Impact modified blends of styrene-methyl methacrylate copolymers and vinylarene-olefin block copolymers

By combining styrene-methyl methacrylate copolymer and vinyl aromatic-olefin block copolymer in the molding composition, the problem of insufficient mechanical properties and light stability in the prior art is solved, and high light transmittance is achieved , low haze and good processability, suitable for a variety of applications.

CN119013344APending Publication Date: 2024-11-22INEOS STYROLUTION GRP GMBH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202380028399.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-03-21
Filing Date
2023-01-11
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

The prior art is difficult to provide molding compositions with good mechanical properties and light stability while maintaining high definition, especially in the case of insufficient processability in the extrusion molding process.

Method used

Using molding compositions containing styrene-methyl methacrylate copolymer (SMMA) and vinyl aromatic-olefin block copolymer, the stiffness, toughness balance and optical composition are improved by adjusting component ratios and structural design. performance, increase processability.

Benefits of technology

Achieve high light transmittance, low haze and good mechanical properties, improve processability, suitable for a variety of applications such as lighting and mask mixtures, caps and protective covers, and exhibit excellent performance in UV stability testing light stability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005047734840000031
    Figure BDA0005047734840000031
  • Figure BDA0005047734840000032
    Figure BDA0005047734840000032
  • Figure BDA0005047734840000091
    Figure BDA0005047734840000091
Patent Text Reader

Abstract

The invention relates to a moulding composition (P) comprising components (a), (b) and (c): a) 30-95 wt.-% of at least one random copolymer component (a) made from 30-70 wt.-% of at least one vinyl aromatic monomer (a11) and 30-70 wt.-% of methyl methacrylate (a12); (b) from 5 to 70 wt.% of at least one block copolymer (b) comprising at least one hard block H, recurring units comprising vinylarene monomers, and at least one elastomeric soft block S1, recurring units comprising olefin monomers, preferably ethylene, and at least one olefin monomer having 3 to 10 carbon atoms, and / or at least one soft block S2, preferably ethylene, comprising recurring units comprising olefin monomers, preferably ethylene, and at least one olefin monomer having 3 to 10 carbon atoms, repeating units comprising an olefin monomer and a vinylarene monomer, in particular ethylene, at least one olefin monomer having 3 to 10 carbon atoms and styrene; wherein the proportion of repeating units of the vinyl aromatic hydrocarbon monomer is 25-85 wt.%, based on the entire block copolymer (b); and (c) from 0 to 2 wt.% of one or more additives and / or processing aids (c); wherein the total amount of the components (a), (b) and (c) is 100 wt.-%.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a molding composition comprising a styrene-methyl methacrylate copolymer (SMMA) and at least one vinyl aromatic hydrocarbon-olefin block copolymer. These molding compositions and articles thereof have good mechanical properties and light stability while maintaining high clarity. The present invention also relates to a method for preparing the molding composition and a thermoplastic molding composition and molded article produced therefrom and their use. Background Art

[0002] For many years, styrene-ethylene / butylene block copolymers have been considered to provide effective modifiers for achieving impact strength when blended with styrene-methyl methacrylate copolymers while still maintaining good clarity and / or low haze.

[0003] JP2005-023267A (2005) discloses a resin composition comprising a copolymer mainly composed of styrene and methyl methacrylate and a styrene-ethylene / butylene-styrene copolymer, wherein the resin composition satisfies the relationship -3<0.101A-0.121B<1, wherein the styrene content of the copolymer mainly composed of styrene and methyl methacrylate is A% by weight, and the styrene content of the styrene copolymer is B% by weight.

[0004] JP2002-234981A discloses a resin composition comprising (a) 55-90 wt.-% of a styrene-methyl methacrylate copolymer, (b) 10-45 wt.-% of a high-density polyethylene and (c) 5-20 parts by weight of an olefin-styrene block copolymer having a styrene content ≥15 wt.-%, based on 100 parts by weight of components (a) and (b). Summary of the invention

[0005] The object of the present invention is to provide a molding composition comprising styrene-methyl methacrylate copolymer (SMMA) and vinyl aromatic-olefin block copolymer, having a good balance of stiffness and toughness, having high light stability, while maintaining high light transmittance and clarity. This combination of good mechanical and optical properties is suitable for many applications, such as lighting and light mask mixtures and cover layers and protective covers, cover layers for hygienic applications, point of purchase displays, container holders, display holders. Another object of the present invention is to provide a molding composition with improved processability, especially in extrusion molding processes.

[0006] According to the invention, this object is achieved by providing a (thermoplastic) molding composition (P) as claimed.

[0007] The present invention relates to a molding composition (P) comprising (or consisting of) components (a), (b) and (c): (a) at least one random copolymer (a) made from 30 to 70 wt.-% of at least one vinyl aromatic monomer (a11), in particular styrene, and 30 to 70 wt.-% of methyl methacrylate (a12); (b) at least one block copolymer (b) comprising: at least one hard block H comprising repeating units of a vinyl aromatic monomer, especially styrene, and at least one elastomeric soft block S1 comprising repeating units of olefin monomers, preferably ethylene and at least one olefin monomer having 3 to 10 carbon atoms, and / or at least one soft block S2 comprising repeating units of olefin monomers and vinyl aromatic monomers, in particular ethylene, at least one olefin monomer having 3 to 10 carbon atoms and styrene, wherein the proportion of the repeating units of the vinyl aromatic hydrocarbon monomer is 25-85 wt.% based on the entire block copolymer (b); as well as (c) optionally, one or more additives and / or processing aids (c); The total amount of components (a), (b) and (c) is 100 wt.-%.

[0008] In one embodiment, the molding composition (P) comprises (or consists of): (a) 30 to 95 wt.-% of at least one random copolymer (a) made from 30 to 70 wt.-% of at least one vinyl aromatic monomer (a11), in particular styrene, and 30 to 70 wt.-% of methyl methacrylate (a12); (b) 5 to 70 wt.-% of at least one block copolymer (b) comprising: at least one hard block H comprising repeating units of a vinyl aromatic monomer, especially styrene, and at least one elastomeric soft block S1 comprising repeating units of olefin monomers, preferably ethylene and at least one olefin monomer having 3 to 10 carbon atoms, and / or at least one soft block S2 comprising repeating units of olefin monomers and vinyl aromatic monomers, in particular ethylene, at least one olefin monomer having 3 to 10 carbon atoms and styrene, wherein the proportion of the repeating units of the vinyl aromatic hydrocarbon monomer is 25-85 wt.% based on the entire block copolymer (b); as well as (c) 0-2 wt.-% of one or more additives and / or processing aids (c); The total amount of components (a), (b) and (c) is 100 wt.-%.

[0009] In another embodiment, the molding composition (P) comprises (or consists of): (a) 30 to 82 wt.-% of at least one random copolymer (a) made from 30 to 70 wt.-% of at least one vinyl aromatic monomer (a11), in particular styrene, and 30 to 70 wt.-% of methyl methacrylate (a12); (b) 18 to 70 wt.-% of at least one block copolymer (b) comprising: at least one hard block H comprising repeating units of a vinyl aromatic monomer, especially styrene, and at least one elastomeric soft block S1 comprising repeating units of olefin monomers, preferably ethylene and at least one olefin monomer having 3 to 10 carbon atoms, and / or at least one soft block S2 comprising repeating units of olefin monomers and vinyl aromatic monomers, in particular ethylene, at least one olefin monomer having 3 to 10 carbon atoms and styrene, wherein the proportion of repeating units of the vinyl aromatic monomer is 25-85 wt.%, preferably 30-85 wt.-%, such as 30-80 wt.-% or 35-75 wt.-%, based on the entire block copolymer (b); and (c) 0-2 wt.-% of one or more additives and / or processing aids (c); The total amount of components (a), (b) and (c) is 100 wt.-%.

[0010] In this context, wt.-% means percent by weight.

[0011] Unless otherwise specified, the olefin monomers of the present invention are monofunctional olefin monomers having one terminal CC double bond, i.e. monomers of the general formula (Ia): in R1 is selected from hydrogen and a saturated hydrocarbon group containing 1 to 10 carbon atoms, preferably hydrogen; and R2 is selected from hydrogen and a saturated hydrocarbon group containing 1 to 10 carbon atoms, preferably a saturated hydrocarbon group containing 1 to 10 carbon atoms.

[0012] The diene monomers (also referred to as dienes) disclosed herein are olefin monomers having at least two CC double bonds, wherein at least one CC double bond is a terminal CC double bond and the second double bond is preferably a conjugated double bond, i.e., monomers of general formula (Ib): in R3 is selected from hydrogen and a saturated hydrocarbon group containing 1 to 10 carbon atoms, preferably selected from hydrogen and a saturated hydrocarbon group containing 1 or 2 carbon atoms; R4 is selected from hydrogen and a saturated hydrocarbon group containing 1 to 10 carbon atoms, preferably selected from hydrogen and a saturated hydrocarbon group containing 1 or 2 carbon atoms. R5 is selected from hydrogen and a saturated hydrocarbon group containing 1 to 10 carbon atoms, preferably selected from hydrogen and a saturated hydrocarbon group containing 1 to 3 carbon atoms.

[0013] According to the present invention, the random copolymer (a) comprises a copolymer having a statistical distribution of repeating units of vinyl monomers and methyl methacrylate.

[0014] The molding composition (P) according to the invention comprises (or consists of) the following amounts of components (a), (b) and (c): 30-95 wt-%, preferably 30-85 wt-%, for example 30-82 wt-%, 40-82 wt-% or 50-82 wt-% of at least one random copolymer component (a); 5-70 wt-%, preferably 15-70 wt-%, e.g., 18-70 wt-%, 18-60 wt-% or 18-50 wt-% of at least one block copolymer component (b); 0-2 wt-%, preferably 0.1-2 wt-% of at least one component (c); Therein, the total amount of components (a), (b) and (c) is 100 wt.-%.

[0015] In one embodiment, the molding composition (P) according to the invention preferably comprises (or consists of) the following amounts of components (a), (b) and (c): 50-85 wt-%, 50-82 wt-%, preferably 55-82 wt-%, e.g. 65-82 wt-% or 65-80 wt-% of at least one random copolymer component (a); 15-50 wt-%, 18-50 wt-%, preferably 18-45 wt-%, e.g. 18-35 wt-% or 20-35 wt-% of at least one block copolymer component (b); 0-2 wt-%, preferably 0.1-2 wt-% of at least one component (c); Therein, the total amount of components (a), (b) and (c) is 100 wt.-%.

[0016] In one embodiment, the molding composition (P) according to the invention preferably comprises (or consists of) the following amounts of components (a), (b) and (c): 50-81.9 wt-%, preferably 55-81.9 wt-%, e.g. 65-81.9 wt-% or 65-77.9 wt-% of at least one random copolymer component (a); 18-49.9 wt-%, preferably 18-44.9 wt-%, such as 18-34.9 wt-%, such as 20-34.9 wt-% of at least one block copolymer component (b); 0.1-2 wt-% of at least one component (c); Therein, the total amount of components (a), (b) and (c) is 100 wt.-%.

[0017] In one embodiment of the present invention, the at least one block copolymer (b) comprises (or consists of) at least one component (b-1), wherein component (b-1) is a block copolymer (b-1) comprising: at least one hard block H comprising repeating units of a vinyl aromatic monomer, especially styrene, and at least one elastomeric soft block S1 comprising repeating units of olefin monomers, preferably ethylene and at least one olefin monomer having 3 to 10 carbon atoms, and / or at least one soft block S2 comprising repeating units of olefin monomers and vinyl aromatic monomers, in particular ethylene, at least one olefin monomer having 3 to 10 carbon atoms and styrene; Therein, the proportion of the repeating units of the vinyl aromatic hydrocarbon monomer is 55-85 wt-%, preferably 55-80 wt-%, usually 60-75 wt-%, based on the entire block copolymer (b-1).

[0018] In one embodiment of the present invention, the at least one block copolymer (b) comprises (or consists of) two or more components (b-1).

[0019] In one embodiment of the present invention, the at least one block copolymer (b) comprises (or consists of) at least one component (b-2), wherein component (b-2) is a copolymer (b-2) comprising: at least one hard block H comprising repeating units of a vinyl aromatic monomer, especially styrene, and at least one elastomeric soft block S1 comprising repeating units of olefin monomers, preferably ethylene and at least one olefin monomer having 3 to 10 carbon atoms, and / or at least one soft block S2 comprising repeating units of olefin monomers and vinyl aromatic monomers, in particular ethylene, at least one olefin monomer having 3 to 10 carbon atoms and styrene; Therein, the proportion of the vinyl aromatic monomer is 25-54 wt-%, preferably 30-54 wt-%, usually 35-50 wt-%, based on the entire block copolymer (b-2).

[0020] In one embodiment of the present invention, the at least one block copolymer (b) comprises (or consists of) two or more components (b-2).

[0021] In one embodiment of the present invention, the at least one block copolymer (b) comprises (or consists of) a combination of at least one component (b-1) and at least one component (b-2), Wherein component (b-1) is a block copolymer (b-1), which comprises: at least one hard block H comprising repeating units of a vinyl aromatic monomer, especially styrene, and at least one elastomeric soft block S1 comprising repeating units of an olefin monomer and, preferably ethylene and at least one olefin monomer having 3 to 10 carbon atoms, and / or at least one soft block S2 comprising repeating units of olefin monomers and vinyl aromatic monomers, in particular ethylene, at least one olefin monomer having 3 to 10 carbon atoms and styrene; Wherein, based on the whole block copolymer (b-1), the proportion of the vinyl aromatic monomer is 55-85 wt-%, preferably 55-80 wt-%, usually 60-75 wt-%; Wherein component (b-2) is a copolymer (b-2), which comprises: at least one hard block H comprising repeating units of a vinyl aromatic monomer, especially styrene, and at least one elastomeric soft block S1 comprising repeating units of olefin monomers, preferably ethylene and at least one olefin monomer having 3 to 10 carbon atoms, and / or at least one soft block S2 comprising repeating units of olefin monomers and vinyl aromatic monomers, in particular ethylene, at least one olefin monomer having 3 to 10 carbon atoms and styrene; Therein, the proportion of the vinyl aromatic monomer is 25-54 wt-%, preferably 30-54 wt-%, usually 35-50 wt-%, based on the entire block copolymer (b-2).

[0022] Preferably, the molding composition (P) comprises, in addition to at least one component (b-1), at least one component (b-1) and optionally at least one component (b-2).

[0023] In one embodiment of the present invention, the molding composition (P) according to the present invention comprises 5 to 70 wt-%, preferably 15 to 70 wt-%, for example 18 to 70 wt-%, 18 to 60 wt-% or 18 to 50 wt-% of at least one block copolymer component (b), based on the total weight of the molding composition (P).

[0024] In one embodiment of the invention, the molding composition (P) according to the invention comprises 5 to 70 wt.-%, preferably 15 to 70 wt.-%, for example 18 to 70 wt.-%, 18 to 60 wt.-% or 18 to 50 wt.-%, based on the total weight of the molding composition (P), of at least one block copolymer component (b-1). For example, the molding composition (P) according to the invention may comprise 18 to 45 wt.-%, for example 18 to 35 wt.-% or 20 to 35 wt.-%, based on the total weight of the molding composition (P), of at least one block copolymer component (b-1).

[0025] In one embodiment of the invention, the molding composition (P) according to the invention comprises 5 to 70 wt.-%, preferably 15 to 70 wt.-%, for example 18 to 70 wt.-%, 18 to 60 wt.-% or 18 to 50 wt.-%, based on the total weight of the molding composition (P), of at least one block copolymer component (b-2). For example, the molding composition (P) according to the invention may comprise 18 to 45 wt.-%, for example 18 to 35 wt.-% or 20 to 35 wt.-%, based on the total weight of the molding composition (P), of at least one block copolymer component (b-2).

[0026] In one embodiment of the invention, the molding composition (P) according to the invention comprises 5-70 wt.-%, preferably 15-70 wt.-%, for example 18-70 wt.-%, 18-60 wt.-% or 18-50 wt.-% of a combination of at least one block copolymer component (b-1) and at least one block copolymer component (b-2), based on the total weight of the molding composition (P). For example, the molding composition (P) according to the invention may comprise 18-29 wt.-%, preferably 19-26.9 wt.-%, typically 19.6-25.5 wt.-% of at least one block copolymer component (b-1), and 3-14 wt.-%, preferably 4-11.9 wt.-%, typically 4.6-6.5 wt.-% of at least one block copolymer component (b-2), based on the total weight of the molding composition (P).

[0027] In one embodiment of the present invention, the molding composition (P) comprises (or consists of) the following amounts of components (a), (b-1), (b-2) and (c): 68-79 wt.-%, preferably 69-76.9 wt.-%, typically 69.6-75.5 wt.-% of at least one random copolymer component (a); 18 to 29 wt.-%, preferably 19 to 26.9 wt.-%, typically 19.6 to 25.5 wt.-% of at least one block copolymer component (b-1); 3 to 14 wt.-%, preferably 4 to 11.9 wt.-%, typically 4.6 to 6.5 wt.-% of at least one block copolymer component (b-2), and 0 to 2 wt.-%, preferably 0.1 to 2 wt.-%, typically 0.3 to 2 wt.-% of at least one component (c), wherein the total amount of components (a), (b-1), (b-2) and (c) is 100 wt.-%, and Component (b-1) is a block copolymer (b-1) comprising: at least one hard block H comprising repeating units of a vinyl aromatic monomer, especially styrene, and at least one elastomeric soft block S1 comprising repeating units of olefin monomers, preferably ethylene and at least one olefin monomer having 3 to 10 carbon atoms, and / or at least one soft block S2 comprising repeating units of olefin monomers and vinyl aromatic monomers, in particular ethylene, at least one olefin monomer having 3 to 10 carbon atoms and styrene; wherein the proportion of the vinyl aromatic monomer is 55-85 wt-%, preferably 55-80 wt-%, usually 60-75 wt-%, based on the entire block copolymer (b-1); and Component (b-2) is a copolymer (b-2) comprising: at least one hard block H comprising repeating units of a vinyl aromatic monomer, especially styrene, and at least one elastomeric soft block S1 comprising repeating units of olefin monomers, preferably ethylene and at least one olefin monomer having 3 to 10 carbon atoms, and / or at least one soft block S2 comprising repeating units of olefin monomers and vinyl aromatic monomers, in particular ethylene, at least one olefin monomer having 3 to 10 carbon atoms and styrene; Therein, the proportion of the vinyl aromatic monomer is 25-54 wt-%, preferably 30-54 wt-%, usually 35-50 wt-%, based on the entire block copolymer (b-2).

[0028] If component (c) is present, the minimum amount of component (c) is generally 0.1 wt.-%.

[0029] Preferably, the refractive index (at 589.3 nm) of components (a) and (b) in the molding composition (P) is in the range of 1.52-1.57. This gives the molding composition (P) particularly high clarity, high light transmittance and low haze. In a preferred embodiment of the present invention, the refractive index (at 589.3 nm) of the molding composition (P) is in the range of 1.52-1.57, more preferably 1.53-1.56.

[0030] Unless otherwise indicated, the refractive indices disclosed herein refer to the The system performs measurements similar to ASTM C 1648-12 at 589.3 nm and 23°C.

[0031] If multiple components (a) and / or (b) are used (for example, components (b-1) and (b-2)), the refractive index (at 589.3 nm) of the mixture of all components (a) is preferably in the range of 1.52-1.57, and the refractive index (at 589.3 nm) of the mixture of all components (b) is preferably in the range of 1.52-1.57.

[0032] The refractive index (at 589.3 nm) of the at least one component (a) is preferably in the range of 1.52-1.57, more preferably in the range of 1.53-1.56, for example in the range of 1.54-1.56.

[0033] The refractive index (at 589.3 nm) of the at least one component (b-1) is preferably in the range of 1.52-1.57, more preferably in the range of 1.54-1.57, for example in the range of 1.54-1.56.

[0034] The refractive index (at 589.3 nm) of the at least one component (b-2) is preferably in the range of 1.52-1.57, more preferably in the range of 1.52-1.55, for example in the range of 1.52-1.54.

[0035] Preferably, the refractive index difference ΔRI (at 589.3 nm) of components (a) and (b) in the molding composition (P) is ≤0.02, preferably ≤0.01, more preferably ≤0.008, typically ≤0.007, for example ≤0.006 or ≤0.005. This allows the molding composition (P) to have particularly high light transmittance, clarity and low haze. According to the invention, the refractive index difference ΔRI is calculated from the refractive indices of the individual components according to the following formula: ΔRI=|RI(a)-RI(b)| in: ΔRI = refractive index RI difference; RI(a) = refractive index of component (a) at 589.3 nm; RI(b) = refractive index of component (b) at 589.3 nm.

[0036] For a composition comprising a single component (a) having a refractive index RI(a) and a single component (b) having a refractive index RI(b), the refractive index difference ΔRI is calculated as follows: ΔRI=|RI(a)-RI(b)|

[0037] For a composition comprising a single component (a) having a refractive index RI(a) and two components (b) (i.e., one component (b1) having a refractive index RI(b1) and the other component (b2) having a refractive index RI(b2)), the refractive index difference ΔRI is calculated from the refractive index of each component and the mass fraction of each component as shown below: in: W(b1) = mass fraction of component (b1); W(b2) = mass fraction of component (b2).

[0038] For a single component (a) and a multi-component (b) (i.e., components (b1) to (b2) having a refractive index of RI (a) m ) has a refractive index of RI(b1) to RI(b m ), the refractive index difference ΔRI is calculated from the refractive index of each component and the mass fraction of each component, as shown below:

[0039] If more than one random copolymer is used as component (a) (i.e., components (a1) to (a2) n ) has a refractive index of RI(a1) to RI(a n )), the refractive index RI(a) of component (a) is calculated from the refractive index of each component and the mass fraction of the component, as shown below: in: W(a1) = mass fraction of component (a1); W(a n ) = component (a n )’s quality score.

[0040] As described below, the random copolymer component (a) may comprise at least one random copolymer of 30-70 wt.-% of a vinyl monomer (a11) and 30-70 wt.-% of methyl methacrylate (a12) in combination with other random copolymers (particularly, the other random copolymers comprise vinyl aromatic repeating units, such as other random copolymers of vinyl monomers and methyl methacrylate or random copolymers of vinyl monomers and acrylonitrile). However, typically, only one random copolymer is used as component (a). Molding compositions (P) comprising only one random copolymer as component (a) generally exhibit lower haze.

[0041] The molding composition (P) according to the invention has a light transmittance of more than 40%. Preferably, the light transmittance of the molding composition (P) according to the invention is greater than 60%, more preferably greater than 70%, typically greater than or equal to 80%, for example greater than or equal to 90%. The light transmittance is determined according to ASTM D1003 on a specimen with a thickness of 3.2 mm (0.125 inches).

[0042] Preferably, the molding composition (P) according to the invention has a clarity greater than 90%, more preferably greater than 95%, typically greater than or equal to 98%, for example greater than or equal to 99%. The clarity is determined according to ASTM D1003 on samples of 3.2 mm (0.125 inch) thickness.

[0043] Preferably, the molding composition (P) according to the invention has a haze of less than 50%, more preferably less than 40%, typically less than 20%.The haze is determined according to ASTM D1003 on samples of 3.2 mm (0.125 inch) thickness.

[0044] Particularly high light transmittance and clarity and low haze are generally achieved by molding compositions (P) in which the refractive index difference ΔRI (at 589.3 nm) of components (a) and (b) is ≤0.02, preferably ≤0.01, more preferably ≤0.008, typically ≤0.007, for example ≤0.006 or ≤0.005.

[0045] In some embodiments, the molding composition (P) according to the present invention is characterized by a haze of less than 20%, more preferably less than or equal to 15% or 10%, measured according to ASTM D1003 on a 3.2 mm (0.125 inch) thick injection molded plaque. This is generally achieved by a molding composition (P) as described above, wherein the refractive index difference ΔRI of the random copolymer (a) and the block copolymer (b) is less than or equal to about 0.003, for example less than or equal to about 0.0026.

[0046] The molding composition (P) according to the invention has good light stability. In particular, the molding composition (P) according to the invention is characterized in that, after a UV stability test (600 hours), the yellowness index increase (ΔYI) is preferably less than 2 units, more preferably less than 1.5 units, typically less than 1 unit of yellowness index increase (ΔYI), wherein the UV stability test is carried out according to AATCC TM16.3, wherein the yellowness index is calculated according to ASTM E313 from the measured CIELAB color space values, and the CIELAB color space values ​​are measured according to ASTM E1348 with D65 light source (observation angle of 10°).

[0047] Furthermore, the molding composition (P) according to the invention is characterized in that after a UV stability test (600 hours), the color change (ΔE) is preferably less than 2 units, more preferably less than 1.5 units, typically less than 1 unit of color change (ΔE), wherein the UV stability test is carried out in accordance with AATCC TM16.3, wherein the color change (ΔE) is calculated in accordance with ASTM D2244 from the measured CIELAB color space values, and the CIELAB color space values ​​are measured in accordance with ASTM E1348 with a D65 light source (observation angle of 10°).

[0048] The molding compositions (P) according to the invention also exhibit improved mechanical properties, as determined by their tensile energy at break. The tensile energy at break determined according to ASTM D638-14 is preferably greater than 17 Nm, more preferably greater than 18 Nm.

[0049] The molding composition (P) according to the invention generally has a melt flow rate (MFR, measured at 200° C. and 5 kg according to ASTM D12385) of ≥ 2 g / 10 min. In some cases, the melt flow rate (MFR, measured at 200° C. and 5 kg according to ASTM D1238) of the molding composition (P) in the absence of the block copolymer component (b) is increased by at least 1.5 times compared to the block copolymer component (a).

[0050] In a preferred embodiment, the molding composition (P) according to the invention consists of components (a) and (b) and optionally (c). In another embodiment, the molding composition (P) according to the invention consists of components (a), (b-1) and (b-2), and optionally (c).

[0051] According to the present invention, the molding composition (P) comprises (or preferably consists of) at least one random copolymer (a), at least one block copolymer (b) and additives and / or processing aids (c) as defined herein. Thus, in addition to the at least one copolymer (a) and the at least one block copolymer (b), the molding composition (P) preferably comprises essentially no other polymer components, in particular no polymer components having a refractive index (at 589.3 nm) outside the range of 1.52-1.57, since these polymer components significantly reduce the optical properties of the molding composition (P). This means that the molding composition (P) preferably comprises less than 1 wt.-%, more preferably less than 0.5 wt.-% of polymer components having a refractive index (at 589.3 nm) outside the range of 1.52-1.57, based on the total weight of the molding composition (P). Examples of undesired polymer components include, but are not limited to, for example, polyolefins (e.g. without polyethylene, polypropylene or ethylene-propylene copolymers), polyamides, polycarbonates or poly(meth)acrylates.

[0052] However, the molding composition (P) optionally comprises polymer components other than the at least one random copolymer (a) and the at least one block copolymer (b) made of vinyl aromatic monomers and methyl methacrylate, as long as the refractive index (at 589.3 nm) of these polymer components is in the range of 1.52 to 1.57. For example, the molding composition (P) may comprise a random copolymer of styrene and acrylonitrile (SAN) in an amount preferably of less than 40 wt.-%, more preferably of less than 30 wt.-%, based on the total weight of the molding composition (P).

[0053] In addition, as described below, the polymer composition (P) may comprise as additive component (c) a polyolefin wax having a weight average molecular weight ≤ 20000 g / mol, as a release agent, in an amount generally < 1 wt.-%, based on the total weight of the polymer composition (P). According to the present invention, unless otherwise stated, the weight average molecular weight is determined by gel permeation chromatography (GPC) according to ASTM D3593. Alternatively, the polymer composition (P) may comprise a polymer component having a refractive index (at 589.3 nm) in the range of 1.52-1.57. Component (a)

[0054] According to the present invention, the molding composition (P) comprises a random copolymer component (a). The random copolymer component (a) comprises (or consists of) at least one (preferably one) random copolymer made from 30-70 wt.-% of a vinyl aromatic monomer (a11), in particular styrene, and 30-70 wt.-% of methyl methacrylate (a12); more preferably a random copolymer made from 40-65 wt.-%, more preferably 45-63 wt.-%, further preferably 48-60 wt.-%, typically 50-58 wt.-% of a vinyl aromatic monomer (a11), and 35-60 wt.-%, more preferably 37-55 wt.-%, further preferably 40-52 wt.-%, typically 42-50 wt.-% of methyl methacrylate (a12). In the composition, the total amount of (a11) and (a12) is 100 wt.-%, and the vinyl aromatic monomer (a11) and methyl methacrylate (a12) are statistically distributed in the random copolymer.

[0055] Styrene-methyl methacrylate (SMMA) copolymer (a) can be obtained by known methods such as bulk polymerization, solution polymerization, suspension polymerization, precipitation polymerization or emulsion polymerization. The details of these methods are described, for example, in Kunststoffhandbuch, ed. R. Vieweg and G. Daumiller, "Polystyrol", Carl-Hanser-Verlag Munich, 1969, Vol. 5, p. 118 et seq. SMMA copolymer (a) is a known product and can be purchased, for example, from Ineos Styrolution (Frankfurt, Germany).

[0056] Furthermore, the random copolymer component (a) may comprise one or more random copolymers other than the vinylarene-methyl methacrylate copolymers (e.g. SMMA) described herein, for example random copolymers of styrene and acrylonitrile (SAN), preferably in an amount of less than 50 wt.-%, typically less than 40 wt.-%, based on the total weight of the random copolymer component (a). However, in order to obtain molding compositions (P) with low haze, it is generally advantageous to use only one random copolymer as random copolymer component (a). Component (b)

[0057] The at least one block copolymer component (b) comprises at least one block copolymer (b), which may be a linear or radial block copolymer, comprising: at least one hard block H comprising repeating units of a vinyl aromatic monomer, especially styrene, and at least one soft block S1 comprising repeating units of olefin monomers, in particular ethylene and at least one olefin monomer having 3 to 10 carbon atoms, and / or At least one soft block S2 comprises repeating units of olefin monomers and vinyl aromatic monomers, in particular ethylene and at least one olefin monomer having 3 to 10 carbon atoms as repeating units of olefin monomers, and styrene as repeating units of vinyl aromatic monomers.

[0058] In one embodiment of the present invention, the at least one block copolymer (b) may be a linear block copolymer comprising: a hard block H comprising repeating units of a vinyl aromatic monomer, especially styrene, and A soft block S1 comprising repeating units of an olefin monomer, in particular ethylene and at least one olefin monomer having 3 to 10 carbon atoms, and / or A soft block S2 comprises repeating units of olefin monomers and vinyl aromatic hydrocarbon monomers, in particular ethylene and at least one olefin monomer having 3 to 10 carbon atoms as repeating units of olefin monomers, and styrene as repeating units of vinyl aromatic hydrocarbon monomers.

[0059] In an alternative embodiment of the present invention, the at least one block copolymer (b) may be a linear or radial block copolymer comprising: at least two hard blocks H comprising repeating units of vinyl aromatic monomers, especially styrene, and at least one soft block S1 comprising repeating units of olefin monomers, in particular ethylene and at least one olefin monomer having 3 to 10 carbon atoms, and / or At least one soft block S2 comprises repeating units of olefin monomers and vinyl aromatic monomers, in particular ethylene and at least one olefin monomer having 3 to 10 carbon atoms as repeating units of olefin monomers, and styrene as repeating units of vinyl aromatic monomers. In a preferred embodiment thereof, the at least two hard blocks H comprising repeating units of vinyl aromatic monomers preferably constitute the terminal blocks of the block copolymer (b).

[0060] Suitable vinyl aromatic monomers that can constitute the repeating units of the hard (polymer) block H or the soft (copolymer) block S2 of component (b) are styrene, α-methylstyrene, p-methylstyrene, ethylstyrene, tert-butylstyrene, vinyltoluene or mixtures of these, preferably styrene. The hard (polymer) block H of the block copolymer (b) is preferably a monomer having a glass transition temperature (T g )>70℃ hard phase.

[0061] T g It is measured by methods well known to polymer chemists, in particular differential scanning calorimetry (DSC).

[0062] The hard block H of component (b) may comprise 95-100 wt.% of repeating units of at least one vinyl aromatic monomer and 0-5 wt.% of repeating units of at least one olefin monomer. Preferably, the hard block H is a homopolymer comprising repeating units of a vinyl aromatic monomer, especially styrene.

[0063] Suitable olefin monomers that can constitute the repeating units of the soft (polymer) block S1 or the soft (copolymer) block S2 of component (b) are monofunctional olefin monomers of formula (Ia), which can preferably be selected from ethylene and at least one olefin monomer having 3 to 10 carbon atoms, such as propylene, butene, 2-methylpropylene, 1-pentene, 1-hexene, vinylcyclohexane or mixtures of these, preferably ethylene and propylene or ethylene and butene, especially ethylene and butene. The soft (polymer) block S1 of the block copolymer (b) is a soft phase, preferably having a glass transition temperature (T g )<0°C, preferably in the range of -60°C to -10°C.

[0064] In addition, the soft (polymer) block S1 or the soft (copolymer) block S2 of component (b) may contain repeating units of diene monomers, for example 1,3-butadiene, isoprene, 2,3-dimethylbutadiene, 1,3-pentadiene or 1,3-hexadiene or mixtures of these, preferably 1,3-butadiene and isoprene, especially 1,3-butadiene. The repeating units of these diene monomers may be retained as residues of incomplete hydrogenation of the vinyl aromatic hydrocarbon-diene block copolymer (b') during the preparation of the vinyl aromatic hydrocarbon-olefin block copolymer (b) described below. The amount of repeating units of diene monomers is preferably ≤10 wt.-%, more preferably ≤5 wt.-%, based on the at least one soft block S1 / or at least one soft block S2, respectively.

[0065] The soft block S1 of component (b) may contain 95-100 wt-% of repeating units of at least one olefin monomer (and optionally repeating units of respective diene monomers) and 0-5 wt-% of repeating units of at least one vinyl aromatic monomer, preferably the soft block S1 is a copolymer of repeating units of at least one olefin monomer (and optionally repeating units of respective diene monomers), preferably ethylene and at least one additional olefin monomer having 3-10 carbon atoms.

[0066] Preferably, the at least one elastomeric soft block S1 comprises repeating units of ethylene and at least one olefin monomer, such as propylene, butene, 2-30 methylpropylene, 1-pentene, 1-hexene, vinylcyclohexane or a mixture of these, preferably selected from propylene and butene, more preferably selected from ethylene and propylene or ethylene and butene, especially ethylene and butene. Likewise, the at least one soft block S2 preferably comprises repeating units of ethylene, at least one olefin monomer selected from propylene and butene and styrene, more preferably ethylene, butene and styrene.

[0067] Typically, based on the entire block copolymer (b), the proportion of repeating units of vinyl aromatic monomers is 25-85wt-%, preferably 30-85wt-%, such as 30-80wt-%, and the proportion of repeating units of olefin monomers is 15-75wt-%, preferably 15-70wt-%, such as 20-70wt-%.

[0068] In one embodiment, component (b) comprises (or consists of) at least two block copolymers (b-1) and (b-2), wherein: (b-1) is at least one block copolymer (b-1) comprising: at least one hard block H comprising repeating units of a vinyl aromatic monomer, especially styrene, and at least one elastomeric soft block S1 comprising repeating units of olefin monomers, in particular ethylene and butene, and / or at least one soft block S2 comprising repeating units of olefin monomers and vinyl aromatic monomers, in particular ethylene, butene and styrene; wherein the proportion of the vinyl aromatic monomer is 55-85 wt-%, preferably 55-80 wt-%, usually 60-75 wt-%, based on the entire block copolymer (b-1); and (b-2) is at least one block copolymer (b-2) comprising: at least one hard block H comprising repeating units of a vinyl aromatic monomer, especially styrene, and at least one elastomeric soft block S1 comprising repeating units of olefin monomers, in particular ethylene and butene, and / or at least one soft block S2 comprising repeating units of olefin monomers and vinyl aromatic monomers, in particular ethylene, butene and styrene; Therein, the proportion of the vinyl aromatic monomer is 25-54 wt-%, preferably 30-54 wt-%, usually 35-50 wt-%, based on the entire block copolymer (b-2).

[0069] In one embodiment, component (b) comprises (or consists of) at least two block copolymers (b-1) and (b-2), wherein: (b-1) is at least one block copolymer (b-1) comprising: at least one hard block H comprising repeating units of a vinyl aromatic monomer, especially styrene, and at least one elastomeric soft block S1 comprising repeating units of olefin monomers, in particular ethylene and butene; wherein the proportion of the vinyl aromatic monomer is 55-85 wt-%, preferably 55-80 wt-%, usually 60-75 wt-%, based on the entire block copolymer (b-1); and (b-2) is at least one block copolymer (b-2) comprising: at least one hard block H comprising repeating units of a vinyl aromatic monomer, especially styrene, and at least one elastomeric soft block S1 comprising repeating units of olefin monomers, in particular ethylene and butene; Wherein, based on the whole block copolymer (b-2), the proportion of vinyl aromatic monomer is 25-54wt-%, preferably 30-54 wt-%, typically 35-50 wt-%.

[0070] The present inventors have found that the combination of two block copolymers (b-1) and (b2) results in unexpected mechanical and optical properties, such as good impact strength, combined with high light transmittance and low haze.

[0071] In one embodiment of the present invention, component (b) comprises (or consists of): (b-1) 45 to 95 wt.-%, preferably 55 to 90 wt.-%, more preferably 65 to 88 wt.-%, based on the total weight of component (b), of at least one block copolymer (b-1); and (b-2) 5 to 55 wt.-%, preferably 10 to 45 wt.-%, more preferably 12 to 35 wt.-%, based on the total weight of component (b), of at least one block copolymer (b-2).

[0072] In some embodiments, the soft block is a block S2, especially a random block S2. A "random" block S2 refers to a copolymer block having a statistical distribution of repeating units of vinyl aromatic monomers and olefin monomers.

[0073] The (copolymer) block S2, in particular the random copolymer block S2, may comprise 5-39 wt-%, in particular 6-39 wt-%, of repeating units of a vinyl aromatic monomer, in particular styrene, and 61-95 wt-% (less than 95 wt-%), in particular 61-94 wt-%, of repeating units of an olefin monomer, preferably ethylene and at least one olefin monomer having 3 to 10 carbon atoms, wherein the total amount of repeating units of the vinyl aromatic monomer and the olefin monomer is 100 wt-%.

[0074] There may also be more than one preferably random (copolymer) block S2. The block copolymer (b) generally comprises at least two, especially random, soft (copolymer) blocks S 2-1 and S 2-2 , which have different ratios of vinyl aromatic monomer repeating units and therefore have different glass transition temperatures.

[0075] Preferably, the block copolymer (b) is a linear block copolymer having one or more hard blocks H, preferably terminal hard blocks H, and at least one soft block S1 and / or at least one soft block S2.

[0076] According to one embodiment, the block copolymer (b) is a (preferably linear) block copolymer of structure H-S1, in particular a styrene-ethylene / butylene block copolymer of structure H-S1.

[0077] According to an alternative embodiment, the block copolymer (b) is a (preferably linear) block copolymer of structure H-S2, in particular a styrene-ethylene / butylene block copolymer of structure H-S2.

[0078] According to another embodiment, the block copolymer (b) is a (preferably linear) block copolymer of the structure H-S1-H, in particular a styrene-ethylene / butylene block copolymer of the structure H-S1-H.

[0079] According to another alternative embodiment, the block copolymer (b) is a (preferably linear) block copolymer of the structure H-S2-H, in particular a styrene-ethylene / butylene block copolymer of the structure H-S2-H.

[0080] Component (b) is preferably obtained by hydrogenation of the non-conjugated double bonds of a vinyl aromatic-diene block copolymer (b'), which comprises at least one hard block H' made of a vinyl aromatic monomer and at least one soft block S1' made of a diene and / or at least one soft block S2' made of a diene and a vinyl aromatic monomer. Typically, component (b) is prepared by hydrogenating a vinyl aromatic-diene block copolymer (b'), wherein preferably at least 90% of the non-conjugated double bonds are hydrogenated, more preferably at least 95%.

[0081] The vinyl aromatic hydrocarbon-diene block copolymer (b') may be a linear or radial block copolymer, comprising: at least one hard block H', made from a vinyl aromatic monomer, especially styrene, and At least one soft block S1' made of a diene and / or At least one soft block S2' is made from diene and vinyl aromatic monomers.

[0082] In one embodiment of the present invention, the at least one vinyl aromatic hydrocarbon-diene block copolymer (b') may be a linear block copolymer comprising: a hard block H' made from a vinyl aromatic monomer, especially styrene; and a soft block S1' made of a diene; and / or At least one soft block S2' is made from diene and vinyl aromatic monomers.

[0083] In an alternative embodiment, the at least one vinyl aromatic hydrocarbon monomer-diene block copolymer (b') may be a linear or radial block copolymer comprising: at least two hard blocks H' made from vinyl aromatic monomers, especially styrene; and at least one soft block S1' made of a diene, and / or At least one soft block S2' is made from diene and vinyl aromatic monomers. In a preferred embodiment thereof, the at least two hard blocks H' made of vinyl aromatic monomers preferably constitute the terminal blocks of the vinyl aromatic-diene block copolymer (b').

[0084] The vinyl aromatic monomers that can be used for the hard (polymer) block H' or for the soft (copolymer) block S2' are styrene, α-methylstyrene, p-methylstyrene, ethylstyrene, tert-butylstyrene, vinyltoluene or mixtures thereof, preferably styrene. The hard (polymer) block H' of the block copolymer (b) is a hard phase having a glass transition temperature (T g )>70℃.

[0085] It is recognized by those skilled in the art that in order to prepare a vinyl aromatic-olefin block copolymer (b) from a vinyl aromatic-diene block copolymer (b'), it is required that the proportion of repeating units of the vinyl aromatic monomer of the vinyl aromatic-diene block copolymer (b') is in the same range, i.e. 25-85 wt.-%, preferably 30-85 wt.-%, e.g. 30-80 wt.-%, based on the entire block copolymer (b). Similarly, the proportion of the vinyl aromatic monomer in the vinyl aromatic-diene block copolymer (b-1') used to prepare the vinyl aromatic-olefin block copolymer (b-1) is 55-85 wt.-%, preferably 55-80 wt.-%, typically 60-75 wt.-%, based on the entire block copolymer (b-1'). Likewise, the proportion of the vinylarene monomer in the vinylarene-diene block copolymer (b-2') used to prepare the vinylarene-olefin block copolymer (b-2) is 25-54 wt.-%, preferably 30-54 wt.-%, typically 35-50 wt.-%, based on the entire block copolymer (b-2').

[0086] The hard block H' of the vinyl aromatic-diene block copolymer (b') may be made from 95-100 wt-% of at least one vinyl aromatic monomer and 0-5 wt-% of at least one diene, preferably the hard block H' is a homopolymer made from a vinyl aromatic monomer, especially styrene.

[0087] Suitable dienes that can be used to prepare the vinyl aromatic hydrocarbon-diene block copolymer (b') are conjugated dienes, preferably conjugated dienes of formula (Ib) as described above. The diene used for at least one soft block S1' or at least one soft block S2' (or optionally for the hard block H') is preferably 1,3-butadiene, isoprene, 2,3-dimethylbutadiene, 1,3-pentadiene or 1,3-hexadiene or a mixture of these, more preferably 1,3-butadiene and isoprene, especially 1,3-butadiene.

[0088] The soft block S1' of the vinyl aromatic-diene block copolymer (b') may be made from 95-100 wt-% of at least one diene and 0-5 wt-% of at least one vinyl aromatic monomer, preferably the soft block B is a homopolymer made from a conjugated diene, especially 1,3-butadiene.

[0089] In some embodiments, the soft block is a block S2' of a vinyl aromatic hydrocarbon-diene block copolymer (b'), especially a random block S2'. A "random" block S2' refers to a copolymer block having a statistical distribution of polymerized units of a vinyl aromatic hydrocarbon monomer and a diene monomer.

[0090] The (copolymer) block S2', especially the random copolymer block S2', of the vinyl aromatic hydrocarbon-diene block copolymer (b') is usually made from 5-39 wt-%, especially 6-39 wt-% of vinyl aromatic hydrocarbon monomers, especially styrene, and 61-95 wt-% (less than 95 wt-%), especially 61-94 wt-% of diene monomers, especially 1,3-butadiene, wherein the total amount of vinyl aromatic hydrocarbon monomers and diene monomers is 100 wt-%.

[0091] There may also be more than one, preferably random, (copolymer) block S2'. Usually the block copolymer (b) comprises at least two, in particular random, soft (copolymer) blocks S 2-1 ' and S 2-2 ', they have different proportions of vinyl aromatic monomers and therefore have different glass transition temperatures. For example, S 2-1 '、S 2-2 ' and all copolymer blocks S2', T g <0°C, generally in the range of -80°C to 0°C, preferably in the range of -70°C to -20°C, particularly preferably in the range of -70°C to -40°C.

[0092] The block copolymer (b') is preferably prepared by sequential anionic polymerization. The block copolymer (b) is preferably prepared by hydrogenation of the non-conjugated double bonds of the block copolymer (b') (i.e., the double bonds mainly present in the soft block S2' or soft block S1' of the block copolymer (b')). For example, hydrogenation can be achieved by reacting the block copolymer (b') with hydrogen under a suitable catalyst. Block copolymers (b) and block copolymers (b') are known. The preparation of block copolymers (b') is described in, for example, "Modern Styrenic Polymers: Polystyrenes and Styrenic Copolymers" (Eds., J. Scheirs, D. Priddy, Wiley, Chichester, UK, (2003), pages 502-507), especially in US6521712 (column 2, line 52 to column 4, line 2). The process for preparing block copolymers (b) by hydrogenation of block copolymers is described, for example, in US 2015 / 0031835 A1.

[0093] Examples of block copolymers (b) are known products available from Asahi Kasei, Japan, such as TUFTEC TM H1043 and TUFTEC TM H1517. Component (c)

[0094] Optionally, the thermoplastic molding composition (P) may comprise up to 2.0 wt.-%, preferably 0.10 to 2 wt.-%, of at least one further additive and / or processing aid (c) (as component (c)).

[0095] Suitable additives and / or processing aids (c) include, besides fillers / fibers and pigments, generally all substances which are used for processing or finishing polymers (see, for example, “Plastics Additives Handbook”, Hans Zweifel, 6th edition, Hanser Publ., Munich, 2009).

[0096] Preferred additives and / or processing aids (c) are, for example, stabilizers (eg UV stabilizers), oxidation inhibitors, antioxidants, agents against thermal and photodecomposition, lubricants and dyes.

[0097] These additives and / or processing aids (c) may be mixed at any stage of the production process, but are preferably mixed at an early stage in order to benefit from the stabilizing effect (or other specific effect) of the added substances as early as possible.

[0098] Suitable antioxidants are, for example, one or more compounds selected from monophosphite antioxidants, diphosphite antioxidants and hindered phenolic antioxidants. If one or more antioxidants are present, they are preferably selected from monophosphite antioxidants (such as trisubstituted monophosphite derivatives), diphosphite antioxidants (such as substituted pentaerythritol diphosphite derivatives), and hindered phenolic antioxidants (such as 2,6-di-tert-butylphenol derivatives).

[0099] Suitable lubricants / glidants and mold release agents include stearic acid, stearyl alcohol, stearic acid esters, amide waxes (bisstearamide, especially ethylene bisstearamide), polyolefin waxes with a weight average molecular weight ≤ 20000 g / mol and / or generally higher fatty acids, their derivatives and corresponding fatty acid mixtures containing 12-30 carbon atoms.

[0100] Suitable dyes are any dyes that can be used for transparent, semi-transparent or opaque coloring of polymers, especially those dyes that are suitable for the coloring of styrene copolymers. Such dyes are well known to those skilled in the art. Preferably, dyes that can be used for transparent coloring of polymers.

[0101] Examples of oxidation inhibitors and heat stabilizers are halides of metals of Group I of the Periodic Table of the Elements, for example sodium, potassium and / or lithium halides, optionally in combination with copper(I) halides, for example chlorides, bromides, iodides, sterically hindered phenols, hydroquinone, different substitutions of these groups and mixtures thereof, in concentrations of up to 1 wt.-%, based on the weight of the molding composition (P).

[0102] Examples of suitable stabilizers against the effects of light (eg UV stabilizers) are various substituted resorcinols, salicylates, benzotriazoles, triazines, benzophenones and HALS (hindered amine light stabilizers), such as those commercially available as The amount thereof may generally be up to 1.7 wt.-%, based on the molding composition (P). Preparation method

[0103] Another aspect of the present invention is a process for preparing the molding composition (P) according to the invention by melt mixing components (a), (b) and (if any) component (c). Preferably, the melt mixing of components (a), (b) and (if any) (c) is carried out in an extruder, preferably a twin-screw extruder.

[0104] Melt mixing may preferably be performed in an extruder at a temperature range of 160-260° C. Preferably, melt mixing is performed in an extruder at a temperature range of 180-230° C.

[0105] The molding compositions (P) obtained by the process show good processability and can therefore be easily processed, i.e. molded into any desired shape, e.g. by extrusion and hot molding (e.g. injection molding). Therefore, another aspect of the present invention is a shaped article produced from the molding composition (P) according to the invention.

[0106] The molding compositions (P) according to the invention and the shaped articles produced therefrom show a good balance of stiffness and toughness, have high light stability, while maintaining high light transmittance and clarity. They can be advantageously used in many applications.

[0107] The molding compositions (P) according to the invention can advantageously be used in many applications, for example in household goods, household appliances, for example lighting and light covering compounds and also cover layers and protective covers.

[0108] The present invention further provides for the use of the molding compositions (P) according to the invention and the shaped articles produced therefrom in various applications in household goods, household appliances, for example lighting and light shielding mixtures and also coverings and protective covers, coverings for hygiene applications, point-of-purchase displays, container stands, display stands.

[0109] The invention is further illustrated by the examples, the drawings and the patent claims. DETAILED DESCRIPTION

[0110] Example:

[0111] Test method:

[0112] Melt flow rate (MFR) is measured according to ASTM D1238 at 200°C and 5 kg.

[0113] Unnotched Izod impact strength is measured according to ASTM D4812.

[0114] The tensile stress at yield, tensile strain at break and tensile energy at break were determined according to the test of ASTM D638-14 standard.

[0115] Rockwell hardness is measured according to ASTM D785.

[0116] Optical properties (haze, light transmittance and clarity) were measured according to ASTM D1003 on samples of 3.2 mm (0.125 inch) thickness.

[0117] UV stability test was conducted according to AATCC TM16.3, at 63°C, the xenon irradiance (420nm) on the black panel was 1.10W / m 2 .

[0118] The refractive index at 589.3 nm and 23° C. was measured using a Metricon Model 2010 / M prism coupler in a manner similar to ASTM C 1648-12 (particularly referring to Section 9.4 of ASTM C 1648-12). The refractive index difference ΔRI of the random copolymer (a) and the block copolymer (b) used in the examples (see the compositions and raw materials of the examples below) was calculated according to the following formula: in RI SMMA =The refractive index of SMMA at 589.3nm; RI SEBS-1 = refractive index of SEBS-1 at 589.3 nm; RI SEBS-2 = refractive index of SEBS-2 at 589.3 nm; w SEBS-1 = mass fraction of SEBS-1 in the composition; w SEBS-2 = mass fraction of SEBS-2 in the composition.

[0119] The yellowness index (YI) was calculated from the measured CIELAB color space values ​​according to ASTM E313. The CIE color space values ​​were measured with a D65 illuminant (observation angle 10°) according to ASTM E1348.

[0120] The color change (ΔE) was calculated from the measured CIELAB color space values ​​according to ASTM D2244. The CIE color space values ​​were measured according to ASTM E1348 with D65 illuminant (observation angle 10°).

[0121] raw material:

[0122] Reference Example 1 (Ref. 1) is a commercial methyl methacrylate butadiene styrene (MBS) polymer composition from INEOS Styrolution 631. Reference Example 2 (Ref. 2) is a blend of 81 wt.-% SMMA and 19 wt.-% styrene block-butadiene block styrene copolymer (SBS).

[0123] The materials shown in Tables 1-5 were melt mixed using a 30 mm twin screw extruder with the zone temperature set at 180-230° C. Samples were injection molded from the obtained molding compositions (P) and the mechanical and optical properties of the parts were tested. Tables 1-5 show the mechanical and optical properties of the injection molded samples of Examples 2-24 and Comparative Example C1. Tables 1-6 further demonstrate the comparison between the samples according to the present invention (Examples 2-24) and the current commercial styrene impact modified transparent molding compositions (P), such as 631 (impact-modified styrene acrylic copolymer (methyl methacrylate butadiene styrene (MBS) resin), as well as a mixture of random styrene / methyl methacrylate copolymer and styrene block-butadiene block styrene copolymer (SBS) (Ref. 1 and Ref. 2; Table 4) and SMMA without impact modification (Comparative Example C1).

[0124] Figure 1 The tensile energy at break (in-lbf, left axis) and the haze (in % , right axis) of Examples 2-24 and Comparative Example C1 according to Tables 1-5 are shown.

[0125] Figure 2 The change in yellowness index (ΔYI) with UV irradiation time (hours) measured according to AATCC TM16.3 for Comparative Example C1, Example 15, and Reference Examples Ref. 1 and Ref. 2 in Table 6 is described.

[0126] Figure 3 The color change (ΔE) with UV irradiation time (hours) measured according to AATCC TM16.3 for Comparative Example C1, Example 15 and Reference Examples Ref. 1 and Ref. 2 according to Table 6 is described.

[0127] Figure 4 The correlation between the refractive index difference (ΔRI) (measured analogously to ASTM C 1648-12 at 589.3 nm and 23° C. and calculated as described above) and the light transmittance (measured according to ASTM D1003 on a sample of 3.2 mm thickness) is shown. Table 1 Composition and properties of SMMA / SEBS-1 blends of Examples 2-5 and Comparative Example C1

[0128] Tables 1 and 2 show that the SMMA compositions comprising at least one SEBS according to the present invention exhibit improved MFR and further exhibit improved mechanical properties, such as tensile energy at break and unnotched Izod impact strength, compared to the non-impact modified SMMA (Comparative Example C1). In addition, it can be seen that the molding compositions (P) having a ΔRI of less than or equal to 0.02 have superior optical properties (Examples 2-5), while the molding compositions having a higher ΔRI have low light transmittance, low clarity and high haze (Examples 6-8). Table 2 Composition and properties of SMMA / SEBS-2 blends of Examples 6-8 and Comparative Example C1 Table 3 Composition and properties of SMMA / SEBS-1 / SEBS-2 blends of Examples 9-13

[0129] Tables 3-5 show the properties of SMMA compositions comprising a SEBS with a high styrene content (SEBS-1) and a SEBS with a low styrene content (SEBS-2). It is particularly surprising that these compositions combine improved mechanical properties with good optical properties (Examples 9-24). Likewise, molding compositions (P) with a ΔRI of less than or equal to 0.02 exhibit excellent optical properties (Examples 9-24), which are further improved in molding compositions with a ΔRI of less than or equal to 0.008, especially 0.006 (Examples 9-19, 21, 23), while molding compositions with higher ΔRI perform poorly in terms of transmittance, clarity and haze (Examples 20, 22, 24). Table 4 Composition and properties of SMMA / SEBS-1 / SEBS-2 blends of Examples 14-18 Table 5 Composition and properties of SMMA / SEBS-1 / SEBS-2 blends of Examples 19-24

[0130] Furthermore, surprisingly, the composition according to the invention exhibits excellent light stability in the UV stability test according to AATCC TM16.3 (see Table 6). The composition of Example 15 exceeds the results of the commercial impact-modified compositions of Ref.1 and Ref.2 and the pure SMMA composition of Comparative Example C1. Table 6 Comparison of UV stability of Examples 1 and 15 with Ref. 1 and Ref. 2

[0131] As shown in Table 6, the evaluation of the light stability of the compositions according to Comparative Example C1 and Example 15 as well as Reference Examples Ref. 1 and Ref. 2 clearly shows that the light stability of the pure SMMA composition of Comparative Example C1 is substantially improved compared to Ref. 1 and Ref. 2. This improvement is even further increased for the composition according to the invention as demonstrated by the light stability of the composition of Example 15, which is impact-modified and therefore exhibits superior mechanical properties compared to Comparative Example C1 (see Tables 1-5).

Claims

1. A molding composition (P) comprising (or consisting of) components (a), (b) and (c): (a) 30 to 95 wt.-% of at least one random copolymer component (a), c made from 30 to 70 wt.-% of at least one vinyl aromatic monomer (a11), in particular styrene, and 30 to 70 wt.-% of methyl methacrylate (a12); (b) 5 to 70 wt.% of at least one block copolymer (b) comprising: at least one hard block H comprising repeating units of a vinyl aromatic monomer, especially styrene, and At least one elastomeric soft block S 1 , comprising repeating units of an olefin monomer, preferably ethylene and at least one olefin monomer having 3 to 10 carbon atoms, and / or At least one soft block S 2 , comprising repeating units of olefin monomers and vinyl aromatic monomers, especially ethylene, at least one olefin monomer having 3 to 10 carbon atoms and styrene; in, The proportion of the repeating units of the vinyl aromatic hydrocarbon monomer is 25 to 85 wt.% based on the entire block copolymer (b); and (c) 0-2 wt.% of one or more additives and / or processing aids (c); Therein, the total amount of components (a), (b) and (c) is 100 wt.-%.

2. The molding composition (P) according to claim 1, It is characterized in that The elastomeric soft block S 1 The at least one soft block S comprises repeating units of ethylene and at least one olefin monomer selected from propylene and butene, more preferably ethylene and butene; wherein the at least one soft block S 2 The repeating unit comprises ethylene, at least one olefin monomer selected from propylene and butene, and styrene, and more preferably ethylene, butene and styrene.

3. The molding composition (P) according to claim 1 or 2, comprising: 30-85 wt-%, preferably 30-82 wt-% of at least one random copolymer component (a); 15-70 wt-%, preferably 18-70 wt-% of at least one block copolymer component (b); and 0-2 wt-%, preferably 0.1-2 wt-% of at least one component (c); in, The total amount of components (a), (b) and (c) is 100 wt.-%.

4. The molding composition (P) according to claim 1 or 2, comprising (or consisting of) the following components as block copolymer component (b): (b-1) at least one block copolymer (b-1) comprising: at least one hard block H comprising repeating units of a vinyl aromatic monomer, especially styrene, and At least one elastomeric soft block S 1 , comprising repeating units of olefin monomers, especially ethylene and butene, in, The proportion of the repeating units of the vinyl aromatic hydrocarbon monomer is 55-85 wt-%, preferably 55-80 wt-%, usually 60-75 wt-%, based on the entire block copolymer (b-1); and (b-2) Optionally, at least one block copolymer (b-2) comprising: at least one hard block H comprising repeating units of a vinyl aromatic monomer, especially styrene, and At least one elastomeric soft block S 1 , comprising repeating units of olefin monomers, especially ethylene and butene, Therein, the proportion of the vinyl aromatic monomer is 25-54 wt-%, preferably 30-54 wt-%, usually 35-50 wt-%, based on the entire block copolymer (b-2).

5. The molding composition (P) according to claim 4, It is characterized in that Component (b) comprises (or consists of): (b-1) 45 to 95 wt.-%, based on the total weight of component (b), of at least one block copolymer (b-1); and (b-2) 5 to 55 wt.-%, based on the total weight of component (b), of at least one block copolymer (b-2).

6. The molding composition (P) according to claim 4, comprising: 68-79 wt.-%, preferably 69-76.9 wt.-%, typically 69.6-75.5 wt.-% of at least one random copolymer component (a); 18 to 29 wt.-%, preferably 19 to 26.9 wt.-%, typically 19.6 to 25.5 wt.-% of at least one block copolymer (b-1); 3 to 14 wt.-%, preferably 4 to 11.9 wt.-%, typically 4.6 to 6.5 wt.-% of at least one block copolymer (b-2); and 0-2 wt.-%, preferably 0.1-2 wt.-%, typically 0.3-2 wt.-% of at least one component (c). in, The total amount of components (a), (b-1), (b-2) and (c) is 100 wt.-%.

7. The molding composition (P) according to any one of claims 1 to 6, It is characterized in that The refractive index values ​​of components (a) and (b) at 589.3 nm are in the range of 1.52-1.57, as measured similarly to ASTM C 1648-12.

8. The molding composition (P) according to any one of claims 1 to 7, It is characterized in that The random copolymer (a) comprises 48-60 wt.-%, preferably 50-58 wt.-% of vinyl aromatic monomer (a11), especially styrene, and 40-52 wt.-%, preferably 42-50 wt.-% of methyl methacrylate (a12).

9. The molding composition (P) according to any one of claims 1 to 8, It is characterized in that Component (b) is obtained by hydrogenation of the non-conjugated double bonds of a vinyl aromatic-diene block copolymer (b'), the vinyl aromatic-diene block copolymer (b') comprising at least one hard block H' made of a vinyl aromatic monomer and at least one soft block S made of a diene. 1 ', and / or at least one soft block S made of diene and vinyl aromatic monomers 2 '.

10. The molding composition (P) according to any one of claims 1 to 9, It is characterized in that Component (b) is a polymer having two terminal hard blocks H and at least one soft block S. 1 and / or at least one soft block S 2 Linear block copolymers.

11. The molding composition (P) according to any one of claims 1 to 10, It is characterized in that The refractive index difference (at 589.3 nm) of components (a) and (b) is ΔRI ≤ 0.02, preferably ≤ 0.

01.

12. The molding composition (P) according to any one of claims 1 to 11, It is characterized in that The molding composition (P) is characterized in that it has: (i) The yellowness index increment after UV stability test (600 hours) is less than 2.0 units; (ii) color change (ΔE) after UV stability testing (600 hours) is less than 2.0 units; (iii) a haze of less than 20% as measured in accordance with ASTM D1003 on an injection molded plaque 3.2 mm (0.125 inches) thick; and (iv) tensile energy at break greater than 17 Nm; Among them, the UV stability test is carried out according to AATCC TM16.3, and The yellowness index is calculated according to ASTM E313 from the measured CIELAB color space values, and the CIELAB color space values ​​are measured according to ASTM E1348 using a D65 light source (observation angle of 10°). Wherein, the color change (ΔE) is calculated according to ASTM D2244 from the measured CIELAB color space values, and the CIELAB color space values ​​are measured according to ASTM E1348 using a D65 light source (observation angle of 10°), The tensile energy at break was measured according to ASTM D638-14.

13. A process for preparing a molding composition (P) according to any one of claims 1 to 12, It is characterized in that Components (a) and (b) and, if present, component (c) are melt mixed preferably by extrusion.

14. A shaped article produced from a molding composition (P) according to any one of claims 1 to 12.

15. Use of the molding composition (P) according to any one of claims 1 to 12 or the shaped article according to claim 14 in household products and household appliances.