Prepolymer solution production method and insulated wire production method
By mixing and controlling reaction conditions in an extruder, a high-concentration prepolymer solution can be continuously manufactured, solving the productivity and cost problems in existing technologies and improving the mechanical strength and heat resistance of insulated wires.
Patent Information
- Application Number
- CN202280094750.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2022-05-31
- Publication Date
- 2024-11-22
AI Technical Summary
Existing technologies struggle to continuously produce high-concentration prepolymer solutions and suffer from difficulties in solvent removal, impacting productivity and costs.
The first raw material, the second raw material, and the solvent are mixed using an extruder. By controlling the reaction conditions and adding a reaction control agent, a high-concentration prepolymer solution is continuously produced. The viscosity and dispersion of the solution are controlled by stirring and viscosity measurement.
It enables continuous production of high-concentration prepolymer solutions, reduces solvent consumption, and improves production efficiency, mechanical strength, and heat resistance of insulated wires.
Smart Images

Figure CN119013328A_ABST
Abstract
Description
Technical Field
[0001] The present disclosure relates to a method for producing a prepolymer solution and a method for producing an insulated wire. Background Art
[0002] Patent document 1 describes a polymer manufacturing system, which uses a raw material fluid containing a first polymerizable compound with polyaddition properties and a raw material powder containing a second polymerizable compound with polyaddition properties as raw materials to manufacture a first polymer, and the above-mentioned polymer manufacturing system comprises: a raw material fluid supply unit, which continuously supplies the above-mentioned raw material fluid; a raw material powder supply unit, which continuously supplies the above-mentioned raw material powder; a first mixing unit, which continuously mixes the above-mentioned raw material fluid and the above-mentioned raw material powder to generate a first mixed fluid; and a first reaction unit, which is arranged on the downstream side of the above-mentioned first mixing unit, and generates a first polymer fluid by performing a polymerization reaction of the above-mentioned first mixed fluid.
[0003] Prior art literature
[0004] Patent Literature
[0005] Patent Document 1: Japanese Patent Application Publication No. 2021-31610 Summary of the invention
[0006] A method for producing a prepolymer solution according to one embodiment of the present disclosure is a method for continuously producing a prepolymer solution in which a prepolymer serving as a precursor of a thermosetting resin is dissolved in a solvent, the method comprising: using an extruder to mix a first raw material, a second raw material that reacts with the first raw material to form the prepolymer, and the solvent. BRIEF DESCRIPTION OF THE DRAWINGS
[0007] Figure 1 This is a schematic diagram for explaining a method for producing a prepolymer solution according to one embodiment of the present disclosure.
[0008] Figure 2 This is a schematic diagram for explaining a method for producing a prepolymer solution according to one embodiment of the present disclosure.
[0009] Figure 3 This is a schematic diagram for explaining a method for producing a prepolymer solution according to one embodiment of the present disclosure. DETAILED DESCRIPTION
[0010] [Problems to be Solved by the Present Disclosure]
[0011] From the viewpoint of improving the productivity of the prepolymer solution and reducing the production cost, a method for continuously producing a prepolymer solution is desired.
[0012] Furthermore, when the prepolymer solution is used as a material for forming an insulating layer of an insulated wire, for example, the solvent contained in the prepolymer solution needs to be removed. Therefore, in order to reduce the solvent to be removed, a method for producing a high-concentration prepolymer solution is required.
[0013] The present disclosure has been made based on the fact that a problem is to provide a method for producing a prepolymer solution capable of continuously producing a prepolymer solution having a high concentration.
[0014] [Effects of the present disclosure]
[0015] A method for producing a prepolymer solution according to one embodiment of the present disclosure can continuously produce a high-concentration prepolymer solution.
[0016] [Description of Embodiments of the Present Disclosure]
[0017] First, embodiments of the present disclosure will be described by way of examples.
[0018] A method for producing a prepolymer solution according to one embodiment of the present disclosure is a method for continuously producing a prepolymer solution in which a prepolymer serving as a precursor of a thermosetting resin is dissolved in a solvent, the method comprising: using an extruder to mix a first raw material, a second raw material that reacts with the first raw material to form the prepolymer, and the solvent.
[0019] The method for producing a prepolymer solution can continuously produce a high-concentration prepolymer solution by mixing the first raw material, the second raw material and the solvent using an extruder. "High concentration" means that the solid content concentration of the prepolymer solution is 25% by mass or more. "Solid content concentration" refers to the ratio of the total mass of all components other than the solvent to the total mass of the prepolymer solution. "Continuously producing" means continuously producing a prepolymer solution within a certain period of time. Moreover, the meaning is different from "intermittent production".
[0020] Preferably, a reaction control agent is further mixed in the mixing step. In this case, the viscosity of the prepolymer solution can be reduced, thereby achieving a viscosity that can be used to manufacture an insulated wire.
[0021] Preferably, the process further comprises a step of measuring the viscosity of the prepolymer solution obtained by the mixing step, and the supply amount of the reaction control agent in the mixing step is determined based on the measured value of the viscosity obtained by the measuring step. In this case, the viscosity of the prepolymer solution can be easily controlled.
[0022] Preferably, the method further comprises stirring the prepolymer solution obtained in the mixing step. In this case, the dispersion of the viscosity of the prepolymer solution can be reduced.
[0023] Preferably, the solid content concentration of the prepolymer solution is 20 mass % or more and 50 mass % or less. In this case, the number of repeated coatings when forming an insulating layer of a target film thickness can be reduced, and the manufacturing efficiency can be improved.
[0024] Preferably, the prepolymer has a group that can form an imide group by dehydration reaction, the first raw material is a carboxylic anhydride, and the second raw material is a diamine compound. In this case, the heat resistance of the thermosetting resin obtained by curing the prepolymer solution can be improved.
[0025] Preferably, the prepolymer is a polyimide prepolymer and the carboxylic anhydride is tetracarboxylic dianhydride. In this case, the heat resistance of the thermosetting resin obtained by curing the prepolymer solution can be further improved.
[0026] Preferably, the extruder is a twin-screw extruder. In this case, the residence time required for the formation of the prepolymer can be sufficiently ensured. By sufficiently ensuring the residence time, the unreacted prepolymer can be reacted, and as a result, the mechanical strength of the insulated wire can be improved.
[0027] Preferably, the viscosity is measured using a vibration viscometer in the above-mentioned measuring step. In this case, the prepolymer can be produced without impairing the continuous productivity of the prepolymer solution.
[0028] The stirring step is preferably performed at a temperature of 20° C. to 200° C. In this case, the dispersion of the viscosity can be reduced by stirring for a short time without causing volatilization of the solvent.
[0029] In the method for manufacturing the insulated wire, the insulated wire comprises a conductor and an insulating layer covering the conductor, and the method for manufacturing the insulated wire comprises: a step of applying a prepolymer solution obtained by the above-mentioned method for manufacturing the prepolymer solution to the outer peripheral side of the conductor; and a step of heating the prepolymer solution applied to the conductor.
[0030] The method for producing an insulated wire can continuously produce an insulated wire having appropriate characteristics by using the prepolymer solution obtained by the above-mentioned method for producing a prepolymer solution as a material for forming an insulating layer.
[0031] [Details of the embodiments of the present disclosure]
[0032] Hereinafter, a method for producing a prepolymer solution and a method for producing an insulated wire according to an embodiment of the present disclosure will be described in detail.
[0033] <Method for producing prepolymer solution>
[0034] The method for producing the prepolymer solution is a method for continuously producing a prepolymer solution in which a prepolymer serving as a precursor of a thermosetting resin is dissolved in a solvent, the method comprising: a step of mixing a first raw material, a second raw material that reacts with the first raw material to form the prepolymer, and the solvent using an extruder (hereinafter also referred to as a "mixing step").
[0035] Preferably, the method for producing a prepolymer solution further comprises a step of measuring the viscosity of the prepolymer solution obtained by the mixing step (hereinafter also referred to as a "viscosity measuring step").
[0036] Preferably, the method for producing a prepolymer solution further comprises a step of stirring the prepolymer solution obtained by the mixing step (hereinafter also referred to as a "stirring step").
[0037] The method for producing the prepolymer solution may also include other steps other than the mixing step, the viscosity measuring step and the stirring step. Other steps include, for example, a supply amount measuring step, a pressure measuring step, a refractive index measuring step, a density measuring step, a temperature measuring step, a flow measuring step, a colorimetric measuring step, an absorbance measuring step, a conductivity measuring step, a turbidity measuring step, and an infrared spectroscopic measuring step.
[0038] The prepolymer solution is a solution of a prepolymer as a precursor of a thermosetting resin dissolved in a solvent. Examples of thermosetting resins include polyimide, polyamide-imide, polyetherimide, polyester, etc. Among them, thermosetting resins having an imide group are preferred, and polyimide is more preferred.
[0039] The prepolymer is a precursor of the thermosetting resin. For example, when the thermosetting resin is polyimide, the prepolymer is a polyamic acid as a precursor thereof. The polyamic acid undergoes a dehydration cyclization reaction by heating or the like, thereby forming a cyclic imide group to become a polyimide.
[0040] As the lower limit of the solid content concentration of the prepolymer solution obtained by the manufacturing method of the prepolymer solution, it is preferably 20% by mass, more preferably 24% by mass, and further preferably 28% by mass. According to the manufacturing method of the prepolymer solution, a high-concentration prepolymer solution with a solid content concentration of more than 20% by mass can be manufactured. In addition, the amount of solvent can be relatively reduced. As the upper limit of the above-mentioned solid content concentration, it is preferably 50% by mass, more preferably 45% by mass, further preferably 40% by mass, and further preferably 36% by mass. The solid content concentration of the prepolymer solution can be adjusted by the supply amount of the first raw material, the second raw material and the solvent, etc.
[0041] The lower limit of the viscosity of the prepolymer solution at 30°C is preferably 5 Pa·s. In addition, the upper limit of the viscosity of the prepolymer solution at 30°C is preferably 450 Pa·s. If the viscosity of the prepolymer solution at 30°C is less than the above lower limit, it is difficult to apply the prepolymer solution evenly, and the coating of the insulated wire may become insufficient. On the other hand, if the viscosity of the prepolymer solution at 30°C exceeds the above upper limit, the application of the prepolymer solution may become difficult. The viscosity of the prepolymer solution is a value measured using an E-type viscometer ("TV-25" of Toki Sangyo Co., Ltd.).
[0042] The lower limit of the weight average molecular weight (Mw) of the prepolymer in terms of polystyrene is preferably 10,000, and more preferably 15,000. In addition, the upper limit of the Mw in terms of polystyrene is preferably 100,000, and more preferably 80,000. If the Mw in terms of polystyrene of the prepolymer is less than the above lower limit, the elongation of the film when forming the insulating layer of the insulated wire may become insufficient. On the other hand, if the Mw in terms of polystyrene of the prepolymer exceeds the above upper limit, the viscosity of the prepolymer solution may be too high.
[0043] The polystyrene-equivalent number average molecular weight (Mn) of the prepolymer is preferably 5,000 or more and 50,000 or less.
[0044] The ratio of Mw to Mn (Mw / Mn) of the prepolymer is preferably 1.5 or more and 4.0 or less.
[0045] Mw, Mn and Mw / Mn of the prepolymer solution are polystyrene-equivalent values measured by gel permeation chromatography in accordance with JIS-K7252-1:2008 “Plastics - Method for determining average molecular weight and molecular weight distribution of polymers measured by size exclusion chromatography - Part 1: General rules”.
[0046] (Mixing process)
[0047] In this step, the first raw material, the second raw material that reacts with the first raw material to form the prepolymer, and the solvent are mixed using an extruder. In this step, a high-concentration prepolymer solution can be continuously produced by using an extruder.
[0048] In this step, the first raw material and the second raw material react to form a prepolymer.
[0049] The mixing time is preferably 30 seconds or more and 60 minutes or less. In this case, the solidification of the prepolymer solution does not excessively proceed to gelation, and the time for forming the polymer can be fully ensured. The mixing temperature is preferably 20° C. or more and 200° C. or less. In this case, the solidification of the prepolymer solution does not excessively proceed to gelation, and the temperature for forming the polymer can be fully ensured.
[0050] The prepolymer is not particularly limited as long as it is a precursor of the above-mentioned thermosetting resin. Among them, a prepolymer having a group capable of forming an imide group by a dehydration reaction is preferred, and a polyimide prepolymer is more preferred.
[0051] In the case where the prepolymer is a prepolymer having a group that can form an imide group by a dehydration reaction, the first raw material is a carboxylic anhydride, and the second raw material is a diamine compound. By making the first raw material and the second raw material respectively the above raw materials, a prepolymer having a group that can form an imide group by a dehydration reaction is formed by this process. In this case, the heat resistance of the thermosetting resin obtained by curing the prepolymer solution can be improved.
[0052] As a carboxylic anhydride, tetracarboxylic dianhydride is mentioned, for example.
[0053] Examples of the diamine compound include aliphatic diamines such as hexamethylenediamine, 1,2-diaminotetradecane, 1,2-diaminoheptadecane, 1,2-diaminooctadecane, 1,9-diaminononane, 2,2-dimethyl-1,3-propylenediamine, and 1,11-diaminoundecane; metaphenylenediamine, paraphenylenediamine, 2,4-diaminotoluene, 4,4'-diamino-3,3'-dimethyl-1,1'-biphenyl, 4,4'-diamino-3,3'-dihydroxy-1,1'-biphenyl, 3,4'-diaminodiphenyl ether, 4,4'-diaminodiphenyl ether, 3,3'-diaminodiphenyl sulfone, 4,4'-diaminodiphenyl sulfone, 4,4'-diaminodiphenyl sulfide, 2,2-diaminodiphenyl ether; Aromatic diamines such as (4-aminophenyl)propane, 2,2-bis(4-aminophenyl)hexafluoropropane, 1,3-bis(4-aminophenoxy)benzene, 1,4-bis(4-aminophenoxy)benzene, 4,4'-bis(4-aminophenoxy)biphenyl, 2,2-bis[4-(4-aminophenoxy)phenyl]propane, 2,2-bis[4-(4-aminophenoxy)phenyl]hexafluoropropane, bis[4-(3-aminophenoxy)phenyl]sulfone, bis[4-(4-aminophenoxy)phenyl]sulfone, 2,6-diaminopyridine, 2,6-diamino-4-methylpyridine, 4,4'-(9-fluorenylene)diphenylamine, and α,α-bis(4-aminophenyl)-1,3-diisopropylbenzene.
[0054] As the diamine compound, an aromatic diamine is preferred. In this case, the mechanical strength of the thermosetting resin obtained by curing the prepolymer solution can be improved.
[0055] When the prepolymer is a polyimide prepolymer, the carboxylic acid anhydride is preferably tetracarboxylic dianhydride. In this case, the heat resistance of the thermosetting resin obtained by curing the prepolymer solution can be further improved.
[0056] Examples of the tetracarboxylic dianhydride include aliphatic tetracarboxylic dianhydrides such as 1,1,2,2-ethanetetracarboxylic dianhydride, 1,2,3,4-butanetetracarboxylic dianhydride, 1,2,3,4-cyclobutanetetracarboxylic dianhydride, and bicyclo[2.2.2]oct-7-ene-2,3,5,6-tetracarboxylic dianhydride; and aromatic tetracarboxylic dianhydrides such as pyromellitic dianhydride, 3,3',4,4'-biphenyltetracarboxylic dianhydride, bis(3,4-dicarboxyphenyl)ether dianhydride, 3,3',4,4'-benzophenonetetracarboxylic dianhydride, 2,2-bis(3,4-dicarboxyphenyl)hexafluoropropane dianhydride and 3,3',4,4'-diphenylsulfonetetracarboxylic dianhydride.
[0057] As the tetracarboxylic dianhydride, aromatic tetracarboxylic dianhydride is preferred. In this case, the mechanical strength of the thermosetting resin obtained by curing the prepolymer solution can be improved.
[0058] The supply amount of the first raw material and the second raw material can be appropriately determined according to the target solid content concentration of the prepolymer solution, etc. As the molar ratio of the first raw material to the second raw material (first raw material: second raw material), for example, it can be set to 95:105 or more and 105:95 or less, more preferably 97:103 or more and 103:97 or less, and further preferably 99:101 or more and 101:99 or less. In addition, it is preferred that the first raw material and the second raw material are substantially equimolar. When the prepolymer solution is used as a forming material for the insulating layer of an insulated wire, an insulated wire having excellent film elongation, insulation breakdown voltage and relative dielectric constant can be formed. "Substantially equimolar" means that the molar ratio of the first raw material to the second raw material (first raw material: second raw material) is in the range of 99:101 or more and 101:99 or less.
[0059] In this step, raw materials other than the first raw material and the second raw material can be supplied within a range that does not impair the effects of the present disclosure.
[0060] As the solvent, a solvent having high solubility for the prepolymer as the reaction product of the first raw material and the second raw material and not reacting with the first raw material, the second raw material and the prepolymer is selected. As such a solvent, a non-protonic polar organic solvent is preferred. By using a solvent having no protons that can react with the prepolymer, side reactions between the solvent and the raw materials or the prepolymer can be avoided. In addition, by being a polar organic solvent, the prepolymer having the same polarity can be fully dissolved.
[0061] Examples of the aprotic polar organic solvent include N-methyl-2-pyrrolidone (NMP), N,N-dimethylacetamide (DMAc), N,N-dimethylformamide, and dimethyl sulfoxide.
[0062] The amount of the solvent to be supplied can be appropriately determined according to the target solid content concentration of the prepolymer solution and the like.
[0063] As an extruder, there is no particular limitation as long as it is a device with an extrusion mechanism, and for example, a single screw extruder, a twin screw extruder, a four screw extruder, an eight screw extruder, etc. can be listed. Among them, a twin screw extruder is preferred. In this case, the equipment cost can be suppressed and the residence time required for the formation of the prepolymer can be fully ensured.
[0064] In this step, in addition to the first raw material, the second raw material and the solvent, a reaction control agent is preferably further mixed. The reaction control agent reacts with a part of the carboxylic anhydride group at the end of the prepolymer to end-cap the polymer chain. By using the reaction control agent, the polymerizability of the first raw material can be controlled, and as a result, the viscosity of the prepolymer solution can be reduced.
[0065] Examples of the reaction control agent include water (H2O) and alcohols having 1 to 15 carbon atoms. Examples of alcohols having 1 to 15 carbon atoms include monohydric alcohols such as ethanol, methanol, propanol, butanol, and pentanol; and polyhydric alcohols such as ethylene glycol, propylene glycol, and glycerol. Among them, water or methanol is preferred from the viewpoint of reactivity and cost.
[0066] The supply amount of the reaction control agent can be appropriately determined based on the molar amount of the carboxylic anhydride, and can be, for example, 0.01 mol or more and 3 mol or less relative to 1 mol of the carboxylic anhydride.
[0067] In this process, components other than the first raw material, the second raw material, the solvent and the reaction control agent may be included for the purpose of improving the performance of the thermosetting resin. For example, functional materials may be included for the purpose of improving the mechanical strength, electrical properties, thermal conductivity, heat resistance, cold resistance, wear resistance, water absorption resistance, chemical resistance, radiation resistance and surge resistance of the thermosetting resin. More specifically, chemical foaming agents, heat-expandable microcapsules, hollow particles of core-shell structure, pore-forming agents such as high-boiling-point solvents, etc. may be cited.
[0068] Reference Figure 1 An example of this process is described below. Figure 1 As shown, the twin-screw extruder 1 comprises: a second raw material supply unit 11 for supplying a second raw material; a solvent supply unit 13 for supplying a solvent; a first raw material supply unit 12 for supplying a first raw material; and a mixing unit 14 for mixing the first raw material, the second raw material and the solvent to perform a polymerization reaction. Figure 1 In the embodiment, the order from upstream is the second raw material supply unit 11, the solvent supply unit 13, and the first raw material supply unit 12, but even when this order is appropriately changed, continuous productivity can be ensured.
[0069] The first raw material is quantitatively supplied from the first raw material supply unit 12, and the second raw material is quantitatively supplied from the second raw material supply unit 11. The first raw material supply unit 12 and the second raw material supply unit 11 may include a feeder.
[0070] The first raw material supply unit 12 and the second raw material supply unit 11 may further include a side feeder.
[0071] The solvent is quantitatively supplied from the solvent supply unit 13. The solvent supply unit 13 may also include a pump. When a reaction control agent is used, it is preferably supplied from the solvent supply unit 13.
[0072] The prepolymer solution obtained in the mixing section 14 is recovered from a discharge port (not shown) disposed on the downstream side of the mixing section 14 .
[0073] (Viscosity measurement process)
[0074] In this step, the viscosity of the prepolymer solution obtained by the mixing step is measured, and the supply amount of the reaction control agent in the mixing step is determined based on the measured value of the viscosity obtained. The method for producing the prepolymer solution can easily control the viscosity of the prepolymer solution by including this step.
[0075] The viscosity in this step is preferably measured using a vibration viscometer. The vibration viscometer can measure the viscosity online, so the prepolymer can be manufactured without damaging the continuous productivity of the prepolymer solution. Furthermore, by automatically measuring the viscosity using the vibration viscometer, the control of the supply amount of the reaction control agent can be automated based on the measured viscosity information, and the control of the viscosity of the prepolymer solution can be automated.
[0076] Reference Figure 2 An example of this process is described below. Figure 2 As shown, the viscosity of the prepolymer solution discharged from the twin-screw extruder 1 is measured by a vibration type viscometer 2 disposed in the flow path. The vibration type viscometer 2 may be disposed not only in the flow path but also in a stirring tank described later.
[0077] (Mixing process)
[0078] In this step, the prepolymer solution obtained in the mixing step is stirred. The method for producing a prepolymer solution can reduce the dispersion of the viscosity of the prepolymer solution by including this step.
[0079] The stirring in this step is preferably performed using a stirrer. The stirring conditions are not particularly limited and can be appropriately determined.
[0080] The stirring temperature is preferably 20° C. to 200° C., more preferably 40° C. to 110° C. In this case, the prepolymer solution does not excessively solidify and gel, and a sufficient temperature for forming a polymer can be ensured.
[0081] Reference Figure 3 An example of this process is described below. Figure 3 As shown, the prepolymer solution discharged from the twin-screw extruder 1 is supplied to the stirring tank 3. The prepolymer solution stirred in the stirring tank 3 is discharged to a flow path by a pump (not shown) or the like.
[0082] <Method for manufacturing insulated electric wire>
[0083] The method for manufacturing an insulated wire is a method for manufacturing an insulated wire comprising a conductor and an insulating layer covering the conductor, the method comprising: a step of applying a prepolymer solution obtained by the method for manufacturing the prepolymer solution on the outer peripheral side of the conductor (hereinafter also referred to as a "coating step"); and a step of heating the prepolymer solution applied to the conductor (hereinafter also referred to as a "heating step").
[0084] The method for producing an insulated wire uses the prepolymer solution obtained by the method for producing the prepolymer solution as a material for forming an insulating layer, so that an insulated wire having appropriate characteristics can be produced. More specifically, according to the method for producing an insulated wire, an insulated wire having excellent film elongation, high insulation breakdown voltage, and low dielectric constant can be produced.
[0085] The conductor generally contains metal as a main component. The metal is not particularly limited, but copper, copper alloy, aluminum or aluminum alloy is preferred. By using the metal in the conductor, an insulated wire having good processability, conductivity and the like can be obtained. In addition to the metal as the main component, the conductor may contain other components such as known additives.
[0086] The cross-sectional shape of the conductor is not particularly limited, and various shapes such as circular, square, rectangular, etc. can be adopted. In addition, the size of the cross section of the conductor is not particularly limited, and can be appropriately determined according to the use of the insulated wire, etc.
[0087] (Coating process)
[0088] In the coating process, the prepolymer solution is coated on the outer circumference of the conductor. As a method for coating the prepolymer solution on the outer circumference of the conductor, for example, a method using a coating device can be cited, the coating device having a storage tank storing the prepolymer solution and a coating die. According to the coating device, the conductor is inserted into the storage tank so that the prepolymer solution adheres to the outer circumference of the conductor, and then passes through the coating die so that the prepolymer solution is coated to a uniform thickness.
[0089] (Heating process)
[0090] In the heating process, the prepolymer solution applied to the conductor in the coating process is heated. By the heating, the solvent of the prepolymer solution is volatilized, and the prepolymer is cured to form a thermosetting resin. In this way, an insulating layer is formed. The prepolymer solution is a solution obtained by the above-mentioned method for producing the prepolymer solution, and therefore has a high concentration. Therefore, the amount of solvent volatilized in the heating process is relatively small, which is advantageous in terms of manufacturing cost.
[0091] The apparatus used in the heating step is not particularly limited, and for example, a cylindrical baking oven that is long in the direction of travel of the conductor can be used. The heating method is not particularly limited, and can be performed by conventionally known methods such as hot air heating, infrared heating, and high-frequency heating.
[0092] In addition, the heating temperature may be set to, for example, 300° C. or higher and 800° C. or lower, and the heating time may be set to 5 seconds or higher and 1 minute or lower. When the heating temperature or the heating time is lower than the lower limit, the volatilization of the solvent and the formation of the insulating layer become insufficient, and the appearance, electrical properties, mechanical properties, thermal properties, etc. of the insulated wire may deteriorate. On the contrary, when the heating temperature exceeds the upper limit, the insulating layer may foam and the mechanical properties may be reduced due to excessive rapid heating. In addition, when the heating time exceeds the upper limit, the productivity of the insulated wire may be reduced.
[0093] The coating process and the heating process are usually repeated for multiple times. This can increase the thickness of the insulating layer. At this time, the aperture of the coating mold is appropriately adjusted according to the number of repetitions.
[0094] [Other embodiments]
[0095] The embodiments disclosed this time should be considered in all respects as illustrative and non-restrictive. The scope of the present invention is not limited to the configuration of the above-mentioned embodiments, but is indicated by the claims, and is intended to include all modifications within the meaning and scope equivalent to the claims.
[0096] Example
[0097] Hereinafter, the present invention will be described in further detail with reference to Examples, but the present invention is not limited to these Examples.
[0098] <Test Example 1>
[0099] In this test example, the effect of different mixing methods on the prepolymer solution was tested according to the following method.
[0100] The abbreviations of the components used in the preparation of the prepolymer solution are as follows.
[0101] PMDA: Pyromellitic Dianhydride
[0102] ODA: 4,4'-diaminodiphenyl ether
[0103] DMAc: N, N-dimethylacetamide
[0104] [No.1-1]
[0105] (Preparation of prepolymer solution)
[0106] PMDA powder as the first raw material, ODA powder as the second raw material and DMAc as the solvent were continuously supplied to a twin-screw extruder ("HYPER KTX30" manufactured by Kobe Steel, Ltd., screw diameter: 32 mm, L / D: 56) in an amount such that the target solid content concentration of the obtained prepolymer solution became 28% by mass. The mixing ratio (molar ratio) of PMDA and ODA was 97:103. In the above-mentioned twin-screw extruder, the first raw material and the second raw material were reacted under the conditions of temperature: 80°C, rotation speed: 200 rpm and raw material residence time: 3 minutes, thereby obtaining prepolymer solution No. 1-1 as a polyimide precursor. Thereafter, the equipment was operated for 2 hours, and it was confirmed that the prepolymer solution could be continuously produced. The solid content concentration of the obtained prepolymer solution was 28.1% by mass, and the viscosity was 29.4 Pa·s. The obtained polyimide precursor had Mw of 45,900, Mn of 15,300, and Mw / Mn of 3.0.
[0107] The solid content concentration and viscosity of the prepolymer solution, and Mw, Mn, and Mw / Mn of the polyimide precursor were measured by the following methods.
[0108] (Solid content concentration)
[0109] The prepolymer solution was dried at 250° C. for 2 hours, and the mass W0 before drying and the mass W1 after drying were measured. The solid content concentration (unit: mass %) was calculated from W1 / W0×100.
[0110] (Viscosity)
[0111] The measurement was performed at a measurement temperature of 30°C using an E-type viscometer ("TV-25" manufactured by Toki Sangyo Co., Ltd.).
[0112] (Mw, Mn and Mw / Mn)
[0113] The prepolymer solution was analyzed using the "GPC system" of Tosoh Corporation, and the Mn, Mw, and Mw / Mn of the prepolymer were calculated. As a developing solvent for the analysis, N-methyl-2-pyrrolidone in which 30 mmol of phosphoric acid and 10 mmol of lithium bromide were dissolved was used. As a standard substance, polystyrene was used. In addition, the chromatographic column used for the analysis was a chromatographic column formed by connecting two "TSKgel GMH HR-H" of Tosoh Corporation in series, and a "TSK Guard Colum HHR-H" was used as a guard column. The measurement was performed at a flow rate of 0.5 mL / min and a measurement time of 60 minutes.
[0114] (Manufacturing of insulated wires)
[0115] As the conductor, a round copper wire with an average conductor diameter (average diameter) of 1 mm was used. The prepolymer solution No. 1-1 was applied to the surface of the conductor, and the conductor coated with the prepolymer solution No. 1-1 was heated in a heating furnace at a set temperature of 450° C., thereby forming an insulation layer with an average thickness of 30 μm, and producing an insulated wire No. 1-1.
[0116] [No.1-2~1-4]
[0117] (Preparation of prepolymer solution)
[0118] Prepolymer solutions No. 1-2 to 1-4 were prepared in the same manner as No. 1-1 except that the target solid content concentration of the prepolymer solution and the mixing ratio (molar ratio) of PMDA and ODA were changed to those shown in Table 1 below. In addition, the equipment was operated for 2 hours to confirm that the prepolymer solution could be produced continuously. The solid content concentration and viscosity of the obtained prepolymer solution, as well as the Mw, Mn, and Mw / Mn of the obtained polyimide precursor are shown in Table 1 below.
[0119] (Manufacturing of insulated wires)
[0120] Insulated wire No. 1-2 was produced in the same manner as No. 1-1 except that prepolymer solution No. 1-2 was used. Insulated wires No. 1-3 and 1-4 were produced in the same manner as No. 1-1 except that prepolymer solutions No. 1-3 and 1-4 were used and heated to 80° C. and applied to the surface of the conductor.
[0121] [No.1-5]
[0122] (Preparation of prepolymer solution)
[0123] PMDA powder as the first raw material, ODA powder as the second raw material, and DMAc as the solvent were continuously supplied to a static mixer ("1,1 / 2-N60-331-1" of NORITAKE CO., LIMITED, inner diameter: 41 mm, total length: 400 mm, number of stirring blades (elements): 6) in an amount such that the target solid content concentration of the obtained prepolymer solution became 15% by mass. The mixing ratio (molar ratio) of PMDA and ODA was 97:103. The above-mentioned static mixer is a static mixer and is a device without an extrusion mechanism. In the above-mentioned static mixer, the first raw material and the second raw material were reacted under the conditions of temperature: 80°C and residence time: 3 minutes, thereby obtaining prepolymer solution No. 1-5 as a polyimide precursor. Thereafter, the equipment was operated for 2 hours, and it was confirmed that the prepolymer solution could be produced continuously. The solid content concentration of the obtained prepolymer solution was 15.1% by mass and the viscosity was 0.20 Pa·s. The obtained polyimide precursor had Mw of 41,200, Mn of 13,600, and Mw / Mn of 3.0.
[0124] (Manufacturing of insulated wires)
[0125] Insulated wire No. 1-5 was produced in the same manner as in No. 1-1 except that prepolymer solution No. 1-5 was used instead of prepolymer solution No. 1-1.
[0126] [No.1-6]
[0127] The preparation of the prepolymer solution was attempted in the same manner as No. 1-5, except that the first raw material, the second raw material and the solvent were supplied in an amount such that the target solid content concentration of the obtained prepolymer solution became 28% by mass. However, 1 minute after the start of the operation of the equipment, a backflow of the material occurred in the static mixer, so the operation of the equipment was stopped. Therefore, a prepolymer solution with a target solid content concentration could not be obtained. As the cause of the backflow of the material, it can be considered that the viscosity of the material in the static mixer increased significantly.
[0128] [evaluate]
[0129] For the insulated wires No. 1-1 to 1-5 produced as described above, the film elongation, the dielectric breakdown voltage, and the relative dielectric constant were measured by the following methods.
[0130] (Film elongation)
[0131] A tensile test was performed on a tubular insulating layer obtained by removing the conductor from the insulated wire using a tensile testing machine ("Autograph AGS-X" manufactured by Shimadzu Corporation) at a chuck distance of 20 mm and a speed of 10 mm / min to measure the film elongation (elongation at break) (unit: %). The results are shown in the "film elongation" row of Table 1 below.
[0132] (Dielectric Breakdown Voltage)
[0133] According to JIS-C3216-5:2011, an AC voltage was applied between two strands, the voltage was increased at 500 V / sec, and the voltage at the time of insulation breakdown was measured (unit: kV / μm). It should be noted that the insulation breakdown voltage was measured with n=5, and the average value was used. The results are shown in the "Insulation Breakdown Voltage" row of Table 1 below.
[0134] (Relative dielectric constant)
[0135] The measurement was performed in accordance with JIS-C2138: 2007. The results are shown in the row of "relative dielectric constant" in Table 1 below.
[0136] The results of No. 1-1 to 1-6 are shown in Table 1 below. In Table 1 below, "-" indicates that the corresponding item was not measured. In Table 1 below, "Twin-screw extrusion" in the "Mixing method" row indicates that the prepolymer solution was prepared using a twin-screw extruder, and "static" indicates that the prepolymer solution was prepared using a static mixer. In Table 1 below, "A" in the "Continuous productivity" row indicates that the prepolymer solution can be continuously produced, "B" indicates that although the prepolymer solution can be continuously produced, due to the high viscosity, a process is required to heat the prepolymer solution to 80°C to reduce the viscosity to a viscosity that can produce an insulated wire, and "C" indicates that the prepolymer solution cannot be continuously produced.
[0137] [Table 1]
[0138] No.1-1 No.1-2 No.1-3 No.1-4 No.1-5 No.1-6 Hybrid Twin screw extrusion Twin screw extrusion Twin screw extrusion Twin screw extrusion still still Target solid content concentration [mass %] 28 32 36 40 15 28 Mixing ratio of PMDA and ODA (molar ratio) 97∶103 97∶103 97∶103 95∶105 97∶103 97∶103 Viscosity [Pa·s] 29.4 81.9 414.2 409.1 0.20 - Solid content concentration [mass %] 28.1 32.4 36.0 40.2 15.1 - M 45,900 46,300 41,200 35,000 41,200 - Mn 15,300 15,900 14,300 12,000 13,600 - Mw / Mn 3.0 2.9 2.9 2.9 3.0 - Continuous productivity A A B B A C Film elongation [%] 43 41 39 23 37 - Insulation breakdown voltage [kV / μm] 0.48 0.47 0.46 0.40 0.45 - Relative dielectric constant 3.2 3.2 3.1 3.2 3.3 -
[0139] As described above, in No.1-1 to 1-4 using a twin-screw extruder, a prepolymer solution with a high solid content concentration can be continuously manufactured. On the other hand, in No.1-5 and No.1-6 using equipment without an extrusion mechanism, only prepolymer solution No.1-5 with a low solid content concentration can be continuously manufactured, and a prepolymer solution with a high solid content concentration cannot be continuously manufactured. Therefore, from the results of Test Example 1, it can be seen that by using an extruder, a prepolymer solution with a high solid content concentration can be continuously manufactured. It can also be seen that compared with the insulated wire No.1-5, the insulated wires No.1-1 to 1-3 are superior in all items including the film elongation, insulation breakdown voltage and relative dielectric constant.
[0140] <Test Example 2>
[0141] In this test example, the effect of adding a reaction control agent to a prepolymer solution was tested according to the following method.
[0142] [No.2-1]
[0143] (Preparation of prepolymer solution)
[0144] Prepolymer solution No. 2-1 was prepared in the same manner as No. 1-1 except that 0.33 mol of H2O as a reaction control agent was supplied to the twin-screw extruder relative to 1 mol of PMDA so that the mixing ratio (molar ratio) of PMDA to ODA was 100:100. The solid content concentration of the obtained prepolymer solution was 28.3% by mass and the viscosity was 8.3 Pa·s. The Mw of the obtained polyimide precursor was 32300, the Mn was 10300, and the Mw / Mn was 3.1.
[0145] (Manufacturing of insulated wires)
[0146] Insulated wire No. 2-1 was produced in the same manner as in No. 1-1 except that prepolymer solution No. 2-1 was used instead of prepolymer solution No. 1-1.
[0147] [No.2-2~2-16]
[0148] A prepolymer solution was prepared in the same manner as in No. 2-1 except that the type and supply amount of the reaction control agent were set to the amounts shown in Table 2 below, and then an insulated wire was produced. The solid content concentration and viscosity of the obtained prepolymer solution, and Mw, Mn, and Mw / Mn of the obtained polyimide precursor are shown in Table 2 below.
[0149] [No.2-17]
[0150] As an example of preparing a prepolymer solution and producing an insulated wire without using a reaction control agent, No. 1-1 in the above-mentioned <Test Example 1> was designated as No. 2-17.
[0151] [evaluate]
[0152] The film elongation, dielectric breakdown voltage and relative dielectric constant of the insulated wires No. 2-1 to 2-16 prepared above were measured in the same manner as in <Test Example 1>. The results are shown in Table 2. In Table 2, the data of No. 2-17 are all the same as the data of No. 1-1 in Table 1 above.
[0153] [Table 2]
[0154]
[0155] As described above, in No. 2-1 to 2-16 using a reaction control agent, PMDA and ODA can be made substantially equimolar, and the viscosity of the prepolymer solution suitable for the manufacture of insulated wires can be formed similarly to No. 2-17. In addition, in No. 2-4 to No. 2-6, No. 2-7 to No. 2-9, the result that the viscosity decreases as the supply amount of the reaction control agent increases is obtained. Therefore, from the results of Test Example 2, it can be seen that the viscosity of the prepolymer solution can be adjusted by using a reaction control agent.
[0156] Furthermore, insulated wires No. 2-1 to 2-16 showed good results in all items of film elongation, dielectric breakdown voltage, and relative dielectric constant compared with insulated wire No. 2-17. This result is considered to be due to the equimolar mixing ratio of PMDA and ODA.
[0157] <Test Example 3>
[0158] In this test example, the correlation between the measured value of the E-type viscometer and the measured value of the vibration viscometer was investigated according to the following method.
[0159] 18 samples were prepared whose viscosity at 30°C measured by an E-type viscometer ("TV-25" produced by Toki Sangyo Co., Ltd.) was uniformly dispersed in the range of 200 mPa·s to 20,000 mPa·s on the logarithmic axis. For these 18 samples, the viscosity at 30°C was measured using a vibration viscometer ("FVM72A-VM-200T3" produced by SEKONIC Co., Ltd.). The measured values of the E-type viscometer and the measured values of the vibration viscometer were plotted on the x-axis and y-axis of the double logarithmic graph, respectively, and the results confirmed that the measured values of the E-type viscometer and the measured values of the vibration viscometer were positively correlated (R 2 =0.96).
[0160] According to the results of Test Example 3, it is considered that by using a vibration viscometer as an online viscometer when continuously manufacturing a prepolymer solution, the viscosity can be measured without stopping the production line, etc. In addition, it is considered that the measurement of the viscosity can be automated. Furthermore, according to the results of Test Examples 2 and 3, it is considered that the viscosity of the prepolymer solution can be adjusted by controlling the supply amount of the reaction control agent based on the measured value of the viscosity measured by the vibration viscometer.
[0161] <Test Example 4>
[0162] In this test example, the effect of the presence or absence of a stirring step on the prepolymer solution was tested according to the following method.
[0163] [No.4-1]
[0164] (Preparation of prepolymer solution)
[0165] Prepolymer solution No. 4-1 was continuously prepared in the same manner as No. 2-3 except that the operation of the equipment was performed for 5 hours.
[0166] (Manufacturing of insulated wires)
[0167] Insulated wire No. 4-1 was produced in the same manner as No. 1-1 except that prepolymer solution No. 4-1 was used.
[0168] [No.4-2]
[0169] (Preparation of prepolymer solution)
[0170] After preparing a prepolymer solution in the same manner as in No. 4-1, the obtained prepolymer solution was supplied to a stirring tank and stirred for 30 minutes at a temperature of 80° C. and a stirring speed of 20 rpm. The stirred prepolymer solution was designated as prepolymer solution No. 4-2.
[0171] (Manufacturing of insulated wires)
[0172] Insulated wire No. 4-2 was produced in the same manner as No. 4-1 except that prepolymer solution No. 4-2 was used.
[0173] [evaluate]
[0174] The viscosity dispersion of the prepolymer solutions No. 4-1 and 4-2 prepared above was evaluated by the following method. Furthermore, the dispersion of the film elongation of the insulated wires No. 4-1 and 4-2 prepared above was evaluated by the following method.
[0175] (Discreteness of viscosity)
[0176] For the samples (N=31) sampled at 10-minute intervals, the viscosity at 30°C was measured using the above-mentioned E-type viscometer. The average value (arithmetic mean), standard deviation σ and coefficient of variation (CV value) of the viscosity were calculated from the measurement results. The coefficient of variation was calculated by dividing the standard deviation σ by the average value. The maximum viscosity and the minimum viscosity and the results are shown in Table 3 below.
[0177] (Discrepancy of film elongation)
[0178] For the samples (N=9) sampled at 75-minute intervals, the film elongation was measured by the same method as in the (film elongation) item of <Test Example 1> above. The average value (arithmetic mean), standard deviation σ, and coefficient of variation (CV value) of the film elongation were calculated based on the measurement results. The coefficient of variation was calculated by dividing the standard deviation σ by the average value. The maximum film elongation and the minimum film elongation and the results are shown in Table 3 below.
[0179] [Table 3]
[0180] No.4-1 No.4-2 With or without stirring none have Average viscosity [Pa·s] 28.2 29.3 Maximum viscosity [Pa·s] 45.7 33.2 Minimum viscosity [Pa·s] 19.2 25.7 Standard deviation of viscosity σ[Pa·s] 5.9 2.1 Coefficient of variation of viscosity 0.21 0.072 Average film elongation [%] 81 80 Maximum film elongation [%] 94 86 Minimum film elongation [%] 53 75 Standard deviation of film elongation σ[%] 13 3.2 Coefficient of variation of film elongation 0.16 0.040
[0181] As described above, in No. 4-2, which was stirred after mixing using a twin-screw extruder, the dispersion of the viscosity of the prepolymer solution was reduced compared to No. 4-1 which was not stirred. In addition, in No. 4-2, the dispersion of the elongation of the film of the insulated wire was also reduced compared to No. 4-1. Therefore, according to the results of Test Example 4, it can be seen that by stirring after mixing using an extruder, the dispersion of the viscosity of the prepolymer solution and the dispersion of the elongation of the film of the insulated wire can be reduced at the same time.
[0182] Description of Reference Numerals
[0183] 1: Twin screw extruder
[0184] 11: Second raw material supply unit
[0185] 12: First raw material supply unit
[0186] 13: Solvent supply unit
[0187] 14: Mixing section
[0188] 2: Vibration Viscometer
[0189] 3: Mixing tank.
Claims
1. A method for producing a prepolymer solution, comprising: continuously producing a prepolymer solution in which a prepolymer serving as a precursor of a thermosetting resin is dissolved in a solvent, the method comprising: A step of mixing a first raw material, a second raw material that reacts with the first raw material to form the prepolymer, and the solvent using an extruder.
2. The method for producing a prepolymer solution according to claim 1, wherein: In the mixing step, a reaction control agent is further mixed.
3. The method for producing a prepolymer solution according to claim 2, wherein: The method further comprises the step of measuring the viscosity of the prepolymer solution obtained by the mixing step. The supply amount of the reaction control agent in the mixing step is determined based on the measured value of the viscosity obtained in the measuring step.
4. The method for producing a prepolymer solution according to claim 1, 2 or 3, wherein: The method further comprises the step of stirring the prepolymer solution obtained in the mixing step.
5. The method for producing a prepolymer solution according to any one of claims 1 to 4, wherein: The solid content concentration of the prepolymer solution is 20 mass % or more and 50 mass % or less.
6. The method for producing a prepolymer solution according to any one of claims 1 to 5, wherein: The prepolymer has a group capable of forming an imide group through a dehydration reaction, the first raw material is a carboxylic anhydride, and the second raw material is a diamine compound.
7. The method for producing a prepolymer solution according to claim 6, wherein: The prepolymer is a polyimide prepolymer, and the carboxylic anhydride is tetracarboxylic dianhydride.
8. The method for producing a prepolymer solution according to any one of claims 1 to 7, wherein: The extruder is a twin-screw extruder.
9. The method for producing a prepolymer solution according to claim 3, wherein: In the above-mentioned measuring step, the viscosity is measured using a vibration viscometer.
10. The method for producing a prepolymer solution according to claim 4, wherein: The stirring step is performed at a temperature of 20° C. to 200° C.
11. A method for manufacturing an insulated wire, wherein: The insulated wire includes a conductor and an insulating layer covering the conductor, and the method for manufacturing the insulated wire includes: A step of applying a prepolymer solution obtained by the method for producing a prepolymer solution according to any one of claims 1 to 10 to the outer peripheral side of the conductor; and A step of heating the prepolymer solution applied to the conductor.