-VI compound includes CuInS; 2 、CuInSe 2 AgInS 2 One or more of; the perovskite semiconductor material includes a doped or undoped inorganic perovskite semiconductor or an organic-inorganic hybrid perovskite semiconductor, and the inorganic perovskite semiconductor has a general structural formula of AMX 3 , where A is Cs + ions, M is a divalent metal cation, including Pb2+ Sn 2+ , Cu 2+ 、Ni 2+ 、Cd 2+ Cr 2+ , Mn 2+ 、Co 2+ , Fe 2+ ,Ge 2+ , Yb 2+ 、Eu 2+ One or more of, X is a halogen anion, including Cl - Br - ,I - One or more of the organic-inorganic hybrid perovskite semiconductor has the general structural formula of BMX 3 , where B is an organic amine cation, including CH 3 (CH 2 ) n-2 NH 3 + or [NH 3 (CH 2 ) n NH 3 ] 2+ , where n≥2, M is a divalent metal cation, including Pb 2+ Sn 2+ , Cu 2+ 、Ni 2+ 、Cd 2+ Cr 2+ , Mn 2+ 、Co 2+ , Fe 2+ ,Ge 2+ , Yb 2+ 、Eu 2+ One or more of, X is a halogen anion, including Cl - Br - ,I - One or more of; and / or

[0017] The photoelectric device further comprises a hole transport layer, which is located on a side of the light-emitting layer away from the electron transport layer, and the material of the hole transport layer comprises 4,4'-N,N'-dicarbazolyl-biphenyl, poly[bis(4-phenyl)(2,4,6-trimethylphenyl)amine], N,N'-diphenyl-N,N'-bis(1-naphthyl)-1,1'-biphenyl-4,4"-diamine, N,N'-diphenyl-N,N'-bis(3-methylphenyl)-(1,1'-biphenyl)-4,4'-diamine, poly(N,N'-bis(4-butyl)amine] phenyl)-N,N'-bis(phenyl)benzidine), N,N'-bis(3-methylphenyl)-N,N'-bis(phenyl)-spiro, N,N'-bis(4-(N,N'-diphenyl-amino)phenyl)-N,N'-diphenylbenzidine, 4,4',4'-tri(N-carbazolyl)-triphenylamine, 4,4',4'-tri(N-3-methylphenyl-N-phenylamino)triphenylamine, poly[(9,9'-dioctylfluorene-2,7-diyl)-co-(4,4'-(N-(4-sec-butylphenyl)diphenylamine))], poly(N-ethylene carbazole) and its derivatives, N,N'-di(1-naphthyl)-N,N'-diphenyl-1,1'-biphenyl-4-4'-diamine, spiro NPB, poly(phenylene vinylene), poly[2-methoxy-5-(2-ethylhexyloxy)-1,4-phenylene vinylene], poly[2-methoxy-5-(3',7'-dimethyloctyloxy)-1,4-phenylene vinylene], 2,2',7,7'-tetrakis[N,N-di(4-methoxyphenyl)amino]-9,9'-spirobifluorene, 4,4'-cyclohexylbis[N,N-di(4 -methylphenyl)aniline], 1,3-di(carbazole-9-yl)benzene, polyaniline, polypyrrole, poly(p-phenylene vinylene), aromatic tertiary amines, polynuclear aromatic tertiary amines, 4,4'-bis(p-carbazolyl)-1,1'-biphenyl compounds, N,N,N',N'-tetraarylbenzidine, PEDOT:PSS and its derivatives, polymethacrylate and its derivatives, poly(9,9-octylfluorene) and its derivatives, poly(spirofluorene) and its derivatives, doped graphene, undoped graphene, C60, doped or undoped NiO, doped or undoped MoO 3 , doped or undoped WO 3 , doped or undoped V 2 O 5 , doped or undoped P-type GaN, doped or undoped CrO 3 , one or more of doped or undoped CuO; and / or

[0018] The photoelectric device further comprises a hole injection layer, which is located on a side of the light-emitting layer away from the electron transport layer, and the material of the hole injection layer comprises 2,3,6,7,10,11-hexacyano-1,4,5,8,9,12-hexaazatriphenylene, PEDOT, PEDOT:PSS, PEDOT:PSS doped with s-MoO 3 One or more of derivatives of, 4,4',4'-tris(N-3-methylphenyl-N-phenylamino)triphenylamine, tetracyanoquinodimethane, copper phthalocyanine, nickel oxide, molybdenum oxide, tungsten oxide, vanadium oxide, molybdenum sulfide, tungsten sulfide and copper oxide.

[0019] Accordingly, the present invention also provides a method for preparing a photoelectric device, comprising the following steps:

[0020] Providing a photovoltaic device preform, wherein the photovoltaic device preform comprises a first electrode;

[0021] Providing a carbon nanocage-inorganic semiconductor particle composite material, and disposing the carbon nanocage-inorganic semiconductor particle composite material on the optoelectronic device preform to obtain an electron transport layer;

[0022] A second electrode is formed on the electron transport layer to obtain a photoelectric device.

[0023] Optionally, in some embodiments of the present application, the method of setting the carbon nanocage-inorganic semiconductor particle composite material on the optoelectronic device preform is: dissolving the carbon nanocage-inorganic semiconductor particle composite material in a first solvent to obtain a dispersion, and spin coating the dispersion on the optoelectronic device preform.

[0024] Optionally, in some embodiments of the present application, the first solvent includes one or more of isopropanol, ethanol, dimethyl sulfoxide, N-methylpyrrolidone and chlorobenzene; and / or

[0025] In the dispersion, the concentration of the carbon nanocage-inorganic semiconductor particle composite material is 10 to 50 mg / mL; and / or

[0026] After spin coating the dispersion on the optoelectronic device preform and before obtaining the electron transport layer, the method further includes: annealing the optoelectronic device preform provided with the dispersion, wherein the annealing temperature is 75-85° C. and the annealing time is 5-10 minutes.

[0027] Optionally, in some embodiments of the present application, the method for preparing the carbon nanocage-inorganic semiconductor particle composite material comprises the following steps:

[0028] Providing an inorganic semiconductor particle dispersion, adding carbon nanocages and a polar solvent to the inorganic semiconductor particle dispersion, and ultrasonically mixing to obtain an intermediate product;

[0029] The intermediate product is calcined to obtain a carbon nanocage-inorganic semiconductor particle composite material.

[0030] Optionally, in some embodiments of the present application, the mass ratio of the carbon nanocage to the inorganic semiconductor particles in the inorganic semiconductor particle dispersion is 1:(2-5); and / or

[0031] The concentration of the inorganic semiconductor particles in the inorganic semiconductor particle dispersion is 30 to 40 mg / ml; and / or

[0032] The mass ratio of the polar solvent to the inorganic semiconductor particles is (0.5-1.5):1; and / or

[0033] The power of the ultrasonic mixing is 200-400W, and the time is 1-3h; and / or

[0034] The calcination temperature is 150-160° C. and the calcination time is 15-25 hours.

[0035] Optionally, in some embodiments of the present application, the carbon nanocage comprises a graphene carbon nanocage; and / or

[0036] The inorganic semiconductor particles include one or more of undoped metal oxides, doped metal oxides, ceramic semiconductor materials, IIB-VIA semiconductor materials, IIIA-VA semiconductor materials, and IB-IIIA-VIA semiconductor materials. The undoped metal oxides include ZnO, TiO 2 SnO 2 、ZrO 2 、 2 O 5 One or more of the following; the metal oxide in the doped metal oxide includes ZnO, TiO 2 SnO 2 、ZrO 2 、 2 O 5 、Al 2 O 3The doping element in the doped metal oxide includes one or more of Al, Mg, Li, Mn, Y, La, Cu, Ni, Zr, Ce, In, and Ga; the ceramic semiconductor material includes barium titanate; the IIB-VIA semiconductor material includes one or more of ZnS, ZnSe, and CdS; the IIIA-VA semiconductor material includes one or more of InP and GaP; the IB-IIIA-VIA semiconductor material includes one or more of CuInS and CuGaS; and / or

[0037] The solvent in the inorganic semiconductor particle dispersion includes one or more of ethanol, butanol, and isopropanol; and / or

[0038] The surfaces of the inorganic semiconductor particles in the inorganic semiconductor particle dispersion are connected with ligands, and the ligands include one or more of hydroxyl groups and carboxyl groups; and / or

[0039] The polar solvent includes one or more of ethanol, butanol, isopropanol, and deionized water.

[0040] Optionally, in some embodiments of the present application, after adding the carbon nanocages and the polar solvent to the inorganic semiconductor particle dispersion and before the ultrasonic mixing, the process further includes: heating the temperature to 60-100° C. at a heating rate of 2-10° C. / min.

[0041] Optionally, in some embodiments of the present application, the first electrode is an anode, the second electrode is a cathode, and the optoelectronic device preform further includes a light-emitting layer disposed on the first electrode; or

[0042] The first electrode is an anode, the second electrode is a cathode, the optical device preform further comprises a hole functional layer and a light emitting layer stacked on the first electrode, the hole functional layer comprises a hole transport layer and / or a hole injection layer; or

[0043] The first electrode is a cathode, the second electrode is an anode, and forming the second electrode on the electron transport layer comprises: forming a stacked light-emitting layer and a second electrode on the electron transport layer; or

[0044] The first electrode is a cathode, the second electrode is an anode, and forming the second electrode on the electron transport layer includes: forming a stacked light-emitting layer, a hole functional layer and a second electrode on the electron transport layer, and the hole functional layer includes a hole transport layer and / or a hole injection layer.

[0045] Correspondingly, an embodiment of the present application also provides a display device, comprising the above-mentioned optoelectronic device.

[0046] The material of the electron transport layer of the optoelectronic device of the present application includes the carbon nanocage-inorganic semiconductor particle composite material, and the inorganic semiconductor particles are filled in the carbon nanocage. In this way, on the one hand, the carbon nanocage can isolate the inorganic semiconductor particles to prevent a large number of inorganic semiconductor particles from gathering together and causing agglomeration, thereby improving the stability of the electron transport layer and the electron transport performance, and further improving the life of the optoelectronic device; on the other hand, the inorganic semiconductor particles are filled in the carbon nanocage, and the carbon nanocage can isolate and protect the inorganic semiconductor particles, preventing water and oxygen from corroding the inorganic semiconductor particles, thereby improving the stability of the inorganic semiconductor particles, and further improving the stability of the electron transport layer, and improving the life of the optoelectronic device. BRIEF DESCRIPTION OF THE DRAWINGS

[0047] In order to more clearly illustrate the technical solutions in the embodiments of the present application, the drawings required for use in the description of the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present application. For those skilled in the art, other drawings can be obtained based on these drawings without paying any creative work.

[0048] Figure 1 is a schematic structural diagram of a photoelectric device provided in an embodiment of the present application;

[0049] Figure 2 This is a schematic structural diagram of a carbon nanocage-inorganic semiconductor particle composite material provided in an embodiment of the present application;

[0050] Figure 3 is a schematic structural diagram of another optoelectronic device provided in an embodiment of the present application;

[0051] Figure 4 is a schematic structural diagram of another optoelectronic device provided in an embodiment of the present application;

[0052] Figure 5 is a schematic structural diagram of another optoelectronic device provided in an embodiment of the present application;

[0053] Figure 6 is a schematic structural diagram of another optoelectronic device provided in an embodiment of the present application;

[0054] Figure 7 is a schematic structural diagram of another optoelectronic device provided in an embodiment of the present application;

[0055] Figure 8 is a schematic structural diagram of another optoelectronic device provided in an embodiment of the present application;

[0056] Fig. 9 is a flow chart of a method for preparing a photoelectric device provided in an embodiment of the present application;

[0057] Fig.10 is a current density-voltage curve diagram of Example 1 and Comparative Example 1 of the present application;

[0058] Fig.11 It is a luminous intensity-current density curve diagram of Example 1 and Comparative Example 1 of the present application.

[0059] Reference numerals:

[0060] Optoelectronic device 100; first electrode 10; electron transport layer 20; composite material 21; carbon nanocage 211; inorganic semiconductor particles 212; second electrode 30; light-emitting layer 40; hole transport layer 50; hole injection layer 60. DETAILED DESCRIPTION

[0061] The technical solutions in the embodiments of the present application will be clearly and completely described below in conjunction with the drawings in the embodiments of the present application. Obviously, the described embodiments are only part of the embodiments of the present application, rather than all of the embodiments. Based on the embodiments in the present application, all other embodiments obtained by those skilled in the art without making creative work belong to the scope of protection of the present application. In addition, it should be understood that the specific implementation methods described herein are only used to illustrate and explain the present application, and are not used to limit the present application.

[0062] In this application, unless otherwise stated, directional words such as "upper" and "lower" generally refer to the upper and lower parts of the device in actual use or working state, specifically the drawing direction in the accompanying drawings; while "inner" and "outer" refer to the outline of the device. In addition, in the description of this application, the term "including" means "including but not limited to". The terms first, second, third, etc. are used only as labels and do not impose numerical requirements or establish an order.

[0063] In this application, "and / or" describes the association relationship of associated objects, indicating that there may be three relationships. For example, A and / or B can mean: A exists alone, A and B exist at the same time, and B exists alone. A and B can be singular or plural.

[0064] In the present application, "at least one" means one or more, and "plurality" means two or more. "At least one", "at least one of the following" or similar expressions refer to any combination of these items, including any combination of single items or plural items. For example, "at least one of a, b, or c", or "at least one of a, b, and c" can all mean: a, b, c, ab (i.e., a and b), ac, bc, or abc, where a, b, c can be single or multiple, respectively.

[0065] In the present application, when a layer is formed "on" another layer, the so-called "on" is a broad concept, which may indicate that the formed another layer is adjacent to the certain layer, or may indicate that there are other spacing structural layers between the another layer and the certain layer. For example, when a second electrode is formed "on" the first carrier functional layer, the so-called "on" may indicate that the formed second electrode is adjacent to the first carrier functional layer, or may indicate that there are other spacing structural layers between the second electrode and the first carrier functional layer, such as a light-emitting layer.

[0066] Various embodiments of the present application may be presented in the form of a range; it should be understood that the description in the form of a range is only for convenience and brevity, and should not be understood as a rigid limitation on the scope of the present application; therefore, the range description should be considered to have specifically disclosed all possible sub-ranges and single numerical values ​​within the range. For example, the range description from 1 to 6 should be considered to have specifically disclosed sub-ranges, such as from 1 to 3, from 1 to 4, from 1 to 5, from 2 to 4, from 2 to 6, from 3 to 6, etc., as well as single numbers within the range, such as 1, 2, 3, 4, 5 and 6, which apply regardless of the range. In addition, whenever a numerical range is indicated herein, it is meant to include any cited number (fractional or integer) within the indicated range.

[0067] Inorganic semiconductor particles are considered to be one of the most popular materials for preparing electron transport layers of high-efficiency optoelectronic devices due to their high electron mobility and hole blocking properties. However, the surface of inorganic semiconductor particles currently prepared by low-temperature solution method or sol-gel method will inevitably be connected with ligands. Although these ligands can prevent inorganic semiconductor particles from agglomerating to a certain extent, these ligands are easily oxidized and easily fall off from the surface of inorganic semiconductor particles, resulting in poor stability of inorganic semiconductor particles, which in turn leads to a short life of optoelectronic devices; in addition, the ligands on the surface of inorganic semiconductor particles will also reduce the conductivity of inorganic semiconductor particles, which in turn leads to low luminescence efficiency of optoelectronic devices.

[0068] The technical solution of this application is as follows:

[0069] First, see Figures 1-2 The embodiment of the present application provides a photoelectric device 100, comprising a first electrode 10, an electron transport layer 20 and a second electrode 30 stacked in sequence. The material of the electron transport layer 20 comprises a carbon nanocage-inorganic semiconductor particle composite material 21, and the carbon nanocage-inorganic semiconductor particle composite material 21 comprises a carbon nanocage 211 and at least one inorganic semiconductor particle 212 filled in the carbon nanocage.

[0070] The material of the electron transport layer 20 includes the carbon nanocage-inorganic semiconductor particle composite material, and the inorganic semiconductor particles are filled in the carbon nanocage. In this way, on the one hand, the carbon nanocage can isolate the inorganic semiconductor particles to prevent a large number of inorganic semiconductor particles from gathering together and causing agglomeration, thereby improving the stability and electron transport performance of the electron transport layer 20, and further improving the life and luminous efficiency of the optoelectronic device 100; on the other hand, the inorganic semiconductor particles are filled in the carbon nanocage, and the carbon nanocage can isolate and protect the inorganic semiconductor particles to prevent water and oxygen from corroding the inorganic semiconductor particles, thereby improving the stability of the inorganic semiconductor particles, and further improving the stability of the electron transport layer 20 and the life of the optoelectronic device 100; on the other hand, the carbon nanocage has better conductivity, which can effectively improve the conductivity of the electron transport layer 20, and further improve the luminous efficiency of the optoelectronic device 100.

[0071] In the carbon nanocage-inorganic semiconductor particle composite material, the mass ratio of the carbon nanocage to the inorganic semiconductor particles is 1:(2-4), for example, 1:2, 1:2.5, 1:3, 1:3.5, 1:4, etc. Within the ratio range, the inorganic semiconductor particles can be fully filled into the carbon nanocage, which is conducive to obtaining a carbon nanocage-inorganic semiconductor particle composite material with good stability and conductivity.

[0072] The carbon nanocages may include but are not limited to graphene carbon nanocages (GCNs).

[0073] In some embodiments, the average particle size of the carbon nano cage is 30 to 50 nm, and the average particle size of the inorganic semiconductor particles is 7 to 12 nm. Within the average particle size range, 1 to 3 inorganic semiconductor particles can be filled in each carbon nano cage, which can effectively reduce the aggregation of a large number of inorganic semiconductor particles, so that the carbon nano cage-inorganic semiconductor particle composite material has better stability.

[0074] The carbon nanocage has a plurality of nanopores. In some embodiments, the pore size of the nanopores is 4 to 16 nm, for example, 4 to 9 nm, 6 to 10 nm, 8 to 12 nm, 11 to 15 nm, 7 to 16 nm, etc. Within the pore size range, it is beneficial for the inorganic semiconductor particles to enter the carbon nanocage through the nanopores.

[0075] In some embodiments, each carbon nanocage is filled with 1 to 3 inorganic semiconductor particles, so that a large number of inorganic semiconductor particles can be effectively reduced from agglomerating together, so that the carbon nanocage-inorganic semiconductor particle composite material has good stability and conductivity.

[0076] The inorganic semiconductor particles include but are not limited to one or more of undoped metal oxides, doped metal oxides, ceramic semiconductor materials, IIB-VIA semiconductor materials, IIIA-VA semiconductor materials, and IB-IIIA-VIA semiconductor materials. The undoped metal oxides include but are not limited to ZnO, TiO 2 SnO 2 、ZrO 2 、 2 O 5 The metal oxides in the doped metal oxides include but are not limited to ZnO, TiO 2 SnO 2 、ZrO 2 、 2 O 5 、Al 2 O 3 One or more of the doped metal oxides, the doping elements in the doped metal oxides include but are not limited to one or more of Al, Mg, Li, Mn, Y, La, Cu, Ni, Zr, Ce, In, and Ga. As an example, the material of the doped inorganic semiconductor particles can be aluminum zinc oxide (AZO), lithium-doped zinc oxide (LZO), and magnesium-doped zinc oxide (MZO). The ceramic semiconductor material includes but is not limited to barium titanate. The IIB-VIA semiconductor materials include but are not limited to one or more of ZnS, ZnSe, and CdS. The IIIA-VA semiconductor materials include but are not limited to one or more of InP and GaP. The IB-IIIA-VIA semiconductor materials include but are not limited to one or more of CuInS and CuGaS.

[0077] See also Figures 3-4 In some embodiments, the optoelectronic device 100 further includes a light-emitting layer 40 , and the light-emitting layer 40 is located between the first electrode 10 and the electron transport layer 20 or between the second electrode 30 and the electron transport layer 20 .

[0078] See also Figure 3 In some embodiments, the first electrode 10 is an anode, the second electrode 30 is a cathode, and the light-emitting layer 40 is located between the first electrode 10 and the electron transport layer 20 .

[0079] See also Figure 4 In some embodiments, the first electrode 10 is a cathode, the second electrode 30 is an anode, and the light-emitting layer 40 is located between the electron transport layer 20 and the second electrode 30 .

[0080] See also Figures 5-6In some embodiments, the optoelectronic device 100 further includes a hole transport layer 50 , and the hole transport layer 50 is located on a side of the light emitting layer 40 away from the electron transport layer 20 .

[0081] See also Figure 5 In some embodiments, the first electrode 10 is an anode, the second electrode 30 is a cathode, and the hole transport layer 50 is located between the first electrode 10 and the light-emitting layer 40 .

[0082] See also Figure 6 In some embodiments, the first electrode 10 is a cathode, the second electrode 30 is an anode, and the hole transport layer 50 is located between the light-emitting layer 40 and the second electrode 30. Figures 7-8 In some embodiments, the optoelectronic device 100 further includes a hole injection layer 60 , and the hole injection layer 60 is located on a side of the hole transport layer 50 away from the light-emitting layer 40 .

[0083] See also Figure 7 In some embodiments, the first electrode 10 is an anode, the second electrode 30 is a cathode, and the hole injection layer 60 is located between the first electrode 10 and the hole transport layer 50 .

[0084] See also Figure 8 In some embodiments, the first electrode 10 is a cathode, the second electrode 30 is an anode, and the hole injection layer 60 is located between the hole transport layer 50 and the second electrode 30 .

[0085] The first electrode 10 and the second electrode 30 are electrodes for optoelectronic devices known in the art, for example, they can independently include but are not limited to doped metal oxide electrodes, composite electrodes, graphene electrodes, carbon nanotube electrodes, metal single substance electrodes or alloy electrodes. The material of the doped metal oxide electrode can include but is not limited to one or more of indium doped tin oxide (ITO), fluorine doped tin oxide (FTO), antimony doped tin oxide (ATO), aluminum doped zinc oxide (AZO), gallium doped zinc oxide (GZO), indium doped zinc oxide (IZO), magnesium doped zinc oxide (MZO), aluminum doped magnesium oxide (AMO), and cadmium doped zinc oxide. The composite electrode is an electrode formed by stacking two or more layers of conductive materials, such as AZO / Ag / AZO, AZO / Al / AZO, ITO / Ag / ITO, ITO / Al / ITO, ZnO / Ag / ZnO, ZnO / Al / ZnO, TiO 2 / Ag / TiO 2 、TiO 2 / Al / TiO 2, ZnS / Ag / ZnS, ZnS / Al / ZnS, Ca / Al, LiF / Ca, LiF / Al, BaF 2 / Al、CsF / Al、CaCO 3 / Al、BaF 2 / Ca / Al, etc., where " / " represents a stacked structure, for example, AZO / Ag / AZO represents a composite electrode including an AZO layer, an Ag layer and an AZO layer stacked in sequence. The material of the metal single substance electrode may include but is not limited to one or more of Ag, Ni, Pt, Au, Ir, Cu, Mo, Al, Ca, Mg and Ba. The alloy electrode includes but is not limited to Au:Mg alloy electrode and Ag:Mg alloy electrode.

[0086] In some embodiments, the anode is an electrode with a relatively high work function, for example, it may include but is not limited to a doped metal oxide electrode with a relatively high work function, a metal single substance electrode with a relatively high work function, and a carbon nanotube electrode. The metal single substance electrode with a relatively high work function may be selected from but is not limited to Ni, Pt, Au, Ag, Ir, etc.

[0087] In some embodiments, the cathode is an electrode with a relatively low work function, such as but not limited to a metal single substance electrode with a relatively low work function, a composite electrode with a relatively low work function, and an alloy electrode with a relatively low work function. The metal single substance electrode with a relatively low work function may be Ca, Ba, Al, Mg, etc. The composite electrode with a relatively low work function may be Ca / Al, LiF / Ca, LiF / Al, BaF 2 / Al、CsF / Al、CaCO 3 / Al、BaF 2 / Ca / Al, etc. The alloy electrodes with relatively low work functions are Au:Mg and Ag:Mg, etc.

[0088] The material of the light-emitting layer 40 may include, but is not limited to, one or more of an organic light-emitting material and a quantum dot light-emitting material.

[0089] The organic light-emitting material may include but is not limited to CBP:Ir(mppy) 3(4,4'-bis(N-carbazole)-1,1'-biphenyl:tris[2-(p-tolyl)pyridine iridium(III)), TCTX:Ir(mmpy)(4,4',4"-tris(carbazole-9-yl)triphenylamine:tris[2-(p-tolyl)pyridine iridium), diaromatic anthracene derivatives, distilbene aromatic derivatives, pyrene derivatives, fluorene derivatives, TBPe fluorescent materials, TTPX fluorescent materials, TBRb fluorescent materials, DBP fluorescent materials, delayed fluorescent materials, TTA materials, TADF (thermally activated delay) materials, polymers containing BN covalent bonds, HLCT (hybridized localized charge transfer excited state) materials, Exciplex (exciplex) luminescent materials, polyacetylene and its derivatives, polyparaphenylene and its derivatives, polythiophene and its derivatives, polyfluorene and its derivatives. One or more thereof.

[0090] The quantum dot light-emitting material may include, but is not limited to, one or more of single structure quantum dots, core-shell structure quantum dots and perovskite semiconductor materials.

[0091] The material of the single structure quantum dots, the core material of the core-shell structure quantum dots and the shell material of the core-shell structure quantum dots may respectively include but are not limited to one or more of II-VI group compounds, IV-VI group compounds, III-V group compounds and I-III-VI group compounds. The II-VI group compounds may include, but are not limited to, one or more of CdS, CdSe, CdTe, ZnS, ZnSe, ZnTe, ZnO, HgS, HgSe, HgTe, CdSeS, CdSeTe, CdSTe, ZnSeS, ZnSeTe, ZnSTe, HgSeS, HgSeTe, HgSTe, CdZnS, CdZnSe, CdZnTe, CdHgS, CdHgSe, CdHgTe, HgZnS, HgZnSe, HgZnTe, CdZnSeS, CdZnSeTe, CdZnSTe, CdHgSeS, CdHgSeTe, CdHgSTe, HgZnSeS, HgZnSeTe and HgZnSTe. The IV-VI group compounds may include, but are not limited to, one or more of SnS, SnSe, SnTe, PbS, PbSe, PbTe, SnSeS, SnSeTe, SnSTe, PbSeS, PbSeTe, PbSTe, SnPbS, SnPbSe, SnPbTe, SnPbSSe, SnPbSeTe, and SnPbSTe. The III-V group compound may include but is not limited to one or more of GaN, GaP, GaAs, GaSb, AlN, AlP, AlAs, AlSb, InN, InP, InAs, InSb, GaNP, GaNAs, GaNSb, GaPAs, GaPSb, AlNP, AlNAs, AlNSb, AlPAs, AlPSb, InNP, InNAs, InNSb, InPAs, InPSb, GaAlNP, GaAlNAs, GaAlNSb, GaAlPAs, GaAlPSb, GaInNP, GaInNAs, GaInNSb, GaInPAs, GaInPSb, InAlNP, InAlNAs, InAlNSb, InAlPAs and InAlPSb. The I-III-VI group compound may include but is not limited to CuInS 2 、CuInSe 2 AgInS 2 One or more of .

[0092] As an example, the core-shell structured quantum dots may include, but are not limited to, one or more of CdSe / CdSeS / CdS, InP / ZnSeS / ZnS, CdZnSe / ZnSe / ZnS, CdSeS / ZnSeS / ZnS, CdSe / ZnS, CdSe / ZnSe / ZnS, ZnSe / ZnS, ZnSeTe / ZnS, CdSe / CdZnSeS / ZnS and InP / ZnSe / ZnS.

[0093] The perovskite semiconductor material may include but is not limited to doped or undoped inorganic perovskite semiconductors, or organic-inorganic hybrid perovskite semiconductors. The inorganic perovskite semiconductor has the general structural formula AMX 3 , where A is Cs + ions, M is a divalent metal cation, including Pb 2+ Sn 2+ , Cu 2+ 、Ni 2+ 、Cd 2+ Cr 2+ , Mn 2+ 、Co 2+ , Fe 2+ ,Ge 2+ , Yb 2+ 、Eu 2+ One or more of, X is a halogen anion, including Cl - Br - ,I - The general structural formula of the organic-inorganic hybrid perovskite semiconductor is BMX 3 , where B is an organic amine cation, including CH 3 (CH 2 ) n-2 NH 3 + or [NH 3 (CH 2 ) n NH 3 ] 2+ , where n≥2, M is a divalent metal cation, including Pb 2+ Sn 2+ , Cu 2+ 、Ni 2+ 、Cd 2+ Cr 2+ , Mn 2+ 、Co 2+ , Fe 2+ ,Ge 2+ , Yb 2+ 、Eu 2+One or more of, X is a halogen anion, including Cl - Br - ,I - One or more of .

[0094] The material of the hole transport layer 50 may also be a material known in the art for a hole transport layer, for example, may be selected from but not limited to 4,4'-N,N'-dicarbazolyl-biphenyl (CBP), poly[bis(4-phenyl)(2,4,6-trimethylphenyl)amine] (PTAA), N,N'-diphenyl-N,N'-bis(1-naphthyl)-1,1'-biphenyl-4,4"-diamine (α-NPD), N,N'-diphenyl-N,N'-bis(3-methylphenyl)-(1,1'-biphenyl)-4,4'-diamine (TPD), poly(N,N'-bis(4-butylphenyl)-N,N'-bis(phenyl)benzidine) (Poly-TPD), N,N'-bis(3-methylphenyl)-N,N'-bis(phenyl)-spiro(spiro-TPD), N,N'-bis(4-(N,N'-diphenyl-amino)phenyl)-N,N'-diphenylbenzidine (DNTPD), 4,4',4'-tri(N-carbazolyl)-triphenylamine (TCTA), 4,4',4'-tri(N-3-methylphenyl-N-phenylamino)triphenylamine (m-MTDATA), poly[(9,9'-dioctylfluorene-2,7-diyl)-co-(4,4'-(N-(4-sec-butylphenyl)diphenylamine))] (TFB), poly(N-vinylcarbazolyl) azole) (PVK) and its derivatives, N,N'-di(1-naphthyl)-N,N'-diphenyl-1,1'-biphenyl-4-4'-diamine (NPB), spiro NPB, poly(phenylene vinylene) (PPV), poly[2-methoxy-5-(2-ethylhexyloxy)-1,4-phenylene vinylene] (MEH-PPV), poly[2-methoxy-5-(3',7'-dimethyloctyloxy)-1,4-phenylene vinylene] (MOMO-PPV), 2,2',7,7'-tetrakis[N,N-di(4-methoxyphenyl)amino]-9,9'-spirobifluorene (spiro-omeTAD), 4,4'-cyclohexylbis[N,N-bis(4-methylphenyl)aniline](TAPC), 1,3-bis(carbazole-9-yl)benzene(MCP), polyaniline, polypyrrole, poly(p-phenylene vinylene), aromatic tertiary amine, polynuclear aromatic tertiary amine, 4,4'-bis(p-carbazolyl)-1,1'-biphenyl compound, N,N,N',N'-tetraarylbenzidine, PEDOT:PSS and its derivatives, polymethacrylate and its derivatives, poly(9,9-octylfluorene) and its derivatives, poly(spirofluorene) and its derivatives, doped graphene, undoped graphene, C60, doped or undoped NiO, doped or undoped MoO 3 , doped or undoped WO3 , doped or undoped V 2 O 5 , doped or undoped P-type GaN, doped or undoped CrO 3 , doped or undoped CuO or more.

[0095] The material of the hole injection layer 60 may also be a material known in the art for a hole injection layer, for example, may be selected from but not limited to 2,3,6,7,10,11-hexacyano-1,4,5,8,9,12-hexaazatriphenylene (HAT-CN), PEDOT, PEDOT:PSS, PEDOT:PSS doped with s-MoO 3 Derivatives (PEDOT:PSS:s-MoO 3 ), one or more of 4,4',4'-tris(N-3-methylphenyl-N-phenylamino)triphenylamine (m-MTDATA), tetracyanoquinodimethane (F4-TCQN), copper phthalocyanine, nickel oxide, molybdenum oxide, tungsten oxide, vanadium oxide, molybdenum sulfide, tungsten sulfide and copper oxide.

[0096] It is understandable that the optoelectronic device 100 may also be provided with some functional layers conventionally used in optoelectronic devices to help improve the performance of the optoelectronic device, such as an electron blocking layer, a hole blocking layer, an electron injection layer, an interface modification layer, etc.

[0097] It can be understood that the materials of each layer of the optoelectronic device 100 can be adjusted according to the light emitting requirements of the optoelectronic device 100 .

[0098] In some embodiments, the optoelectronic device 100 further includes a substrate, and the substrate is disposed on a side of the first electrode 10 away from the light-emitting layer 40 , or the substrate is disposed on a side of the second electrode 30 away from the light-emitting layer 40 .

[0099] The substrate may be a rigid substrate or a flexible substrate. In some embodiments, the material of the substrate may include but is not limited to one or more of glass, silicon wafer, polycarbonate, polymethyl methacrylate, polyethylene terephthalate, polyethylene naphthalate, polyamide and polyether sulfone.

[0100] It is understood that the optoelectronic device 100 may be an upright optoelectronic device or an inverted optoelectronic device. The optoelectronic device 100 may be a quantum dot optoelectronic device or an organic optoelectronic device.

[0101] Second, see Fig. 9 The present application also provides a method for preparing a photoelectric device, comprising the following steps:

[0102] Step S11, providing a photoelectric device preform, wherein the photoelectric device preform includes a first electrode 10;

[0103] Step S12, providing a carbon nanocage-inorganic semiconductor particle composite material, disposing the carbon nanocage-inorganic semiconductor particle composite material on the optoelectronic device preform, and annealing to obtain an electron transport layer 20;

[0104] Step S13 , forming a second electrode 30 on the electron transport layer 20 to obtain a photoelectric device 100 .

[0105] When the first electrode 10 is an anode and the second electrode 30 is a cathode:

[0106] See also Figure 3 In some embodiments, the optoelectronic device preform further includes a light-emitting layer 40 disposed on the first electrode 10 , and the composite material is disposed on the light-emitting layer 40 .

[0107] See also Figure 5 and Figure 7 In some other embodiments, the optical device preform also includes a hole functional layer and a light-emitting layer 40 stacked in sequence on the first electrode 10, the hole functional layer includes a hole transport layer 50 and / or a hole injection layer 60, and the composite material is arranged on the light-emitting layer 40.

[0108] When the first electrode 10 is a cathode and the second electrode 30 is an anode:

[0109] See also Figure 4 In some embodiments, the step S13 includes: sequentially forming a stacked light-emitting layer 40 and a second electrode 30 on the electron transport layer 20 to obtain a photoelectric device 100 .

[0110] See also Figure 6 and Figure 8 In some other embodiments, the step S13 includes: sequentially forming a stacked light-emitting layer 40, a hole functional layer and a second electrode 30 on the electron transport layer 20 to obtain a photoelectric device 100, wherein the hole functional layer includes a hole transport layer 50 and / or a hole injection layer 60.

[0111] The method of forming the first electrode 10, the second electrode 30, the light-emitting layer 40, the hole transport layer 50, and the hole injection layer 60, as well as the method of setting the carbon nano cage-inorganic semiconductor particle composite material on the optoelectronic device preform can be implemented by conventional techniques in the art, such as chemical methods or physical methods. Among them, the chemical method includes chemical vapor deposition, continuous ion layer adsorption and reaction, anodization, electrolytic deposition, and coprecipitation. The physical method includes physical coating and solution method, wherein the physical coating method includes: thermal evaporation coating, electron beam evaporation coating, magnetron sputtering, multi-arc ion coating, physical vapor deposition, atomic layer deposition, pulsed laser deposition, etc.; the solution method can be spin coating, printing, inkjet printing, blade coating, printing, dip pulling, immersion, spraying, rolling, casting, slit coating, and strip coating.

[0112] In at least some embodiments, the method of placing the carbon nanocage-inorganic semiconductor particle composite material on the optoelectronic device preform is: dissolving the carbon nanocage-inorganic semiconductor particle composite material in a first solvent to obtain a dispersion, and spin coating the dispersion on the optoelectronic device preform.

[0113] The first solvent includes, but is not limited to, one or more of isopropanol, ethanol, DMSO (dimethyl sulfoxide), NMP (N-methylpyrrolidone) and chlorobenzene.

[0114] In some embodiments, in the dispersion, the concentration of the composite material is 10 to 50 mg / mL, for example, 10 to 30 mg / mL, 15 to 35 mg / mL, 20 to 40 mg / mL, 25 to 45 mg / mL, 30 to 50 mg / mL, etc. Within the concentration range, the composite material can be uniformly dispersed in the solvent, which is conducive to preparing an electron transport layer 20 with a good film-forming effect.

[0115] In some embodiments, the annealing temperature is 75-85° C., such as 75-80° C., 80-85° C., etc., and the annealing time is 5-10 min., such as 5-8 min., 6-9 min., 7-10 min., etc. Within the temperature and time range, it is beneficial to prepare an electron transport layer 20 with a good film-forming effect.

[0116] The preparation method of the carbon nano cage-inorganic semiconductor particle composite material comprises the following steps:

[0117] Step S21, providing an inorganic semiconductor particle dispersion, wherein the inorganic semiconductor particles in the inorganic semiconductor particle dispersion have ligands connected to their surfaces, adding a carbon nanocage and a polar solvent to the inorganic semiconductor particle dispersion, and ultrasonically mixing the inorganic semiconductor particles so that the inorganic semiconductor particles enter the interior of the carbon nanocage through the nanopores of the carbon nanocage to obtain an intermediate product, wherein the intermediate product includes a carbon nanocage and at least one inorganic semiconductor particle in the carbon nanocage having a ligand connected to its surface;

[0118] Step S22, calcining the intermediate product to remove the ligands connected to the surface of the inorganic semiconductor particles to obtain a carbon nanocage-inorganic semiconductor particle composite material.

[0119] In step S21:

[0120] The mass ratio of the carbon nanocage to the inorganic semiconductor particles in the inorganic semiconductor particle dispersion is 1:(2-5), such as 1:(2-3), 1:(2.5-3.5), 1:(3-4), 1:(4.5-5), etc. Within the ratio range, the inorganic semiconductor particles can be fully filled in the carbon nanocage, which is conducive to preparing a carbon nanocage-inorganic semiconductor particle composite material with good stability and conductivity.

[0121] In some embodiments, the concentration of the inorganic semiconductor particles in the inorganic semiconductor particle dispersion is 30-40 mg / ml, for example, 30-35 mg / ml, 32-36 mg / ml, 34-38 mg / ml, 33-40 mg / ml, etc. Within the concentration range, it is beneficial for the inorganic semiconductor particles to fully dissolve and for preparing a carbon nanocage-inorganic semiconductor particle composite material with good stability and conductivity.

[0122] The inorganic semiconductor particles in the inorganic semiconductor particle dispersion are as described above and will not be described in detail here.

[0123] The ligands on the surface of the inorganic semiconductor particles are ligands known to exist on the surface of inorganic semiconductor particles, for example, they may include but are not limited to one or more of hydroxyl groups and carboxyl groups.

[0124] The solvent in the inorganic semiconductor particle dispersion may include, but is not limited to, one or more of ethanol, butanol, and isopropanol.

[0125] It can be understood that the inorganic semiconductor particles can be prepared by known preparation methods. In at least some embodiments, the inorganic semiconductor particles are prepared by a solution method.

[0126] The polar solvent may include, but is not limited to, one or more of ethanol, butanol, isopropanol, and deionized water. The polar solvent is conducive to the dispersion of the inorganic semiconductor particles and the carbon nanocage, and during the ultrasonic process, it is conducive to the inorganic semiconductor particles entering the interior of the carbon nanocage through the nanopores of the carbon nanocage.

[0127] In some embodiments, the mass ratio of the polar solvent to the inorganic semiconductor particles is (0.5-1.5):1, for example, 0.5:1, 1:1, 1.2:1, 1.5:1, and the like.

[0128] In some embodiments, the power of the ultrasonic mixing is 200-400 W, for example, 200-300 W, 220-320 W, 240-340 W, 250-350 W, 280-380 W, 270-400 W, etc., and the time is 1-3 h, for example, 1 h, 1.5 h, 2 h, 2.5 h, 3 h, etc. Within the power and time range, it is beneficial for the inorganic semiconductor particles to enter the interior of the carbon nanocage through the nanopores of the carbon nanocage.

[0129] In some embodiments, before ultrasonic mixing, the method further comprises: heating the temperature to 60-100° C. at a heating rate of 2-10° C. / min. This is conducive to allowing the inorganic semiconductor particles to enter the interior of the carbon nanocage through the nanopores of the carbon nanocage.

[0130] In the center, each carbon nano cage is filled with 1 to 3 inorganic semiconductor particles with ligands connected to the surface.

[0131] In step S22: In some embodiments, the calcination temperature is 150-160°C. For example, 150°C, 152°C, 154°C, 156°C, 158°C, 160°C, etc., and the time is 15-25h, for example, 15h, 18h, 20h, 22h, 24h, 25h, etc. The calcination can effectively remove the ligands on the surface of the inorganic semiconductor particles. In addition, since the inorganic semiconductor particles are filled in the carbon nanocage, even if the surface ligands are removed by calcination, a large number of inorganic semiconductor particles will not agglomerate.

[0132] It is understood that the carbon nanocage can be prepared by a known preparation method. In at least some embodiments, the preparation method of the carbon nanocage is: providing graphene, pre-treating the graphene with a poly (dimethyldiallyl ammonium) chloride (PDDA) solution to obtain more oxygen-containing functional groups; 2 / FeCl 3 Growth of Fe on the PDDA surface by in situ hydrolysis of x O y Nanoparticles (FexOyNPs) to obtain G@FeO y; Then 80 mg of G@FexOy and 2 g of sucrose were added to 40 mL of water and ultrasonically treated for 1 h to form a uniform black suspension; then the solution was hydrothermally reacted at 180 ° C for 15 h to obtain a dark brown precursor solution, which was centrifugally washed and dried to obtain a dried precursor; the dried precursor was then calcined at 800 ° C in argon for 3 h, with a heating rate of 5 ° C / min and a gas flow rate of 50 mL / min; finally, the material was placed in a 60 ° C HCl solution and stirred for 48 h to remove Fe x O y NPs to obtain hollow carbon nanocages.

[0133] The graphene can be prepared by a known preparation method. In at least some embodiments, the preparation method of the graphene includes:

[0134] A. Add ice cubes to a 250 mL beaker to provide an ice water bath. Use a test tube to measure 23 mL of H 2 SO 4 , and then weigh 1g of graphite, 0.5g of sodium nitrate and 3g of potassium permanganate with an electronic balance; place the conical flask in an ice-water bath, then gently pour concentrated sulfuric acid into the conical flask, and then put it in an electromagnetic stirrer; mix the graphite and sodium nitrate and add them to the conical flask, stir and react for 3min, and then add potassium permanganate to the conical flask; control the temperature to less than 20°C, stir and react for 2h; heat to 35°C and continue stirring for 30min; prepare 46mL of deionized water (14°C) with water and distilled water, add deionized water to the conical flask, and then increase the temperature to 98°C, continue heating for 20min, the solution is brown-yellow and red smoke emerges; take 5g of hydrogen peroxide (30%) and add it to the conical flask; remove the conical flask and filter it while hot, and wash it with hydrochloric acid and deionized water. After the remaining solid is stable on the filter paper, take out the filter paper with tweezers, and then line the bottom with a clean filter paper, and put one piece in a drying oven at 60°C to fully dry to obtain dried graphene;

[0135] B. Remove 100 mg of the dried graphene oxide and disperse it in 100 g of water to obtain a brown-yellow suspension; put the suspension into an ultrasonic washing box and disperse it under ultrasonic conditions for 1 hour; take out the solution and put it into a four-necked beaker, heat it to 80°C, then add 20 ml of hydrazine hydrate dropwise, react for 24 hours, filter, rinse the obtained product with methanol and water, and fully dry the obtained solid in a 60°C drying oven to obtain graphene.

[0136] It can be understood that when the optoelectronic device 100 also includes functional layers conventionally used in optoelectronic devices that help improve the performance of the optoelectronic device, such as an electron blocking layer, a hole blocking layer, an electron injection layer, an interface modification layer, etc., the preparation method of the optoelectronic device 100 may also include the step of preparing the above-mentioned functional layers using conventional techniques in the field.

[0137] The optoelectronic device 100 prepared by the preparation method described in the present application has good luminous efficiency and long life.

[0138] In a third aspect, the present application further relates to a display device, wherein the display device comprises the optoelectronic device 100 .

[0139] The display device can be any electronic product with a display function, including but not limited to smart phones, tablet computers, laptops, digital cameras, digital video cameras, smart wearable devices, smart weighing electronic scales, car displays, televisions or e-book readers, among which smart wearable devices can be, for example, smart bracelets, smart watches, virtual reality (VR) helmets, etc.

[0140] The present application is described in detail below through specific embodiments. The following embodiments are only partial embodiments of the present application and are not limitations of the present application.

[0141] Example 1

[0142] Preparation of carbon nanocage-inorganic semiconductor particle composite materials:

[0143] Add ice cubes to a 250 mL beaker to provide an ice water bath; use a test tube to measure 23 ml of H 2 SO 4 , and then weigh 1g of graphite, 0.5g of sodium nitrate and 3g of potassium permanganate with an electronic balance; place the conical flask in an ice-water bath, then gently pour concentrated sulfuric acid into the conical flask, and then put it in an electromagnetic stirrer; mix the graphite and sodium nitrate and add them to the conical flask, stir and react for 3min, and then add potassium permanganate to the conical flask; control the temperature to less than 20°C, stir and react for 2h; heat to 35°C and continue stirring for 30min; prepare 46mL1 of deionized water (14°C) with water and distilled water, add deionized water to the conical flask, and then increase the temperature to 98°C, continue heating for 20min, the solution is brown-yellow and red smoke emerges; take 5g of hydrogen peroxide (30%) and add it to the conical flask; remove the conical flask and filter it while hot, and wash it with hydrochloric acid and deionized water. After the remaining solid is stable on the filter paper, take out the filter paper with tweezers, and then line the bottom with a clean filter paper, and put one piece in a drying oven at 60°C to fully dry to obtain dried graphene;

[0144] 100 mg of the dried graphene oxide was dispersed in 100 g of water to obtain a brown-yellow suspension; the suspension was placed in an ultrasonic washing box and dispersed under ultrasonic conditions for 1 hour; the solution was taken out and placed in a four-necked beaker, the temperature was raised to 80°C, and 20 ml of hydrazine hydrate was added dropwise, the reaction was carried out for 24 hours, and the obtained product was filtered, and the obtained product was washed with methanol and water, and the obtained solid was fully dried in a drying oven at 60°C to obtain graphene;

[0145] Graphene was pretreated with poly(dimethyldiallylammonium) chloride (PDDA) solution to obtain more oxygen-containing functional groups; FeCl 2 / FeCl 3 Growth of Fe on the PDDA surface by in situ hydrolysis of x O y Nanoparticles (FexOyNPs) to obtain G@FeO y ; Then 80 mg of G@FexOy and 2 g of sucrose were added to 40 mL of water and ultrasonically treated for 1 h to form a uniform black suspension; then the solution was hydrothermally reacted at 180 ° C for 15 h to obtain a dark brown precursor solution, which was centrifugally washed and dried to obtain a dried precursor; the dried precursor was then calcined at 800 ° C in argon for 3 h, with a heating rate of 5 ° C / min and a gas flow rate of 50 mL / min; finally, the material was placed in a 60 ° C HCl solution and stirred for 48 h to remove Fe x O y NPs, to obtain carbon nanocages;

[0146] 1.5 g of carbon nanocage was added to an ethanol dispersion of ZnO particles with a concentration of 30 mg / mL and a volume of 200 mL, the temperature was raised to 80°C at a heating rate of 5°C / min, and then ultrasonically mixed at a power of 300 W for 2 hours to obtain an intermediate product, wherein the intermediate product includes a carbon nanocage and at least one ZnO particle with a ligand connected to its surface located in the carbon nanocage; and the mixture was calcined at 155°C for 20 hours to obtain a carbon nanocage-ZnO particle composite material.

[0147] Preparation of optoelectronic devices:

[0148] Providing an ITO anode having a thickness of 30 nm;

[0149] Spin coating PEDOT:PSS material on the anode, annealing at 150° C. for 30 min, to obtain a hole injection layer 60 with a thickness of 20 nm;

[0150] Spin coating TFB material on the hole injection layer 60, annealing at 200°C for 30 minutes to obtain a hole transport layer 50 with a thickness of 25 nm;

[0151] Spin-coat CdZnSe / ZnSe / ZnS on the hole transport layer 50 2 The blue light quantum dot material is annealed at 80° C. for 5 min to obtain a light-emitting layer 40 with a thickness of 20 nm;

[0152] Providing a carbon nanocage-inorganic semiconductor particle composite material, dissolving the carbon nanocage-inorganic semiconductor particle composite material in DMF to obtain a dispersion, spin-coating the dispersion on the light-emitting layer 40, and annealing at 80° C. for 30 minutes to obtain an electron transport layer 20 with a thickness of 35 nm;

[0153] Ag is evaporated on the electron transport layer 20 to obtain a cathode with a thickness of 35 nm;

[0154] After packaging, the optoelectronic device 100 is obtained.

[0155] Example 2

[0156] This embodiment is substantially the same as Embodiment 1, except that, in this embodiment, Mg-doped ZnO is used to replace the ZnO in Embodiment 1.

[0157] Example 3

[0158] This embodiment is basically the same as embodiment 1, except that in this embodiment, TiO 2 The particles replace the ZnO particles in Example 1.

[0159] Example 4

[0160] This embodiment is substantially the same as Embodiment 1, except that, in this embodiment, the amount of carbon nanocage used is 4 g.

[0161] Example 5

[0162] This embodiment is basically the same as Embodiment 1, except that, in this embodiment, the amount of carbon nanocage used is 1 g.

[0163] Comparative Example 1

[0164] This comparative example is basically the same as Example 1, except that, in this comparative example, the method for preparing the electron transport layer is: providing an ethanol dispersion of ZnO particles, spin coating the ethanol dispersion of ZnO particles on the light-emitting layer 40, annealing at 80°C for 5 minutes, to obtain an electron transport layer 20 with a thickness of 35 nm.

[0165] The maximum external quantum efficiency EQE of the optoelectronic devices of Examples 1 to 5 and Comparative Example 1 was respectively max , lifespan T95@1000nits and current density J test, the maximum external quantum efficiency EQE shown in Table 1 is obtained max , lifespan T95@1000nits and current density J, Fig.10 The JV curves of Example 1 and Comparative Example 1 shown, Fig.11 The luminous intensity-current density curves of Example 1 and Comparative Example 1 are shown.

[0166] Maximum external quantum efficiency EQE max The test method is: using FSD FPD optical property measurement equipment, controlling the efficiency test system built by QE PRO spectrometer, Keithley 2400, and Keithley 6485 through LabView, measuring parameters such as voltage, current, brightness, and luminous spectrum, and calculating the maximum external quantum efficiency EQE of the device. max .

[0167] The test method for life span T95@1000nit is: in CDA gas, under constant current or voltage drive, measure the time taken for the device brightness to decay to a certain proportion of the maximum brightness, and the time taken for the brightness to decay to 95% of the maximum brightness is defined as T95, and this life span is the measured life span. In order to shorten the life span test cycle, the device life span test is usually carried out at high brightness by accelerating device aging, and the life span at low brightness is obtained by fitting the decay fitting formula. For example, the life span at 1000nits is recorded as T95@1000nits, and the calculation formula is:

[0168]

[0169] Among them, T95 L The lifespan under low brightness, generally 1000nits, T95 H is the lifespan under high brightness, that is, the measured lifespan, L H is the maximum brightness that the device is accelerated to, L L Generally, it is 1000nits, A is the acceleration factor, which is 1.7. The constant current is 2mA.

[0170] The test method of current density J is: use Keithley 2400 to test the current of the device, obtain the current density according to the light-emitting area, and record the current density of the device under a voltage of 5V.

[0171] Depend on Fig.10 It can be seen that under the same voltage, the photovoltaic device of Example 1 has a higher current density. Fig.11 It can be seen that under the same current density, the optoelectronic device of Example 1 has a higher luminous intensity. It can be seen that under the same voltage, the optoelectronic device of Example 1 has a higher luminous intensity. The reason may be that the electron transport layer material carbon nanocage-inorganic semiconductor particle composite material of Example 1 has no ligand on the surface of inorganic semiconductor particles, and the carbon nanocage has good conductivity, so that the electron transport layer has a higher conductivity.

[0172] Table 1:

[0173]

[0174] From Table 1 we can see that:

[0175] Compared with the optoelectronic device of comparative example 1, the optoelectronic devices prepared by using the carbon nanocage-inorganic semiconductor particle composite material of the present application as the electron transport layer material in Examples 1 to 3 have a higher maximum external quantum efficiency EQE max , and a longer lifespan. The reason may be that the inorganic semiconductor particles of the electron transport layer material carbon nanocage-inorganic semiconductor particle composite material of Examples 1 to 3 have no ligands on the surface and are not easy to aggregate, which can make the electron transport layer have higher stability and conductivity.

[0176] Under the same voltage, compared with the optoelectronic device of Comparative Example 1, the optoelectronic devices of Examples 1 to 3 prepared by using the carbon nanocage-inorganic semiconductor particle composite material of the present application as the electron transport layer material may be because the electron transport layer material carbon nanocage-inorganic semiconductor particle composite material of Examples 1 to 3 has no ligands on the surface of the inorganic semiconductor particles, and the carbon nanocage has good conductivity, which makes the electron transport layer have higher conductivity.

[0177] Compared with the optoelectronic device of Example 1, the maximum external quantum efficiency EQE of the optoelectronic device of Example 4 is max The reason may be that the carbon nanocages and inorganic semiconductor particles in the carbon nanocage-inorganic semiconductor particle composite material of Example 4 are relatively large in mass, resulting in a relatively small content of inorganic semiconductor particles and weaker electron transport performance.

[0178] Compared with the optoelectronic device of Example 1, the maximum external quantum efficiency EQE of the optoelectronic device of Example 5 is max The smaller the carbon nanocage, the shorter the lifespan and the lower the current density, the possible reason is that in the carbon nanocage-inorganic semiconductor particle composite material of Example 4, the mass of the carbon nanocage and the inorganic semiconductor particles are relatively small, resulting in a relatively high content of inorganic semiconductor particles, and there are inorganic semiconductor particles not filled in the carbon nanocage. These inorganic semiconductor particles not filled in the carbon nanocage are easy to agglomerate, resulting in poor stability and poor electron transport performance.

[0179] The optoelectronic devices and their preparation methods, and display devices provided in the embodiments of the present application are introduced in detail above. Specific examples are used herein to illustrate the principles and implementation methods of the present application. The description of the above embodiments is only used to help understand the methods and core ideas of the present application. At the same time, for technical personnel in this field, according to the ideas of the present application, there will be changes in the specific implementation methods and application scopes. In summary, the content of this specification should not be understood as a limitation on the present application.

Claims

1. A photoelectric device comprising a stacked first electrode, an electron transport layer and a second electrode, characterized in that: The material of the electron transport layer includes a carbon nanocage-inorganic semiconductor particle composite material, and the carbon nanocage-inorganic semiconductor particle composite material includes a carbon nanocage and at least one inorganic semiconductor particle filled in the carbon nanocage.

2. The optoelectronic device according to claim 1, characterized in that In the carbon nanocage-inorganic semiconductor particle composite material, the mass ratio of the carbon nanocage to the inorganic semiconductor particle is 1:(2-4); and / or The average particle size of the carbon nano cage is 30 to 50 nm; and / or The average particle size of the inorganic semiconductor particles is 7 to 12 nm; and / or The carbon nano cage has a plurality of nanopores, and the diameter of the nanopores is 4-16 nm.

3. The optoelectronic device according to claim 1, characterized in that Each carbon nanocage is filled with 1 to 3 inorganic semiconductor particles.

4. The optoelectronic device according to claim 1, characterized in that The carbon nanocage comprises a graphene carbon nanocage; and / or The material of the inorganic semiconductor particles includes one or more of undoped metal oxides, doped metal oxides, ceramic semiconductor materials, IIB-VIA semiconductor materials, IIIA-VA semiconductor materials and IB-IIIA-VIA semiconductor materials. The undoped metal oxides include one or more of ZnO, TiO2, SnO2, ZrO2, and Ta2O5; the metal oxides in the doped metal oxides include one or more of ZnO, TiO2, SnO2, ZrO2, Ta2O5, and Al2O3; the doping elements in the doped inorganic semiconductor particles include one or more of Al, Mg, Li, Mn, Y, La, Cu, Ni, Zr, Ce, In, and Ga; the ceramic semiconductor material includes barium titanate; the IIB-VIA semiconductor materials include one or more of ZnS, ZnSe, and CdS; the IIIA-VA semiconductor materials include one or more of InP and GaP; and the IB-IIIA-VIA semiconductor materials include one or more of CuInS and CuGaS.

5. The optoelectronic device according to claim 1, wherein: The optoelectronic device further includes a light-emitting layer, which is located between the first electrode and the electron transport layer or between the second electrode and the electron transport layer.

6. The optoelectronic device according to claim 5, characterized in that The first electrode and the second electrode independently include a doped metal oxide electrode, a composite electrode, a graphene electrode, a carbon nanotube electrode, a metal single substance electrode or an alloy electrode. The material of the doped metal oxide electrode includes one or more of indium doped tin oxide, fluorine doped tin oxide, antimony doped tin oxide, aluminum doped zinc oxide, gallium doped zinc oxide, indium doped zinc oxide, magnesium doped zinc oxide, aluminum doped magnesium oxide, and cadmium doped zinc oxide. The composite electrode includes AZO / Ag / AZO, AZO / Al / AZO, ITO / Ag / ITO, ITO / Al / ITO, ZnO / Ag, / ZnO, ZnO / Al / ZnO, TiO2 / Ag / TiO2, TiO2 / Al / TiO2, ZnS / Ag / ZnS, ZnS / Al / ZnS, Ca / Al, LiF / Ca, LiF / Al, BaF2 / Al, CsF / Al, CaCO3 / Al or BaF2 / Ca / Al, the material of the metal single substance electrode includes one or more of Ag, Ni, Pt, Au, Ir, Cu, Mo, Al, Ca, Mg and Ba, and the alloy electrode includes Au:Mg alloy electrode or Ag:Mg alloy electrode; and / or The material of the light-emitting layer includes one or more of an organic light-emitting material and a quantum dot light-emitting material, and the organic light-emitting material includes one or more of 4,4'-bis(N-carbazole)-1,1'-biphenyl:tri[2-(p-tolyl)pyridine iridium(III), 4,4',4"-tri(carbazole-9-yl)triphenylamine:tri[2-(p-tolyl)pyridine iridium, diaromatic anthracene derivatives, distilbene aromatic derivatives, pyrene derivatives, fluorene derivatives, TBPe fluorescent materials, TTPX fluorescent materials, TBRb fluorescent materials, DBP fluorescent materials, delayed fluorescent materials, TTA materials, thermally activated delayed materials, polymers containing covalent bonds of BN, hybrid localized charge transfer excited state materials, exciplex light-emitting materials, polyacetylene and its derivatives, polyparaphenylene and its derivatives, polythiophene and its derivatives, polyfluorene and its derivatives;The quantum dot luminescent material includes one or more of a single structure quantum dot, a core-shell structure quantum dot and a perovskite semiconductor material. The material of the single structure quantum dot, the core material of the core-shell structure quantum dot and the shell material of the core-shell structure quantum dot are independently selected from one or more of II-VI group compounds, IV-VI group compounds, III-V group compounds and I-III-VI group compounds. The II-VI group compounds include CdS, CdSe, CdTe, ZnS, ZnSe, ZnTe, ZnO, HgS, HgSe, HgTe, CdSeS, CdSeTe, CdSTe, ZnSeS, ZnSeTe, Zn STe, HgSeS, HgSeTe, HgSTe, CdZnS, CdZnSe, CdZnTe, CdHgS, CdHgSe, CdHgTe, HgZnS, HgZnSe, HgZnTe, CdZnSeS, CdZnSeTe, CdZnSTe, CdHgSeS, CdHgSeTe, CdHgSTe, HgZnSeS, HgZnSeTe and HgZnSTe, and the IV-VI group compound includes SnS, SnSe, SnTe, PbS, PbSe, PbTe, SnSeS, SnSeTe, SnSTe, PbSeS, One or more of PbSeTe, PbSTe, SnPbS, SnPbSe, SnPbTe, SnPbSSe, SnPbSeTe, SnPbSTe, the III-V group compound includes GaN, GaP, GaAs, GaSb, AlN, AlP, AlAs, AlSb, InN, InP, InAs, InSb, GaNP, GaNAs, GaNSb, GaPAs, GaPSb, AlNP, AlNAs, AlNSb, AlPAs, AlPSb, InNP, InNAs, InNSb, InPAs, InPSb, GaAlNP, GaAlN As, GaAlNSb, GaAlPAs, GaAlPSb, GaInNP, GaInNAs, GaInNSb, GaInPAs, GaInPSb, InAlNP, InAlNAs, InAlNSb, InAlPAs and InAlPSb, the I-III-VI group compound includes one or more of CuInS2, CuInSe2 and AgInS2; the perovskite semiconductor material includes a doped or undoped inorganic perovskite semiconductor or an organic-inorganic hybrid perovskite semiconductor, and the general structural formula of the inorganic perovskite semiconductor is AMX3, wherein A is Cs; + ions, M is a divalent metal cation, including Pb 2+ Sn 2+ , Cu 2+ 、Ni 2+ 、Cd 2+ Cr 2+ , Mn 2+ 、Co 2+ , Fe 2+ ,Ge 2+ , Yb 2+ 、Eu 2+ One or more of, X is a halogen anion, including Cl - Br - ,I - One or more of; the general structural formula of the organic-inorganic hybrid perovskite semiconductor is BMX3, wherein B is an organic amine cation, including CH3(CH2) n-2 NH3 + or [NH3(CH2) n NH3] 2+ , where n≥2, M is a divalent metal cation, including Pb 2+ Sn 2+ , Cu 2+ 、Ni 2+ 、Cd 2+ Cr 2+ , Mn 2+ 、Co 2+ , Fe 2+ ,Ge 2+ , Yb 2+ 、Eu 2+ One or more of, X is a halogen anion, including Cl - Br - ,I - One or more of; and / or The photoelectric device also includes a hole transport layer, which is located on a side of the light-emitting layer away from the electron transport layer, and the material of the hole transport layer includes 4,4'-N,N'-dicarbazolyl-biphenyl, poly[bis(4-phenyl)(2,4,6-trimethylphenyl)amine], N,N'-diphenyl-N,N'-bis(1-naphthyl)-1,1'-biphenyl-4,4"-diamine, N,N'-diphenyl-N,N'-bis(3-methylphenyl)-(1,1'-biphenyl)-4,4'-diamine, poly(N,N'-bis(4-butylphenyl)-N,N'-bis(phenyl)benzidine) 、N,N'-bis(3-methylphenyl)-N,N'-bis(phenyl)-spiro、N,N'-bis(4-(N,N'-diphenyl-amino)phenyl)-N,N'-diphenylbenzidine、4,4',4'-tri(N-carbazolyl)-triphenylamine、4,4',4'-tri(N-3-methylphenyl-N-phenylamino)triphenylamine、poly[(9,9'-dioctylfluorene-2,7-diyl)-co-(4,4'-(N-(4-sec-butylphenyl)diphenylamine))]、poly(N-vinylcarbazole) and its derivatives、N,N'-di(1-naphthyl)-N,N'-diphenyl-1,1' -biphenyl-4-4'-diamine, spiro NPB, poly(phenylene vinylene), poly[2-methoxy-5-(2-ethylhexyloxy)-1,4-phenylene vinylene], poly[2-methoxy-5-(3',7'-dimethyloctyloxy)-1,4-phenylene vinylene], 2,2',7,7'-tetrakis[N,N-di(4-methoxyphenyl)amino]-9,9'-spirobifluorene, 4,4'-cyclohexylbis[N,N-di(4-methylphenyl)aniline], 1,3-bis(carbazol-9-yl)benzene, polyaniline, polypyrrole, poly(p-)phenylene vinylene, aromatic tertiary amines, polynuclear aromatic One or more of fragrant tertiary amine, 4,4'-bis(p-carbazolyl)-1,1'-biphenyl compound, N,N,N',N'-tetraarylbenzidine, PEDOT:PSS and its derivatives, polymethacrylate and its derivatives, poly(9,9-octylfluorene) and its derivatives, poly(spirofluorene) and its derivatives, doped graphene, undoped graphene, C60, doped or undoped NiO, doped or undoped MoO3, doped or undoped WO3, doped or undoped V2O5, doped or undoped P-type gallium nitride, doped or undoped CrO3, doped or undoped CuO; and / or The photoelectric device also includes a hole injection layer, which is located on a side of the light-emitting layer away from the electron transport layer, and the material of the hole injection layer includes one or more of 2,3,6,7,10,11-hexacyano-1,4,5,8,9,12-hexaazatriphenylene, PEDOT, PEDOT:PSS, a derivative of PEDOT:PSS doped with s-MoO3, 4,4',4'-tris(N-3-methylphenyl-N-phenylamino)triphenylamine, tetracyanoquinodimethane, copper phthalocyanine, nickel oxide, molybdenum oxide, tungsten oxide, vanadium oxide, molybdenum sulfide, tungsten sulfide and copper oxide.

7. A method for preparing a photoelectric device, characterized in that: The steps include: Providing a photovoltaic device preform, wherein the photovoltaic device preform comprises a first electrode; Providing a carbon nanocage-inorganic semiconductor particle composite material, and disposing the carbon nanocage-inorganic semiconductor particle composite material on the optoelectronic device preform to obtain an electron transport layer; A second electrode is formed on the electron transport layer to obtain a photoelectric device.

8. The preparation method according to claim 7, characterized in that: The method for arranging the carbon nano cage-inorganic semiconductor particle composite material on the optoelectronic device preform is: dissolving the carbon nano cage-inorganic semiconductor particle composite material in a first solvent to obtain a dispersion, and spin coating the dispersion on the optoelectronic device preform.

9. The preparation method according to claim 8, characterized in that: The first solvent comprises one or more of isopropanol, ethanol, dimethyl sulfoxide, N-methylpyrrolidone and chlorobenzene; and / or In the dispersion, the concentration of the carbon nanocage-inorganic semiconductor particle composite material is 10 to 50 mg / mL; and / or After spin coating the dispersion on the optoelectronic device preform and before obtaining the electron transport layer, the method further includes: annealing the optoelectronic device preform provided with the dispersion, wherein the annealing temperature is 75-85° C. and the annealing time is 5-10 minutes.

10. The preparation method according to claim 7, characterized in that: The preparation method of the carbon nano cage-inorganic semiconductor particle composite material comprises the following steps: Providing an inorganic semiconductor particle dispersion, adding carbon nanocages and a polar solvent to the inorganic semiconductor particle dispersion, and ultrasonically mixing to obtain an intermediate product; The intermediate product is calcined to obtain a carbon nanocage-inorganic semiconductor particle composite material.

11. The preparation method according to claim 10, characterized in that: The mass ratio of the carbon nanocage to the inorganic semiconductor particles in the inorganic semiconductor particle dispersion is 1:(2-5); and / or In the inorganic semiconductor particle dispersion, the concentration of the inorganic semiconductor particles is 30 to 40 mg / ml; and / or The mass ratio of the polar solvent to the inorganic semiconductor particles is (0.5-1.5):1; and / or The power of the ultrasonic mixing is 200-400W, and the time is 1-3h; and / or The calcination temperature is 150-160° C. and the calcination time is 15-25 hours.

12. The preparation method according to claim 10, characterized in that: The carbon nanocage comprises a graphene carbon nanocage; and / or The inorganic semiconductor particles include one or more of undoped metal oxides, doped metal oxides, ceramic semiconductor materials, IIB-VIA semiconductor materials, IIIA-VA semiconductor materials and IB-IIIA-VIA semiconductor materials. The undoped metal oxides include one or more of ZnO, TiO2, SnO2, ZrO2 and Ta2O5; the metal oxides in the doped metal oxides include one or more of ZnO, TiO2, SnO2, ZrO2, Ta2O5 and Al2O3; the doping elements in the doped metal oxides include one or more of Al, Mg, Li, Mn, Y, La, Cu, Ni, Zr, Ce, In and Ga; the ceramic semiconductor material includes barium titanate; the IIB-VIA semiconductor materials include one or more of ZnS, ZnSe and CdS; the IIIA-VA semiconductor materials include one or more of InP and GaP; the IB-IIIA-VIA semiconductor materials include one or more of CuInS and CuGaS; and / or The solvent in the inorganic semiconductor particle dispersion includes one or more of ethanol, butanol, and isopropanol; and / or The surfaces of the inorganic semiconductor particles in the inorganic semiconductor particle dispersion are connected with ligands, and the ligands include one or more of hydroxyl groups and carboxyl groups; and / or The polar solvent includes one or more of ethanol, butanol, isopropanol, and deionized water.

13. The preparation method according to claim 10, characterized in that: After adding the carbon nano cage and the polar solvent into the inorganic semiconductor particle dispersion and before the ultrasonic mixing, the method further comprises: heating the temperature to 60-100° C. at a heating rate of 2-10° C. / min.

14. The preparation method according to claim 7, characterized in that: The first electrode is an anode, the second electrode is a cathode, and the photoelectric device preform further comprises a light-emitting layer disposed on the first electrode; or The first electrode is an anode, the second electrode is a cathode, the optical device preform further comprises a hole functional layer and a light emitting layer stacked on the first electrode, the hole functional layer comprises a hole transport layer and / or a hole injection layer; or The first electrode is a cathode, the second electrode is an anode, and forming the second electrode on the electron transport layer comprises: forming a stacked light-emitting layer and a second electrode on the electron transport layer; or The first electrode is a cathode, the second electrode is an anode, and forming the second electrode on the electron transport layer includes: forming a stacked light-emitting layer, a hole functional layer and a second electrode on the electron transport layer, and the hole functional layer includes a hole transport layer and / or a hole injection layer.

15. A display device, characterized in that: The display device comprises the optoelectronic device according to any one of claims 1 to 6, or the display device comprises the optoelectronic device prepared by the preparation method according to any one of claims 7 to 14.