Catalyst for preparing neopentyl glycol and preparation method thereof
By using a catalyst composed of support, fiber-based binder and CuO/SiO2 under high temperature and high pressure conditions, the problem of insufficient catalyst strength and stability is solved, the yield and process stability of neopentyl glycol are improved, and the catalyst is realized Maintain activity and improve production efficiency.
Patent Information
- Application Number
- CN202480002126.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2024-02-14
- Filing Date
- 2024-02-15
- Publication Date
- 2024-11-22
AI Technical Summary
In the prior art, when preparing neopentyl glycol under high temperature and high pressure conditions, the strength and stability of the catalyst are insufficient, resulting in process stability and catalyst support elution problems, affecting production efficiency.
Using a catalyst composed of a carrier, a fiber-based binder and CuO/SiO2, XRD analysis ensures that the weight ratio of Cu to Si is in the range of 30:70 to 70:30, and the CuO content is 5-40 parts by weight, and is coated with aqueous alcohol solution. The support is coated to improve the strength and reactivity of the catalyst.
Even under high temperature and high pressure conditions, the catalyst activity is maintained, which improves the yield and process stability of neopentyl glycol, extends the catalyst life and reduces the preparation cost.
Smart Images

Figure CN119013097A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to a catalyst for preparing neopentyl glycol and a method for preparing the catalyst.
[0002] This application claims priority to and the benefits of Korean Patent Applications No. 10-2023-0028645 and No. 10-2024-0020773 filed in the Korean Intellectual Property Office on March 3, 2023 and February 14, 2024, respectively, the entire contents of which are incorporated into this specification by reference. Background Art
[0003] Neopentyl glycol (NPG) is a white crystalline material with a melting point above 130°C. It is used as an important intermediate for various synthetic resins and is also widely used in industry as a raw material for various plastic powder coatings, synthetic lubricants, plasticizers, surfactants, fiber processing agents, etc.
[0004] Such NPG is usually prepared by reacting isobutylaldehyde with formaldehyde to produce hydroxypivalaldehyde (HPA), and then reacting the HPA with hydrogen in the presence of a catalyst. In this case, the reaction is carried out under high temperature (above 130° C.) and high pressure (above 35 bar) in the presence of a copper-based catalyst in order to obtain a high yield.
[0005] Since the reaction is carried out under such high temperature and high pressure conditions, a problem of reduced strength of the catalyst may occur. When the strength of the catalyst is reduced, this may cause problems in terms of process stability.
[0006] Furthermore, since the reaction is carried out under high temperature and high pressure conditions, the catalyst support components are eluted, so that the catalyst may be physically crushed, increasing the pressure difference in the reactor and making the production process impossible.
[0007] Therefore, efforts are being made to develop a catalyst having improved catalyst stability and excellent catalyst activity due to excellent catalyst strength even under high temperature and high pressure conditions. In addition, efforts are being made to develop a technology capable of preventing elution of the catalyst support.
[0008] [Citation List] (Patent Document 1) Korean Patent Application Laid-Open No. 10-2011-0038324 Summary of the invention
[0009] Technical issues
[0010] The present invention is directed to providing a catalyst for preparing neopentyl glycol having excellent catalyst strength and catalyst activity and a method for preparing the catalyst.
[0011] Technical Solution
[0012] An exemplary embodiment of the present invention provides a catalyst for preparing neopentyl glycol (NPG), comprising: a carrier; a fiber-based binder; and CuO and SiO2, wherein the weight ratio of Cu to Si is 30:70 to 70:30, and based on 100 parts by weight of the catalyst for preparing neopentyl glycol, the catalyst for preparing neopentyl glycol comprises 5 to 40 parts by weight of CuO through XRD analysis.
[0013] An exemplary embodiment of the present invention provides a method for preparing a catalyst for preparing neopentyl glycol, the method comprising: preparing a coprecipitate comprising a copper (Cu) precursor and a silicon dioxide (SiO2) sol; drying the coprecipitate; preparing a coating powder by adding a fiber-based binder to the dried coprecipitate; and coating a carrier with the coating powder using an alcohol aqueous solution, wherein the catalyst for preparing neopentyl glycol is the above-mentioned catalyst for preparing neopentyl glycol.
[0014] Beneficial Effects
[0015] The catalyst for preparing neopentyl glycol according to the present invention can maintain the activity of the catalyst even in a high temperature and high pressure reaction due to the excellent strength, reactivity and stability of the catalyst, and thus the stability of the process for preparing neopentyl glycol can be improved. That is, since the process can be carried out for a long time, the productivity can be improved.
[0016] Since the catalyst for preparing neopentyl glycol according to the present invention has excellent catalyst activity, when neopentyl glycol is prepared using the catalyst, the yield of neopentyl glycol is high. BRIEF DESCRIPTION OF THE DRAWINGS
[0017] Figure 1 1 is a photographed image showing the catalyst of Example 1. DETAILED DESCRIPTION
[0018] Hereinafter, the present invention will be described in detail so that those skilled in the art to which the present invention pertains can easily implement the present invention. However, the present invention can be implemented in various different forms and is not limited to the configurations described in this specification.
[0019] In the present specification, when a part “comprises” one component, unless otherwise specifically described, this does not mean excluding another component but means that another component may be further included.
[0020] In the present specification, "p to q" or "p~q" means "p or more and q or less".
[0021] In this specification, "Dn" refers to particle size distribution, which refers to the particle size at the n% point of the cumulative distribution of the number of particles according to the particle size. That is, D50 is the particle size (average particle size) at the 50% point of the cumulative distribution of the number of particles according to the particle size, D90 is the particle size at the 90% point of the cumulative distribution of the number of particles according to the particle size, and D10 is the particle size at the 10% point of the cumulative distribution of the number of particles according to the particle size. At the same time, the particle size distribution can be measured using a laser diffraction method. Specifically, after the powder to be measured is dispersed in a dispersion medium, the particle size distribution is calculated by introducing the obtained dispersion into a commercially available laser diffraction particle size measuring device (e.g., Microtrac S3500) to measure the difference in diffraction patterns according to the particle size when the particles pass through the laser beam.
[0022] In this specification, "fiber-based adhesive" refers to an adhesive containing fiber materials, specific types of which will be described below.
[0023] Furthermore, in describing the present invention, detailed descriptions of related known technologies that may unnecessarily obscure the gist of the present invention will be omitted.
[0024] An exemplary embodiment of the present invention provides a catalyst for preparing neopentyl glycol (NPG), comprising: a carrier; a fiber-based binder; and CuO and SiO2, wherein the weight ratio of Cu to Si is 30:70 to 70:30, and based on 100 parts by weight of the catalyst for preparing neopentyl glycol, the catalyst for preparing neopentyl glycol comprises 5 to 40 parts by weight of CuO through XRD analysis.
[0025] That is, the catalyst for preparing neopentyl glycol according to the present invention is a copper-based catalyst for preparing neopentyl glycol.
[0026] Furthermore, the catalyst for producing neopentyl glycol according to the present invention corresponds to a coated catalyst in which a carrier is coated with a catalyst component.
[0027] In order to obtain the weight ratio of Cu to Si, the content (weight %) of Cu can be measured by inductively coupled plasma emission spectrometer (ICP-OES) analysis. More specifically, the content can be measured using an Optima8300DV device manufactured by Perkin Elmer Inc. After obtaining the content of Cu using the following mathematical formula 1, the content of Si can be obtained using the following mathematical formula 2.
[0028] [Mathematical formula 1]
[0029] Copper content (weight %) = concentration to be measured (μg / mL) × (dilution volume of catalyst (mL) / weight (μg)) × 100
[0030] [Mathematical formula 2]
[0031] Si content (weight %) = 100 weight % - Cu content (weight %)
[0032] The catalyst for preparing neopentyl glycol according to the present invention can improve the strength, reactivity and stability of the catalyst by including a carrier and a fiber-based binder. In other words, the catalyst for preparing neopentyl glycol according to the present invention can maintain the activity of the catalyst even in high temperature and high pressure reactions due to the excellent strength, reactivity and stability of the catalyst. In addition, since the catalyst for preparing neopentyl glycol according to the present invention has a weight ratio of Cu to Si and excellent activity of the catalyst by including CuO within the above content range, there is an advantage that when the catalyst is used to prepare neopentyl glycol, the yield of neopentyl glycol is high.
[0033] In an exemplary embodiment of the present invention, the catalyst for preparing neopentyl glycol may include 5 to 40 parts by weight, preferably 10 to 35 parts by weight, more preferably 10 to 30 parts by weight, and still more preferably 5 to 20 parts by weight of CuO, based on 100 parts by weight of the catalyst for preparing neopentyl glycol by XRD analysis.
[0034] As described above, when the weight ratio of Cu to Si and the content of CuO satisfy the above ranges, the catalyst for preparing neopentyl glycol according to the present invention has even better catalyst activity, so that the yield of neopentyl glycol can be increased when the catalyst is used to prepare neopentyl glycol.
[0035] In an exemplary embodiment of the present invention, the catalyst for preparing neopentyl glycol may include CuO / SiO2, CuO / BaO / SiO2, CuO / ZnO / SiO2, CuO / Al2O3 / SiO2, CuO / MnO / SiO2 or CuO / Cr2O3 / SiO2, but is not limited thereto. That is, the catalyst for preparing neopentyl glycol according to the present invention is a copper-based catalyst for preparing neopentyl glycol.
[0036] In an exemplary embodiment of the present invention, the fiber-based binder may be one or more selected from glass fiber, carbon fiber, aramid fiber, alumina fiber, silicon carbide fiber, and boron fiber. When the fiber-based binder is included, there is an effect of easily improving the strength of the catalyst by bonding to the carrier and improving the reactivity by increasing the degree of dispersion of copper.
[0037] In an exemplary embodiment of the present invention, the carrier may have a mass of 600 kg / m 3 Up to 1500kg / m 3 The packing density.
[0038] In an exemplary embodiment of the present invention, the carrier may have a strength of 30N to 250N, preferably 40N to 200N.
[0039] In an exemplary embodiment of the present invention, the carrier may have a mass of 600 kg / m 3 Up to 1,500kg / m 3 , preferably 700kg / m 3 Up to 1,400kg / m 3 The packing density.
[0040] In an exemplary embodiment of the present invention, the support may include zirconium oxide, aluminum silicate oxide, silicon oxide, or aluminum oxide.
[0041] When the carrier satisfies the above-mentioned strength and packing density or includes an oxide type, there is an effect of satisfying both the above-mentioned catalyst reactivity and catalyst stability at the same time.
[0042] In this specification, "strength" refers to the desorption strength of a single catalyst, specifically, FGN-50B manufactured by SHIMPO, calculated by the average of 20 maximum desorption strengths at the initial collapse point. That is, in the present invention, strength may refer to the strength measured by the above-mentioned measurement method.
[0043] In this specification, "packing density" is a value calculated by measuring the apparent density, specifically, a value obtained by measuring the weight of an empty measuring cylinder, filling the measuring cylinder with 100cc of the molded catalyst, measuring the weight, and dividing the weight difference by the volume of the molded catalyst. That is, in the present invention, the packing density may refer to the apparent density measured by the above-mentioned measurement method.
[0044] In an exemplary embodiment of the present invention, the shape of the carrier may be a spherical shape, a cylindrical shape, a flat surface type, etc., but is not limited thereto.
[0045] In an exemplary embodiment of the present invention, the carrier may be a spherical carrier, and the spherical carrier may have an average particle diameter of 3 mm to 7 mm.
[0046] In an exemplary embodiment of the present invention, the spherical carrier may have an average particle size of 3 to 7 mm, preferably 3 to 5 mm. As described above, the average particle size refers to a particle size (D50) at a 50% point of the cumulative distribution of the number of particles depending on the particle size.
[0047] When the spherical carrier meets the above average particle size range, it has the effect of further improving the reactivity and stability of the above catalyst.
[0048] An exemplary embodiment of the present invention provides a method for preparing a catalyst for preparing neopentyl glycol, the method comprising: preparing a coprecipitate comprising a copper (Cu) precursor and a silicon dioxide (SiO2) sol; drying the coprecipitate; preparing a coating powder by adding a fiber-based binder to the dried coprecipitate; and coating a carrier with the coating powder using an alcohol aqueous solution, wherein the catalyst for preparing neopentyl glycol is the above-mentioned catalyst for preparing neopentyl glycol. For reference, silicon dioxide corresponds to another expression of silicon dioxide.
[0049] In an exemplary embodiment of the present invention, the copper precursor may be Cu(NO 3 ) 2 ·3H 2 O, but is not limited thereto.
[0050] In an exemplary embodiment of the present invention, the coprecipitate may further include sodium hydroxide. Sodium hydroxide may be used as a precipitant to prepare the coprecipitate.
[0051] The method for preparing a catalyst for preparing neopentyl glycol according to an exemplary embodiment of the present invention may further include preparing an alcohol aqueous solution. The type and content of the alcohol aqueous solution described below may be used.
[0052] The method for preparing a catalyst for preparing neopentyl glycol according to an exemplary embodiment of the present invention may further include filtering and washing the coprecipitate before drying the coprecipitate. The washing may be performed with distilled water.
[0053] In an exemplary embodiment of the present invention, the content of the fiber-based binder may be 5 to 20 parts by weight, preferably 5 to 15 parts by weight, based on 100 parts by weight of the coprecipitate. The above content may be suitable for the type of the fiber-based binder, and when the fiber-based binder in the coprecipitate satisfies the above content, the fiber-based binder may be more easily bonded to the carrier and the activity of the catalyst may be improved.
[0054] In an exemplary embodiment of the present invention, the drying of the coprecipitate may be performed at a temperature of 80 to 120° C. for 12 to 48 hours, but is not limited thereto, and the temperature and time conditions may be changed according to the total amount of the coprecipitate. A drying oven may be used for drying.
[0055] In an exemplary embodiment of the present invention, preparing the coating powder by adding the fiber-based binder to the dried coprecipitate may include: pulverizing the material in which the fiber-based binder is added to the dried coprecipitate; and preparing the powder by classifying the pulverized material.
[0056] In an exemplary embodiment of the present invention, the classification range of the powder may be 5 μm to 100 μm, preferably 5 μm to 85 μm. In this specification, classification refers to dividing powders / particles having the same density into two or more particle groups according to particle size. That is, the classification range of the powder means that the particle size of the powder is 5 μm to 100 μm, preferably 5 μm to 85 μm, and the powder can be classified according to the diameter. When the above classification range is met, it is easier to enhance the activation of the catalyst.
[0057] In an exemplary embodiment of the present invention, coating a carrier with a coating powder using an alcohol aqueous solution may include: introducing the carrier into a sugar coating machine; and spraying the coating powder and the alcohol aqueous solution onto the carrier while rotating the sugar coating machine, but is not limited thereto, and any method may be used as long as it can coat the carrier with the coating powder and the alcohol aqueous solution.
[0058] In an exemplary embodiment of the present invention, the alcohol aqueous solution may be an aqueous solution including one or more selected from methanol, ethanol, and isopropanol.
[0059] In an exemplary embodiment of the present invention, the concentration of the alcohol aqueous solution may be 0.1 parts by weight to 80 parts by weight of alcohol based on 100 parts by weight of the alcohol aqueous solution.
[0060] The method of preparing a catalyst for preparing neopentyl glycol according to an exemplary embodiment of the present invention may further include: drying the carrier coated with the coating powder; and calcining the dried carrier coated with the coating powder.
[0061] In an exemplary embodiment of the present invention, the drying of the carrier coated with the coating powder may be performed at a temperature of 80° C. to 120° C. for 6 to 24 hours, but is not limited thereto, and the temperature and time conditions may vary depending on the total amount of the coating powder and the alcohol aqueous solution and the size of the carrier. However, the drying time of the carrier may be shorter than the drying time of the coprecipitate. Even in this case, a drying oven may be used for drying.
[0062] In an exemplary embodiment of the present invention, the calcination of the dried carrier coated with the coating powder may be performed at a temperature of 250° C. to 650° C. for 2 to 8 hours. A calcination furnace may be used for the calcination.
[0063] In an exemplary embodiment of the present invention, the calcination of the dried support coated with the coating powder may be performed at a temperature of 250°C to 650°C, preferably 250°C to 450°C.
[0064] In an exemplary embodiment of the present invention, the calcination of the dried support coated with the coating powder may be performed for 2 hours to 8 hours, preferably 3 hours to 5 hours.
[0065] In an exemplary embodiment of the present invention, the calcination of the dried support coated with the coating powder may be performed in an air atmosphere.
[0066] An exemplary embodiment of the present invention provides a method for preparing neopentyl glycol, the method comprising introducing a hydroxypivalaldehyde (HPA) solution and hydrogen into a hydrogenation reactor for a hydrogenation reaction, wherein the hydrogenation reactor comprises a catalyst for preparing neopentyl glycol according to the present invention.
[0067] In an exemplary embodiment of the present invention, the method for preparing neopentyl glycol may be a method known in the art except for including the catalyst for preparing neopentyl glycol according to the present invention.
[0068] For example, the hydrogenation reactor may be a fixed bed reactor (FBR) filled with a catalyst for preparing neopentyl glycol, in which case the catalyst and the reaction product do not need to be separated, and since the reaction temperature and the reaction pressure can be lowered compared to the prior art, the hydrogenation reactor can be operated stably and economically, and since the catalyst is easy to replace and the scale of the reactor can be reduced, there is an effect of significantly reducing investment costs.
[0069] In an exemplary embodiment of the present invention, the hydroxypivalaldehyde solution may include 50 to 80 wt % of hydroxypivalaldehyde, 1 to 5 wt % of neopentyl glycol, 15 to 35 wt % of alcohol, 1 to 10 wt % of water, and 1 to 10 wt % of hydroxypivalylhydroxypivalate (hereinafter, HPNE), in which case, since the reaction heat can be minimized without reducing the reactivity, there is an effect of suppressing the generation of by-products.
[0070] Furthermore, in an exemplary embodiment of the present invention, the hydrogenation reaction may be performed at a reaction temperature of 100°C to 250°C, preferably 100°C to 200°C, and more preferably 100°C to 180°C.
[0071] In addition, in an exemplary embodiment of the present invention, the hydrogenation reaction may be performed at a reaction pressure of 35 bar or more. The reaction pressure refers to a measured pressure.
[0072] When the catalyst for preparing neopentyl glycol according to an exemplary embodiment of the present invention is applied to the preparation of neopentyl glycol, it is possible to prevent the problem that the catalyst component (eg, copper component) in the neopentyl glycol solution to be prepared is eluted.
[0073] Therefore, when the catalyst for preparing neopentyl glycol according to an exemplary embodiment of the present invention is applied to the preparation of neopentyl glycol, a purification process due to elution of the catalyst component (e.g., copper component) is not required, and the catalyst life is extended, thereby obtaining an effect of being able to reduce the preparation cost. [Specific implementation method]
[0075] Hereinafter, the present invention will be described in detail with reference to the embodiments for specifically describing the present invention. However, embodiments according to the present invention may be modified in various forms, and should not be construed as limiting the scope of the present invention to the embodiments described in detail below. Embodiments of the present invention are provided to more fully illustrate the present invention to those of ordinary skill in the art.
[0076] <Example 1>
[0077] A coprecipitate in the form of slurry was prepared by introducing silica sol and NaOH into a Cu(NO3)2·3H2O aqueous solution for coprecipitation, so that the weight ratio of Cu to Si satisfied Cu:Si=40:60. The coprecipitate in the form of slurry was filtered and washed with distilled water to obtain a cake-like coprecipitate. The coprecipitate cake was dried in an oven at a temperature of 80°C for 15 hours.
[0078] Subsequently, based on the total weight of the dried coprecipitate cake, 7% by weight of ceramic wool corresponding to a fiber-based adhesive is added to the dried coprecipitate cake. After adding the ceramic wool, the coprecipitate cake to which the ceramic wool is added is crushed to prepare a mixed powder (coating powder) classified as less than 45 μm. Afterwards, in order to coat the carrier described below with the mixed powder, the mixed powder, isopropyl alcohol (IPA) and water are mixed to prepare a mixed solution. Here, ceramic wool refers to a fiber-based adhesive that is formed into a roll by stacking ceramic fibers and sewing and punching the layers.
[0079] After that, alumina balls with a size of 3.2 mm (strength of about 150 N) corresponding to the carrier were placed in the chamber, and the alumina balls were coated with the mixed solution while spraying the mixed solution. In this case, the coating thickness was 2 to 4 mm. For reference, the coating thickness refers to a calculated value obtained by subtracting the size of the alumina balls from the size of the catalyst for preparing neopentyl glycol and dividing it by 2.
[0080] After the alumina balls are completely coated, the alumina balls coated with the mixed solution are dried at 80°C for 7 hours using an oven, and the dried alumina balls coated with the mixed solution are calcined in a calcination furnace at a temperature of 250°C to 550°C for 8 hours to prepare the catalyst for preparing neopentyl glycol in Example 1.
[0081] Figure 1is a photographic image showing the catalyst of Example 1 prepared by this method.
[0082] <Example 2 to Example 9 and Comparative Examples 1 to Comparative Examples 4, 7 and 8>
[0083] The catalysts for preparing neopentyl glycol in Examples 2 to 9 and Comparative Examples 1 to 4, 7 and 8 were prepared in the same manner as in Example 1, except that in Example 1, a coprecipitate was prepared, a mixed powder was used, and alumina ball coating was performed so that the weight ratio of Cu to Si, the type of fiber-based adhesive, the amount of powder used and the coating thickness satisfied the requirements of Table 1 below.
[0084] <Comparative Example 5>
[0085] Powder was prepared in the same manner as in Example 1, except that only Cu(NO3)2·3H2O was used and a fiber-based binder (quartz wool) was not used in Example 1. Thereafter, in order to coat a support described below with the powder, the powder, isopropyl alcohol (IPA) and water were mixed to prepare a mixed solution. In this case, it is referred to as powder rather than mixed powder in the sense that a fiber-based binder is not used.
[0086] Subsequently, an alumina ball having a size of 3.2 mm (strength of about 150 N) corresponding to the carrier was placed in the chamber, and the alumina ball was coated with a mixed solution containing only Cu(NO3)2·3H2O while spraying a mixed solution containing only Cu(NO3)2·3H2O. In this case, the coating thickness was 0.3 mm to 1 mm.
[0087] Afterwards, the alumina balls coated with the mixed solution containing only Cu(NO3)2·3H2O were dried at 80°C for 7 hours using an oven, and the dried alumina balls coated with the mixed solution were calcined in a calcination furnace at a temperature of 250°C to 550°C for 8 hours to prepare the catalyst for preparing neopentyl glycol of Comparative Example 1.
[0088] <Comparative Example 6>
[0089] A catalyst for preparing neopentyl glycol of Comparative Example 6 was prepared in the same manner as in Example 1, except that hydroxypropylmethylcellulose (HPMC) was used instead of the ceramic wool in Example 1. Hydroxypropylmethylcellulose (HPMC) is not a fiber-based binder but a material corresponding to an organic binder.
[0090] The catalysts for preparing neopentyl glycol of Examples 1 to 9 and Comparative Examples 1 to 8 were analyzed by XRD to measure the content of CuO, and the results are shown in the following Table 1. In this case, in order to measure the content of CuO by performing XRD analysis, the diffraction angle (2θ) of the CuK-α characteristic X-ray wavelength was measured by X-ray diffraction (XRD) analysis.
[0091] More specifically, as a quantitative spike during measurement of the CuO content, MgO heat-treated at 800° C. for 5 hours was introduced at arbitrary contents (5 wt %, 10 wt %, and 20 wt %) to calculate the relative contents of crystalline CuO and amorphous Cu-silicate.
[0092] In addition, the types of materials used in the catalysts for preparing neopentyl glycol in Examples 1 to 9 and Comparative Examples 1 to 8, the weight ratio of Cu to Si (Cu:Si), coating thickness, and the amount of powder used are also shown in Table 1 below.
[0093] <Reference Example 1>
[0094] In order to evaluate the performance of the catalyst for preparing neopentyl glycol of Examples 1 to 9 and Comparative Examples 1 to 8, an existing extruded catalyst (CuO / SiO2, having a CuO content of 40 wt%) was prepared. The catalyst of Reference Example 1 was prepared in the same manner as Example 1, up to the process of preparing the coprecipitate cake using a coprecipitate having a Cu:Si weight ratio of Cu to Si of 40:60 and a fiber-based binder, and finally using an extruder to prepare a catalyst having a size of 5 mm x 5 mm without coating a carrier.
[0095] <Reference Example 2>
[0096] In order to evaluate the performance of the catalyst for preparing neopentyl glycol of Examples 1 to 9 and Comparative Examples 1 to 8, a conventional tablet catalyst (CuO / SiO2, having a CuO content of 40 wt%) was prepared. The catalyst of Reference Example 2 was prepared in the same manner as in Example 1, up to the process of preparing the coprecipitate cake using a coprecipitate having a Cu:Si weight ratio of Cu to Si of 40:60 and a fiber-based binder, and finally using a tablet press to prepare a catalyst having a size of 5 mm x 5 mm without coating a carrier.
[0097] Information on the catalysts used for preparing neopentyl glycol in Reference Examples 1 and 2 is also shown in the following Table 1. For reference, the type of alumina balls is the same, and therefore, the alumina balls are not shown in the following Table 1.
[0098] In order to obtain the weight ratio of Cu to Si (Cu:Si in Table 1 below), the content of Cu can be measured by inductively coupled plasma emission spectrometer (ICP-OES) analysis. The content of Cu is measured using the Optima 8300DV device manufactured by PerkinElmer Inc. Specifically, the measured catalyst and nitric acid are added to a platinum crucible and then diluted to a concentration of 10M with ultrapure water. Afterwards, the content of Cu is calculated according to the following mathematical formula 1. Afterwards, the content of Si is obtained according to the following mathematical formula 2.
[0099] [Mathematical formula 1]
[0100] Copper content (weight %) = concentration to be measured (μg / mL) × (dilution volume of catalyst (mL) / weight of catalyst (μg)) × 100
[0101] [Mathematical formula 2]
[0102] Si content (weight %) = 100 weight % - Cu content (weight %)
[0103] [Table 1]
[0104]
[0105] In Table 1 above, the materials described in parentheses with respect to the catalyst types refer to the type of binder used, and Cu:Si refers to the weight ratio of Cu to Si in the coprecipitate or catalyst.
[0106] In this case, Reference Example 1 corresponds to an extruded catalyst, and Reference Example 2 corresponds to a tableted catalyst, respectively.
[0107] In addition, the CuO content indicates the CuO content in the catalyst, and as for the coating thickness, as described above, the coating thickness refers to a calculated value obtained by subtracting the size of the alumina balls from the size of the catalyst for preparing neopentyl glycol and dividing it by 2, and the amount of powder used refers to a relative amount (%) when the amount used (based on mass) of Example 1 is defined as 1 (100%).
[0108] In the case of Comparative Example 5, only the copper precursor was used, and Reference Examples 1 and 2 correspond to existing extruded catalysts and tableted catalysts, and thus the amount of powder used is not described.
[0109] <Experimental Example 1>
[0110] Neopentyl glycol was produced using a fixed bed reactor (FBR) filled with each of the catalysts for producing neopentyl glycol of Reference Examples 1 and 2, Examples 1 to 9, and Comparative Examples 1 to 8. Specifically, a reaction raw material consisting of 65 wt % of hydroxypivalaldehyde (HPA), 2 wt % of neopentyl glycol (NPG), 25 wt % of 2-isopropylethanol (2-EH), 5 wt % of water (HO), and 3 wt % of HPNE was used, and a hydrogenation reaction was carried out in an air atmosphere at a temperature of 160° C. and a pressure of 35 bar for 1 hour.
[0111] In this case, the amount of consumed hydrogen was measured to determine the catalyst activity of each of the catalysts for preparing neopentyl glycol of Reference Examples 1 and 2, Examples 1 to 9, and Comparative Examples 1 to 8.
[0112] The results are shown in Table 2 below.
[0113] <Experimental Example 2>
[0114] The Si content of each of the catalysts for preparing neopentyl glycol of Reference Examples 1 and 2, Examples 1 to 9, and Comparative Examples 1 to 8 was measured by intensity and ICP-OES analysis.
[0115] For the stability test, the catalysts for preparing neopentyl glycol of Reference Examples 1 and 2, Examples 1 to 9 and Comparative Examples 1 to 8 were immersed in the liquid reaction raw material of Experimental Example 1 and reacted in a hydrogen atmosphere at a temperature of 180° C. for 6 hours.
[0116] As another form of stability test, the catalysts for preparing neopentyl glycol of Reference Examples 1 and 2, Examples 1 to 9, and Comparative Examples 1 to 8 were immersed in a neopentyl glycol solution and reacted in a hydrogen atmosphere at a temperature of 180° C. for 18 hours.
[0117] Thereafter, the strengths of the catalysts for preparing neopentyl glycol of Reference Examples 1 and 2, Examples 1 to 9, and Comparative Examples 1 to 8 after the reaction were measured and compared with the strengths of the catalysts measured before the reaction to confirm the difference.
[0118] Afterwards, after the stability test reaction under the reaction raw material conditions of Experimental Example 1, the Si content of the catalyst for preparing neopentyl glycol of Reference Example 1 and Reference Example 2, Examples 1 to 9, and Comparative Examples 1 to 8 was measured by ICP-OES analysis, and compared with the Si content of the catalyst measured before the reaction to confirm the difference.
[0119] The results are shown in Table 2 below.
[0120] [Table 2]
[0121]
[0122] In the above Table 2, Si elution (%) is a value calculated as follows: [{Si content (weight) of initial catalyst (before reaction) - Si content (weight) of catalyst after stability test (after reaction)} / Si content (weight) of initial catalyst (before reaction)]×100.
[0123] In addition, the catalyst activity is a value indicating the relative catalyst activity when the catalyst activity (unit: mL / min·catalyst mL) of Example 1 is set to 1 as a reference (100%). That is, for example, when the catalytic activity of Example 1 is 100 mL / min·catalyst mL, this means that the catalyst activity of Example 2 is 119 mL / min·catalyst mL. In addition, the examples are arbitrary values and do not mean the activity values of actual catalysts.
[0124] From the results in Table 2, it can be confirmed that the catalysts for preparing neopentyl glycol of Examples 1 to 9 have excellent catalyst activity as coated catalysts when compared with the extruded catalyst of Reference Example 1 and the tableted catalyst of Reference Example 2.
[0125] In addition, it can be confirmed that the catalysts for preparing neopentyl glycol of Examples 1 to 9 used as coated catalysts have fresh strength similar to that of the extruded catalyst of Reference Example 1 and the tableted catalyst of Reference Example 2, and show small strength changes and Si elution amounts after the stability test. Small strength changes and small Si elution amounts mean that the catalyst has excellent physical stability. That is, this means that the durability of the catalyst is improved, which has the advantage of being able to improve the stability of the catalyst process and the service life of the catalyst.
[0126] In addition, the catalysts for preparing neopentyl glycol in Examples 6 and 7 are coated catalysts using carbon fiber and alumina fiber as fiber-based binders, respectively, and physical stability was confirmed by confirming that the catalysts had similar fresh strength and low Si elution amount as the coated catalyst using ceramic wool as fiber-based binder in Example 1. That is, this means that the binder is not limited to ceramic wool as long as the binder is an available fiber-based binder and exhibits the desired effect.
[0127] Furthermore, it can also be confirmed that Comparative Examples 1 to 3 and Comparative Examples 5 to 8 are physically unstable compared to the embodiment.
[0128] Specifically, Comparative Example 1 is a case where the weight of Cu in the coprecipitate is lower than the weight of Si as in the example, but the specific weight ratio of Cu to Si in the coprecipitate does not satisfy the weight ratio of the catalyst for preparing neopentyl glycol according to the present invention, and it can be confirmed that when it is necessary to load the same content of copper as in Example 1 to ensure the performance of the catalyst, the coating thickness must be very thick. When the coating thickness becomes very thick, the physical stability of the catalyst will deteriorate. That is, since the catalyst of Comparative Example 1 does not have good catalyst durability, there is a problem of reduced stability of the catalyst process operation and reduced service life of the catalyst.
[0129] Comparative Examples 2 and 3 are cases where the weight ratio of Cu to Si of the catalyst for preparing neopentyl glycol according to the present invention is satisfied, but the content of CuO deviates from that of the catalyst for preparing neopentyl glycol, and it can be confirmed that the catalyst activity is not good even after the stability test, and the change in strength and the elution amount of Si are also large.
[0130] Comparative Example 4 is a case where the weight of Cu in the coprecipitate is greater than the weight of Si, and even in this case, it can be confirmed that the catalyst activity is not good. It can be determined that the activity is reduced because the particle size of Cu, which is known to be an active material in hydrogenation reactions, becomes larger than that in the examples.
[0131] Unlike the catalysts for preparing neopentyl glycol using a coprecipitate containing Cu and Si in Examples 1 to 9, Comparative Example 5 is a catalyst for preparing neopentyl glycol prepared by coating a material containing only Cu. That is, Comparative Example 5 also corresponds to a coated catalyst.
[0132] However, when the same comparison was performed under the conditions of Experimental Example 1, it was confirmed that Comparative Example 5 showed no catalytic activity. This was determined to be due to the following effect: for the catalyst (coated catalyst) for preparing neopentyl glycol in the examples, the particle size growth of Cu, which is known to be an active material in the hydrogenation reaction, was regulated by Si. That is, in Comparative Example 5, as in Comparative Example 4, it was determined that the particle size of Cu became large enough to have no catalytic activity.
[0133] Similar to the catalysts for preparing neopentyl glycol in Examples 1 to 9, Comparative Example 6 is a coated catalyst prepared using a coprecipitate containing Cu and Si, and it can be confirmed that the catalyst activity is similar to that in the examples, but the coating strength is too weak to use the catalyst in the catalytic process. Comparative Example 6 is a case where a fiber-based binder is not used, and it can be confirmed that, as in the catalyst for preparing neopentyl glycol according to the present invention, the use of a fiber-based binder is effective in increasing the strength (durability) of the catalyst.
[0134] Furthermore, the catalysts for preparing neopentyl glycol in Comparative Examples 7 and 8 were coated catalysts using carbon fiber and alumina fiber as fiber-based binders, respectively, and were prepared in the same manner as the coated catalyst using ceramic wool in Comparative Example 1, and although the fiber-based binder was changed, the fresh strength was low and Si elution occurred at a high rate as in Comparative Example 1. That is, this means that even if the type of fiber-based binder used is changed, when the Cu:Si ratio of the coprecipitate deviates from the appropriate range, the effect of improving physical stability by the fiber-based binder cannot be ensured.
[0135] That is, since the catalyst for preparing neopentyl glycol according to the present invention can maintain the activity of the catalyst even in high temperature and high pressure reactions due to the excellent strength, reactivity and stability of the catalyst, it can be confirmed that the stability of the process for preparing neopentyl glycol can be improved and the activity of the catalyst is excellent.
[0136] As a result, when the catalyst for preparing neopentyl glycol according to the present invention is used, the process can be performed for a long time and the yield of neopentyl glycol can be increased, thereby confirming an advantage of being able to improve productivity.
Claims
1. A catalyst for preparing neopentyl glycol (NPG), comprising: Carrier; Fiber-based adhesives; and CuO and SiO2, in, The weight ratio of Cu to Si is 30:70 to 70:30, According to XRD analysis, the catalyst for preparing neopentyl glycol includes 5 to 40 parts by weight of CuO based on 100 parts by weight of the catalyst.
2. The catalyst according to claim 1, wherein The catalyst includes CuO / SiO2, CuO / BaO / SiO2, CuO / ZnO / SiO2, CuO / Al2O3 / SiO2, CuO / MnO / SiO2 or CuO / Cr2O3 / SiO2.
3. The catalyst according to claim 1, wherein The fiber-based binder is one or more selected from glass fiber, carbon fiber, aramid fiber, alumina fiber, silicon carbide fiber and boron fiber.
4. The catalyst according to claim 1, wherein The carrier has a mass of 600 kg / m 3 Up to 1500kg / m 3 The packing density.
5. The catalyst according to claim 1, wherein The support includes zirconium oxide, aluminum silicate oxide, silicon oxide or aluminum oxide.
6. A method for preparing a catalyst for preparing neopentyl glycol, the method comprising: preparing a co-precipitate comprising a copper (Cu) precursor and a silicon dioxide (SiO2) sol; drying the coprecipitate; preparing a coated powder by adding a fiber-based binder to the dried coprecipitate; and coating a support with the coating powder using an alcohol aqueous solution, Wherein, the catalyst for preparing neopentyl glycol is the catalyst according to any one of claims 1 to 5.
7. The method according to claim 6, wherein: The fiber-based binder may be included in an amount of 5 parts by weight to 20 parts by weight based on 100 parts by weight of the coprecipitate.
8. The method according to claim 6, wherein: The preparation of a coated powder by adding a fiber-based binder to a dried coprecipitate comprises: comminuting the material wherein the fiber-based binder is added to the dried coprecipitate; and The powder is prepared by classifying the pulverized material.
9. The method according to claim 8, wherein: The powder is classified in the range of 5 μm to 100 μm.
10. The method according to claim 6, wherein: The weight ratio of copper (Cu) to silicon (Si) in the coprecipitate is 20:80 to 50:
50.
11. The method according to claim 6, wherein: The alcohol aqueous solution is an aqueous solution containing one or more selected from methanol, ethanol and isopropanol.