Porous polyester-based film, resin composition, and method for manufacturing resin composition

By adding silicone resin to the polyolefin resin, the problems of easy deformation and poor heat resistance of the polypropylene resin holes are solved, and the lightweight, film-forming and whiteness of the polyester film is achieved, and it is suitable for labels and cards. , packaging materials and other uses.

CN119013144APending Publication Date: 2024-11-22TOYOBO CO LTD

Patent Information

Application Number
CN202380031725.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-04-15
Filing Date
2023-04-04
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

In the prior art, when using polypropylene resin as the hole embodier, the holes are easily crushed, resulting in poor lightweight and buffering properties. At the same time, the heat resistance of surfactants and polyethylene glycol is poor, resulting in a decrease in the whiteness of the film and The membrane-forming properties deteriorate.

Method used

Add extremely small amounts of silicone resin to the polyolefin resin, adjust the laminated composition and the amount of silicone resin to improve the heat resistance and stiffness of the polyolefin dispersed particles, reduce deformation, and suppress side effects such as coating and printing deterioration.

Benefits of technology

The polyester-based film has excellent lightweight, film-making properties, covering properties and whiteness, and the holes are not easily crushed under high temperature environments, maintaining the hole embodying.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005066511520000211
    Figure BDA0005066511520000211
Patent Text Reader

Abstract

Provided is a void-containing polyester film having excellent lightness, film-forming properties, covering properties, and whiteness even when mainly using a polyolefin resin (e.g., a polypropylene resin) as a void-embodying agent. The void-containing polyester film is a laminate in which a first coating layer (B1) containing a polyester resin containing an inorganic pigment, a void-containing layer (A) having voids therein, and a second coating layer (B2) containing a polyester resin containing an inorganic pigment are laminated in this order. The void-containing layer A contains a composition containing a polyester resin, a polyolefin resin, and a silicone resin. In addition, the apparent density of the void-containing polyester film is from 0.80 g / cm3 to 1.20 g / cm3 (inclusive). The inorganic pigment in the first coating layer B1 and the second coating layer B2 is, for example, titanium oxide.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a void-containing polyester film having voids inside, a resin composition obtained by material recovery of the void-containing polyester film, and a method for producing the resin composition. Background Art

[0002] As a method for obtaining a film having a function similar to that of paper, a method of making a film contain a large number of fine pores inside the film is known.

[0003] The method is as follows: a non-miscible thermoplastic resin (hereinafter referred to as non-miscible resin) is mixed in a polyester resin to obtain a sheet in which the non-miscible resin is dispersed in the polyester resin, and the sheet is stretched at least in a uniaxial direction. Thus, the method forms voids by peeling off the interface between the polyester resin and the non-miscible resin. As such non-miscible resins, polyolefin resins such as polyethylene resin, polypropylene resin, and polymethylpentene resin (for example, see patent documents 1 to 3), and polystyrene resin (for example, see patent documents 4 and 5) are proposed. Among these, polypropylene resin is particularly preferred in terms of void formation and cost performance.

[0004] Here, when the polypropylene resin is simply dispersed in the polyester resin, the dispersion diameter of the polypropylene dispersed particles becomes larger. Therefore, the holes are easy to form, but on the other hand, the holes become larger, sufficient covering power cannot be obtained, and the film-forming property also deteriorates. Therefore, a method of microdispersing the polypropylene resin is adopted. So far, as a method for the microdispersion, a method of adding a dispersant such as a surfactant or polyethylene glycol has been proposed (for example, refer to Patent Documents 6 and 7).

[0005] Prior art literature

[0006] Patent Literature

[0007] Patent Document 1: Japanese Patent Application Laid-Open No. 49-134755

[0008] Patent Document 2: Japanese Patent Application Laid-Open No. 2-284929

[0009] Patent Document 3: Japanese Patent Application Laid-Open No. 2-180933

[0010] Patent Document 4: Japanese Patent Publication No. 54-29550

[0011] Patent Document 5: Japanese Patent Application Laid-Open No. 11-116716

[0012] Patent Document 6: Japanese Patent Publication No. 7-17779

[0013] Patent Document 7: Japanese Patent Application Laid-Open No. 8-252857 Summary of the invention

[0014] Problem that the invention aims to solve

[0015] However, when a dispersant such as a surfactant or polyethylene glycol is added, although there is a micro-dispersion effect on the polypropylene resin, the polypropylene resin will deform in the heating and stretching process and the heat setting process. Therefore, the obtained holes are also easily crushed, and sufficient lightness and cushioning properties cannot be obtained. In addition, the heat resistance of surfactants and polyethylene glycol is poor, so in the melt extrusion process combined with polyester resin, thermal degradation is easily generated, and the whiteness of the obtained film will be reduced. Depending on the situation, there is a problem of promoting the degradation of the polyester resin and worsening the film-forming property.

[0016] The object of the present invention is to improve the above-mentioned problems of the prior art and provide a void-containing polyester film which is excellent in lightness, film-forming properties, hiding power and whiteness when a polyolefin resin (e.g., polypropylene resin) is mainly used as a void-forming agent. Another object of the present invention is to provide a resin composition obtained by material recycling of a void-containing polyester film and a method for producing the resin composition.

[0017] Solutions for solving problems

[0018] The inventors of the present invention have conducted in-depth research and found the following by adding a very small amount of silicone resin to a polyolefin resin (e.g., polypropylene resin). That is, the inventors of the present invention have found that the heat resistance or rigidity of polyolefin dispersed particles (e.g., polypropylene dispersed particles) in the polyester resin can be improved by silicone resin, and the deformation of polyolefin dispersed particles (e.g., polypropylene dispersed particles) during heating, stretching, and heat setting can be reduced. As a result, the inventors of the present invention have found that a porous polyester film with excellent lightness, film-forming properties, hiding properties, and whiteness can be obtained. Furthermore, the inventors of the present invention have found that by adjusting the stacking structure and the amount of silicone resin added, the deterioration of coating and printing properties, which are side effects of silicone resin, can be suppressed.

[0019] That is, the void-containing polyester film of the present invention has the following configuration.

[0020] 1. A porous polyester film comprising:

[0021] The first cover layer B1 comprises a polyester resin containing an inorganic pigment,

[0022] A hole-containing layer A having holes inside, and

[0023] The second cover layer B2 comprises a polyester resin containing an inorganic pigment,

[0024] The porous polyester film is sequentially laminated with a first covering layer B1, a porous layer A and a second covering layer B2.

[0025] The void-containing layer A comprises a composition containing polyester resin, polyolefin resin and silicone resin. The apparent density of the void-containing polyester film is 0.80 g / cm 3 Above and 1.20g / cm 3 the following.

[0026] 2. The void-containing polyester film according to 1., wherein in the void-containing layer A, the content of polydimethylsiloxane in the silicone resin is 1 ppm or more and 2500 ppm or less relative to the total mass of the void-containing layer A.

[0027] 3. The void-containing polyester film according to 1. or 2., wherein in the void-containing layer A, the content of polydimethylsiloxane in the silicone resin is 0.005 mass % or more and 2.000 mass % or less relative to 100 mass % of the polyolefin resin.

[0028] 4. The void-containing polyester film according to any one of 1. to 3., wherein the inorganic pigment in the first covering layer B1 and the second covering layer B2 is titanium oxide.

[0029] 5. The void-containing polyester film according to any one of 1. to 4., wherein the ratio of the total thickness of the first covering layer B1 and the second covering layer B2 to the total thickness of the first covering layer B1, the void-containing layer A and the second covering layer B2 is greater than 6% and less than 40%.

[0030] 6. The void-containing polyester film according to any one of 1. to 5., wherein the total light transmittance is 1% to 30%.

[0031] 7. The void-containing polyester film according to any one of 1. to 6., wherein the apparent density is 0.80 g / cm 3 Above and 1.10g / cm 3 the following.

[0032] 8. The void-containing polyester film according to any one of 1. to 7., which is used for labels, cards, packaging materials or release films.

[0033] 9. A resin composition obtained by material recovery of the void-containing polyester film according to any one of 1. to 8., the resin composition comprising an inorganic pigment, a polyester resin, a polyolefin resin and a silicone resin.

[0034] 10. A method for producing a resin composition, comprising recovering the void-containing polyester film according to any one of 1. to 8. to produce a resin composition containing an inorganic pigment, a polyester resin, a polyolefin resin and a silicone resin.

[0035] 11. The method for producing the void-containing polyester film according to any one of 1. to 8., the resin composition according to 9., or the resin composition according to 10., wherein the polyolefin resin is a polypropylene resin.

[0036] Effects of the Invention

[0037] The present invention can provide a void-containing polyester film which is excellent in lightness, film-forming properties, hiding power, and whiteness when the film mainly contains a polyolefin resin (for example, a polypropylene resin) as a void-developing agent. DETAILED DESCRIPTION

[0038] The present invention is described in detail below. It should be noted that in this specification, expressions such as "at least a first covering layer B1, a hole-containing layer A, and a second covering layer B2 are stacked in sequence" are sometimes used. This expression and expressions similar to it are expressions that allow the existence of any layer between the first covering layer B1 and the hole-containing layer A, and / or between the hole-containing layer A and the second covering layer B2.

[0039] The void-containing polyester film of the present invention includes a void-containing layer A containing a polyolefin resin. Examples of the polyolefin resin include polypropylene resin, polyethylene resin, and polymethylpentene resin. Examples of the polyolefin resin include cyclic polyolefin resins. Examples of the cyclic polyolefin resin include: polymers obtained by hydrogenating ring-opening copolymers of cyclic olefins as needed; addition (co)polymers of cyclic olefins; random copolymers of cyclic olefins and α-olefins; and grafted modified products obtained by modifying at least one of them with unsaturated carboxylic acids or their derivatives. Among them, polypropylene resin is preferred in terms of void expression and cost performance.

[0040] Hereinafter, an embodiment in which the polyolefin resin is a polypropylene resin will be described. The description of polyolefin resins other than the polypropylene resin overlaps with the description of the polypropylene resin and is therefore omitted. Therefore, the description of the polypropylene resin described later (e.g., the description of the melt flow rate, the deflection temperature under load, the weight average molecular weight, the molecular weight distribution, and the content) can also be treated as the description of the polyolefin resin other than the polypropylene resin. For example, the description of the melt flow rate of the polypropylene resin described later can also be treated as the description of the melt flow rate of the polyolefin resin, and the description of the content of the polypropylene resin described later can also be treated as the description of the content of the polyolefin resin.

[0041] The void-containing polyester film of the present invention is a laminated body in which a first covering layer B1 containing a polyester resin containing an inorganic pigment, a void-containing layer A having voids inside, and a second covering layer B2 containing a polyester resin containing an inorganic pigment are sequentially laminated. The void-containing layer A contains a composition containing a polyester resin, a polyolefin resin, and a silicone resin. In addition, the apparent density of the void-containing polyester film is 0.80 g / cm 3 Above and 1.20g / cm 3 the following.

[0042] The polyester resin that is the main component of the void-containing layer A, the first cover layer B1, and the second cover layer B2 is a polymer synthesized from dicarboxylic acid or its ester-forming derivative and diol or its ester-forming derivative. Representative examples of such polyester resins include polyethylene terephthalate, polybutylene terephthalate, and polyethylene 2,6-naphthalate. Among these, polyethylene terephthalate is preferred from the viewpoints of mechanical properties, heat resistance, cost, etc.

[0043] In addition, other components may be copolymerized in these polyester resins as long as they do not impair the purpose of the present invention. Specifically, as copolymerization components, among the dicarboxylic acid components, isophthalic acid, naphthalene dicarboxylic acid, 4,4-diphenyl dicarboxylic acid, adipic acid, sebacic acid and ester-forming derivatives thereof may be cited. In addition, as diol components, diethylene glycol, hexamethylene glycol, neopentyl glycol and cyclohexanedimethanol may be cited. In addition, polyoxyalkylene glycols such as polyethylene glycol and polypropylene glycol may also be cited. As the copolymerization amount, it is preferably within 10 mol% and more preferably within 5 mol% in the unit repeating unit.

[0044] The polyester resin is produced by, for example, firstly using the above-mentioned dicarboxylic acid or its ester-forming derivative and diol or its ester-forming derivative as main starting materials, then subjecting them to esterification or transesterification reaction according to a conventional method, and then subjecting them to polycondensation reaction under high temperature and reduced pressure.

[0045] The intrinsic viscosity of the polyester resin is preferably 0.50 dl / g to 0.9 dl / g, more preferably 0.55 dl / g to 0.85 dl / g, from the viewpoints of film forming properties, recyclability, and the like.

[0046] The content of the polyester resin is preferably 70% by mass or more and 97% by mass or less, and more preferably 75% by mass or more and 95% by mass or less, relative to 100% by mass of the total of all components contained in the void-containing layer A. When the content of the polyester resin is 70% by mass or more, the void-containing polyester film can suppress the deterioration of film-forming properties. When the content of the polyester resin is 97% or less, the void-containing polyester film can form voids by adding polypropylene resin and silicone resin.

[0047] Next, the incompatible resin used as the void-developing agent in the present invention, that is, the polypropylene resin, is described. The void-containing polyester film of the present invention can maintain void-developing properties by adopting a specific layer structure and using a polypropylene resin. As a result, the void-containing polyester film of the present invention has sufficient lightness and cushioning properties, and is excellent in film-forming properties, hiding properties, and whiteness.

[0048] The polypropylene resin used in the present invention is preferably a crystalline polypropylene having 95 mol% or more, more preferably 98 mol% or more of propylene units, and is particularly preferably a crystalline polypropylene homopolymer having 100 mol% of propylene units.

[0049] For the polypropylene resin used in the present invention, from the viewpoint of hole expression and film forming property, the melt flow rate (MFR) is preferably 1.0 g / 10 minutes or more and 10.0 g / 10 minutes or less, and more preferably 1.5 g / 10 minutes or more and 7.0 g / minute or less. When the MFR is 1.0 g / 10 minutes or more and 10.0 g / 10 minutes or less, the polypropylene dispersed particles are not easily deformed when extruded from the die, so it becomes easy to form holes. Furthermore, when the MFR is 1.0 g / 10 minutes or more and 10.0 g / 10 minutes or less, the dispersibility of the polypropylene dispersed particles is also excellent, sufficient covering property is obtained, and film forming property is also excellent. It should be noted that the melt flow rate (MFR) is a measured value based on JIS K 7210 at 230°C and a load of 2.16 kg.

[0050] In the polypropylene resin used in the present invention, from the viewpoint of void expression, the deflection temperature under load is preferably 85°C or more, more preferably 90°C or more, and further preferably 95°C or more. The upper limit is not particularly limited, but is preferably 135°C or less. When the deflection temperature under load is 85°C or more, in particular, in the longitudinal stretching process of heating and stretching the film at a temperature above the glass transition temperature of the polyester resin described later, the dispersed particles of the polypropylene become less likely to be crushed, and therefore, voids become easily formed. It should be noted that the deflection temperature under load is a measured value when the bending stress of the test piece is 0.45 MPa according to the B method of JIS K 7191-1, 2.

[0051] For the polypropylene resin used in the present invention, from the viewpoint of hole manifestation, suppression of thermal degradation in the extrusion process and the recycling process, the weight average molecular weight (Mw) is preferably 200,000 or more and 450,000 or less, and more preferably 250,000 or more and 400,000 or less. When Mw is 450,000 or less, the dispersibility of the polypropylene dispersed particles becomes good, sufficient covering property is obtained, and excellent film forming property is obtained. When Mw is 200,000 or more, the polypropylene dispersed particles become less deformable, and therefore, holes are easily formed. When Mw is 200,000 or more, when recycled raw materials are used, the decrease in hole manifestation can also be suppressed, so it is preferred.

[0052] In addition, the ratio of weight average molecular weight (Mw) to number average molecular weight (Mn), i.e. molecular weight distribution (Mw / Mn), is preferably 2 or more and 6 or less, more preferably 2 or more and 5 or less. Mw / Mn is an index representing the molecular weight distribution amplitude, and the larger the value, the wider the molecular weight distribution. When Mw / Mn is less than 6, low molecular weight components are reduced, and therefore, when using recycled raw materials, the reduction of whiteness and hole embodiment can also be suppressed and is preferred. In addition, if Mw / Mn is more than 2, it is suitable for industrial production from the viewpoint of cost. It should be noted that weight average molecular weight (Mw) and number average molecular weight (Mn) are values ​​measured by gel permeation chromatography (GPC).

[0053] The content of the polypropylene resin is preferably 3% by mass or more and 30% by mass or less, and more preferably 5% by mass or more and 25% by mass or less, based on 100% by mass of the total of all components contained in the void-containing layer A. When the content of the polypropylene resin is 3% by mass or more and 30% by mass or less, voids can be formed to obtain sufficient lightness and cushioning properties, and excellent film forming properties are achieved.

[0054] Examples of the silicone resin used in the present invention include silicone polymers, such as partially cross-linked silicone polymers (i.e., silicone resins belonging to silicone resins in a narrow sense) and linear silicone polymers (i.e., silicone rubbers). Specifically, examples include methyl silicone resins, methylphenyl silicone resins, phenyl silicone resins, alkyd-modified silicone resins, polyester-modified silicone resins, urethane-modified silicone resins, epoxy-modified silicone resins, and acrylic-modified silicone resins. From the perspective of being able to withstand the extrusion temperature of the polyester resin belonging to the base resin and suppressing process contamination caused by sublimation, silicone resins having a cross-linked structure are preferred.

[0055] There is no particular limitation on the method of adding the silicone resin. The silicone resin may be added directly by dry-mixing the silicone resin in powder or pellet form with the base resin. It may also be prepared in advance as a masterbatch of melt-mixed polyester resin, polypropylene resin, and silicone resin. It may also be added by recovering the silicone resin contained in the release layer of the release polyester film together with the polyester film and adding the obtained polyester pellets containing the silicone resin.

[0056] The amount of the silicone resin added is preferably 1 ppm or more and 10,000 ppm or less, and more preferably 100 ppm or more and 8,000 ppm or less, relative to the total mass of the hole-containing layer A, from the viewpoints of hole expression, film forming property, and manufacturing cost. By setting it to 1 ppm or more, the apparent density can be efficiently reduced. By setting it to 10,000 ppm or less, the process pollution and the deterioration of film forming property can be suppressed. The manufacturing cost can be further suppressed.

[0057] The content of polydimethylsiloxane derived from silicone resin is obtained by NMR (nuclear magnetic resonance) method. For the content of polydimethylsiloxane derived from silicone resin, from the viewpoint of pore manifestation, film forming property, and manufacturing cost, relative to the total mass of the hole-containing layer A, it is preferably 1 ppm or more and 2500 ppm or less, and further preferably 100 ppm or more and 2400 ppm or less. It is further more preferably 100 ppm or more and 1400 ppm or less. By setting it to more than 1 ppm, the apparent density can be efficiently reduced. By setting it to less than 2500 ppm, the deterioration of process pollution and film forming property can be suppressed. The manufacturing cost can be further suppressed. The silicone resin has a cross-linked structure and is insoluble in solvents. Therefore, the content of polydimethylsiloxane present in the silicone resin is obtained by the NMR measurement method described later, so that an index of the content of the silicone resin in the hole-containing layer A can be formed.

[0058] The content of polydimethylsiloxane in the silicone resin contained in the hole-containing layer A obtained by the NMR method is preferably 0.005% by mass or more and 2.000% by mass or less relative to 100% by mass of the polypropylene resin in the hole-containing layer A. It is further preferably 0.010% by mass or more and 1.800% by mass or less. It is even more preferably 0.100% by mass or more and 0.800% by mass or less. Relative to 100% by mass of the polypropylene resin, it contains 0.005% by mass or more, thereby improving the heat resistance or rigidity of the polypropylene resin, and the holes can be efficiently embodied without loss during stretching. By setting it to 2.000% by mass or less, the deterioration of film forming properties can be suppressed.

[0059] The void-containing layer A can impart heat resistance or rigidity to the polypropylene resin by containing a small amount of silicone resin. Therefore, the thermal degradation of the polypropylene resin can be suppressed during material recycling, and the void-embodying effect can be maintained. As a void-containing polyester film, the voids are not easily crushed in a high temperature environment, and therefore, the uneven thickness caused by the partial loss of the polypropylene resin as a void-embodying agent can be suppressed.

[0060] In addition, non-miscible resins other than polypropylene resins can be contained as long as the scope does not damage the purpose of the present invention. As non-miscible resins, for example, polyethylene resins, polymethylpentene resins, and cyclic polyolefin resins can be cited. Polycarbonate resins, polysulfone resins, cellulose resins, etc. can also be cited. Relative to the total non-miscible resins in the hole-containing layer A of 100 mass%, the polypropylene resin preferably contains more than 90 mass%, more preferably more than 95 mass%, and most preferably 100 mass%. In addition, from the viewpoint of whiteness and hole manifestation, it is preferably free of dispersants such as polyethylene glycol and surfactants.

[0061] In addition, within the scope of not impairing the purpose of the present invention, a small amount of other polymers, antioxidants, heat stabilizers, matting agents, pigments, ultraviolet absorbers, fluorescent whitening agents, plasticizers or other additives may also be contained in these polyester resins or polypropylene resins. In order to inhibit the oxidative degradation of the polypropylene resin, it is particularly preferred to contain an antioxidant or a thermal stabilizer. There is no particular limitation on the types of antioxidants and thermal stabilizers, for example, hindered phenol systems, phosphorus systems, hindered amine systems, etc., which can be used alone or in combination. As an added amount, it is preferably more than 1ppm and less than 50000ppm relative to the total mass of the hole-containing layer A. It should be noted that in the present invention, even if a fluorescent whitening agent is not added to the hole-containing layer A, excellent whiteness can be ensured.

[0062] In the present invention, in the polyester film containing holes, the polyester resin or the polypropylene resin may contain inorganic pigments as needed to improve hiding power and whiteness. As inorganic pigments, silicon dioxide, kaolinite, talc, calcium carbonate, zeolite, aluminum oxide, barium sulfate, titanium oxide, zinc sulfide, etc. can be cited. Among these, titanium oxide, calcium carbonate, and barium sulfate are preferred from the viewpoint of hiding power and whiteness. In addition, these inorganic pigments can be used alone or in combination of two or more. These inorganic pigments can be included in the polyester film containing holes by being added to the polyester resin or the polypropylene resin in advance.

[0063] The method of mixing the inorganic pigment into the polyester resin or the polypropylene resin is not particularly limited, and the following methods may be mentioned: that is, a method of dry-mixing the polyester resin and the polypropylene resin and directly feeding the mixture into a film-making machine; a method of dry-mixing the polyester resin and the polypropylene resin and then melt-mixing and preparing a masterbatch using various common mixers; and the like.

[0064] The void-containing polyester film of the present invention has a laminated structure in which a first covering layer B1 formed of a polyester resin containing an inorganic pigment, a void-containing layer A having voids inside, and a second covering layer B2 formed of a polyester resin containing an inorganic pigment are sequentially laminated. That is, the first covering layer B1, the void-containing layer A, and the second covering layer B2 are sequentially arranged along the thickness direction of the void-containing polyester film. Here, when the void-containing layer A containing a polypropylene resin is exposed on the surface, a part of the exposed polypropylene dispersed particles may cause process contamination such as roller contamination. In addition, the first covering layer B1 containing an inorganic pigment and the second covering layer B2 have the effect of preventing the whiteness from being reduced by covering the void-containing layer A.

[0065] It should be noted that any layer may exist between the first covering layer B1 and the hole-containing layer A, but preferably no layer exists between the two. That is, it is preferred that the first covering layer B1 is laminated on the hole-containing layer A without the aid of any layer. That is, it is preferred that the first covering layer B1 is in contact with the hole-containing layer A. On the other hand, any layer may exist between the hole-containing layer A and the second covering layer B2, but preferably no layer exists between the two. That is, it is preferred that the second covering layer B2 is laminated on the hole-containing layer A without the aid of any layer. That is, it is preferred that the second covering layer B2 is in contact with the hole-containing layer A.

[0066] From the viewpoint of the manifestation of voids and the suppression of the exposure of the polypropylene resin and the silicone resin, the ratio of the total thickness of the first covering layer B1 and the thickness of the second covering layer B2 (hereinafter sometimes referred to as the layer ratio) is preferably 6% or more and 40% or less, and more preferably 8% or more and 30% or less. When the layer ratio is 6% or more and 40% or less, the exposure of the polypropylene resin and the silicone resin can be suppressed, and the contact angle of water and the contact angle of diiodomethane can be reduced. Furthermore, when the layer ratio is 6% or more and 40% or less, it is easy to form voids for obtaining sufficient lightness and cushioning properties.

[0067] As the inorganic pigment contained in the first covering layer B1 and the second covering layer B2, silicon dioxide, kaolinite, talc, calcium carbonate, zeolite, aluminum oxide, barium sulfate, titanium oxide, zinc sulfide, etc. can be cited. Among these, titanium oxide, calcium carbonate, and barium sulfate are preferred from the viewpoint of hiding power and whiteness, and titanium oxide is particularly preferred. In addition, these inorganic pigments can be used alone or in combination of two or more. These pigments can be included in the film by being added to the polyester resin in advance.

[0068] The amount of the inorganic pigment added to the first covering layer B1 is not particularly limited, but is preferably 1% by mass or more and 35% by mass or less, and more preferably 2% by mass or more and 30% by mass or less, relative to 100% by mass of all components constituting the first covering layer B1. When the amount of the inorganic pigment added is 1% by mass or more and 35% by mass or less, the hiding power and whiteness of the void-containing polyester film are easily improved, and the film forming properties and mechanical strength of the void-containing polyester film can be improved.

[0069] The description of the amount of inorganic pigment added in the second covering layer B2 overlaps with the description of the amount of inorganic pigment added in the first covering layer B1, and is therefore omitted. Therefore, the description of the amount of inorganic pigment added in the first covering layer B1 can also be treated as the description of the amount of inorganic pigment added in the second covering layer B2. The amount of inorganic pigment added in the second covering layer B2 and the amount of inorganic pigment added in the first covering layer B1 can be independent of each other. Therefore, the amount of inorganic pigment added in the second covering layer B2 can be the same as or different from the amount of inorganic pigment added in the first covering layer B1. Preferably, the amount of inorganic pigment added in the second covering layer B2 is the same as the amount of inorganic pigment added in the first covering layer B1.

[0070] In addition, in the void-containing polyester film of the present invention, a coating layer may be provided on at least one side thereof in order to improve the coating properties and adhesiveness of printing ink, coating agent, etc. As the compound constituting the coating layer, a polyester resin is preferred. In addition, polyurethane resin, polyester polyurethane resin, acrylic resin, etc., which are generally disclosed as a solution for improving the adhesiveness of polyester films, can be used.

[0071] As a method for providing a coating layer, commonly used methods such as gravure coating, kiss coating, dipping, spraying, curtain coating, air knife coating, blade coating, reverse roll coating, etc. can be applied. As a coating stage, any method such as a method of coating before stretching the film, a method of coating after longitudinal stretching, and a method of coating on the surface of the film after the stretching treatment is completed can be used.

[0072] The method for producing the void-containing polyester film of the present invention is described below. For example, a mixed pellet formed by a composition containing a polyester resin, a polypropylene resin and a silicone resin is dried, melt-extruded from a T-shaped nozzle into a sheet, and then closely bonded to a casting drum by an electrostatic application method, etc., and cooled and solidified to obtain an unstretched film.

[0073] Next, when the unstretched film is stretched / oriented, the most commonly used sequential biaxial stretching method, in particular, a method in which the unstretched film is longitudinally stretched in the length direction and then transversely stretched in the width direction, is described as an example. First, in the longitudinal stretching process in the length direction, the film is heated and stretched to 2.5 to 5.0 times between two or more rollers with different peripheral speeds. As the heating means at this time, it can be a method using a heated roller or a method using a non-contact heating medium, and they can be used in combination. At this time, it is preferred to make the temperature of the film in the range of (Tg-10°C) to (Tg+50°C). Next, the uniaxially stretched film is introduced into a tenter and stretched to 2.5 to 5 times in the width direction at a temperature below (Tg-10°C) to Tm-10°C, thereby obtaining a biaxially stretched film.

[0074] Here, Tg is the glass transition temperature of the polyester resin, and Tm is the melting point of the polyester resin. The film obtained as described above is preferably subjected to heat treatment as necessary, and the treatment temperature is preferably in the range of (Tm-60°C) to Tm.

[0075] In addition, the void-containing polyester film of the present invention may contain recycled raw materials formed by the used void-containing polyester film of the present invention in the void-containing layer A. The used void-containing polyester film of the present invention refers to scrap films generated from the edge portion, fracture failure, etc. generated in the film-making process, and market recyclers. In the case of adding recycled raw materials to the void-containing layer A, as long as the recycled raw materials of the void-containing polyester film of the present invention are used, a small amount of silicone resin is added to the polypropylene resin, so that the void expression can be maintained. As a result, the void-containing polyester film has sufficient lightness and cushioning properties, and can obtain a void-containing polyester film with excellent covering properties and whiteness. In particular, in the current situation where it is required to cope with environmental loads, it is expected that the used void-containing polyester film can be recycled, so the amount of recycled raw materials added can be increased compared to the past. However, if silicone resin is added, the void expression can be maintained even when the amount of recycled raw materials added is increased.

[0076] The amount of the recycled raw material added is preferably 5 to 70% by mass relative to 100% by mass of the total mass of the void-containing layer A from the viewpoint of reducing the raw material cost, whiteness, and film forming properties.

[0077] The first covering layer B1 or the second covering layer B2 may contain recycled materials, but preferably does not contain recycled materials from the viewpoint of avoiding deterioration of whiteness and exposure of polypropylene resin in the recycled materials.

[0078] The apparent density of the void-containing polyester film of the present invention is preferably 0.80 g / cm 3 Above and 1.20g / cm3 Below, more preferably 0.80g / cm 3 Above and 1.10g / cm 3 Below. Apparent density is 0.80g / cm 3 Above and 1.20g / cm 3 In the following cases, the total number of pores in the pore-containing polyester film is appropriate, and it becomes easy to handle during post-processing such as printing and use. In addition, the apparent density is 0.80 g / cm 3 Above and 1.20g / cm 3 In the following cases, sufficient lightness and cushioning properties can be obtained.

[0079] In particular, when the void-containing polyester film of the present invention contains a trace amount of silicone resin, it has excellent lightness, film-forming properties, hiding power, and whiteness even if the apparent density is 0.80 to 1.10.

[0080] In addition, the apparent density is a value obtained by the measurement method described in the evaluation method described later.

[0081] The total light transmittance of the hole-containing polyester film of the present invention is preferably 30% or less, more preferably 25% or less. When the total light transmittance is 30% or less, sufficient hiding power is obtained. For example, when used for labels, the image printed on the label becomes clear. It should be noted that the total light transmittance is a value converted to a thickness of 50 μm obtained by the measurement method described in the evaluation method described later.

[0082] The tone b value of the void-containing polyester film of the present invention is preferably 4.0 or less, and more preferably 3.0 or less. When the tone b value is greater than 4.0, the whiteness is poor, and when forming a label, the clarity during printing is reduced, which may damage the product value.

[0083] The thickness of the void-containing polyester film of the present invention is arbitrary, but is preferably 20 μm or more and 300 μm or less.

[0084] The water contact angle of the void-containing polyester film of the present invention after heating at 150°C for 30 minutes is preferably 50 to 90°. It is further preferably 55 to 85°. When the water contact angle is 90° or less, the void-containing polyester film can suppress coating penetration and printing penetration in the processing step. However, as long as a polyester resin is used, the possibility of the water contact angle being 50° or less is extremely low. In addition, the contact angle of diiodomethane after heating at 150°C for 30 minutes is preferably 10 to 40°. When the contact angle of diiodomethane is 40° or less, the void-containing polyester film can suppress coating penetration and printing penetration in the processing step. When the contact angle of diiodomethane is 10° or more, the void-containing polyester film can improve the adhesion between the coating and the blank in the processing step.

[0085] The water contact angle of the void-containing polyester film of the present invention after 72 hours at 85°C and 85%RH is preferably 50 to 90°. It is further preferably 55 to 85°. When the water contact angle is 90° or less, the void-containing polyester film can suppress coating penetration and printing penetration when it is processed after long-term storage in a warehouse. However, when the water contact angle becomes 50° or less, it is sufficient to use polyester resin, and the possibility is as low as possible. In addition, the contact angle of diiodomethane after 72 hours at 85°C and 85%RH is preferably 10 to 40°. When the contact angle of diiodomethane is 40° or less, the coating penetration and printing penetration can be suppressed when the void-containing polyester film is processed after long-term storage in a warehouse. When the contact angle of diiodomethane is 10° or more, the void-containing polyester film can improve the adhesion between the coating and the blank in the processing step.

[0086] As described above, the void-containing polyester film of the present invention has excellent lightness, film-forming properties, hiding power, whiteness, and the like.

[0087] Specifically, the hole-containing layer A contains both polyolefin resin and silicone resin, so compared with the case where the silicone resin is not contained, the holes can be efficiently formed during the manufacturing process of the hole-containing polyester film (for example, during the stretching process). It is believed that this is because the heat resistance or rigidity of the polyolefin resin, i.e., the polyolefin dispersed particles, dispersed in the hole-containing layer A is improved by the silicone resin, thereby suppressing the excessive deformation of the polyolefin dispersed particles during the manufacturing process of the hole-containing polyester film (for example, excessive deformation of the polyolefin dispersed particles during stretching). As a result (i.e., the result that the holes can be efficiently formed), the covering property can be improved, and the lightness (i.e., lightweight) can also be improved.

[0088] Furthermore, the first covering layer B1 containing an inorganic pigment, the pore-containing layer A, and the second covering layer B2 containing an inorganic pigment are sequentially stacked, so that the hiding power can be further improved and the whiteness can be improved. In addition, the silicone resin of the pore-containing layer A can be prevented from being exposed on the surface of the pore-containing polyester film, so that the water contact angle and the diiodomethane contact angle can be prevented from being excessively increased by the silicone resin, so that the deterioration of the coating and printing properties that may be caused by the silicone resin of the pore-containing layer A can be suppressed (for example, when coating and printing are performed on the pore-containing polyester film, coating penetration and printing penetration can be suppressed).

[0089] In addition, the apparent density is 0.80 g / cm 3 As above, the lightweight property is excellent.

[0090] Furthermore, the apparent density is 1.20 g / cm 3 Therefore, the volume of the pores does not become excessively large, and thus the film forming property is excellent.

[0091] Therefore, the void-containing polyester film of the present invention can be suitably used as a substrate for labels, cards, packaging materials, release films used in the production of polarizing plates and laminated ceramic capacitors.

[0092] The resin composition can be manufactured by material recovery of the hole-containing polyester film. As a material recovery method, for example, the following method can be cited: the hole-containing polyester film is masked as required, crushed, supplied to an extruder, extruded from a die head, and formed into any shape as required (for example, the strands extruded from the die head are cut with a granulator). The resin composition can be formed into a strand, a pellet, or a sheet.

[0093] The resin composition contains an inorganic pigment, a polyester resin, a polyolefin resin and a silicone resin. Specifically, the resin composition contains: an inorganic pigment derived from a void-containing polyester film, a polyester resin derived from a void-containing polyester film, a polyolefin resin derived from a void-containing polyester film and a silicone resin derived from a void-containing polyester film. The use of the resin composition is not particularly limited, but the resin composition can be suitably used as one of the raw materials of the void-containing layer A of the void-containing polyester film.

[0094] Example

[0095] The present invention is specifically described below by way of examples. It should be noted that the present invention is not limited to the following examples. It should be noted that each evaluation item in the examples and comparative examples was measured by the following method.

[0096] (1) Film-forming properties

[0097] Under the film-forming conditions described in the production of the void-containing polyester film described later, the number of breakages during the production within a film-forming time of 2 hours was evaluated as follows.

[0098] ○: No breakage

[0099] △: Broken 1 to 3 times

[0100] ×: Broken more than 4 times, unable to form film

[0101] (2) Apparent density

[0102] Cut the porous polyester film into 4 square sheets of 5.0 cm square, overlap the 4 sheets, and use a micrometer to change the position of the total thickness by 4 significant figures to measure 10 points, and find the average thickness of the 4 overlapping sheets. Divide the average by 4, approximate to 3 significant figures, and record it as the average thickness of each sheet (t: μm). Measure the mass (w: g) of 4 sheets of the same sample with an automatic plate balance to 4 significant figures, and find the apparent density according to the following formula. It should be noted that the apparent density is approximated to 3 significant figures.

[0103] Apparent density (g / cm 3 ) = w / (5.0×5.0×t×10 -4 ×4)

[0104] (3) Total light transmittance

[0105] The haze was measured using a haze meter (NDH5000 manufactured by Nippon Denshoku Industries Co., Ltd.) and converted into a value per 50 μm of film thickness. The same measurement was performed three times, and the arithmetic mean value was used.

[0106] (4) Hue b value

[0107] The color tone b value is measured using a colorimeter (ZE6000) manufactured by Nippon Denshoku Co., Ltd. in accordance with JIS-8722. The smaller the color tone b value is, the higher the whiteness is and the weaker the yellow tone is.

[0108] (5) Water contact angle after heating at 150°C for 30 minutes

[0109] After heating the sample for 30 minutes in a Gir aging thermostat at 150°, the contact angle with distilled water was measured 1 minute after the sample was dropped using a FACE contact angle meter (CA-X model, manufactured by Kyowa Interface Chemical Co., Ltd.) It should be noted that 5 measurements were performed for each sample, and the average of the three measured values ​​after removing the maximum and minimum values ​​of the measured values ​​was taken as the contact angle.

[0110] (6) Diiodomethane contact angle after heating at 150°C for 30 minutes

[0111] After heating the sample for 30 minutes in a Gir aging thermostat at 150°, the contact angle with diiodomethane was measured 1 minute after the dropwise addition using a FACE contact angle meter (CA-X model, manufactured by Kyowa Interface Chemical Co., Ltd.) It should be noted that 5 measurements were performed for each sample, and the average of the three measured values ​​after removing the maximum and minimum values ​​of the measured values ​​was taken as the contact angle.

[0112] (7) Water contact angle after 72 hours at 85°C and 85% RH

[0113] After the sample was placed in a constant temperature and humidity chamber at 85°C and 85% RH for 72 hours, the contact angle with distilled water was measured 1 minute after the drop was added using a FACE contact angle meter (CA-X model, manufactured by Kyowa Interface Chemical Co., Ltd.) It should be noted that 5 measurements were performed on each sample, and the average of the three measured values ​​after removing the maximum and minimum values ​​of the measured values ​​was taken as the contact angle.

[0114] (8) Diiodomethane contact angle after 72 hours at 85°C and 85% RH

[0115] After the sample was placed in a constant temperature and humidity chamber at 85°C and 85% RH for 72 hours, the contact angle with diiodomethane was measured 1 minute after the dropwise addition using a FACE contact angle meter (CA-X model, manufactured by Kyowa Interface Chemical Co., Ltd.) It should be noted that 5 measurements were performed for each sample, and the average of the three measured values ​​after removing the maximum and minimum values ​​of the measured values ​​was taken as the contact angle.

[0116] (9) Determination of polydimethylsiloxane content

[0117] After dissolving in 0.1 ml of CDCl3 (deuterated chloroform) / HFIP-d (deuterated hexafluoroisopropanol) (1 / 1 volume ratio), add 0.5 ml of TCE (tetrachloroethane)-d and dissolve at 130°C. For this solution, H-NMR measurement is carried out at 120°C, and the mass ratio of polydimethylsiloxane is calculated from the ratio of the integral values ​​of the obtained components. The peak of polydimethylsiloxane used is the peak detected near 0.2 ppm of the NMR spectrum. The content of polydimethylsiloxane in the void-containing layer A is calculated using the layer ratio. Since the silicone resin is cross-linked and has a lot of insoluble components, it is difficult to quantify the amount of addition, but if the above method is used, the soluble component of polydimethylsiloxane in the silicone resin can be quantified. It can be confirmed that the amount of silicone resin added is related to the polydimethylsiloxane content.

[0118] (10) Determination of the mass ratio of polypropylene resin content to polydimethylsiloxane content

[0119] H-NMR measurement was carried out in the same manner as above, and the mass ratio was calculated from the ratio of the integrated values ​​of the peaks of the polypropylene resin and the polydimethylsiloxane in the obtained NMR spectrum.

[0120] (Example 1)

[0121] [Manufacture of masterbatch pellets (M1) containing titanium oxide]

[0122] 50% by mass of anatase-type titanium dioxide having an average particle size of 0.3 μm (by electron microscopy) was mixed with 50% by mass of polyethylene terephthalate resin having an intrinsic viscosity of 0.62, and the mixture was supplied to a vented twin-screw extruder and kneaded to produce masterbatch pellets (M1) containing titanium oxide.

[0123] [Manufacturing of Silicone Resin S]

[0124] A thermosetting silicone resin (KS-774 manufactured by Shin-Etsu Chemical Co., Ltd.) was diluted with a solvent, and 3 parts by mass of a catalyst (CAT-PL-3 manufactured by Shin-Etsu Chemical Co., Ltd.) was added to 100 parts by mass of the silicone resin, and heated at 150° C. for 60 seconds. The cured silicone resin after heating was powdered to obtain silicone resin S.

[0125] [Manufacturing of unstretched film]

[0126] 93% by mass of polyethylene terephthalate resin with an intrinsic viscosity of 0.62, 6.92% by mass of polypropylene resin with MFR=2.5, Mw=320000, Mw / Mn=4.0, and load deflection temperature=92°C, and 800ppm of silicone resin S are mixed. Then, the mixture is vacuum dried to form a raw material for the void-containing layer A. On the other hand, 30% by mass of the master batch pellets (M1) containing titanium oxide and 70% by mass of polyethylene terephthalate resin with an intrinsic viscosity of 0.62 are pelletized. Then, the mixture is vacuum dried to form a raw material for the first covering layer B1 and the second covering layer B2. These raw materials are supplied to respective extruders, melted at 285°C, and the void-containing layer A, the first covering layer B1, and the second covering layer B2 are stacked in a manner of B1 / A / B2. The stacked body is joined in a feed head in a manner of a thickness ratio of 10 / 80 / 10. This bonded body was extruded from a T-die onto a cooling drum adjusted to 30° C. to produce an unstretched film having two types of three-layer structures.

[0127] [Production of porous polyester film]

[0128] A void-containing polyester film was prepared under the following film-forming conditions. That is, the obtained unstretched film was uniformly heated to 70°C by a heating roller, and longitudinally stretched to 3.4 times between two pairs of rollers with different peripheral speeds. At this time, as an auxiliary heating device for the unstretched film, an infrared heating heater (rated at 20 W / cm) with a gold reflective film was placed in the middle of the rollers (1 cm away from the film surface) facing both sides of the film to heat it. The uniaxially stretched film thus obtained was introduced into a tenter, heated to 140°C, transversely stretched to 4.0 times, fixed in width, heat treated at 235°C, and then relaxed by 3% in the width direction at 210°C, thereby obtaining a void-containing polyester film with a thickness of 50 μm. The results of apparent density, water contact angle, diiodomethane contact angle, color tone b value, total light transmittance and film-forming properties are shown in Table 1.

[0129] (Examples 2, 3, 5)

[0130] In Example 1, except that the raw material ratio of the void-containing layer A was changed as shown in Table 1, the same method as in Example 1 was used to obtain a void-containing polyester film.

[0131] (Example 4)

[0132] In Example 1, except that the raw material ratio and layer ratio of the void-containing layer A were changed as shown in Table 1, the same method as in Example 1 was used to obtain a void-containing polyester film.

[0133] (Example 6)

[0134] [Manufacture of polyester pellets containing silicone resin]

[0135] A polyester film containing voids was prepared in the same manner as in Example 1 except that the silicone resin S of the void-containing layer A was not added. On this basis, a release layer containing a silicone resin as a main component was coated on one side of the polyester film containing voids at a thickness of 0.075 g / m 2 The release polyester film is recycled together with the release layer to obtain polyester pellets containing silicone resin.

[0136] [Made from recycled polyester film containing holes]

[0137] A void-containing polyester film is obtained by mixing 61.3 mass % of polyethylene terephthalate resin (intrinsic viscosity 0.62), 13.7 mass % of polypropylene resin (MFR = 2.5, Mw = 320000, Mw / Mn = 4.0, load deflection temperature = 92°C), and 25 mass % of polyester pellets containing silicone resin. Except for this, the same method as Example 1 is used to obtain a void-containing polyester film.

[0138] It should be noted that the composition of Example 6 is shown in Table 1 in the same manner as in Example 1. The amount of polyethylene terephthalate resin in Example 6 in Table 1 is the total amount of polyethylene terephthalate resin having an intrinsic viscosity of 0.62 and polyethylene terephthalate resin derived from polyester pellets containing silicone resin. The amount of polypropylene resin in Example 6 in Table 1 is the total amount of polypropylene resin having MFR=2.5, Mw=320000, Mw / Mn=4.0, and load deflection temperature=92°C and polypropylene resin derived from polyester pellets containing silicone resin. The amount of silicone resin in Example 6 in Table 1 is the amount of silicone resin derived from polyester pellets containing silicone resin.

[0139] (Comparative Example 1)

[0140] In Example 1, the void-containing polyester film was obtained in the same manner as in Example 1 except that the silicone resin in the void-containing layer A was changed to 0 ppm and the polyethylene terephthalate resin was changed to 93.08 mass %. In the void-containing polyester film of Comparative Example 1, the apparent density exceeded 1.20 g / cm 3 , therefore, it is not within the scope of the present invention. Therefore, the lightness and cushioning properties are poor. The mass is large, so the manufacturing cost is also high. In addition, the total light transmittance of the hole-containing polyester film of Comparative Example 1 is also high, and the hiding property is also poor compared with Examples 1 to 6.

[0141] (Comparative Example 2)

[0142] In Example 1, except that the aforementioned layer ratio was set to 0%, a void-containing polyester film was obtained by the same method as in Example 1. Comparative Example 2 does not have the first covering layer B1 and the second covering layer B2, and therefore is not within the scope of the present invention. In Comparative Example 2, the voids of the void-containing layer A are exposed on the surface, and the surface of Comparative Example 2 becomes extremely rough. In Comparative Example 2, the total light transmittance is high, and the hiding power is poor compared with Examples 1 to 6. In addition, in Comparative Example 2, the color tone b value is large, and the whiteness is low and the yellow tone is strong compared with Examples 1 to 6. In addition, the contact angle of the void-containing polyester film of Comparative Example 2 becomes high due to the influence of the silicone resin. In detail, the water contact angle exceeds 90°, and Comparative Example 2 cannot suppress the coating penetration and printing penetration in the processing steps of the void-containing polyester film. In addition, the contact angle of diiodomethane also exceeds 40°, and Comparative Example 2 cannot suppress the coating penetration and printing penetration in the processing steps of the void-containing polyester film.

[0143] (Comparative Example 3)

[0144] In Example 1, the raw material ratio of the void-containing layer A was changed as shown in Table 1. The same method as in Example 1 was used to obtain a void-containing polyester film. The apparent density of Comparative Example 3 was less than 0.80 g / cm3 Therefore, the film forming property of Comparative Example 3 is inferior to that of Examples 1 to 6.

[0145] As described above, the void-containing polyester film of the present invention can suppress the thermal degradation of the polypropylene resin during the processing step, for example, by virtue of the void-containing layer A containing a silicone resin, and can maintain the void expression. Therefore, the void-containing polyester film of the present invention has excellent lightness, film-forming properties, hiding properties, and whiteness even if the apparent density is 0.80 to 1.20. In particular, the void-containing polyester films of Examples 12 to 6 have excellent lightness, film-forming properties, hiding properties, and whiteness even if the apparent density is 0.80 to 1.10.

[0146] [Table 1]

[0147]

[0148] Industrial Applicability

[0149] As described above, the void-containing polyester film of the present invention is excellent in lightness, film-forming property, hiding power and whiteness, and is therefore suitable for use as a substrate for release films used in, for example, labels, cards, packaging materials, polarizing plates, and laminated ceramic capacitor manufacturing.

Claims

1. A porous polyester film, include: The first cover layer B1 comprises a polyester resin containing an inorganic pigment, A hole-containing layer A having holes inside, and The second cover layer B2 comprises a polyester resin containing an inorganic pigment, The porous polyester film is sequentially laminated with a first covering layer B1, a porous layer A and a second covering layer B2. The void-containing layer A comprises a composition containing a polyester resin, a polyolefin resin and a silicone resin. The apparent density of the porous polyester film is 0.80 g / cm 3 Above and 1.20g / cm 3 the following.

2. The void-containing polyester film according to claim 1, in, In the void-containing layer A, the content of the polydimethylsiloxane in the silicone resin is 1 ppm or more and 2500 ppm or less relative to the total mass of the void-containing layer A.

3. The void-containing polyester film according to claim 1, in, In the void-containing layer A, the content of the polydimethylsiloxane in the silicone resin is 0.005 mass % or more and 2.000 mass % or less relative to 100 mass % of the polyolefin resin.

4. The void-containing polyester film according to claim 1, in, The inorganic pigment in the first covering layer B1 and the second covering layer B2 is titanium oxide.

5. The void-containing polyester film according to claim 1, in, The ratio of the total thickness of the first covering layer B1 and the second covering layer B2 to the total thickness of the first covering layer B1, the void-containing layer A, and the second covering layer B2 is 6% to 40%. 6 . The void-containing polyester film according to claim 1 , wherein the total light transmittance is greater than or equal to 1% and less than or equal to 30%.

7. The porous polyester film according to claim 1, wherein the apparent density is 0.80 g / cm 3 Above and 1.10g / cm 3 the following. 8 . The void-containing polyester film according to claim 1 , which is used for labels, cards, packaging materials or release films. 9 . A resin composition obtained by material recycling the void-containing polyester film according to claim 1 , wherein the resin composition contains an inorganic pigment, a polyester resin, a polyolefin resin and a silicone resin.

10. A method for producing a resin composition, in, The void-containing polyester film according to any one of claims 1 to 7 is subjected to material recovery to produce a resin composition containing an inorganic pigment, a polyester resin, a polyolefin resin and a silicone resin.

Citation Information

Patent Citations

  • White surface-roughened polyester film and its production

    JP1990180933A

  • White polyester film

    JP1990284929A

  • Manufacture of laminated white polyester film

    JP1996252857A

  • White polyester film

    JP1999116716A

  • Fine bubble-containing laminated polyester film and mounting sheet for seal print

    JP1998029286A

Cited By