Spot-welded joint, method for manufacturing spot-welded joint, high-strength steel member for spot-welded joint, and method for manufacturing high-strength steel member for spot-welded joint

By forming a specific surface treatment part on the high-strength steel plate and controlling the oxygen concentration in the plastic metal ring area, the problem of spot welded joints of high-strength steel components is solved, the tensile shear strength is improved, and efficient spot welded joint manufacturing is achieved.

CN119013116AInactive Publication Date: 2024-11-22NIPPON STEEL CORPORATION
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202380023328.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-03-15
Filing Date
2023-03-15
Publication Date
2024-11-22
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

The prior art is difficult to effectively improve the tensile shear strength of the spot welded joint of a high-strength steel member with a tensile strength of 1800 MPa or a Vickers hardness of 530 HV, and the problem of embrittlement of the welded part has not been effectively solved.

Method used

By forming a specific surface treatment part on the surface of the high-strength steel plate, the oxygen concentration in the plastic metal ring region is less than 15.0 mass%, and no plating is provided during spot welding to form a spot welding joint with a melting core diameter of 4.5√t or more, a spot welding joint with a melting core diameter of 4.5√t or more is formed. , to improve the tensile shear strength of the spot welded joint.

Benefits of technology

The tensile shear strength of the spot welded joint is significantly improved, and the embrittlement of the welded part is avoided, and the excellent spot welded joint manufacturing of high-strength steel components is achieved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119013116A_ABST
    Figure CN119013116A_ABST
Patent Text Reader

Abstract

A spot-welded joint according to one embodiment of the present invention is provided with: a plurality of steel plate sections including high-strength steel plate sections having a Vickers hardness of 530 HV or more; a nugget that joins a high-strength steel sheet part among the plurality of steel sheet parts to another steel sheet part; and a plastic metal ring region which is formed in a ring shape around the nugget in a plan view viewed from a direction perpendicular to the surface of the high-strength steel plate section, and in which the high-strength steel plate section and another steel plate section are solid-bonded, and in which there is no plating layer in a region where the plastic metal ring region is present. The oxygen concentration of the plastic metal ring region at a position 50 [mu] m outside the outer periphery of the nugget in a plan view is 15.0 mass% or less.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a spot welded joint, a method for manufacturing a spot welded joint, a high-strength steel member for a spot welded joint, and a method for manufacturing a high-strength steel member for a spot welded joint.

[0002] This application claims priority based on Japanese Patent Application No. 2022-040299 filed in Japan on March 15, 2022, and the contents are incorporated herein by reference. Background Art

[0003] In the spot welded joint manufactured by spot welding a high-strength steel member, there is a problem that the joint strength of the welded portion becomes low. In particular, if the tensile strength of the high-strength steel member reaches 1800MPa or more (or the Vickers hardness of the high-strength steel member reaches 530HV or more), the tensile shear strength (TSS) of the spot welded portion is significantly reduced. It is believed that this is due to the large amount of C contained in the high-strength steel member causing the embrittlement of the welded portion.

[0004] Various studies have been conducted to improve the joining strength of spot welded joints using high-strength steel plates as base materials.

[0005] Patent document 1 discloses a spot-welded component, which is a spot-welded component formed by spot-welding a plurality of steel plates, wherein at least one of the plurality of steel plates is a high-strength cold-rolled steel plate having a tensile strength of 780 MPa or more and having no coating on the surface, and at least one of the plurality of steel plates is a zinc-plated steel plate having a zinc-plated layer on the surface, and the surface Zn concentration inside the plastic metal ring region (corona bond) of the spot weld portion is 1 mass % or more and less than 25 mass %.

[0006] Patent document 2 discloses a steel plate for spot welding, which has a tensile strength of 400 to 700 MPa, a C content in the component composition of the base material in the range of 0.05 to 0.12 mass %, a carbon equivalent Ceqt represented by the following formula {Ceqt=C+Si / 30+Mn / 20+2P+4S} in the range of 0.18 mass % to 0.22 mass %, and a carbon equivalent Ceqh represented by the following formula {Ceqh=C+Si / 40+Cr / 20} is greater than 0.08 mass %, and further, at a depth ranging from the surface to 3 μm of the steel plate, the average oxygen concentration OC (%) measured by the GDS analysis method is in the range represented by the following formula {OC≤0.5}.

[0007] Patent document 3 discloses a high-strength resistance welded joint, wherein the average composition in the nugget contains, by mass%, P: 0.03% or less, S: 0.01% or less, O: 0.02% or less, and further contains one or more of Mg, La, and Ce in a total amount of 0.005% or less, and the remainder is Fe and unavoidable impurities, the average hardness in the nugget is 320 to 500 in HV, and the distribution density of oxide-based inclusions with a particle size of 1 μm or more present in the nugget is 20 pieces / mm 2 The maximum grain size of all inclusions is 50 μm or less, and the metal structure in the nugget contains tempered martensite and lower bainite.

[0008] Prior art literature

[0009] Patent Literature

[0010] Patent Document 1: Japanese Patent Application Publication No. 2020-179413

[0011] Patent Document 2: Japanese Patent Application Publication No. 2012-102370

[0012] Patent Document 3: Japanese Patent Application Publication No. 2014-180698 Summary of the invention

[0013] Problems to be solved by the invention

[0014] However, the maximum tensile strength of the steel plate studied in Patent Document 1 is 1570 MPa. Patent Document 1 does not make any study on high-strength steel members with a tensile strength of 1800 MPa or more (or a Vickers hardness of 530 HV or more), which may cause more significant embrittlement of spot welds.

[0015] The maximum tensile strength of the steel plate studied in Patent Document 2 is 700 MPa. No research has been conducted in Patent Document 2 on high-strength steel members with a tensile strength of 1800 MPa or more (or a Vickers hardness of 530 HV or more), in which the embrittlement of the spot weld is more pronounced. In addition, Patent Document 2 seeks to improve the weld strength of the spot welded joint by adjusting the oxygen concentration of the base steel plate, but no special research has been conducted on the structure of the spot welded joint.

[0016] The Vickers hardness of the nugget disclosed in Patent Document 3 is within the range of 320 HV to 500 HV. If the nugget hardness is taken into consideration, it is estimated that the tensile strength of the steel plate studied in Patent Document 3 is lower than 1800 MPa (or the Vickers hardness is lower than 530 HV). It is estimated that no research has been conducted in Patent Document 3 on high-strength steel components with a tensile strength of 1800 MPa or more (or a Vickers hardness of 530 HV or more), which further increases the embrittlement of the spot weld.

[0017] In view of the above situation, the subject of the present invention is to provide a spot welded joint having excellent TSS despite including one or more high-strength steel plate portions having a Vickers hardness of 530 HV or more, and a method for manufacturing the same. Furthermore, the subject of the present invention is to provide a high-strength steel member for a spot welded joint capable of manufacturing a spot welded joint having excellent TSS despite having a Vickers hardness of 530 HV or more, and a method for manufacturing the same.

[0018] Means for solving problems

[0019] The gist of the present invention is as follows.

[0020] (1) A spot welding joint according to a first embodiment of the present invention comprises: a plurality of steel plate portions including a high-strength steel plate portion having a Vickers hardness of 530 HV or more; a nugget for joining the high-strength steel plate portion among the plurality of steel plate portions to the other steel plate portions; and a plastic metal ring zone, which is formed in a ring shape around the nugget in a plan view observed from a direction perpendicular to the surface of the high-strength steel plate portion, and solid-phase joins the high-strength steel plate portion to the other steel plate portions, wherein no plating layer is present in the region where the plastic metal ring zone exists, and an oxygen concentration of the plastic metal ring zone at a position 50 μm outside the outer periphery of the nugget in the plan view is 15.0 mass % or less.

[0021] (2) In the spot welded joint described in (1) above, preferably, the carbon content of the high-strength steel sheet portion exceeds 0.30 mass %.

[0022] (3) In the spot welded joint described in (1) or (2), preferably, the carbon content of the nugget is 0.29 mass % or more.

[0023] (4) Preferably, in the spot welded joint described in any one of (1) to (3), the diameter of the nugget measured along the boundary line of the adjacent steel plate parts in a cross section passing through the center of the nugget and perpendicular to the surface of the steel plate part is 4.5√t or more. Here, t refers to the smaller of the respective thicknesses of the two adjacent steel plate parts constituting the boundary line.

[0024] (5) A method for manufacturing a spot welded joint according to a second embodiment of the present invention comprises the following steps: a step of providing a high-strength steel member having a surface treated portion having a Vickers hardness of 530 HV or more; a step of overlapping a plurality of the above-mentioned steel members in a manner of arranging the above-mentioned surface treated portion on a joining surface between the above-mentioned high-strength steel member and other steel members; a step of spot welding the plurality of the above-mentioned steel members in a manner of accommodating a nugget and a plastic metal ring zone on the inner side of the above-mentioned surface treated portion in a top view observed from a direction perpendicular to the above-mentioned surface treated portion, wherein in the above-mentioned overlapping step, no plating layer is provided on the above-mentioned surface treated portion and a region in contact with the above-mentioned surface treated portion, the ten-point average roughness of the above-mentioned surface treated portion is less than 3.5 μm, and the oxygen concentration of the above-mentioned surface treated portion is less than 18.0 mass %.

[0025] (6) Preferably, the method for manufacturing a spot welded joint described in (5) above further comprises a step of forming the surface treated portion on a surface of the high-strength steel member before the step of providing the high-strength steel member.

[0026] (7) Preferably, the method for manufacturing a spot welding joint described in (6) above further comprises a step of hot stamping the high-strength steel plate before forming the above-mentioned surface treatment portion, and in the step of forming the above-mentioned surface treatment portion, the above-mentioned surface treatment portion is formed on the surface of the high-strength steel component after the above-mentioned hot stamping.

[0027] (8) Preferably, the method for manufacturing a spot welding joint described in (6) or (7) above includes a step of removing a portion of a coating on the surface of a high-strength steel member before forming the surface treatment portion, and in the step of forming the surface treatment portion, the surface treatment portion is formed in a region where the coating has been removed.

[0028] (9) In the method for producing a spot welded joint according to any one of (5) to (8) above, it is preferred that the carbon content of the high-strength steel member be set to exceed 0.30 mass %.

[0029] (10) In the method for manufacturing a spot welded joint according to any one of (5) to (9) above, it is preferred that the carbon content of the nugget formed by the spot welding be set to 0.29 mass % or more.

[0030] (11) Preferably, in the method for manufacturing a spot welded joint described in any one of (5) to (10), the diameter of the nugget formed by the spot welding is set to be 4.5√t or more. Here, the diameter of the nugget refers to the size of the nugget measured along the boundary line of the adjacent steel members in a plane passing through the center of the nugget and perpendicular to the surface of the steel member, and t refers to the smaller of the thicknesses of the two adjacent steel members constituting the boundary line.

[0031] (12) In the method for manufacturing a spot welded joint according to any one of (6) to (11) above, it is preferred that the surface treated portion is formed by shot blasting or wet blasting.

[0032] (13) The high-strength steel component for spot welding joints according to the third embodiment of the present invention has a Vickers hardness of 530 HV or more, has a surface-treated portion without a coating, has a ten-point average roughness of 3.5 μm or less, and has an oxygen concentration of 18.0 mass % or less.

[0033] (14) In the high-strength steel member for a spot welded joint described in (13) above, it is preferred that the carbon content exceeds 0.30 mass %.

[0034] (15) Preferably, in the high-strength steel member for a spot welded joint described in (13) or (14), the surface treated portion is provided on the entire surface of the high-strength steel member.

[0035] (16) The fourth embodiment of the present invention is a method for manufacturing a high-strength steel component for a spot welding joint, which comprises a step of forming a surface treatment portion on the surface of the high-strength steel component having a Vickers hardness of 530 HV or more, wherein no plating is provided on the surface treatment portion, the ten-point average roughness of the surface treatment portion is set to be less than 3.5 μm, and the oxygen concentration of the surface treatment portion is set to be less than 18.0 mass %.

[0036] (17) Preferably, the method for manufacturing a high-strength steel component for a spot welding joint described in (16) above further comprises a step of hot stamping the high-strength steel plate before forming the above-mentioned surface treatment portion, and in the step of forming the above-mentioned surface treatment portion, the above-mentioned surface treatment portion is formed on the surface of the high-strength steel component after the above-mentioned hot stamping.

[0037] (18) Preferably, the method for manufacturing a high-strength steel component for a spot welding joint described in (16) or (17) above includes a step of removing a portion of a plating layer on the surface of the high-strength steel component before forming the above-mentioned surface treatment portion, and in the step of forming the above-mentioned surface treatment portion, the above-mentioned surface treatment portion is formed in the area where the above-mentioned plating layer is removed.

[0038] (19) Preferably, in the method for manufacturing a high-strength steel member for a spot welded joint according to any one of (16) to (18), the carbon content of the high-strength steel member is set to exceed 0.30 mass %.

[0039] (20) Preferably, in the method for manufacturing a high-strength steel member for a spot welded joint according to any one of (16) to (19) above, the surface treated portion is provided on the entire surface of the high-strength steel member.

[0040] (21) Preferably, in the method for manufacturing a high-strength steel member for a spot welded joint according to any one of (16) to (20) above, the surface treated portion is formed by shot blasting or wet blasting.

[0041] Effects of the Invention

[0042] According to the present invention, a spot welded joint having excellent TSS despite including one or more high-strength steel plate portions having a Vickers hardness of 530 HV or more and a method for manufacturing the same can be provided. Furthermore, according to the present invention, a high-strength steel member for a spot welded joint capable of manufacturing a spot welded joint having excellent TSS despite having a Vickers hardness of 530 HV or more and a method for manufacturing the same can be provided. BRIEF DESCRIPTION OF THE DRAWINGS

[0043] Figure 1 It is a cross-sectional view of the spot welded joint according to the first embodiment.

[0044] Figure 2A It is a graph showing the relationship between the diameter of the weld core and the surface oxygen concentration of the plastic metal ring area.

[0045] Figure 2B It is a graph showing the relationship between the diameter of the weld core and the surface oxygen concentration of the plastic metal ring area.

[0046] Figure 3A It is a schematic diagram of the surface treatment portion forming step S1.

[0047] Figure 3B It is a schematic diagram of the step S2 of superimposing the steel members.

[0048] Figure 3C This is a schematic diagram of step S3 of spot welding a steel member. DETAILED DESCRIPTION

[0049] <Spot Welded Joint of First Embodiment>

[0050] First, a spot welding joint 1 according to a first embodiment of the present invention will be described. The spot welding joint 1 according to the first embodiment is, for example, Figure 1As shown in the cross-sectional view, it comprises: a plurality of steel plate portions 11 including a high-strength steel plate portion 11H having a Vickers hardness of 530 HV or more; a weld core 121 for joining the high-strength steel plate portion 11H among the plurality of steel plate portions 11 with the other steel plate portions 11; and a plastic metal ring zone 122, wherein the plastic metal ring zone 122 is formed in a ring shape around the weld core 121 in a top view (hereinafter referred to as the top view) observed from a direction perpendicular to the surface of the high-strength steel plate portion, and solid-phase joins the high-strength steel plate portion 11H with the other steel plate portions 11, and in the region where the plastic metal ring zone 122 is formed, there is no plating layer 13, and the oxygen concentration of the plastic metal ring zone 122 at a position 50 μm outside the outer periphery of the weld core 121 in the top view is 15.0 mass % or less. Hereinafter, the surface oxygen concentration of the plastic metal ring zone 122 formed on the surface of the high-strength steel plate portion 11H at a position 50 μm outside the outer periphery of the nugget is sometimes referred to as "surface oxygen concentration of the plastic metal ring zone" etc. In addition, the area where the plastic metal ring zone 122 exists between the high-strength steel plate portion 11H and other steel plate portions 11 is sometimes referred to as "plastic metal ring zone portion 123".

[0051] In the spot welded joint 1 of the first embodiment, TSS is improved by modifying the plastic metal ring region 122. The inventors of the present invention have found that the TSS of the spot welded joint 1 including the high-strength steel plate portion 11H having a Vickers hardness of 530 HV or more is dramatically improved by reducing the oxygen concentration in the plastic metal ring region 122 formed in the high-strength steel plate portion 11H. The spot welded joint 1 of the first embodiment will be described in detail below.

[0052] (Steel plate portion 11, high-strength steel plate portion 11H)

[0053] The details of the manufacturing method will be described below, but the spot welding joint 1 is formed by spot welding a steel member formed by forming a steel plate that becomes a base material (joint material). The steel plate portion 11 represents a flat portion on the same surface as the spot welding portion in the portion corresponding to the steel member or steel plate before spot welding in the spot welding joint 1. For example, in the case where the steel member before spot welding is a hat-shaped component, the steel plate portion 11 is a flange portion that is spot welded. Alternatively, in the case where a flat plate component is spot welded to form the spot welding joint 1, the steel plate portion 11 is the entirety of the flat plate component.

[0054] The number of the steel plate portion 11 is as follows: Figure 1As shown in the example, it can be 2 or more than 3. In addition, one or more of the multiple steel plate portions 11 is set to a high-strength steel plate portion 11H with a Vickers hardness of 530HV or more. As a result, the parent material strength of the spot welding joint 1 is greatly improved. It should be noted that there is a good correlation between the tensile strength and Vickers hardness of steel, and a Vickers hardness of 530HV is equivalent to a tensile strength of about 1800MPa. A Vickers hardness of 580HV is equivalent to a tensile strength of about 2000MPa.

[0055] According to the conventional technology, if the Vickers hardness of the steel plate portion 11 is 530 HV or more, the TSS of the spot welded joint 1 is reduced. However, in the spot welded joint 1 of the first embodiment, the TSS is ensured by reducing the oxygen concentration of the plastic metal ring region 122 described later.

[0056] The number of high-strength steel plate portions 11H is not limited. Figure 1 In the spot welded joint 1 illustrated in the example, the high-strength steel sheet portion 11H is combined with the steel sheet portion 11 having a Vickers hardness lower than 530 HV, but two high-strength steel sheet portions 11H may also be combined. Hereinafter, for convenience, the steel sheet portion 11 having a Vickers hardness lower than 530 HV is referred to as a "normal steel sheet portion 11".

[0057] (Nuclear core 121 and plastic metal ring area 122)

[0058] The nugget 121 is a molten and solidified portion generated in the weld during spot welding. The nugget 121 joins at least the high-strength steel sheet portion 11H among the plurality of steel sheet portions 11 to the other steel sheet portions 11. Preferably, the nugget 121 joins all of the plurality of steel sheet portions 11.

[0059] The plastic metal ring region 122 is an annular solid phase joint between two steel plate portions 11 located around the nugget 121 during spot welding. The plastic metal ring region 122 solid phase joins the high-strength steel plate portion 11H to the other steel plate portions 11. However, in the plastic metal ring region 122, melting and solidification of the steel plate portion 11 does not occur, and only the two steel plate portions 11 are solid phase joined.

[0060] It should be noted that in Figure 1 In the spot welding joint 1 illustrated in the figure, since there is only one overlapping surface of the steel plate portion 11, only one plastic metal ring area 122 is formed for one spot welding portion. If there are overlapping surfaces of multiple steel plate portions 11, the plastic metal ring area 122 is formed on the multiple overlapping surfaces. Hereinafter, the portion including the nugget 121 and the plastic metal ring area 122 that joins the multiple steel plate portions 11 is collectively referred to as the "spot welding portion 12".

[0061] (Oxygen concentration of plastic metal ring area 122 and presence or absence of coating)

[0062] As a result of conducting various studies on TSS of the spot welded joint 1 including the high-strength steel plate portion 11H, the inventors of the present invention found the following.

[0063] First, it was found that in the spot welded joint 1 including the high-strength steel plate portion 11H having a Vickers hardness of 530 HV or more, the plastic metal ring region 122 has a significant influence on the joint strength of the spot welded joint 1. It is inferred that a large amount of C contained in the high-strength steel plate portion 11H causes embrittlement of the welded portion and reduces the joint strength of the molten solidified portion, so that the joint strength of the plastic metal ring region 122 has a relatively significant influence on the joint strength of the spot welded joint 1.

[0064] Next, a good correlation was observed between the oxygen concentration of the plastic metal ring region 122 formed on the surface of the high-strength steel plate portion 11H and the TSS of the spot welded joint 1. The lower the oxygen concentration, the higher the TSS. It is presumed that this is because the higher the oxygen concentration of the plastic metal ring region 122, the larger the oxide of the plastic metal ring region 122, which leads to the peeling of the plastic metal ring region 122.

[0065] On the other hand, no correlation was observed between the oxygen concentration of the plastic metal ring zone and TSS between the two ordinary steel plate parts 11. For example, in a spot welded joint composed of ordinary steel plate parts 11 and not containing a high-strength steel plate part 11H, even if the oxygen concentration of the plastic metal ring zone is reduced, the TSS improvement effect cannot be obtained. It should be noted that in the previous technology of spot welded joints that do not contain a high-strength steel plate part 11H with a Vickers hardness of 530HV or more, the relationship between the oxygen concentration, oxide and TSS in the plastic metal ring zone has not been reported. It is presumed that this is because: in a spot welded joint composed of ordinary steel plate parts 11 and not containing a high-strength steel plate part 11H, the plastic metal ring zone has basically no effect on the joining strength of the spot welded joint 1.

[0066] Furthermore, in the spot welded joint 1 composed of two ordinary steel sheet portions 11 and one high-strength steel sheet portion 11H, even if the oxygen concentration in the plastic metal ring region between the two ordinary steel sheet portions 11 is reduced, the TSS improvement effect is still not obtained.

[0067] In addition, when a coating layer such as a hot-dip Zn coating layer is included in the plastic metal ring section 123 between the high-strength steel plate section 11H and the other steel plate sections 11 adjacent thereto, the TSS improvement effect due to the reduction in oxygen concentration cannot be obtained. If spot welding is performed in a state where a coating layer exists at the contact surface between the steel members, inclusions of the coating layer and the like are formed in the plastic metal ring section 123 in addition to oxides. It is presumed that the inclusions derived from the coating component will hinder the manifestation of the TSS improvement effect. Here, the so-called plastic metal ring section 123 refers to an area where a plastic metal ring section 122 exists between the high-strength steel plate section 11H and the other steel plate sections 11.

[0068] According to the above reasons, in the spot welding joint 1 of the first embodiment, the plating layer 13 does not exist in the plastic metal ring section that joins the high-strength steel plate portion 11H with the other steel plate portion 11. It should be noted that the plating layer 13 does not exist in the plastic metal ring section between the high-strength steel plate portion 11H and the other steel plate portion 11 (that is, as long as the plating layer 13 is excluded from the plastic metal ring section). Since the plastic metal ring section 122 is not formed in the surface of the high-strength steel plate portion 11H that does not overlap with the other steel plate portion 11, the plating layer 13 can also be formed. In the surface of the high-strength steel plate portion 11H that overlaps with the other steel plate portion 11, the plating layer 13 can also be formed in the area outside the plastic metal ring section. The plating layer 13 located outside the plastic metal ring section of the high-strength steel plate portion 11H will not adversely affect the TSS of the spot welding joint 1. In addition, the plating layer can also exist in the plastic metal ring section between the ordinary steel plate portions 11.

[0069] Furthermore, in the top view, the oxygen concentration of the plastic metal ring zone 122 for solid phase bonding the high-strength steel plate portion 11H and other steel plate portions 11 at a position 50 μm outside the periphery of the nugget 121 is set to 15.0 mass % or less. Preferably, the oxygen concentration of the plastic metal ring zone 122 at a position 50 μm outside the periphery of the nugget 121 is 14.0 mass % or less, 13.0 mass % or less, 12.0 mass % or less, or 10.0 mass % or less. The lower limit of the oxygen concentration of the plastic metal ring zone 122 between the high-strength steel plate portion 11H and other steel plate portions 11 is not particularly limited, and may be 0 mass %. However, it is difficult to completely remove oxygen if the manufacturing cost of the spot welding joint 1 is considered. Therefore, the oxygen concentration of the plastic metal ring region 122 between the high-strength steel sheet portion 11H and the other steel sheet portions 11 may be set to 1.0 mass % or more, 2.0 mass % or more, or 5.0 mass % or more.

[0070] It should be noted that the oxygen concentration of the plastic metal ring area 122 that is not in contact with the high-strength steel plate portion 11H is not particularly limited. As described above, this is because: in the joint surface of the ordinary steel plate portion 11 with a tensile strength of less than 1800 MPa (i.e., a Vickers hardness of less than 530 HV), no correlation between oxygen concentration and TSS is observed.

[0071] The spot welded joint 1 of the first embodiment can obtain the TSS improvement effect as long as the above-mentioned necessary conditions are satisfied. On the other hand, by applying the preferred aspects described below, the TSS and other mechanical properties of the spot welded joint 1 of the first embodiment can be further improved.

[0072] (Carbon content of high-strength steel sheet portion 11H: preferably more than 0.30 mass %)

[0073] The carbon amount of the high-strength steel plate portion 11H is not particularly limited, but is preferably set to more than 0.30 mass%, more than 0.31 mass%, more than 0.33 mass%, more than 0.36 mass% or more than 0.40 mass%. Thus, the strength improvement effect brought by the technology disclosed in the present invention can be obtained. On the other hand, by setting the carbon amount of the high-strength steel plate portion 11H to less than 0.50 mass%, less than 0.48 mass%, less than 0.45 mass%, less than 0.42 mass% or less than 0.40 mass%, the hardness of the nugget 121 can be reduced, and the joining strength of the spot welding joint 1 can be further improved. It should be noted that the carbon amount of the ordinary steel plate portion 11 that may be combined with the high-strength steel plate portion 11H is not particularly limited, but, for example, it can also be set to less than 0.2 mass%.

[0074] It should be noted that the C contained in the high-strength steel plate portion 11H may cause embrittlement of the weld. However, in the spot welded joint 1 of the first embodiment, the plastic metal ring zone is used to improve TSS. Therefore, even when the carbon content of the high-strength steel plate portion 11H is high, in the spot welded joint 1 of the first embodiment, the joining strength of the weld is improved.

[0075] (Carbon content of nugget 121: preferably 0.29 mass % or more)

[0076] The carbon content of the nugget 121 is not particularly limited either, and can be set to, for example, 0.29 mass % or more, 0.31 mass % or more, 0.35 mass % or more, or 0.38 mass % or more. Thus, the strength improvement effect brought about by the technology disclosed in the present invention can be obtained. On the other hand, the carbon content of the nugget 121 can also be set to 0.45 mass % or less, 0.42 mass % or less, or 0.38 mass % or less. Thus, excessive hardening of the nugget 121 can be avoided, and the joining strength of the spot welded joint 1 can be further improved.

[0077] (Diameter of the nugget 121: preferably 4.5√t or more)

[0078] The diameter of the nugget 121 is not particularly limited, and various values ​​can be selected within the range in which the high-strength steel plate portion and the other steel plate portion can be joined. On the other hand, according to the experimental results of the inventors of the present invention, it is found that the larger the diameter of the nugget 121, the further the oxygen concentration of the plastic metal ring area 122 is reduced, and the further the TSS is improved.

[0079] This is presumably due to the amount of thermal expansion during the formation of the nugget 121. Figure 2A and Figure 2B As shown in , during spot welding, the nugget 121 undergoes thermal expansion. Due to this thermal expansion, pressure is applied to the plastic metal ring area 122 in the direction of the outside of the nugget 121. It is believed that this pressure causes the plastic metal ring area to produce plastic flow, and discharges the oxide Ox to the outside of the plastic metal ring area. The greater the heat input during spot welding and the larger the nugget diameter, the greater the pressure applied to the plastic metal ring area 122. Therefore, it is believed that the larger the nugget diameter, the greater the discharge amount of the oxide Ox, and the further the TSS is improved.

[0080] According to the experimental results of the inventors of the present invention, when the diameter D of the nugget 121 is 4.5√t or more, a further improvement in TSS is observed. The diameter D of the nugget 121 here refers to the size of the nugget 121 measured along the boundary line of the adjacent steel plate parts 11 in the cross section passing through the center of the nugget 121 and perpendicular to the surface of the steel plate part 11. The so-called "t" refers to the smaller of the plate thicknesses of the two adjacent steel plate parts 11 constituting the boundary line that serves as the measurement reference of the nugget 121. When the number of steel plate parts 11 contained in the spot welding joint 1 is 3 or more and there are 2 or more boundary lines, determine more than 2 D and more than 2 t corresponding to each of the more than 2 boundary lines.

[0081] For example, when the number of steel plate portions 11 included in the spot welded joint 1 is two, there is one boundary line of the steel plate portion 11. The diameter D of the nugget 121 refers to the width of the nugget 121 measured along the boundary line, and t refers to the thinner thickness of the two steel plate portions 11. In the boundary line, D ≥ 4.5√t is preferably satisfied. In this case, a further improvement in TSS can be observed.

[0082] When the number of steel plate portions 11 included in the spot welded joint is 3 or more, the number of boundary lines of the steel plate portion 11 is 2 or more. In this case, preferably, in at least one boundary line, the diameter D of the nugget 121 and the thinner plate thickness t in the steel plate portion 11 constituting the boundary line satisfy D≥4.5√t, and more preferably, in all boundary lines, D≥4.5√t is satisfied. It is further preferred to set the diameter of the nugget 121 to be 4.8√t or more or 5.0√t or more. In addition, it is preferred that, in the boundary line constituted by the high-strength steel plate portion 11H, the diameter D of the nugget 121 and the thinner plate thickness t in the steel plate portion 11 constituting the boundary line satisfy D≥4.5√t.

[0083] (Thickness, Hardness, Tensile Strength and Surface Treatment of Steel Plate 11)

[0084] As mentioned above, the Vickers hardness of the high-strength steel plate portion 11H is more than 530HV. From the viewpoint of improving the strength of the spot welding joint 1, the larger the Vickers hardness of the high-strength steel plate portion 11H, the more preferred. Therefore, the Vickers hardness of the high-strength steel plate portion 11H can also be set to more than 550HV, more than 580HV, more than 600HV or more than 620HV. The upper limit of the Vickers hardness of the high-strength steel plate portion 11H is not particularly limited, but from the viewpoint of improving the bonding strength of the spot welding joint 1, the Vickers hardness of the high-strength steel plate portion 11H can also be set to less than 700HV, less than 680HV or less than 650HV.

[0085] The tensile strength of the high-strength steel plate portion 11H is not particularly limited. In general, there is a good correlation between the tensile strength and Vickers hardness of steel, and a Vickers hardness of 530HV is equivalent to a tensile strength of about 1800MPa. A Vickers hardness of 580HV is equivalent to a tensile strength of about 2000MPa. Therefore, if the hardness of the high-strength steel plate portion 11H is specified, it is not necessary to separately specify the tensile strength of the high-strength steel plate portion 11H. On the other hand, the tensile strength of the high-strength steel plate portion 11H can also be specified to be above 1900MPa, above 2000MPa, or above 2100MPa. The upper limit of the tensile strength of the high-strength steel plate portion 11H is not particularly limited. For example, the tensile strength of the high-strength steel plate portion 11H can also be specified to be below 2800MPa, below 2500MPa, or below 2300MPa.

[0086] The tensile strength of the ordinary steel sheet portion 11 having a Vickers hardness of less than 530 HV combined with the high-strength steel sheet portion 11H is not particularly limited. For example, the tensile strength of the ordinary steel sheet portion 11 may be set to 1700 MPa or less, 1500 MPa or less, or 1200 MPa or less.

[0087] The metal structure of the steel plate portion 11 and the high-strength steel plate portion 11H is not particularly limited. For example, more than 90 area%, more than 92 area%, or more than 95 area% of the metal structure of the high-strength steel plate portion 11H may be martensite. It should be noted that the so-called martensite refers to a concept that includes both untempered martensite, i.e., primary martensite, and tempered martensite, i.e., tempered martensite. The upper limit of the proportion of martensite in the metal structure of the high-strength steel plate portion 11H is not particularly limited, but for example, the proportion may be less than 100 area%, less than 99 area%, or less than 98 area%.

[0088] In the spot welding joint 1 of the first embodiment, it is required that there is no coating in the area (plastic metal ring area) where the high-strength steel plate portion 11H is solid-phase bonded with the other steel plate portions 11, where the plastic metal ring area 122 is solid-phase bonded. On the other hand, as long as this requirement is met, the steel plate portion 11 may also have a coating 13 on a part or all of its surface. For example, the coating 13 disposed on the surface of the steel plate group will not have an adverse effect on the plastic metal ring area 122. In addition, the coating 13 present between two adjacent steel plate portions 11 will not have an adverse effect on the plastic metal ring area 122 as long as it is disposed outside the plastic metal ring area. Examples of the coating 13 are, for example, hot-dip galvanizing layer, hot-dip alloy zinc layer, alloyed hot-dip galvanizing layer, electroplated zinc layer, electroplated Al layer, etc. In addition, surface treatment films such as coating and chemical conversion treatment films may also be disposed on a part or all of the surface of the steel plate portion 11.

[0089] (Measurement method)

[0090] Hereinafter, the determination method of the parameters of the spot welding joint 1 defining the first embodiment will be described. It should be noted that it is not necessary to implement all the measurements described below to the sample of one spot welding portion. Generally speaking, two or more spot welding portions are provided in the same steel plate portion in the spot welding joint, and the parameters of these spot welding portions are substantially the same. Therefore, the measurement results of the samples of two or more spot welding portions can be regarded as the measurement results of the parameters of one spot welding portion. It should be noted that, in the case of determining whether the manufacturing method of the spot welding joint complies with the manufacturing method of the spot welding joint of the second embodiment described later, the measurement results of the samples of two or more spot welding portions can also be regarded as the measurement results of the parameters of one spot welding portion.

[0091] The method for measuring the Vickers hardness of the steel plate portion 11 is as follows. In the cross-sectional view, a cut surface perpendicular to the surface of the steel plate portion is made at a position more than 10 mm away from the periphery of the plastic metal ring zone. The position more than 10 mm away from the periphery of the plastic metal ring zone in the cut surface for measuring the carbon content of the molten core 121 described later can also be used as a sample for measuring the hardness of the steel plate portion. In this cut surface, the Vickers hardness is measured at a position 1 / 4t away from the surface of the steel plate portion. The measuring points are set to 3 points. The load is set to 0.5 kgf. The measuring points are set to be arranged roughly parallel to the surface of the steel plate portion, and the interval between the measuring points is set to 0.5 mm. The average value of the measured values ​​at the 3 points is regarded as the Vickers hardness of the steel plate portion. The cut surface for measuring the hardness of a steel component can be formed in any flat part such as a flange portion, for example.

[0092] The tensile strength of the steel plate portion 11 is measured by a tensile test in accordance with JIS Z 2241:2011 "Methods for tensile testing of metallic materials". The test piece is set to be a No. 13B test piece. The test piece is collected from the flat portion. In addition, the test piece is collected from the outside of the heat-affected zone of the spot weld. The collection location of the test piece can also be greatly away from the nugget. For example, in the case where the high-strength steel plate portion is a flange portion of a hat-shaped component, the tensile test piece can also be collected from the flange portion where the nugget is set, or the tensile test piece can be collected from the longitudinal wall portion or the transverse wall portion. It should be noted that this measurement method is also applied to the measurement of the tensile strength of the steel component before spot welding described later.

[0093] The method for measuring the oxygen concentration of the plastic metal ring zone 122 at a position 50 μm outside the outer periphery of the nugget 121 is as follows. First, in accordance with the provisions of JIS Z 3144:2013 "Field Test Methods for Spot Welds and Projection Welds", a peeling test is performed on the spot weld joint 1 to break the spot weld 12. As a result, the surface (also called the fracture surface) of the plastic metal ring zone 122 that solid-phase bonds the high-strength steel plate portion to the other steel plate portion is revealed. Next, the oxygen concentration of the plastic metal ring zone 122 is measured by surface EDX analysis. The acceleration voltage is set to 15 kV. The position of the measurement point is set to the plastic metal ring zone 122 at a position 50 μm outside the outer periphery of the nugget 121 in the top view. The number of measurement points is set to 20 points for each plastic metal ring zone 122. The measurement points are set in a manner distributed at approximately equal intervals along the outer periphery of the nugget 121. When the nugget 121 is circular, the angle formed by the adjacent measurement points and the center of the nugget 121 is approximately 18°.

[0094] This measurement is performed on the surface (fracture surface) of the high-strength steel sheet portion 11H side that is solid-phase bonded by the plastic metal ring zone 122. However, in the case where the high-strength steel sheet portions 11H are solid-phase bonded to each other, the surface (fracture surface) of each of the two high-strength steel sheet portions 11H is measured at 20 points, thereby obtaining measurement results at a total of 40 points. The average value of these measurement results is regarded as the oxygen concentration of the plastic metal ring zone 122 that solid-phase bonds the high-strength steel sheet portion and the other steel sheet portion at a position 50 μm outside the outer periphery of the nugget 121.

[0095] The method for determining the presence or absence of a coating at the plastic metal ring region 122 is as follows. The surface (fracture surface) of the plastic metal ring region 122 is visualized by the same procedure as the determination of the oxygen concentration of the plastic metal ring region 122. The chemical composition of the coating is different from that of the base steel plate. Therefore, by performing EDX analysis on the surface (fracture surface) of the plastic metal ring region, the presence or absence of a coating can be easily visually identified. The presence or absence of a coating can also be determined for the sample used in the determination of the oxygen concentration of the plastic metal ring region 122.

[0096] The carbon content of the steel plate portion 11 is measured by JIS G 1211-3: 2018 "Iron and steel - Carbon quantitative method - Part 3: Combustion - Infrared absorption method". The sample for measuring the carbon content is extracted from a position 10 to 30 mm away from the center of the spot weld. When the sample is extracted, the surface of the steel plate portion is shaved off by more than 0.1 mm to remove the coating and contamination. It should be noted that this measurement method is also applied to the measurement of the carbon content of the steel member before spot welding described later.

[0097] The method for measuring the carbon content of the nugget 121 is as follows. First, the nugget 121 is cut in a plane that passes through the center of the nugget 121 when the nugget 121 is viewed from above in a direction perpendicular to the surface of the steel plate portion 11 and is perpendicular to the surface of the steel plate portion 11. Next, the cut surface is etched to reveal the nugget 121. The area of ​​each steel plate portion of the nugget 121 revealed in the cut surface is measured, and the carbon content of the nugget 121 is calculated by dividing the total product of the carbon content of each steel plate and the area of ​​the nugget 121 in each steel plate by the area of ​​the nugget 121. The so-called "area of ​​the nugget 121" refers to the area of ​​the nugget measured in the cut surface. The "area of ​​the nugget 121 in each steel plate portion" refers to the area of ​​each nugget region existing on each steel plate portion side in the divided nugget region, in which the nugget 121 is divided by connecting the plastic metal ring regions appearing at both ends of the nugget 121 in the cut surface as a boundary line (hereinafter referred to as the boundary line). Specifically, the carbon content of the nugget is calculated by the following formula.

[0098] Carbon content of nugget (%) =

[0099] (S1×C1+S2×C2+……+Sn×Cn) / (S1+S2+……+Sn)

[0100] S1: The nugget area of ​​the first steel plate (mm 2 )

[0101] C1: Carbon content of the first steel plate (mass %)

[0102] S2: The nugget area of ​​the second steel plate (mm 2 )

[0103] C2: Carbon content of the second steel plate portion (mass %)

[0104] Sn: The nugget area of ​​the nth steel plate (mm 2 )

[0105] Cn: Carbon content of the nth steel plate portion (mass %)

[0106] For example, in Figure 1 In the cross-sectional view of the spot welded joint shown in , when the steel plate portion 11 arranged on the upper side is regarded as the "first steel plate portion" and the high-strength steel plate portion 11H arranged on the lower side is regarded as the "second steel plate portion", the dotted line shown inside the weld core 121 is the boundary line, the area of ​​the weld core 121 that is higher than the dotted line is S1, and the area of ​​the weld core 121 that is lower than the dotted line is S2.

[0107] It should be noted that, if it is on the same steel plate portion 11, the oxygen concentration of the plastic metal ring zone around another nugget different from the nugget being the object of carbon concentration measurement is regarded as the oxygen concentration of the plastic metal ring zone around the same nugget. Specifically, from the spot welded joint, a sample is taken as the same plate-shaped portion having a plurality of spot welds, and two adjacent spot welds are taken as the measurement objects, and the measurement results in each spot weld are regarded as the measurement results in the same spot weld.

[0108] The diameter of the nugget 121 is measured as follows: First, the nugget 121 is cut along a plane passing through the center of the nugget 121 when viewed from above in a direction perpendicular to the surface of the steel plate portion 11 and perpendicular to the surface of the steel plate portion 11 .

[0109] Next, the cut surface is etched to reveal the nugget 121. Then, the diameter of the nugget associated with the thinnest steel plate portion is measured. In JIS Z 3001-6:2013, the diameter of the nugget portion measured at the joint interface by a cross-sectional test of the spot weld is defined as the nugget diameter. In this embodiment, the diameter of the nugget refers to the nugget width measured on the boundary line between two adjacent steel plate portions. When there are more than two boundary lines, the diameter of the nugget is measured at each boundary line.

[0110] The diameter of the nugget may also be measured on the cross section of the nugget on which the above-mentioned carbon concentration is measured. On the other hand, if it is on the same steel plate portion 11, the diameter of another nugget different from the nugget that is the object of the oxygen concentration measurement and the carbon concentration measurement may also be measured as the diameter of the same nugget. Specifically, from the spot welded joint, a sample is taken as the same plate-shaped portion having a plurality of spot welds, and two adjacent spot welds are taken as the measurement object, and the average value of the measurement results in each spot weld is regarded as the measurement result in the same spot weld.

[0111] <Method for Manufacturing Spot Welded Joint 1 of Second Embodiment>

[0112] Next, a method for manufacturing a spot welding joint 1 according to a second embodiment of the present invention will be described. Figure 3A to Figure 3C As shown in the example, the following steps are included: a step of forming a surface treatment portion 24 on the surface of a high-strength steel member 2H having a Vickers hardness of 530 HV or more; a step of overlapping a plurality of steel members 2 in a manner of arranging the surface treatment portion 24 on the joint surface between the high-strength steel member 2H and other steel members 2; a step of spot welding a plurality of steel members 2 in a manner of accommodating a nugget 121 and a plastic metal ring zone 122 on the inner side of the surface treatment portion 24 in a plan view observed from a direction perpendicular to the surface of the surface treatment portion 24, wherein in the overlapping step, no plating is provided on the surface treatment portion 24 and a region in contact with the surface treatment portion 24, the ten-point average roughness of the surface treatment portion 24 is set to be 3.5 μm or less, and the oxygen concentration of the surface treatment portion 24 is set to be 18.0 mass % or less.

[0113] It should be noted that the term "steel member 2" refers to the material (i.e., the parent material) of the "steel plate portion 11" of the spot welding joint 1 of the first embodiment. The flat portion on the same surface as the spot welding portion in the spot-welded steel member 2 is the steel plate portion 11. Similarly, the term "high-strength steel member 2H" refers to the material of the "high-strength steel plate portion 11H" of the spot welding joint 1 of the first embodiment. The flat portion on the same surface as the spot welding portion in the high-strength steel member 2H to be spot-welded is the high-strength steel plate portion 11H.

[0114] (Step S1 of Forming Surface Treatment Portion 24)

[0115] First, if Figure 3A As shown in , a surface treatment portion 24 is formed on the surface of a high-strength steel member 2H having a Vickers hardness of 530 HV or more. However, in the case of providing a high-strength steel plate pre-set with a surface treatment portion 24 to manufacture a spot welding joint, the step S1 of forming the surface treatment portion 24 can be omitted from the manufacturing method of the spot welding joint. It should be noted that the "surface" of the high-strength steel member 2H on which the surface treatment portion 24 is formed refers to the surface on which electrodes for spot welding can be configured. Therefore, the so-called "surface" refers to a concept that does not contain an "end face" (i.e., a cut surface formed by cutting a steel member from a steel plate as a raw material, etc.). As described below, a nugget 121 and a plastic metal ring zone 122 are formed in the surface treatment portion 24. By controlling the surface state of the surface treatment portion 24 in advance, the oxygen concentration of the plastic metal ring zone 122 can be set to less than 15.0 mass%.

[0116] In the surface treatment portion 24, the ten-point average roughness of the surface treatment portion 24 is set to 3.5 μm or less, and the oxygen concentration is set to 18.0 mass % or less. By setting the ten-point average roughness of the surface treatment portion 24 of the high-strength steel member 2H to 3.5 μm or less, the surface area of ​​the surface treatment portion 24 can be reduced, and the amount of oxygen in the surface treatment portion 24 can be reduced. In addition, according to the experimental results of the inventors of the present invention, the oxides are discharged to the outside of the plastic metal ring area 122 by the thermal expansion of the nugget 121 during spot welding, and the oxygen concentration is reduced. Therefore, if the ten-point average roughness of the surface treatment portion 24 is set to 3.5 μm or less, and the oxygen concentration of the surface treatment portion 24 is set to 18.0 mass % or less before spot welding, the oxygen concentration of the plastic metal ring area 122 formed in the surface treatment portion 24 can be set to 15.0 mass % or less. It should be noted that, when the high-strength steel member 2H is combined with the ordinary steel member 2, it is not necessary to control the ten-point average roughness and oxygen concentration in the surface of the ordinary steel member 2 in contact with the high-strength steel member 2H. In addition, the oxygen concentration of the surface treatment portion 24 can also be set to 16.5 mass% or less, 16.0 mass% or less, or 15.0 mass% or less. It should be noted that the surface treatment portion having the above-mentioned structure only needs to be formed on the surface of the high-strength steel member 2H having a Vickers hardness of 530HV or more. It is further preferred that the surface treatment portion having the above-mentioned structure is also formed on the surface of the ordinary steel member 2 having a Vickers hardness of less than 530HV.

[0117] The method for measuring the Vickers hardness of the high-strength steel member 2H is the same as the method for measuring the Vickers hardness of the steel plate portion of the spot welded joint 1 of the first embodiment except for the measurement position. The measurement position is set to a position 1 / 4t from the surface of the high-strength steel member 2H in the cross section of the high-strength steel member 2H.

[0118] The method for measuring the ten-point average roughness of the surface treated portion 24 of the high-strength steel member 2H is as follows. Based on the appendix JA "ten-point average roughness" of JIS B 0601:2013, the ten-point average roughness of any measurement point of the surface treated portion 24 is measured. The definition of the ten-point average roughness is based on the standard of 2013. The measurement length is set to 4 mm, and the cut-off is set to 0.8 mm.

[0119] The method for measuring the oxygen concentration of the surface treated portion 24 of the high-strength steel member 2H is the same as the method for measuring the oxygen concentration of the plastic metal ring zone 122 of the spot welded joint 1 of the first embodiment, except for the peeling test and the measurement position. That is, in the surface treated portion 24 of the high-strength steel plate portion 11H, the surface EDX analysis can be performed at an acceleration voltage of 15KV. However, since no nugget 121 is formed in the surface treated portion 24, the interval of the measurement points is set to 10μm, the number of the measurement points is set to 5 points, and the positions of these measurement points are set to any position inside the surface treated portion 24.

[0120] The steel member 2 and the high-strength steel member 2H may have a plating layer. However, the surface treatment portion 24 is not provided with a plating layer.

[0121] When the high-strength steel member 2H is a non-plated steel member 2 , it is not necessary to remove the plating layer, and the ten-point average roughness and oxygen concentration of the surface treated portion 24 are set to the above-mentioned ranges.

[0122] When the high-strength steel member 2H is a plated steel member 2, it is necessary to first remove the plating layer from the surface treated portion 24, and then set the ten-point average roughness and oxygen concentration of the surface treated portion 24 to the above ranges. When the plating layer is removed and the surface treated portion is formed by one treatment, the temperature of the surface treated portion rises, making it difficult to set the oxygen concentration to the above range.

[0123] The surface treatment portion 24 only needs to be formed on the surface of the high-strength steel member 2H. When two high-strength steel members 2H are overlapped, the surface treatment portion 24 is provided on the two high-strength steel members 2H. On the other hand, when the high-strength steel member 2H is overlapped with the ordinary steel member 2 having a Vickers hardness of less than 530 HV, it is not necessary to provide the surface treatment portion 24 on the ordinary steel member 2. In addition, when the ordinary steel member 2 overlapped with the high-strength steel member 2H is a plated steel member 2, it is necessary to remove the plating layer at least in at least a portion of the plated steel member 2.

[0124] In the case where the high-strength steel member 2H is arranged on the surface of the steel plate group, the surface treatment portion 24 only needs to be arranged on one surface of the high-strength steel member 2H. In the case where the high-strength steel member 2H is sandwiched by two other steel members 2, the surface treatment portion 24 is arranged on both surfaces of the high-strength steel member 2H. In either case, the surface treatment portion 24 can be arranged only in a part of the surface of the high-strength steel member 2H, or it can be arranged on the entire surface. For example, in the case where the high-strength steel member is a hat-shaped member having a flange portion, a longitudinal wall portion and a transverse wall portion (top plate portion), spot welding is performed on the flange portion. The surface treatment portion can be formed only on the surface of the flange portion, or on the surface of all parts including the flange portion, the longitudinal wall portion and the transverse wall portion. The surface treatment portion can be arranged on one or both of the inner side surface and the outer side surface of the hat-shaped member. However, as described above, it is not necessary to set the surface treatment portion on the end face.

[0125] (Step S2 of overlapping a plurality of steel members 2)

[0126] Then, if Figure 3B As shown in , a plurality of steel members 2 including the above-mentioned high-strength steel member 2H are overlapped. At this time, the surface treatment portion 24 formed in the high-strength steel member 2H is arranged on the joint surface of the steel member 2. In addition, the surface treatment portion 24 formed in the high-strength steel member 2H is not in contact with the coating. That is, not only is the coating not provided in the surface treatment portion 24, but also the coating is not provided in the area in contact with the surface treatment portion 24. In the case where the high-strength steel members 2H are overlapped with each other, no special treatment is required because the surface treatment portions 24 are overlapped with each other. On the other hand, in the case where the steel member 2 overlapped with the high-strength steel member 2H is an ordinary steel plate and has a coating on its overlapping surface, it is necessary to remove the coating in advance as described above, and align the steel member 2 in such a way that the removed portion of the coating overlaps with the surface treatment portion 24.

[0127] (Step S3 of spot welding a plurality of steel members 2)

[0128] Then, if Figure 3CAs shown in , a plurality of steel members 2 are spot welded. At this time, in a plan view observed from a direction perpendicular to the surface of the surface treated portion 24, the steel members 2 are spot welded so that the position where the electrode E contacts the steel member 2, i.e., the spot, overlaps with the surface treated portion 24 so that the nugget and the plastic metal ring area are contained inside the surface treated portion 24.

[0129] By manufacturing the spot welded joint 1 according to the above steps, the nugget 121 and the plastic metal ring zone 122 can be formed in the surface treated portion 24 having a low ten-point average roughness and oxygen concentration and having no plating layer. That is, the manufacturing method of the second embodiment can make it possible to prevent the plating layer from existing in the plastic metal ring zone 122 formed on the surface of the high-strength steel plate portion 11H of the spot welded joint 1, and can set the oxygen concentration of the plastic metal ring zone 122 formed on the surface of the high-strength steel plate portion 11H to 15.0 mass % or less.

[0130] The method for manufacturing the spot welded joint 1 of the second embodiment can obtain the TSS improvement effect as long as the above-mentioned necessary conditions are satisfied. On the other hand, the preferred aspects of the spot welded joint 1 of the first embodiment can also be applied to the manufacturing method of the second embodiment.

[0131] (Hot stamping and removal of plating)

[0132] The method for manufacturing the spot welded joint 1 may further include a step of hot stamping the high-strength steel sheet. In this case, it is preferred that the high-strength steel sheet be hot stamped before the surface treatment portion 24 is formed in the high-strength steel sheet. Then, in the step of forming the surface treatment portion 24, it is preferred that the surface treatment portion 24 be formed on the surface of the high-strength steel sheet after hot stamping. Thus, it is possible to avoid an increase in the oxygen concentration of the surface treatment portion 24 caused by heating for hot stamping.

[0133] The method for manufacturing the spot welding joint 1 may also include a step of removing a portion of the plating layer at the surface of the high-strength steel member before forming the surface treatment portion. In this case, in the step of forming the surface treatment portion, the surface treatment portion is preferably formed in the region where the plating layer is removed. Thus, a plastic metal ring region without plating layer can be manufactured.

[0134] (Carbon content of high-strength steel member 2H: preferably more than 0.30 mass %)

[0135] (Carbon content of nugget 121: preferably 0.29 mass % or more)

[0136] For example, similarly to the spot welding joint 1 of the first embodiment, in the manufacturing method of the second embodiment, the carbon content of the high-strength steel member 2H may be set to more than 0.30 mass%. In addition, the carbon content of the nugget 121 may be set to more than 0.29 mass%. Thus, various mechanical properties of the spot welding joint 1 can be further improved. The preferred upper and lower limits of the carbon content of the high-strength steel plate portion 11H and the nugget 121 illustrated with respect to the first embodiment may also be applied to the high-strength steel member 2H and the nugget 121 in the manufacturing method of the second embodiment, respectively.

[0137] The carbon content of the nugget 121 can be controlled by the carbon content and plate thickness of the steel member 2. The higher the carbon content of the steel member 2, the higher the carbon content of the nugget 121. In addition, when a high-carbon steel member and a low-carbon steel member are combined to manufacture the spot welded joint 1, the carbon content of the nugget 121 can be increased by increasing the ratio of the plate thickness of the high-carbon steel member to the total plate thickness t.

[0138] The method of measuring the carbon amount of the high-strength steel member 2H and the oxygen amount of the nugget 121 is the same as the method of measuring the carbon amount of the high-strength steel plate portion 11H and the oxygen amount of the nugget 121 of the spot welded joint 1 of the first embodiment.

[0139] (Hardness of high-strength steel components 2H: 530HV or more)

[0140] (Metallic structure of high-strength steel member 2H: preferably 90 area % or more of martensite)

[0141] As mentioned above, the Vickers hardness of the high-strength steel member 2H is more than 530HV. From the viewpoint of improving the strength of the spot welding joint 1, the larger the Vickers hardness of the high-strength steel member 2H, the more preferred. Therefore, the Vickers hardness of the high-strength steel member 2H can also be set to more than 550HV, more than 580HV, more than 600HV or more than 620HV. The upper limit of the Vickers hardness of the high-strength steel member 2H is not particularly limited, but from the viewpoint of improving the bonding strength of the spot welding joint 1, the Vickers hardness of the high-strength steel member 2H can also be set to less than 700HV, less than 680HV or less than 650HV.

[0142] The metal structure of the steel member 2 and the high-strength steel member 2H is not particularly limited. For example, more than 90% by area, more than 92% by area, or more than 95% by area of ​​the metal structure of the high-strength steel member 2H may also be martensite. It should be noted that the so-called martensite refers to a concept that includes both untempered martensite, i.e., primary martensite, and tempered martensite, i.e., tempered martensite. The upper limit of the proportion of martensite in the metal structure of the high-strength steel member 2H is not particularly limited, but for example, the proportion may be less than 100% by area, less than 99% by area, or less than 98% by area.

[0143] (Diameter of the nugget 121: preferably 4.5√t or more)

[0144] The diameter D of the nugget 121 may be set to be greater than 4.5√t. The diameter D of the nugget 121 here refers to the size of the nugget 121 measured along the boundary line of the adjacent steel members 2 in a plane passing through the center of the nugget 121 and perpendicular to the surface of the steel member 2. The so-called "t" refers to the smaller of the plate thicknesses of the two adjacent steel members 2 constituting the boundary line that serves as the measurement reference of the nugget 121. When the number of the steel members 2 to be spot welded is 3 or more and there are 2 or more boundary lines, 2 or more D and 2 or more t corresponding to each of the 2 or more boundary lines are determined.

[0145] By satisfying D≥4.5√t, the amount of oxides discharged from the plastic metal ring zone 122 can be increased, and the oxygen concentration of the plastic metal ring zone 122 can be further reduced. The diameter of the nugget 121 can be controlled by the heat input of spot welding. The larger the diameter of the nugget 121 becomes, the larger the diameter of the plastic metal ring zone 122 becomes. Therefore, it is preferred to specify the size of the surface treatment portion 24 in such a way that the plastic metal ring zone 122 is formed on the inner side of the surface treatment portion 24. When the number of steel members 2 is more than 3 and the number of boundary lines is more than 2, it is preferred to satisfy D≥4.5√t at least at one boundary, and it is further preferred to satisfy D≥4.5√t at all boundaries. In addition, it is preferred that, in the boundary line formed by the high-strength steel member 2H, the diameter D of the nugget 121 and the thinner plate thickness t in the steel member 2 constituting the boundary line satisfy D≥4.5√t.

[0146] The method of measuring the diameter of the nugget 121 is the same as the method of measuring the diameter of the nugget 121 of the spot welding joint 1 of the first embodiment.

[0147] (Means for forming the surface treatment portion 24: preferably shot blasting or wet sand blasting)

[0148] The means for forming the surface treatment portion 24 is not particularly limited, but shot blasting or wet blasting is preferred. Shot blasting refers to surface treatment by blasting a projection material as a polishing powder. Wet blasting refers to surface treatment by blasting a slurry obtained by mixing an abrasive and a liquid.

[0149] The high-strength steel member 2H having a Vickers hardness of 530 HV or more is preferably manufactured through heat treatments such as quenching and tempering and hot stamping. Therefore, a large amount of oxide scale is attached to the surface of the high-strength steel member 2H. The oxide scale is usually removed by means such as pickling and shot blasting. However, the inventors of the present invention have confirmed that the oxygen concentration of the high-strength steel member 2H after the oxide scale is removed by these common means exceeds 18.0 mass %, and the ten-point average roughness also exceeds 3.5 μm.

[0150] Therefore, the inventors of the present invention have repeatedly conducted various investigations, and the result is that if wet sandblasting is used, the oxygen concentration of the high-strength steel component 2H can be reduced to 18.0 mass%. The effect of wet sandblasting on reducing the oxygen concentration of the high-strength steel component 2H is greater than that of shot blasting, and this purpose is unknown so far. In addition, for wet sandblasting, there is a disadvantage that the time required for removing the oxide scale is longer than that of shot blasting. Because wet sandblasting applies water resistance when the abrasive collides, the processing capacity is small compared with shot blasting. In addition, due to the use of water, wet sandblasting has the disadvantage of requiring the installation of drainage equipment, additional drying and other processes. Therefore, the example of using wet sandblasting as a pre-treatment for spot welding has not been reported so far. However, in the manufacturing method of the second embodiment, based on the above-mentioned understanding of the inventors of the present invention, wet sandblasting is adopted as the preferred surface treatment means.

[0151] The material of the abrasive used in wet sandblasting is preferably set to steel, zirconium oxide, stainless steel or aluminum oxide, for example. The shape of the abrasive is preferably set to a spherical or grid shape, for example. The average diameter of the abrasive is preferably set to 0.03 to 0.50 mm, for example. During wet sandblasting, the pressure of the air used to spray the projection material (i.e., a slurry obtained by mixing the abrasive with a liquid) is preferably set to 0.2 to 0.8 MPa, for example. The projection distance (i.e., the distance between the nozzle for spraying the projection material and the high-strength steel member 2H) is preferably set to 1 to 30 cm, for example.

[0152] It should be noted that it is believed that by reducing the diameter of the particles sprayed in shot peening, the oxygen concentration and ten-point average roughness of the high-strength steel component 2H can be reduced even if shot peening is used. However, as far as shot peening is concerned, frictional heat and other heat may be generated during surface processing, and the oxygen concentration of the high-strength steel component 2H increases. Therefore, when using shot peening to perform surface processing of the high-strength steel component 2H, it is preferred that in addition to making the particle size suitable, conditions such as the particle ejection speed are also made suitable and a cooling mechanism is used. In addition, there are the following disadvantages for reducing the particle size of shot peening: the influence of air resistance becomes larger, and it may become difficult for the particles to reach the high-strength steel component 2H; moisture is easily generated, and it is possible that the particles will not be ejected evenly and the nozzle will be clogged; and dust becomes easy to be raised, which may cause the working environment to deteriorate.

[0153] The material of the particles (projection material) used in shot peening is preferably set to steel, zirconia, stainless steel or alumina, for example. The shape of the projection material is preferably set to a spherical or grid shape, for example. The average diameter of the projection material is preferably set to 0.03 to 0.70 mm, for example. During shot peening, the pressure of the air used to spray the projection material is preferably set to 0.2 MPa to 1.0 MPa, for example. The projection distance (i.e., the distance between the nozzle for spraying the projection material and the high-strength steel member 2H) is preferably set to 5 to 40 cm, for example.

[0154] The projection pressure in wet blasting or shot peening, i.e., the pressure of the air used to blast the projection material, is obtained by measuring the pressure of the air pipe equipped with the projection material. The particle size of the projection material in wet blasting or shot peening is obtained by measuring 20 random particles with a microscope and calculating the average value. The projection distance in wet blasting or shot peening is obtained by measuring the distance from the front end of the projection material spray nozzle to the workpiece.

[0155] In addition, the oxygen concentration and the ten-point average roughness can also be reduced by grinding or cutting. If grinding or cutting is used, the coating can also be removed. However, as with shot peening, in grinding and cutting, it is also possible to generate heat such as frictional heat during surface processing, which increases the oxygen concentration of the high-strength steel component 2H. Therefore, when using grinding or cutting to perform surface processing on the high-strength steel component 2H, it is preferred to make conditions such as processing speed suitable and use a cooling mechanism. In addition, for grinding or cutting, there are disadvantages such as high processing cost and long processing time. Due to the above reasons, wet sandblasting is considered to be the most preferred means for forming the surface treatment portion 24.

[0156] When the surface treatment portion is formed by grinding, it is preferred to suppress frictional heat by controlling the rotation speed of the grindstone, i.e., the peripheral speed, feed speed, cutting depth, and the type and flow rate of the grinding fluid. When the surface treatment portion is formed by cutting, it is preferred to suppress frictional heat by controlling the rotation speed, feed speed, and cutting depth of the tool.

[0157] <High Strength Steel Member for Spot Welded Joint of Third Embodiment>

[0158] Next, a high-strength steel component for spot welding joints according to a third embodiment of the present invention is described. The high-strength steel component for spot welding joints according to the third embodiment has a Vickers hardness of 530 HV or more, has a surface treatment portion without a coating, has a ten-point average roughness of 3.5 μm or less, and has an oxygen concentration of 18.0 mass % or less.

[0159] The Vickers hardness of the high-strength steel component of the third embodiment is 530HV or more. Therefore, according to the high-strength steel component of the third embodiment, a very high-strength spot welding joint 1 can be manufactured. However, the TSS of the spot weld 12 obtained by spot welding a high-strength steel component with a Vickers hardness of 530HV or more is poor. Therefore, the high-strength steel component of the third embodiment has a surface treatment portion 24 without a coating, the ten-point average roughness of the surface treatment portion 24 is less than 3.5μm, and the oxygen concentration of the surface treatment portion 24 is less than 18.0 mass%. In the plastic metal ring area 122 obtained by spot welding the surface treatment portion 24, there is no coating, and the oxygen concentration becomes less than 15.0 mass%. Thus, the TSS of the spot welding joint 1 can be dramatically improved.

[0160] As long as the high-strength steel member for the spot welded joint of the third embodiment satisfies the above-mentioned necessary conditions, the TSS improvement effect of the spot welded joint 1 can be obtained. On the other hand, the preferred embodiments of the manufacturing methods of the spot welded joint 1 of the first embodiment and the spot welded joint 1 of the second embodiment can also be applied to the high-strength steel member of the third embodiment.

[0161] The method for measuring the Vickers hardness of the high-strength steel member according to the third embodiment is the same as the method for measuring the Vickers hardness of the high-strength steel member described in the method for manufacturing the spot welded joint 1 according to the second embodiment.

[0162] The method for measuring the ten-point average roughness of the surface treated portion 24 of the high-strength steel member of the third embodiment is the same as the method for measuring the ten-point average roughness of the surface treated portion 24 described in the method for manufacturing a spot welded joint of the second embodiment.

[0163] The method for measuring the oxygen concentration of the surface treated portion 24 of the high-strength steel member according to the third embodiment is the same as the method for measuring the oxygen concentration of the surface treated portion described in the method for manufacturing a spot welded joint according to the second embodiment.

[0164] (Carbon content: preferably more than 0.30 mass %)

[0165] (Position of the surface treatment portion 24: preferably the entire one surface or the entire two surfaces)

[0166] For example, similarly to the spot welding joint 1 of the first embodiment, the carbon content of the high-strength steel component for the spot welding joint of the third embodiment can also be set to more than 0.30 mass %. Thus, the various mechanical properties of the spot welding joint 1 can be further improved. It should be noted that the C contained in the high-strength steel component may cause the embrittlement of the weld. However, according to the high-strength steel component for the spot welding joint of the third embodiment, the plastic metal ring zone is modified using the surface treatment portion, which improves the joint strength of the joint of the spot welding joint. Therefore, even when the carbon content is high, according to the high-strength steel component for the spot welding joint of the third embodiment, a weld with high joint strength can be manufactured.

[0167] The carbon amount of the high-strength steel member for spot welding joint is more preferably 0.31 mass %, 0.33 mass %, 0.36 mass % or 0.40 mass %. The carbon amount of the high-strength steel member for spot welding joint is more preferably 0.50 mass %, 0.48 mass %, 0.45 mass %, 0.42 mass % or 0.40 mass %. In addition, similarly to the manufacturing method of the spot welding joint 1 of the second embodiment, the surface treatment portion 24 can also be provided on the entire one surface or the entire two surfaces of the high-strength steel member.

[0168] The method for measuring the carbon content of the high-strength steel member is the same as the method for measuring the carbon content of the high-strength steel plate portion 11H of the spot welded joint 1 of the first embodiment. However, the sample for measuring the carbon content is extracted from a portion 10 to 30 mm away from the end face of the high-strength steel member. When extracting the sample, the surface of the steel plate portion is shaved off by more than 0.1 mm to remove the plating layer and contamination.

[0169] <Method for Manufacturing High-Strength Steel Member According to Fourth Embodiment>

[0170] Next, a method for manufacturing a high-strength steel member 2H for a spot welded joint according to a fourth embodiment of the present invention is described. The method for manufacturing a high-strength steel member 2H for a spot welded joint according to the fourth embodiment of the present invention includes a step of forming a surface treatment portion 24 on the surface of a high-strength steel member having a Vickers hardness of 530 HV or more, not providing a plating layer in the surface treatment portion 24, setting the ten-point average roughness of the surface treatment portion 24 to 3.5 μm or less, and setting the oxygen concentration of the surface treatment portion 24 to 18.0 mass % or less.

[0171] The Vickers hardness of the high-strength steel component 2H obtained by the manufacturing method of the fourth embodiment is 530HV or more. Therefore, according to the manufacturing method of the high-strength steel component of the fourth embodiment, it is possible to provide a steel plate portion 11 that can manufacture a very high-strength spot welding joint 1. However, the TSS of the spot weld 12 obtained by spot welding a high-strength steel component having a Vickers hardness of 530HV or more is poor. Therefore, in the manufacturing method of the high-strength steel component of the fourth embodiment, the ten-point average roughness is less than 3.5μm, the oxygen concentration is less than 18.0 mass%, and a surface treatment portion 24 without a coating is formed. In the plastic metal ring area 122 obtained by spot welding the surface treatment portion 24, there is no coating 13, and the oxygen concentration becomes less than 15.0 mass%. Therefore, according to the manufacturing method of the high-strength steel component of the fourth embodiment, it is possible to provide a high-strength steel component that can dramatically improve the TSS of the spot welding joint 1.

[0172] As long as the above-mentioned necessary conditions are satisfied, the method for manufacturing the high-strength steel member of the fourth embodiment can obtain the TSS improvement effect of the spot welded joint 1. On the other hand, the preferred embodiments of the spot welded joint 1 of the first embodiment, the method for manufacturing the spot welded joint 1 of the second embodiment, and the high-strength steel member for the spot welded joint of the third embodiment can also be applied to the method for manufacturing the high-strength steel member of the fourth embodiment.

[0173] The method for measuring the Vickers hardness of the high-strength steel member is the same as the method for measuring the Vickers hardness of the high-strength steel plate portion in the method for manufacturing the spot welded joint 1 of the second embodiment.

[0174] The method for measuring the ten-point average roughness and oxygen concentration of the surface treated portion 24 of the high-strength steel member is the same as the method for measuring the ten-point average roughness and oxygen concentration of the surface treated portion 24 in the method for manufacturing a spot welded joint of the second embodiment.

[0175] (Hot stamping and removal of plating)

[0176] The method for manufacturing a high-strength steel member may further include a step of hot stamping the high-strength steel sheet. In this case, it is preferred that the high-strength steel sheet be hot stamped before the surface treatment portion 24 is formed in the high-strength steel sheet. Then, in the step of forming the surface treatment portion 24, it is preferred that the surface treatment portion 24 be formed on the surface of the high-strength steel member after hot stamping. Thereby, it is possible to avoid an increase in the oxygen concentration of the surface treatment portion 24 caused by heating for hot stamping.

[0177] The method for manufacturing the spot welded joint 1 may also include a step of removing a portion of the plating layer on the surface of the high-strength steel member before forming the surface treated portion 24. In this case, in the step of forming the surface treated portion, the surface treated portion is preferably formed in the region where the plating layer is removed. Thus, a high-strength steel member can be provided in which a plastic metal ring region without a plating layer can be manufactured.

[0178] (Carbon content: preferably more than 0.30 mass %)

[0179] (Position of the surface treatment portion 24: preferably the entire one surface or the entire two surfaces)

[0180] (Means for forming the surface treatment portion 24: preferably wet sandblasting)

[0181] For example, similarly to the high-strength steel plate portion 11H of the spot welding joint 1 of the first embodiment, the carbon amount of the high-strength steel member 2H provided for the manufacturing method of the fourth embodiment can also be set to more than 0.30 mass%. Thus, the various mechanical properties of the spot welding joint 1 can be further improved. In addition, similarly to the manufacturing method of the spot welding joint 1 of the second embodiment, a surface treatment portion 24 can also be provided on the entire surface or the entire two surfaces of the high-strength steel member 2H. In addition, similarly to the manufacturing method of the spot welding joint of the second embodiment, the means for forming the surface treatment portion 24 is not particularly limited, but it is preferred that the means is set to shot blasting or wet sand blasting. In addition, the surface treatment portion 24 can also be formed by grinding. The various processing conditions for forming the surface treatment portion 24 illustrated in the second embodiment can also be applied to the manufacturing method of the fourth embodiment.

[0182] The method for measuring the carbon amount of the high-strength steel member 2H is the same as the method for measuring the carbon amount of the high-strength steel member according to the third embodiment.

[0183] Example

[0184] The effects of one embodiment of the present invention are described in more detail by way of an embodiment. However, the conditions in the embodiment are merely a conditional example adopted to confirm the feasibility and effects of the present invention. The present invention is not limited to this conditional example. As long as it does not deviate from the gist of the present invention and achieves the purpose of the present invention, the present invention may adopt various conditions.

[0185] (Example 1)

[0186] Spot welding is performed on two high-strength steel plates with a thickness of 1.6 mm and a Vickers hardness of 580 HV (tensile strength of 2000 MPa) to produce a spot welding joint. However, for the example of No. 20, it is not set to the above-mentioned high-strength steel plate, but is set to a spot welding joint obtained by spot welding two ordinary steel plates with a thickness of 1.6 mm and a Vickers hardness of 310 HV (tensile strength of 980 MPa), and for the example of No. 22, it is not set to the above-mentioned high-strength steel plate, but is set to a spot welding joint obtained by spot welding two ordinary steel plates with a thickness of 1.6 mm and a Vickers hardness of 460 HV (tensile strength of 1500 MPa). It should be noted that the high-strength steel plate with a tensile strength of 2000 MPa is a steel plate that has been subjected to heat treatment of a steel member after simulating hot stamping, and the steel plate with a tensile strength of 980 MPa and the steel plate with a tensile strength of 1500 MPa are ordinary cold-rolled steel plates that are not subjected to heat treatment.

[0187] A surface treatment portion was formed on each surface of the two steel plates before spot welding. Table 1 shows the ten-point average roughness and oxygen concentration of the surface treatment portion.

[0188] The oxygen concentration and nugget diameter of the plastic metal ring zone of each spot welded joint obtained by the above-mentioned procedure were measured and are shown in Table 1. Furthermore, the TSS increase rate of each spot welded joint was evaluated and is shown in Table 1.

[0189] The so-called TSS increase rate refers to the increase rate of TSS relative to the TSS reference value recorded in Table 2. The TSS reference value is the TSS of the spot welded joint obtained by performing ordinary shot peening on two high-strength steel plates of each tensile strength of 1.6 mm in thickness and then spot welding. It should be noted that TSS varies depending on the diameter of the nugget, so the reference value corresponding to the nugget diameter is recorded in Table 2. The meanings of the symbols of the TSS increase rate recorded in Table 1 are as follows.

[0190] · Spot welds with TSS below the reference value: D

[0191] Spot welds with a TSS increase rate of more than 0% and less than 5% relative to the reference value: C

[0192] Spot welds with a TSS increase rate of more than 5% and less than 20% relative to the reference value: B

[0193] · Spot welds with a TSS increase of 20% or more relative to the reference value: A

[0194] [Table 1]

[0195]

[0196] [Table 2]

[0197]

[0198] The oxygen concentrations in the plastic metal ring region of Comparative Examples 2, 5 and 7 are outside the scope of the invention. In these Comparative Examples, no increase in TSS relative to the TSS reference value was observed. It is presumed that the reason why the oxygen concentrations in the plastic metal ring region are high in these Comparative Examples is that the oxygen concentration in the surface treated portion before spot welding is excessive.

[0199] Although the oxygen concentration in the plastic metal ring zone of Comparative Example 20 is within the scope of the invention, no increase in TSS relative to the TSS baseline value is observed. It is presumed that this is because the tensile strength of the base material of the spot welded joints of Comparative Example 20 is 980 MPa. Similarly, in Comparative Example 22, although the oxygen concentration in the plastic metal ring zone is also within the scope of the invention, no increase in TSS relative to the TSS baseline value is observed. It is presumed that this is because the tensile strength of the base material of the spot welded joints of Comparative Example 22 is 1500 MPa. The correlation between the oxygen concentration in the plastic metal ring zone and TSS is only confirmed in high-strength steel plates with a Vickers hardness of 530 HV or more.

[0200] The oxygen concentration of the plastic metal ring region of Comparative Example 21 is outside the scope of the invention. In these comparative examples, no increase in TSS relative to the TSS reference value was observed. It is presumed that the reason why the oxygen concentration of the plastic metal ring region is high in this comparative example is that the ten-point average roughness of the surface treatment portion before spot welding is excessive, so the oxygen concentration of the plastic metal ring region increases through spot welding.

[0201] On the other hand, in the examples within the scope of the present invention, it is possible to provide a spot welded joint having excellent TSS despite including one or more high-strength steel sheets having a Vickers hardness of 530 HV or more.

[0202] (Example 2)

[0203] The various high-strength steel plates listed in Table 3 were subjected to hot stamping treatment to manufacture high-strength steel components. In the hot stamping treatment, the high-strength steel plate was heated to 890°C, maintained for 5 minutes, and then cooled using a water-cooled mold. Then, the test piece was taken out from the flat surface of the high-strength steel component by laser cutting. The test pieces of these high-strength steel components were subjected to wet sandblasting according to the conditions listed in Table 4, shot peening according to the conditions listed in Table 5, or cutting according to the conditions listed in Table 6, thereby forming a surface treatment portion. The ten-point average roughness and oxygen concentration of the surface treatment portion were measured by the above-mentioned means and are recorded in Table 7.

[0204] [Table 3]

[0205]

[0206] [Table 4]

[0207]

[0208] [Table 5]

[0209]

[0210] [Table 6]

[0211]

[0212] [Table 7]

[0213]

[0214] In Sample No. 1, wet blasting was performed under appropriate conditions. In Sample No. 1, the ten-point average roughness and oxygen concentration of the surface treated portion formed by wet blasting were appropriate.

[0215] In the case of Sample No. 2, the projection distance during wet blasting was too long. In the case of Sample No. 2, the oxygen concentration of the surface treatment portion formed by wet blasting became excessive. It is presumed that this is because the projection distance was too long, and therefore the oxides present on the surface of the steel member were not sufficiently removed.

[0216] In Sample No. 3, the diameter of the abrasive used in wet blasting was too large. In Sample No. 3, both the ten-point average roughness and the oxygen concentration of the surface treated portion formed by wet blasting became excessive. This is presumed to be because the diameter of the abrasive was too large, so the surface of the steel member became rough, and the removal of oxides existing on the surface became insufficient.

[0217] In Sample No. 4, shot peening was performed under appropriate conditions. In Sample No. 4, the ten-point average roughness and oxygen concentration of the surface treated portion formed by shot peening were appropriate.

[0218] In the case of sample No. 5, the projection distance during shot peening was too long. In the case of sample No. 5, the oxygen concentration of the surface treatment portion formed by shot peening became excessive. It is estimated that this is because the projection distance was too long, so the oxides existing on the surface of the steel member were not removed sufficiently.

[0219] In the case of Sample No. 6, the diameter of the projection material used in shot peening was too large. In the case of Sample No. 6, both the ten-point average roughness and the oxygen concentration of the surface treatment portion formed by shot peening became excessive. It is estimated that this is because the diameter of the projection material was too large, so the surface of the steel member became rough, and the removal of oxides existing on the surface became insufficient.

[0220] In Sample No. 7, cutting was performed under appropriate conditions. In Sample No. 7, the ten-point average roughness and oxygen concentration of the surface treated portion formed by cutting were appropriate.

[0221] In the case of sample No. 8, the cutting depth during cutting was too large. In the case of sample No. 8, the ten-point average roughness of the surface treatment portion formed by cutting became excessive. This is presumably because the cutting depth was too large, causing chattering and making the surface rough.

[0222] For Sample 9, cutting was performed under appropriate conditions. For Sample No. 9, the ten-point average roughness and oxygen concentration of the surface treatment portion formed by cutting were appropriate. It should be noted that the TSS of Sample 9 was measured for reference, and the evaluation was performed based on the TSS evaluation standard used in Example 1. As a result, the TSS increase rate of Sample 9 was more than 20%. It should be noted that the reference value of the TSS increase rate in the weld joint formed by combining the steel member No. 1 and the steel member No. 2 recorded in Table 3 is 23 kN when the nugget diameter is 5.0 mm, 25 kN when the nugget diameter is 5.5 mm, and 27 kN when the nugget diameter is 6.0 mm.

[0223] In the case of Sample 10, a steel member having a zinc-based coating is used as a starting material. In the case of Sample 10, first, the zinc-based coating of the steel member is removed to form a coating removal portion. Next, after waiting for the temperature of the coating removal portion to drop to room temperature, cutting is performed to form a surface treatment portion. In the case of Sample 10, the zinc-based coating is removed before forming the surface treatment portion, and then cutting is performed under appropriate conditions. In the case of Sample No. 10, the ten-point average roughness and oxygen concentration of the surface treatment portion formed by cutting are appropriate.

[0224] As for Sample No. 11, similarly to Sample No. 10, a steel member having a zinc-based coating was used as a starting material. However, in Sample No. 11, the zinc-based coating was not removed before cutting to form the surface treatment portion. Specifically, the zinc-based coating was removed and the surface treatment portion was formed in one process by cutting the portion where the zinc-based coating existed under Condition G1. In Sample No. 11, the oxygen concentration of the surface treatment portion formed by cutting became excessive.

[0225] Explanation of symbols

[0226] 1 spot welding joint

[0227] 11 Steel Plate Department

[0228] 11H High strength steel plate

[0229] 12 Spot welding

[0230] 121 Core

[0231] 122 Plastic metal ring area

[0232] 123 Plastic metal ring area

[0233] 13 Plating

[0234] 2 Steel components

[0235] 2H High Strength Steel Components

[0236] 24 Surface treatment department

[0237] E Electrode

[0238] Ox Oxide

Claims

1. A spot welding joint, comprising: A plurality of steel plate portions including a high-strength steel plate portion having a Vickers hardness of 530 HV or more; a nugget for joining the high-strength steel sheet portion to the other steel sheet portions among the plurality of steel sheet portions; and a plastic metal ring region formed in a ring shape around the nugget in a top view observed from a direction perpendicular to the surface of the high-strength steel plate portion, and solid-phase bonding the high-strength steel plate portion with the other steel plate portions, In the area where the plastic metal ring zone is present, there is no plating layer, The oxygen concentration of the plastic metal ring region at a position 50 μm outside the outer periphery of the nugget in the plan view is 15.0 mass % or less.

2. The spot welding joint according to claim 1, It is characterized in that The carbon content of the high-strength steel sheet portion exceeds 0.30 mass %.

3. The spot welding joint according to claim 1 or 2, It is characterized in that The carbon content of the nugget is 0.29 mass % or more.

4. The spot welding joint according to claim 1 or 2, It is characterized in that In a cross section passing through the center of the nugget and perpendicular to the surface of the steel sheet portion, a diameter of the nugget measured along a boundary line of adjacent steel sheet portions is 4.5√t or more, Here, t refers to the smaller one of the plate thicknesses of the two adjacent steel plate portions constituting the boundary line.

5. A method for manufacturing a spot welding joint, comprising the following steps: A process for providing a high-strength steel member having a surface-treated portion with a Vickers hardness of 530 HV or more; A step of overlapping a plurality of the steel members in such a manner that the surface treatment portion is arranged on a joining surface between the high-strength steel member and other steel members; In a plan view viewed from a direction perpendicular to the surface treatment portion, a plurality of the steel members are spot welded in such a manner that a nugget and a plastic metal ring area are contained inside the surface treatment portion. In the overlapping step, no plating layer is provided on the surface treatment portion and a region in contact with the surface treatment portion. The ten-point average roughness of the surface treated portion is 3.5 μm or less, and the oxygen concentration of the surface treated portion is 18.0 mass % or less.

6. The method for manufacturing a spot welding joint according to claim 5, It is characterized in that Before the step of providing the high-strength steel member, the method further includes forming the surface treated portion on the surface of the high-strength steel member.

7. The method for manufacturing a spot welding joint according to claim 6, It is characterized in that Before forming the surface treatment portion, the process further comprises hot stamping the high-strength steel sheet. In the step of forming the surface treated portion, the surface treated portion is formed on the surface of the high-strength steel member after the hot stamping.

8. The method for manufacturing a spot welding joint according to claim 6 or 7, It is characterized in that Before forming the surface treated portion, a step of removing a portion of the plating layer on the surface of the high-strength steel member is provided. In the step of forming the surface treatment portion, the surface treatment portion is formed in a region where the plating layer is removed.

9. The method for manufacturing a spot welding joint according to claim 5 or 6, It is characterized in that The carbon content of the high-strength steel member is set to exceed 0.30 mass %.

10. The method for manufacturing a spot welding joint according to claim 5 or 6, It is characterized in that The carbon content of the nugget formed by the spot welding is set to 0.29 mass % or more.

11. The method for manufacturing a spot welding joint according to claim 5 or 6, It is characterized in that The diameter of the nugget formed by the spot welding is set to be 4.5√t or more, Here, the diameter of the nugget refers to the size of the nugget measured along the boundary line of the adjacent steel members in a plane passing through the center of the nugget and perpendicular to the surface of the steel member, and t refers to the smaller of the plate thicknesses of the two adjacent steel members constituting the boundary line.

12. The method for manufacturing a spot welding joint according to claim 6 or 7, It is characterized in that The surface treatment portion is formed by shot blasting or wet blasting.

13. A high-strength steel component for spot welding joints, having a Vickers hardness of 530 HV or more, Has a surface treatment portion without a plating layer, The ten-point average roughness of the surface treatment portion is 3.5 μm or less, The surface treated portion has an oxygen concentration of 18.0 mass % or less.

14. The high-strength steel member for spot welding joint according to claim 13, It is characterized in that The carbon content exceeds 0.30 mass %.

15. The high-strength steel member for spot welding joint according to claim 13 or 14, It is characterized in that The surface treatment portion is provided on the entire surface of the high-strength steel member.

16. A method for manufacturing a high-strength steel member for a spot welding joint, comprising the step of forming a surface treatment portion on a surface of a high-strength steel member having a Vickers hardness of 530 HV or more, No plating layer is provided on the surface treatment portion, The ten-point average roughness of the surface treatment portion is set to 3.5 μm or less. The oxygen concentration of the surface treated portion is set to 18.0 mass % or less.

17. The method for manufacturing a high-strength steel member for a spot welded joint according to claim 16, It is characterized in that Before forming the surface treatment portion, the process further comprises hot stamping the high-strength steel sheet. In the step of forming the surface treated portion, the surface treated portion is formed on the surface of the high-strength steel member after the hot stamping.

18. The method for manufacturing a high-strength steel member for a spot welded joint according to claim 16 or 17, It is characterized in that Before forming the surface treated portion, a step of removing a portion of the plating layer on the surface of the high-strength steel member is provided. In the step of forming the surface treatment portion, the surface treatment portion is formed in a region where the plating layer is removed.

19. The method for manufacturing a high-strength steel member for a spot welded joint according to claim 16 or 17, It is characterized in that The carbon content of the high-strength steel member is set to exceed 0.30 mass %.

20. The method for manufacturing a high-strength steel member for a spot welded joint according to claim 16 or 17, It is characterized in that The surface treatment portion is provided on the entire surface of the high-strength steel member.

21. The method for manufacturing a high-strength steel member for a spot welded joint according to claim 16 or 17, It is characterized in that The surface treatment portion is formed by shot blasting or wet blasting.