Manufacturing method of perovskite solar cell and perovskite solar cell
By combining CsX and PbX2 in DMF and DMSO and controlling the halide distribution using the dual solution diffusion method, the band gap control problem of perovskite layer is solved, the preparation of high-quality perovskite layer is achieved, and the performance of solar cells is improved.
Patent Information
- Application Number
- CN202411088386.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-08
- Publication Date
- 2024-11-22
AI Technical Summary
In the prior art, it is difficult to achieve accurate band gap control in the formation of perovskite layers, especially in the presence of large halide ions such as bromide, resulting in poor uniformity of the perovskite layer, and the band gap deviates from the design value, affecting solar energy. Photoelectric conversion performance of the battery.
By combining CsX and PbX2 in DMF and DMSO, a solid inorganic membrane template is formed, combined with organic salts such as FAX and MAX, and the distribution and proportion of halides are controlled using a dual solution diffusion method to achieve uniform and orderly growth of the perovskite layer and Fine control.
The preparation of high-quality perovskite layers is realized, the crystallinity is enhanced, the complexity of halide control is solved, the wide band gap characteristics and precise adjustment of optical band gap is ensured, defects are reduced, and the performance of solar cells is improved.
Smart Images

Figure CN119012879A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of solar cell manufacturing, and in particular to a manufacturing method of a perovskite solar cell and a perovskite solar cell. Background Art
[0002] Solar energy is renewable and clean, with abundant availability and cost-effectiveness. Converting solar energy into electrical energy using photovoltaic cells is one of the most efficient utilization methods currently used. It is worth noting that solar cells, especially those composed of polycrystalline silicon and single-crystalline silicon, already have mature industrial technology. However, in recent years, there has been a surge in scientific and industrial attention to perovskite solar cells due to their remarkable properties, including high photoelectric conversion efficiency, adjustable bandgap width, strong tolerance to impurities, lowest temperature coefficient and simple preparation procedures. The efficiency of perovskite / crystalline silicon tandem solar cells has now reached an impressive 33.9%, exceeding the 26.8% of single-junction devices.
[0003] The formation of a perovskite layer is of great significance for achieving higher solar cell efficiency, especially when considering wide bandgap perovskites used in the formation of tandem solar cells. In the prior art, one of the methods for the formation of a perovskite layer is a full solution method (double solution mutual diffusion method). Among them, the double solution diffusion method includes a layered method, first forming an inorganic precursor film or template (a template refers to an inorganic precursor solution spread on a substrate to be formed, including a structure of a substrate and a liquid film), and then forming an organic film and then mixing a perovskite absorption layer. This method encounters challenges in controlling carrier dynamics in the formation of a wide bandgap perovskite layer, and it is difficult to achieve the preparation of an accurate bandgap perovskite layer. Especially in the presence of large halide ions, such as bromide (Br), the uniformity of the perovskite layer is poor, and defects are prone to occur, resulting in the final product bandgap deviating from the design value, making the photoelectric conversion performance of the final solar cell unsatisfactory. Therefore, it is urgent to solve the application of this method for a wide bandgap perovskite layer. Summary of the invention
[0004] Therefore, the present invention provides a method for manufacturing a perovskite solar cell and a perovskite solar cell to solve the problem that it is difficult to achieve a precise band gap when preparing a wide band gap perovskite layer.
[0005] The invention provides a method for manufacturing a perovskite solar cell. The formation of a perovskite layer of the perovskite solar cell comprises the following steps: forming an inorganic precursor solution, and further forming an inorganic precursor film layer; the solvent of the inorganic precursor solution comprises a mixture of DMF and DMSO; the inorganic precursor material forming the inorganic precursor solution comprises at least CsX and PbX2; wherein X in CsX is Br or I, and X in PbX2 is I; forming an organic precursor solution, applying the organic precursor solution on the surface of the inorganic precursor film layer, and mixing with the inorganic precursor film layer to form a mixed precursor solution layer; the organic precursor material of the organic precursor solution comprises at least two of FAX and MAX, wherein X in FAX is Br or I, and X in MAX is Cl; and diffusion annealing to convert the mixed precursor solution layer into a perovskite layer.
[0006] Optionally, the steps of forming an inorganic precursor solution and further forming an inorganic precursor film layer include: mixing two or more inorganic precursor materials and modulating them according to corresponding preset molar contents to form an inorganic precursor solution; spreading the inorganic precursor solution on a substrate to be formed with a film layer; the spreading method includes spin coating; annealing the spread inorganic precursor solution to form an inorganic precursor film layer, wherein the inorganic precursor film layer is a liquid film layer.
[0007] Optionally, in the inorganic precursor solution, the molar content of CsX is different from the molar content of PbX2. The molar content of CsX is 0.10 mol / L to 0.20 mol / L; the molar content of PbX2 is 1.00 mol / L to 2.00 mol / L; in the mixed solvent of DMF and DMSO, the ratio of DMF to DMSO is DMF:DMSO=900:100 to 990:10.
[0008] Optionally, in the mixed solvent of DMF and DMSO, the ratio of DMF to DMSO is DMF:DMSO=950:50; and the difference between the molar content of CsX and the molar content of PbX2 is 0.1 mol / L.
[0009] Optionally, the steps of forming an organic precursor solution, applying the organic precursor solution on the surface of the inorganic precursor film layer, and mixing the organic precursor solution with the inorganic precursor film layer to form a mixed precursor solution layer include: modulating at least one organic precursor material into an organic precursor solution according to a corresponding preset molar content; the solvent of the organic precursor solution includes IPA; spreading and mixing the organic precursor solution on the surface of the inorganic precursor film layer; and the spreading method includes spin coating.
[0010] Optionally, in the step of diffusion annealing to convert the mixed precursor solution layer into a perovskite layer: the annealing temperature is 100° C. to 200° C.; the annealing time is 10 min to 60 min; and the ambient humidity is 20% to 60% relative humidity.
[0011] Optionally, the method for manufacturing a perovskite solar cell also includes: providing a substrate layer; forming an i-type hydrogenated amorphous silicon layer, a P-type amorphous silicon doped layer, a first transparent electrode layer and a first metal electrode layer stacked in sequence on the surface of one side of the substrate layer; forming an i-type hydrogenated amorphous silicon layer, an N-type amorphous silicon doped layer, a transparent conductive layer, a hole transport layer, a passivation layer, an electron transport layer, a second transparent conductive layer, a second metal electrode layer and an anti-reflection layer stacked in sequence on the surface of the other side of the substrate layer; the perovskite layer is formed on the surface of the hole transport layer on the side facing away from the substrate layer; the passivation layer is formed on the surface of the perovskite layer on the side facing away from the substrate layer.
[0012] The present invention also provides a perovskite solar cell, characterized in that it is manufactured using the manufacturing method of the perovskite solar cell provided by the present invention; the perovskite solar cell includes a single-junction perovskite cell device, a perovskite-perovskite stacked cell or a perovskite heterojunction stacked cell and other stacked cells containing a perovskite cell portion.
[0013] Optionally, the perovskite solar cell provided by the present invention includes: a substrate layer; an i-type hydrogenated amorphous silicon layer, a P-type amorphous silicon doped layer, a first transparent electrode layer and a first metal electrode layer stacked in sequence on one side of the substrate layer; an i-type hydrogenated amorphous silicon layer, an N-type amorphous silicon doped layer, a transparent conductive layer, a hole transport layer, a passivation layer, an electron transport layer, an electron transport layer modified layer, a second transparent conductive layer, a second metal electrode layer and an anti-reflection layer stacked in sequence on the other side of the substrate layer; the perovskite layer is located between the hole transport layer and the passivation layer.
[0014] Optionally, the first transparent conductive layer includes ITO conductive glass or FTO conductive glass; the second transparent conductive layer includes ITO conductive glass or FTO conductive glass; the material of the passivation layer includes phenylethylamine iodide or ethylamine iodide; the material of the first metal electrode layer includes one of Au, Ag, Cu, Cu-Al alloy, and C; the material of the second metal electrode layer includes one of Au, Ag, Cu, Cu-Al alloy, and C.
[0015] The technical solution of the present invention has the following advantages:
[0016] The method for manufacturing a perovskite solar cell provided by the present invention is to establish a strong inorganic film template by combining CsX and PbX2 (especially PbI2) in DMF and DMSO, thereby forming a structured substrate to promote the uniform and orderly growth of the perovskite film. Subsequently, a double solution diffusion method is used in combination with organic salts such as FAX and / or MAX to control the penetration of the template and promote the formation of the final perovskite layer. The method includes preparing a separate precursor solution with a specific molar ratio of inorganic and organic components, thereby allowing fine control of the halide composition at the molecular level. The deposition process includes applying the organic precursor solution to the preformed inorganic precursor film layer, and promoting the controlled interdiffusion of the halide during the annealing process to achieve the desired halide distribution. By carefully managing the specific concentrations of different halides (I and Br) in the separate precursor solutions, this method provides a unique solution to solve the complexity of halide control in the double-step deposition method, and ultimately produces a high-quality perovskite layer with the desired wide bandgap properties. The present approach enhances the crystallization of perovskites and addresses challenges associated with support dynamics, particularly in the presence of larger halide ions such as bromide (Br), leading to a more uniform and defect-free structure. Furthermore, tuning the ratio of organic precursors in the perovskite enables the realization of different optical bandgaps within the perovskite layer.
[0017] The perovskite solar cell provided by the present invention is manufactured using the manufacturing method of the perovskite solar cell provided by the present invention. By combining CsX and PbX2 (especially PbI2) in DMF and DMSO, a strong inorganic film template is established to form a structured substrate to promote the uniform and orderly growth of the perovskite film. Subsequently, a double solution diffusion method is used in combination with organic salts such as FAX and / or MAX to control the penetration of the template and promote the formation of the final perovskite layer. The method includes preparing a separate precursor solution with a specific molar ratio of inorganic and organic components, thereby allowing fine control of the halide composition at the molecular level. The deposition process includes applying the organic precursor solution to the preformed inorganic precursor film layer, and promoting the controlled interdiffusion of the halide during the annealing process to achieve the desired halide distribution. By carefully managing the specific concentrations of different halides (I and Br) in the separate precursor solutions, this method provides a unique solution to solve the complexity of halide control in the double-step deposition method, and ultimately produces a high-quality perovskite layer with the desired wide bandgap properties. The method enhances the crystallization of perovskites and addresses challenges associated with carrier dynamics, particularly in the presence of larger halide ions such as bromide (Br), leading to a more uniform and defect-free structure. Furthermore, tuning the ratio of organic precursors in the perovskite enables the realization of different optical bandgaps within the perovskite layer. BRIEF DESCRIPTION OF THE DRAWINGS
[0018] In order to more clearly illustrate the specific implementation methods of the present invention or the technical solutions in the prior art, the drawings required for use in the specific implementation methods or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are some implementation methods of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0019] Figure 1 A schematic diagram of a process for manufacturing a perovskite solar cell according to an embodiment of the present invention;
[0020] Figure 2A and Figure 2B It is a schematic diagram of forming an organic precursor film layer in a method for manufacturing a perovskite solar cell according to an embodiment of the present invention;
[0021] Figure 3A and Figure 3B It is a schematic diagram of a process of forming a mixed precursor film layer and converting it into a perovskite layer in a method for manufacturing a perovskite solar cell according to an embodiment of the present invention;
[0022] Figure 4 is a JV characteristic curve diagram of a perovskite solar cell according to a specific embodiment of the present invention;
[0023] Figure 5A An electron microscope image of the interface between the perovskite layer and the underlying film layer of a perovskite solar cell according to another specific embodiment of the present invention;
[0024] Figure 5B FIG. 4 is a JV characteristic curve diagram of a perovskite solar cell according to another specific embodiment of the present invention. DETAILED DESCRIPTION
[0025] One of the main challenges facing the dual-step deposition method for perovskite formation is the precise control of the halide composition, especially when dealing with multiple halides such as I and Br. The mixture of these halides in the second precursor solution can make it difficult to achieve the desired halide ratio in the perovskite structure. This challenge becomes more pronounced when aiming to make perovskites for larger bandgap cells, where the specific halide concentration plays a crucial role in determining the optical properties.
[0026] In order to solve the problem of accurate preparation of the band gap of a perovskite solar cell in which it is difficult to prepare a wide band gap perovskite layer in the prior art, the present invention provides a method for manufacturing a perovskite solar cell and a perovskite solar cell.
[0027] The technical solution of the present invention will be clearly and completely described below in conjunction with the accompanying drawings. Obviously, the described embodiments are part of the embodiments of the present invention, rather than all of the embodiments. Based on the embodiments in the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention. In the description of the present invention, it should be noted that the terms "first", "second" and "third" are used for descriptive purposes only and cannot be understood as indicating or implying relative importance.
[0028] Example 1
[0029] refer to Figure 1 This embodiment provides a method for manufacturing a perovskite solar cell, wherein the formation of a perovskite layer of the perovskite solar cell comprises the following steps:
[0030] An inorganic precursor solution is formed, and an inorganic precursor film layer is further formed; the solvent of the inorganic precursor solution includes a mixture of DMF and DMSO; the inorganic precursor material forming the inorganic precursor solution includes at least CsX and PbX2; wherein X in CsX is Br or I, and X in PbX2 is I;
[0031] Forming an organic precursor solution, applying the organic precursor solution on the surface of the inorganic precursor film layer, and mixing with the inorganic precursor film layer to form a mixed precursor solution layer; the organic precursor material of the organic precursor solution includes at least two of FAX and MAX, wherein X in FAX is Br or I, and X in MAX is Cl;
[0032] Diffusion annealing allows the inorganic precursor solution and the organic precursor solution to be more fully mixed to form a mixed precursor solution layer, and then converted into a perovskite layer.
[0033] The method for manufacturing perovskite solar cells provided in this embodiment is to establish a strong inorganic film template by accurately combining CsX and PbX2 (especially PbI2) in DMF and DMSO, thereby forming a structured substrate to promote the uniform and orderly growth of the perovskite film. Subsequently, the double solution diffusion method is used in combination with organic salts such as FAX and / or MAX to control the penetration of the template and promote the formation of the final perovskite layer. The method of this embodiment includes preparing a separate precursor solution with a specific molar ratio of inorganic and organic components, thereby allowing fine control of the halide composition at the molecular level. The deposition process includes applying the organic precursor solution to the pre-formed inorganic precursor film layer, and promoting the controlled interdiffusion of the halide during the annealing process to achieve the desired halide distribution. By carefully managing the specific concentrations of different halides (I and Br) in the separate precursor solutions, this method provides a unique solution to solve the complexity of halide control in the double-step deposition method, and ultimately produces a high-quality perovskite layer with the desired wide bandgap properties. The present approach enhances the crystallization of perovskites and addresses challenges associated with support dynamics, particularly in the presence of larger halide ions such as bromide (Br), leading to a more uniform and defect-free structure. Furthermore, tuning the ratio of organic precursors in the perovskite enables the realization of different optical bandgaps within the perovskite layer.
[0034] Furthermore, the steps of forming an inorganic precursor solution and further forming an inorganic precursor film layer include: mixing two or more inorganic precursor materials and modulating them according to corresponding preset molar contents to form an inorganic precursor solution; spreading the inorganic precursor solution on a substrate to be formed with a film layer; the spreading method includes spin coating; annealing the spread inorganic precursor solution to form an inorganic precursor film layer, wherein the inorganic precursor film layer is a liquid film layer.
[0035] Furthermore, in the inorganic precursor solution, the molar content of CsX is different from the molar content of PbX2. The molar content of CsX is 0.10 mol / L to 0.20 mol / L; the molar content of PbX2 is 1.00 mol / L to 2.00 mol / L; in the mixed solvent of DMF and DMSO, the ratio of DMF to DMSO is DMF:DMSO=900:100 to 990:10. By precisely controlling the above material range, precise adjustment of the band gap can be achieved.
[0036] Furthermore, in different embodiments, the molar content of CsX and the molar content of PbX2 differ by 0.1 mol / L. In this way, the components can be precisely controlled and the band gap can be precisely adjusted.
[0037] In a preferred embodiment, in the mixed solvent of DMF and DMSO, the ratio of DMF to DMSO is
[0038] 950:50 (parts), CsI or CsBr is 0.13 mol / L, PbI2 is 1.3 mol / L. This ratio is helpful for the subsequent precise adjustment of the band gap of the final perovskite layer by regulating the proportion of organic precursor materials in the organic precursor solution.
[0039] Furthermore, the steps of forming an organic precursor solution, applying the organic precursor solution on the surface of the inorganic precursor film layer, and mixing the organic precursor solution with the inorganic precursor film layer to form a mixed precursor solution layer include: modulating at least two organic precursor materials into an organic precursor solution according to corresponding preset molar contents; the solvent of the organic precursor solution includes IPA; spreading and mixing the organic precursor solution on the surface of the inorganic precursor film layer; and the spreading method includes spin coating.
[0040] Furthermore, in the organic precursor solution, the organic precursor material includes FAI, FABr and MACl; in the organic precursor solution, the content of FAI is 0.12mol / L to 0.22mol / L, the content of FABr is 0.16mol / L to 0.32mol / L, and the content of MACl is 0.1mol / L.
[0041] In a preferred embodiment, the content of FAI is 0.12 mol / L, the content of FABr is 0.32 mol / L, and the content of MACl is 0.1 mol / L. In this ratio, combined with the ratio of the aforementioned inorganic precursors, a band gap of 1.67 eV can be obtained. In another preferred embodiment, the content of FAI is 0.22 mol / L, the content of FABr is 0.16 mol / L, and the content of MACl is 0.1 mol / L. In this ratio, combined with the ratio of the aforementioned inorganic precursors, a band gap of 1.61 eV can be obtained.
[0042] Furthermore, in the step of diffusion annealing to convert the mixed precursor solution layer into a perovskite layer, the annealing temperature is 100°C to 200°C; the annealing time is 10min to 60min; and the ambient humidity is 20% to 60% relative humidity. Within such a range of conditions, it is helpful to mix and convert the materials and maintain a stable ratio. A ratio lower than the lower limit or higher than the upper limit is not conducive to the precise control of the ratio.
[0043] Furthermore, the method for manufacturing a perovskite solar cell also includes: providing a substrate layer; forming an i-type hydrogenated amorphous silicon layer, a P-type amorphous silicon doped layer, a first transparent electrode layer and a first metal electrode layer stacked in sequence on the surface of one side of the substrate layer; forming an i-type hydrogenated amorphous silicon layer, an N-type amorphous silicon doped layer, a transparent conductive layer, a hole transport layer, a passivation layer, an electron transport layer (in different embodiments, it can also be an electron transport layer modification layer), a second transparent conductive layer, a second metal electrode layer and an anti-reflection layer stacked in sequence on the surface of the other side of the substrate layer; the perovskite layer is formed on the surface of the hole transport layer on the side facing away from the substrate layer; the passivation layer is formed on the surface of the perovskite layer on the side facing away from the substrate layer.
[0044] Example 2
[0045] refer to Figure 2A to Figure 3B This embodiment is a specific implementation process of manufacturing a solar cell using the method of the above-mentioned embodiment 1, and the details are as follows:
[0046] Nickel oxide was prepared as a hole transport layer on a clean ITO substrate and dispersed in deionized water at a concentration of 10-20 mg / mL and processed by spin coating. MeO2Paz was prepared at a concentration of 0.5 mg / mL-1.0 mg / mL and processed by spin coating. Raw materials based on cesium bromide, iodide and lead iodide were prepared according to a 1.3M molar ratio, dissolved in a mixed solvent of DMF:DMSO=950:50 (molar ratio), stirred for 5-10 minutes, then spin coated on the substrate and annealed at 70°C for one minute to prepare a conformal inorganic template. Raw materials based on formamidine, methylamine iodide and bromide were prepared according to FAI: FABr:MACl was weighed at a molar ratio of 30:40, dissolved in isopropanol, stirred for 5-10 minutes, and then spin coated on the inorganic template. The substrate was placed in a 30% RH environment and annealed at 150°C for 15 minutes to complete the perovskite conversion process. In this experiment, PCBM was selected as the electron transport layer. Phenylethylamine iodide (PEAI) with a concentration of 0.5 mg / mL to 1.0 mg / mL was prepared by spin coating. PCBM was dissolved in a chlorobenzene solvent with a concentration of 20 mg / ml and processed by spin coating. Finally, in this experiment, silver was deposited on the electron transport layer as the back electrode with an evaporation rate of 1 A / s and a film thickness of 100 nm. The photovoltaic performance parameters of the device are as follows Figure 4 As shown in Table 1 below.
[0047] Table 1 Photovoltaic performance parameters of perovskite solar cells
[0048] <![CDATA[V oc (V)]]> <![CDATA[J sc (mA / cm 2 )]]> FF(%) PCE(%) Example 2 1.168 21.638 83.273 21.05
[0049] Example 3
[0050] refer to Figure 1 as well as Figure 5A , Figure 5B This embodiment is a specific implementation process of manufacturing a solar cell using the method of the above-mentioned embodiment 1, and the details are as follows:
[0051] First, a single crystal silicon substrate is provided, and on one surface, an i-type hydrogenated amorphous silicon and a P-type amorphous silicon doping layer are sequentially prepared using plasma enhanced chemical vapor deposition (PECVD), wherein the i-type layer has a specific thickness of 5nm, and the P-type layer has a specific thickness of 5nm to 30nm. Subsequently, a first transparent electrode layer having a thickness in the range of 50nm to 500nm is deposited using magnetron sputtering, vacuum evaporation or reactive plasma deposition technology.
[0052] Subsequently, a first metal electrode layer is applied on the surface of the first transparent electrode layer using a method such as magnetron sputtering, vacuum evaporation, reactive plasma deposition or printing, with a thickness ranging from 50 nm to 3000 nm. On the other surface of the silicon substrate, i-type hydrogenated amorphous silicon, N-type amorphous silicon doping layer and transparent conductive oxide (TCO) composite layer are sequentially prepared according to specific thickness requirements using PECVD and methods such as magnetron sputtering, vacuum evaporation, reactive plasma deposition or chemical vapor deposition.
[0053] Subsequently, a hole transport layer with a thickness ranging from 0 to 50 nm is formed on the TCO composite layer, including treatments such as UV ozone and techniques such as spin coating, magnetron sputtering and static spin coating of different layers.
[0054] The subsequent steps include preparing a perovskite absorption layer on the bottom hole transport layer, that is, preparing raw materials based on cesium bromide, iodide and lead iodide according to 1.3 mol / L, dissolving them in a mixed solvent of DMF:DMSO=950:50 (molar ratio), stirring for 5 minutes to 10 minutes, and then spin-coating on the HTL and annealing at 70°C for one minute to prepare a conformal inorganic template. Prepare raw materials based on formamidine, methylamine iodide and bromide according to FAI: weigh FABr:MACl at 30:40 (molar ratio), take 7 mg, weigh and dissolve in isopropanol, stir for 5 minutes to 10 minutes, and then spin-coat on the inorganic template. Place the substrate in a 30% RH environment and anneal at 150 degrees Celsius for 15 minutes to complete the perovskite conversion process, and then use vapor deposition technology to deposit a top passivation layer with materials such as magnesium fluoride and lithium fluoride. Then prepare an electron transport layer or an electron transport layer modification layer on top of the passivation layer, and outline the specific deposition method and thickness.
[0055] Finally, a second transparent electrode layer and a second metal electrode layer are applied on the electron transport layer modification layer using magnetron sputtering and vapor deposition, respectively. An anti-reflection layer is deposited on the second metal electrode layer to complete the fabrication of the perovskite / crystalline silicon tandem solar cell. Each step in the process involves precise control of the deposition method, vacuum conditions, temperature, evaporation rate, and material composition to ensure the successful construction of the solar cell structure.
[0056] Example 4
[0057] The present invention also provides a perovskite solar cell, characterized in that it is manufactured using the manufacturing method of the perovskite solar cell provided by the present invention; the perovskite solar cell includes a single-junction perovskite cell device, a perovskite-perovskite stacked cell or a perovskite heterojunction stacked cell and other stacked cells containing a perovskite cell portion.
[0058] The perovskite solar cell provided in this embodiment is manufactured using the manufacturing method of the perovskite solar cell provided by the present invention. By accurately combining CsX and PbX2 (especially PbI2) in DMF and DMSO, a strong inorganic film template is established to form a structured substrate to promote the uniform and orderly growth of the perovskite film. Subsequently, a double solution diffusion method is used in combination with organic salts such as FAX and / or MAX to control the penetration of the template and promote the formation of the final perovskite layer. The method includes preparing a separate precursor solution having a specific molar ratio of inorganic and organic components, thereby allowing fine control of the halide composition at the molecular level. The deposition process includes applying the organic precursor solution to the preformed inorganic precursor film layer, and promoting the controlled interdiffusion of the halide during the annealing process to achieve the desired halide distribution. By carefully managing the specific concentrations of different halides (I and Br) in the separate precursor solutions, this method provides a unique solution to solve the complexity of halide control in the double-step deposition method, and ultimately produces a high-quality perovskite layer with the desired wide bandgap properties. The method enhances the crystallization of perovskites and addresses challenges associated with support dynamics, particularly in the presence of larger halide ions such as bromide (Br), leading to a more uniform and defect-free structure. Furthermore, tuning the ratio of organic precursors in the perovskite enables the realization of different optical bandgaps within the perovskite layer.
[0059] Furthermore, the perovskite solar cell provided by the present invention includes: a substrate layer; an i-type hydrogenated amorphous silicon layer, a P-type amorphous silicon doped layer, a first transparent electrode layer and a first metal electrode layer stacked in sequence on one side of the substrate layer; an i-type hydrogenated amorphous silicon layer, an N-type amorphous silicon doped layer, a transparent conductive layer, a hole transport layer, a passivation layer, an electron transport layer, an electron transport layer modified layer, a second transparent conductive layer, a second metal electrode layer and an anti-reflection layer stacked in sequence on the other side of the substrate layer; the perovskite layer is located between the hole transport layer and the passivation layer.
[0060] Furthermore, the first transparent conductive layer includes ITO conductive glass or FTO conductive glass; the second transparent conductive layer includes ITO conductive glass or FTO conductive glass; the material of the passivation layer includes phenylethylamine iodide or ethylamine iodide; the material of the first metal electrode layer includes one of Au, Ag, Cu, Cu-Al alloy, and C; the material of the second metal electrode layer includes one of Au, Ag, Cu, Cu-Al alloy, and C.
[0061] Obviously, the above embodiments are merely examples for the purpose of clear explanation, and are not intended to limit the implementation methods. For those skilled in the art, other different forms of changes or modifications can be made based on the above description. It is not necessary and impossible to list all the implementation methods here. The obvious changes or modifications derived therefrom are still within the scope of protection of the invention.
Claims
1. A method for manufacturing a perovskite solar cell, characterized in that: The formation of the perovskite layer of the perovskite solar cell comprises the following steps: An inorganic precursor solution is formed, and an inorganic precursor film layer is further formed; the solvent of the inorganic precursor solution includes a mixture of DMF and DMSO; the inorganic precursor material forming the inorganic precursor solution includes at least CsX and PbX2; wherein X in CsX is Br or I, and X in PbX2 is I; Forming an organic precursor solution, applying the organic precursor solution on the surface of the inorganic precursor film layer, and mixing with the inorganic precursor film layer to form a mixed precursor solution layer; the organic precursor material of the organic precursor solution includes at least two of FAX and MAX; wherein X in FAX is Br or I, and X in MAX is Cl; Diffusion annealing is performed to transform the mixed precursor solution layer into a perovskite layer.
2. The method for manufacturing a perovskite solar cell according to claim 1, characterized in that: The steps of forming an inorganic precursor solution and further forming an inorganic precursor film layer include: Mixing two or more inorganic precursor materials and modulating them according to corresponding preset molar contents to form an inorganic precursor solution; Spreading the inorganic precursor solution on the substrate to be formed into a film layer; the spreading method includes spin coating; The spread inorganic precursor solution is annealed to form an inorganic precursor film layer, wherein the inorganic precursor film layer is a liquid film layer.
3. The method for manufacturing a perovskite solar cell according to claim 2, characterized in that: In the inorganic precursor solution, the molar content of CsX and the molar content of PbX2 are different; The molar content of CsX is 0.10 mol / L to 0.20 mol / L; The molar content of PbX2 is 1.00mol / L to 2.00mol / L; In the mixed solvent of DMF and DMSO, the ratio of DMF to DMSO is DMF: DMSO=900:100~990:10; Preferably, in the mixed solvent of DMF and DMSO, the ratio of DMF to DMSO is DMF:DMSO=950:50; In the inorganic precursor solution, the difference between the molar content of CsX and the molar content of PbX2 is 0.1 mol / L.
4. The method for manufacturing a perovskite solar cell according to claim 1, characterized in that: The step of forming an organic precursor solution, applying the organic precursor solution on the surface of the inorganic precursor film layer, and mixing the organic precursor solution with the inorganic precursor film layer to form a mixed precursor solution layer comprises: preparing at least two organic precursor materials into an organic precursor solution according to corresponding preset molar contents; The solvent of the organic precursor solution includes IPA; The organic precursor solution is spread and mixed on the surface of the inorganic precursor film layer; the spreading method includes spin coating.
5. The method for manufacturing a perovskite solar cell according to claim 4, characterized in that: In the organic precursor solution, the organic precursor material includes FAI, FABr and MACl; In the organic precursor solution, the content of FAI is 0.12 mol / L to 0.22 mol / L, the content of FABr is 0.16 mol / L to 0.32 mol / L, and the content of MACl is 0.1 mol / L.
6. The method for manufacturing a perovskite solar cell according to claim 1, characterized in that: In the step of diffusion annealing to convert the mixed precursor solution layer into a perovskite layer: Annealing temperature is 100°C to 200°C; Annealing time is 10min~60min; The ambient humidity is 20% to 60% relative humidity.
7. The method for manufacturing a perovskite solar cell according to claim 1, characterized in that: Also includes: providing a substrate layer; Forming an i-type hydrogenated amorphous silicon layer, a P-type amorphous silicon doping layer, a first transparent electrode layer and a first metal electrode layer stacked in sequence on a surface of one side of the substrate layer; On the other side surface of the substrate layer, a stacked i-type hydrogenated amorphous silicon layer, an N-type amorphous silicon doped layer, a transparent conductive layer, a hole transport layer, a passivation layer, an electron transport layer, a second transparent conductive layer, a second metal electrode layer and an anti-reflection layer are sequentially formed; The perovskite layer is formed on a surface of the hole transport layer facing away from the substrate layer; and the passivation layer is formed on a surface of the perovskite layer facing away from the substrate layer.
8. A perovskite solar cell, characterized in that: Manufactured using the method for manufacturing a perovskite solar cell according to any one of claims 1 to 7; The perovskite solar cell includes a single-junction perovskite cell device, a perovskite-perovskite stacked cell or a perovskite heterojunction stacked cell and other stacked cells containing a perovskite cell portion.
9. The perovskite solar cell according to claim 8, characterized in that: include: substrate layer; An i-type hydrogenated amorphous silicon layer, a P-type amorphous silicon doping layer, a first transparent electrode layer and a first metal electrode layer are sequentially stacked on one side of the substrate layer; An i-type hydrogenated amorphous silicon layer, an N-type amorphous silicon doped layer, a transparent conductive layer, a hole transport layer, a passivation layer, an electron transport layer, an electron transport layer modification layer, a second transparent conductive layer, a second metal electrode layer and an anti-reflection layer are sequentially stacked on the other side of the substrate layer; The perovskite layer is located between the hole transport layer and the passivation layer.
10. The perovskite solar cell according to claim 9, characterized in that: The first transparent conductive layer comprises ITO conductive glass or FTO conductive glass; The second transparent conductive layer comprises ITO conductive glass or FTO conductive glass; The material of the passivation layer includes phenylethylamine iodide or ethylamine iodide; The material of the first metal electrode layer includes one of Au, Ag, Cu, Cu-Al alloy, and C; The material of the second metal electrode layer includes one of Au, Ag, Cu, Cu-Al alloy and C.
Citation Information
Cited By
Manufacturing method for perovskite solar cell and perovskite solar cell
EP4734728A1
Manufacturing method for perovskite solar cell and perovskite solar cell
WO2026031579A1