Resin composition

By combining liquid epoxy resin and carbon-containing inorganic filler in the resin composition, the problems of uneven insulation layer thickness and decreased insulation reliability in circuit boards and semiconductor chip packaging are solved, and the flowability and insulation performance are improved.

CN119013347APending Publication Date: 2024-11-22AJINOMOTO CO INC
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202380034279.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-04-18
Filing Date
2023-03-08
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

In circuit boards and semiconductor chip packaging, with the development of larger size, higher wiring density and higher communication speed, existing resin compositions, when reducing viscosity to improve flowability, lead to problems such as uneven insulation layer thickness and reduced insulation reliability.

Method used

A resin composition containing a specific ratio of liquid epoxy resin and carbon-containing inorganic filler is used. The composition of the resin composition is adjusted to improve flowability and insulation reliability. The specific method includes using a specific range of liquid epoxy resin and inorganic filler, combined with an appropriate amount of curing agent and thermoplastic resin to form a dense cross-linked structure.

Benefits of technology

This improved the uniformity of insulation layer thickness and insulation reliability, ensured the flowability and heat resistance of the resin composition, suppressed the reduction in insulation reliability caused by chlorine, and improved the overall insulation performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119013347A_ABST
    Figure CN119013347A_ABST
Patent Text Reader

Abstract

A resin composition containing (A) an epoxy resin and (B) an inorganic filler, in which (A) the epoxy resin contains (A-1) a liquid epoxy resin, (B) the inorganic filler contains (B-1) a carbon-containing inorganic filler having a carbon content of 0.2% by mass or more, and the content of the inorganic filler is less than or equal to 100% by mass per 100% by mass of non-volatile components of the resin composition. The amount of the liquid epoxy resin (A-1) is 0.5 mass% or more with respect to 100 mass% of non-volatile components of the resin composition, and the amount of the carbon-containing inorganic filler (B-1) is 10 mass% or more with respect to 100 mass% of the non-volatile components of the resin composition.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a resin composition and also to a cured product, a sheet-like laminate, a resin sheet, a circuit board, a semiconductor chip package, and a semiconductor device using the resin composition. Background Art

[0002] In circuit substrates and semiconductor chip packages, an insulating layer is usually provided. For example, an interlayer insulating layer is sometimes provided as an insulating layer on a printed wiring board which is a type of circuit substrate. In addition, for example, in semiconductor chip packages, a rewiring forming layer is sometimes provided as an insulating layer. These insulating layers can be formed from a cured product obtained by curing a resin composition (Patent Documents 1 to 2). In addition, the technology of Patent Document 3 is known.

[0003] Prior art literature Patent Document 1: Japanese Patent No. 3644761 Patent Document 2: International Publication No. 2019 / 216388 Patent Document 3: Japanese Patent Application Publication No. 2020-37643 Summary of the invention

[0004] Technical problem to be solved by the invention In recent years, the enlargement of circuit substrates and semiconductor chip packages, the high density of wiring, and the high speed of communication are in progress. From the viewpoint of appropriately embedding the fine wiring resin composition formed with high density, high fluidity is required for the resin composition. In order to achieve high fluidity, it is considered to reduce the viscosity of the resin composition. However, when the viscosity of the resin composition is reduced, when the wiring resin composition is embedded, the resin composition will flow, and sometimes the stability of the thickness of the insulating layer obtained by curing the resin composition becomes low. For example, when the wiring formed on the surface on the substrate is embedded in the resin composition, the thickness of the resin composition differs between the part on the wiring and the gap between the wiring, and sometimes the thickness of the insulating layer becomes uneven. Especially in large-scale circuit substrates and semiconductor chip packages, because the area of ​​the insulating layer becomes large, it is more difficult to make the thickness stable and uniform on the whole of the insulating layer.

[0005] In addition, due to the progress of the above-mentioned enlargement of circuit boards and semiconductor chip packages, high-density wiring, and high-speed communication, the insulation reliability of the insulation layer has been required to be higher in recent years. However, when a low-viscosity epoxy resin is used to reduce the viscosity of the resin composition, the low-viscosity epoxy resin generally contains a large amount of chlorine, so the insulation reliability tends to be reduced.

[0006] The present invention is invented in view of the above-mentioned problems, and therefore, the purpose of the present invention is to provide: a resin composition that can obtain a cured product with excellent insulation reliability and excellent fluidity; a cured product of the above-mentioned resin composition; a sheet-like laminated material and a resin sheet containing the above-mentioned resin composition; a circuit substrate, a semiconductor chip package and a semiconductor device containing the above-mentioned cured product.

[0007] Means for solving technical problems The present inventors have conducted in-depth research to solve the above-mentioned problems. As a result, the present inventors have found that a resin composition comprising (A) an epoxy resin and (B) an inorganic filler, wherein the (A) epoxy resin comprises a specific range of amounts of (A-1) a liquid epoxy resin, and the (B) epoxy resin comprises a specific range of amounts of (B-1) a carbonaceous inorganic filler, can solve the above-mentioned problems, thereby completing the present invention.

[0008] That is, the present invention includes the following contents. [1] A resin composition comprising (A) an epoxy resin and (B) an inorganic filler, wherein: (A) the epoxy resin comprises (A-1) a liquid epoxy resin, (B) the inorganic filler includes (B-1) a carbon-containing inorganic filler having a carbon content of 0.1 mass % or more, The amount of (A-1) the liquid epoxy resin is 0.5% by mass or more relative to 100% by mass of the nonvolatile components of the resin composition, and the amount of (B-1) the carbonaceous inorganic filler is 10% by mass or more relative to 100% by mass of the nonvolatile components of the resin composition. [2] The resin composition according to [1], further comprising (C) a curing agent. [3] The resin composition according to [1] or [2], wherein the amount of the carbon-containing inorganic filler (B-1) is 20% by mass or more relative to 100% by mass of the total amount of the inorganic filler (B). [4] The resin composition according to any one of [1] to [3], wherein the (B-1) carbon-containing inorganic filler is silica particles having a carbon content of 0.2 mass % or more. [5] The resin composition according to any one of [1] to [4], wherein the carbon content of the carbon-containing inorganic filler (B-1) is 5% by mass or less. [6] The resin composition according to any one of [1] to [5], wherein the (A-1) liquid epoxy resin has a weight average molecular weight of 1,000 or less. [7] The resin composition according to any one of [1] to [6], wherein the (A-1) liquid epoxy resin is a non-aromatic epoxy resin. [8] The resin composition according to any one of [1] to [7], wherein the (A-1) liquid epoxy resin has a viscosity of 15,000 mPa·s or less at 25°C. [9] The resin composition according to any one of [1] to [8], further comprising (D) a curing accelerator.

[10] The resin composition according to any one of [1] to [9], comprising (E) a thermoplastic resin.

[11] The resin composition according to any one of [1] to

[10] , which has a minimum melt viscosity of less than 4,000 poise.

[12] The resin composition according to any one of [1] to

[11] , wherein the resin composition is thermally cured at 190° C. for 90 minutes to obtain a cured product, and when a voltage of 3.3 V is applied to the cured product at 130° C. and 85% RH for 100 hours, the insulation resistance of the cured product measured using a comb-shaped electrode with a line width / line spacing of 15 μm / 15 μm is 1.0×10 8 Ω or more.

[13] The resin composition according to any one of [1] to

[12] , which is used for forming an insulating layer.

[14] A cured product of the resin composition according to any one of [1] to

[13] .

[15] A sheet-like laminated material comprising the resin composition according to any one of [1] to

[13] .

[16] A resin sheet comprising a support and a resin composition layer formed on the support, The resin composition layer includes the resin composition according to any one of [1] to

[13] .

[17] A circuit board comprising a cured product of the resin composition according to any one of [1] to

[13] .

[18] A semiconductor chip package comprising a cured product of the resin composition according to any one of [1] to

[13] .

[19] A semiconductor device comprising the circuit substrate described in

[17] .

[20] A semiconductor device comprising the semiconductor chip package described in

[18] . Effects of the Invention

[0009] According to the present invention, there can be provided: a resin composition capable of obtaining a cured product having excellent insulation reliability and excellent fluidity; a cured product of the resin composition; a sheet-like laminate material and a resin sheet comprising the resin composition; and a circuit substrate, a semiconductor chip package and a semiconductor device comprising the cured product. BRIEF DESCRIPTION OF THE DRAWINGS

[0010] Figure 1 It is a cross-sectional view schematically showing a fan-out type WLP as an example of a semiconductor chip package according to an embodiment of the present invention. DETAILED DESCRIPTION

[0011] The present invention will be described below with reference to the embodiments and examples. However, the present invention is not limited to the embodiments and examples described below, and can be implemented with arbitrary modifications within the scope of the claims and their equivalents.

[0012] In the following description, the term "(meth)acrylic acid" includes acrylic acid, methacrylic acid and a combination thereof. In addition, the term "(meth)acrylate" includes acrylate, methacrylate and a combination thereof.

[0013] In the following description, unless otherwise specified, the term "dielectric constant" means a relative dielectric constant.

[0014] [Overview of resin composition] The resin composition involved in one embodiment of the present invention comprises (A) epoxy resin and (B) inorganic filler. (A) epoxy resin comprises (A-1) liquid epoxy resin in a specific range of amount. In addition, (B) inorganic filler comprises (B-1) carbon-containing inorganic filler in a specific range of amount. Here, (B-1) carbon-containing inorganic filler refers to an inorganic filler containing carbon in a specific range of amount.

[0015] The resin composition according to one embodiment of the present invention may have excellent fluidity. In addition, the resin composition according to one embodiment of the present invention may obtain a cured product with excellent insulation reliability. Therefore, the resin composition according to one embodiment of the present invention may improve both fluidity and insulation reliability. Furthermore, the resin composition according to one embodiment of the present invention may generally have a low minimum melt viscosity. In addition, the resin composition according to one embodiment of the present invention may generally obtain a cured product with excellent heat resistance.

[0016] The present inventors have speculated the mechanism by which the resin composition according to one embodiment of the present invention can obtain the above-mentioned excellent effects as follows. However, the scope of the present invention is not limited to the mechanism described below.

[0017] The resin composition according to one embodiment of the present invention includes a specific range of amounts of (A-1) liquid epoxy resin, and thus can have a low viscosity. Thus, excellent fluidity can be achieved. However, the generally low-viscosity (A-1) liquid epoxy resin tends to contain a large amount of chlorine due to its preparation method. Such a composition containing a large amount of chlorine generally has poor insulation reliability.

[0018] In contrast, in the resin composition according to one embodiment of the present invention, a specific range of amounts of (A-1) liquid epoxy resin is combined and further includes a specific range of amounts of (B-1) carbonaceous inorganic filler. In such a resin composition, the carbon contained in the (B-1) carbonaceous inorganic filler can capture chlorine, and thus the reduction in insulation reliability caused by chlorine can be suppressed. Therefore, both fluidity and insulation reliability can be improved.

[0019] As another method for suppressing the reduction of insulation reliability caused by chlorine, it can be a method for introducing ion catcher into resin combination. However, ion catcher usually has poor affinity with the resin component in the resin combination, so the uniformity of the composition of the resin combination comprising the ion catcher on a micro level is poor. In addition, ion catcher usually has a tendency of poor heat resistance. Therefore, the resin combination comprising ion catcher in the past, as a whole composition, has a high viscosity, or locally produces a part with poor fluidity and heat resistance, and the result is that, as a whole resin combination, fluidity and heat resistance are poor. In contrast, in the resin composition according to one embodiment of the present invention, the carbon that captures chlorine does not reduce the affinity and heat resistance of the inorganic filler and the resin component. Therefore, while the insulation reliability can be improved by capturing chlorine, the fluidity improvement effect brought by the (A-1) liquid epoxy resin can be fully utilized while maintaining heat resistance, thereby achieving improvements in both fluidity and insulation reliability.

[0020] Furthermore, the (A-1) liquid epoxy resin generally has a small molecular weight and thus tends to have a small epoxy equivalent. Thus, when a resin composition containing a specific range of the (A-1) liquid epoxy resin is cured, a large number of crosslinking points formed by the reaction of epoxy groups can be formed. Therefore, since a network of crosslinked structures can be densely formed, high heat resistance can be obtained. Therefore, for example, a cured product with a high glass transition temperature can be obtained.

[0021] In addition, as described above, unlike the resin composition comprising an ion trapping agent, the resin composition involved in one embodiment of the present invention can have a higher uniformity of composition. Therefore, the cured product can also have a higher uniformity of composition, so the generation of the uneven points of the composition that become the starting point of destruction due to stress can be suppressed. Therefore, a conductor layer is formed on the insulating layer of the cured product comprising the resin composition, and when the insulating layer is heated and stress is generated in the insulating layer, the destruction of the insulating layer caused by the stress can be suppressed. Therefore, the peeling of the conductor layer accompanied by the destruction of the insulating layer can be suppressed, so excellent reflow resistance can be obtained.

[0022] [(A) Epoxy resin] The resin composition involved in one embodiment of the present invention contains (A) epoxy resin as (A) component. (A) Epoxy resin can be a curable resin having an epoxy group. Examples of (A) epoxy resin include trimethylolpropane type epoxy resin, neopentyl glycol type epoxy resin, biphenyl type epoxy resin, bisphenol A type epoxy resin, bisphenol F type epoxy resin, bisphenol S type epoxy resin, bisphenol AF type epoxy resin, dicyclopentadiene type epoxy resin, trisphenol type epoxy resin, naphthol novolac type epoxy resin, phenol novolac type epoxy resin, tert-butyl-catechol type epoxy resin, naphthalene type epoxy resin, naphthol type epoxy resin, anthracene type epoxy resin, glycidylamine type epoxy resin, glycidylester type epoxy resin. The epoxy resins include epoxy resins of cresol novolac type, phenol aralkyl type, biphenyl type, linear aliphatic, butadiene structure, alicyclic, heterocyclic, spiro ring-containing, cyclohexane type, cyclohexanedimethanol type, naphthyl ether type, trimethylol type, tetraphenylethane type, isocyanurate type, phenolphthalimidine type, etc. The epoxy resins (A) may be used alone or in combination of two or more.

[0023] The (A) epoxy resin contains the (A-1) liquid epoxy resin in an amount within a specific range. The (A-1) liquid epoxy resin is an epoxy resin that is liquid at a temperature of 20° C. The (A-1) liquid epoxy resin preferably has two or more epoxy groups in one molecule.

[0024] Examples of the (A-1) liquid epoxy resin include bisphenol A type liquid epoxy resin, bisphenol F type liquid epoxy resin, bisphenol AF type liquid epoxy resin, naphthalene type liquid epoxy resin, glycidyl ester type liquid epoxy resin, glycidyl amine type liquid epoxy resin, phenol novolac type liquid epoxy resin, trimethylolpropane type liquid epoxy resin, neopentyl glycol type liquid epoxy resin, alicyclic liquid epoxy resin having an ester skeleton, cyclohexane type liquid epoxy resin, cyclohexanedimethanol type liquid epoxy resin, and liquid epoxy resin having a butadiene structure. The (A-1) liquid epoxy resin may be used alone or in combination of two or more.

[0025] (A-1) Liquid epoxy resin preferably contains non-aromatic epoxy resin, preferably only contains non-aromatic epoxy resin. Non-aromatic epoxy resin refers to an epoxy resin that does not contain an aromatic ring in its molecule. In addition, "aromatic ring" means a ring that follows the Huckel rule and has 4p+2 electrons (p is an integer greater than 0) contained in the π electron system on the ring, including a monocyclic aromatic ring and a condensed polycyclic aromatic ring formed by condensing more than two monocyclic aromatic rings. In addition, the aromatic ring includes an aromatic carbocyclic ring and an aromatic heterocyclic ring. Therefore, the non-aromatic epoxy resin is preferably an aliphatic epoxy resin. The non-aromatic epoxy resin may contain an alicyclic structure. When using the (A-1) liquid epoxy resin containing a non-aromatic epoxy resin, the fluidity and insulation reliability can be effectively improved, and the minimum melt viscosity and heat resistance can usually be made particularly good. (A-1) Among the liquid epoxy resins, examples of non-aromatic epoxy resins include trimethylolpropane type liquid epoxy resins, neopentyl glycol type liquid epoxy resins, hexanediol type liquid epoxy resins, polypropylene glycol type liquid epoxy resins, alicyclic liquid epoxy resins having an ester skeleton, cyclohexane type liquid epoxy resins, cyclohexanedimethanol type liquid epoxy resins, and liquid epoxy resins having a butadiene structure.

[0026] Specific examples of the (A-1) liquid epoxy resin include "HP4032", "HP4032D", and "HP4032SS" (naphthalene-based liquid epoxy resins) manufactured by DIC Corporation; "828US", "828EL", "jER828EL", "825", and "EPIKOTE "828EL" (bisphenol A type liquid epoxy resin); "jER807", "1750" (bisphenol F type liquid epoxy resin) manufactured by Mitsubishi Chemical Corporation; "jER152" (phenol novolac type liquid epoxy resin) manufactured by Mitsubishi Chemical Corporation; "630", "630LSD", "604" (glycidylamine type liquid epoxy resin) manufactured by Mitsubishi Chemical Corporation; "ED-523T" (GLYCIROL type liquid epoxy resin) manufactured by ADEKA; "EP-3950L", "EP-3980S" (glycidylamine type liquid epoxy resin) manufactured by ADEKA; "EP-4088S" (dicyclopentadiene type liquid epoxy resin) manufactured by ADEKA; "ZX1059" (a mixture of bisphenol A type liquid epoxy resin and bisphenol F type liquid epoxy resin) manufactured by Nippon Steel Chemical Materials Co., Ltd.; " EX-721" (glycidyl ester type liquid epoxy resin); "CELLOXIDE2021P" manufactured by Daicel Corporation (alicyclic liquid epoxy resin with ester skeleton); "PB-3600" manufactured by Daicel Corporation, "JP-100" and "JP-200" manufactured by Nippon Soda Co., Ltd. (liquid epoxy resin with butadiene structure); "ZX1658" and "ZX1658GS" manufactured by Nippon Steel Chemical Materials (liquid 1,4-glycidylcyclohexane type liquid epoxy resin); "ED-503" and "ED-503G" (hexanediol type liquid epoxy resin) manufactured by ADEKA Corporation; "ED-505" (trimethylolpropane type liquid epoxy resin) manufactured by ADEKA Corporation; "ED-506" (polypropylene glycol type liquid epoxy resin) manufactured by ADEKA Corporation; "ED-523T" (neopentyl glycol type liquid epoxy resin) manufactured by ADEKA Corporation, etc.

[0027] (A-1) liquid epoxy resin preferably has a small weight average molecular weight within a specific range. The weight average molecular weight of (A-1) liquid epoxy resin is specifically preferably less than 1000, more preferably less than 500, and further preferably less than 300. When using (A-1) liquid epoxy resin having a weight average molecular weight in this range, fluidity and insulation reliability can be effectively improved, and the minimum melt viscosity and heat resistance can generally be made particularly good. The lower limit is not particularly limited, for example, it can be more than 50, more than 80, more than 100, etc. The weight average molecular weight of the resin can be measured as a polystyrene-converted value by gel permeation chromatography (GPC).

[0028] (A-1) The liquid epoxy resin preferably has a small viscosity within a specific range. The above-mentioned viscosity range of the liquid epoxy resin (A-1) is preferably 15,000 mPa·s or less, more preferably 3,000 mPa·s or less, further preferably 1,000 mPa·s or less, and particularly preferably 500 mPa·s or less. When using the (A-1) liquid epoxy resin having a viscosity within this range, the fluidity and insulation reliability can be effectively improved, and the minimum melt viscosity and heat resistance can generally be made particularly good. There is no particular restriction on the lower limit value, for example, it can be 5 mPa·s or more, 10 mPa·s or more, etc. The viscosity of the liquid epoxy resin can be measured using an E-type viscometer under the conditions of 25°C and 20 rpm. The specific viscosity measurement method can adopt the method described in <Measurement of Viscosity of Epoxy Resin> in the examples described later.

[0029] As described above, the (A-1) liquid epoxy resin having a relatively low viscosity may generally contain chlorine. The amount of chlorine contained in the (A-1) liquid epoxy resin may be 0.03% by mass or more, 0.1% by mass or more, 0.3% by mass or more, etc., relative to 100% by mass of the (A-1) liquid epoxy resin. Even in the case of using such a (A-1) liquid epoxy resin containing chlorine, a resin composition containing a specific range of amounts of (B-1) a carbon-containing inorganic filler can also achieve high insulation. The upper limit of the amount of chlorine contained in the (A-1) liquid epoxy resin is preferably 5% by mass or less, more preferably 3% by mass or less, and further preferably 1% by mass or less.

[0030] From the above viewpoints, as specific examples of particularly preferred (A-1) liquid epoxy resins, there can be mentioned hexanediol liquid epoxy resins represented by the following formula (a-1), trimethylolpropane liquid epoxy resins represented by the following formula (a-2), polypropylene glycol liquid epoxy resins represented by the following formula (a-3), and neopentyl glycol liquid epoxy resins represented by the following formula (a-4). In formula (a-3), n represents a number greater than 0. As examples of commercially available products of hexanediol liquid epoxy resins, there can be mentioned "ED-503" (viscosity 25 mPa·s, chlorine content 6.5% by mass) and "ED-503G" (viscosity 15 mPa·s, chlorine content 0.3% by mass) manufactured by ADEKA. As examples of commercially available products of trimethylolpropane liquid epoxy resins, there can be mentioned "ED-505" (viscosity 150 mPa·s, chlorine content 8.0% by mass) manufactured by ADEKA. Examples of commercially available polypropylene glycol liquid epoxy resins include "ED-506" manufactured by ADEKA Corporation (viscosity 60 mPa·s, chlorine content 6.0 mass %). Examples of commercially available neopentyl glycol liquid epoxy resins include "ED-523T" manufactured by ADEKA Corporation (viscosity 15 mPa·s, chlorine content 5.0 mass %).

[0031] [Chemical formula 1]

[0032] The epoxy equivalent of the (A-1) liquid epoxy resin is preferably in the range of 50 g / eq. to 5,000 g / eq., more preferably 60 g / eq. to 3,000 g / eq., further preferably 80 g / eq. to 2,000 g / eq., and particularly preferably 110 g / eq. to 1,000 g / eq. The epoxy equivalent represents the mass of the resin per 1 equivalent of epoxy group. The epoxy equivalent can be measured according to JIS K 7236.

[0033] The resin composition involved in one embodiment of the present invention contains (A-1) liquid epoxy resin in an amount within a specific range. The range of the amount of (A-1) liquid epoxy resin is generally 0.5% by mass or more, preferably 1% by mass or more, more preferably 2% by mass or more, preferably 20% by mass or less, more preferably 10% by mass or less, and further preferably 5% by mass or less, relative to 100% by mass of the non-volatile component in the resin composition. When the amount of (A-1) liquid epoxy resin is within the above range, both fluidity and insulation reliability can be improved, and the minimum melt viscosity and heat resistance can generally be improved.

[0034] The range of the amount of (A-1) liquid epoxy resin is preferably 1% by mass or more, preferably 1.5% by mass or more, more preferably 2% by mass or more, particularly preferably 5% by mass or more, preferably 40% by mass or less, more preferably 30% by mass or less, and further preferably 20% by mass or less, relative to 100% by mass of the resin component in the resin composition. The resin component of the resin composition represents the components other than (B) inorganic filler in the non-volatile components of the resin composition. When the amount of (A-1) liquid epoxy resin is within the above range, the fluidity and insulation reliability can be effectively improved, and the minimum melt viscosity and heat resistance can generally be made particularly good.

[0035] The (A-1) liquid epoxy resin preferably contains a large amount of a liquid epoxy resin having a viscosity in the above-mentioned specific range (e.g., 1,000 mPa·s or less) at 25°C. The amount of the liquid epoxy resin having a viscosity in the above-mentioned specific range at 25°C is preferably 30% by mass or more, more preferably 40% by mass or more, further preferably 50% by mass or more, and usually 100% by mass or less, relative to the total amount of 100% by mass of the (A-1) liquid epoxy resin. Among them, it is preferred that all of the (A-1) liquid epoxy resin is a liquid epoxy resin having a viscosity of 1,000 mPa·s or less at 25°C. When the amount of the liquid epoxy resin having a viscosity in the above-mentioned specific range at 25°C is within the above-mentioned range, the fluidity and insulation reliability can be effectively improved, and the minimum melt viscosity and heat resistance can generally be made particularly good.

[0036] The (A) epoxy resin may include a (A-2) solid epoxy resin in combination with the (A-1) liquid epoxy resin. The (A-2) solid epoxy resin refers to an epoxy resin that is solid at a temperature of 20° C. As the (A-2) solid epoxy resin, a solid epoxy resin having two or more epoxy groups in one molecule is preferred, and a solid epoxy resin having three or more epoxy groups in one molecule is more preferred.

[0037] As (A-2) solid epoxy resin, for example, there can be mentioned biphenylol type solid epoxy resin, naphthalene type solid epoxy resin, naphthalene type tetrafunctional solid epoxy resin, naphthol novolac type solid epoxy resin, cresol novolac type solid epoxy resin, dicyclopentadiene type solid epoxy resin, trisphenol type solid epoxy resin, naphthol type solid epoxy resin, biphenyl type solid epoxy resin, naphthyl ether type solid epoxy resin, anthracene type solid epoxy resin, bisphenol A type solid epoxy resin, bisphenol AF type solid epoxy resin, phenol aralkyl type solid epoxy resin, tetraphenylethane type solid epoxy resin, phenol benzopyrrolidone type solid epoxy resin. (A-2) solid epoxy resin can be used alone or in combination of two or more.

[0038] From the viewpoint of obtaining a cured product with excellent heat resistance, (A-2) solid epoxy resin preferably includes solid epoxy resin containing aromatic rings, and may also include only solid epoxy resin containing aromatic rings. As solid epoxy resin containing aromatic rings, for example, biphenylol type solid epoxy resin, naphthalene type solid epoxy resin, naphthalene type tetrafunctional solid epoxy resin, naphthol novolac type solid epoxy resin, cresol novolac type solid epoxy resin, trisphenol type solid epoxy resin, naphthol type solid epoxy resin, biphenyl type solid epoxy resin, naphthyl ether type solid epoxy resin, anthracene type solid epoxy resin, bisphenol A type solid epoxy resin, bisphenol AF type solid epoxy resin, phenol aralkyl type solid epoxy resin, tetraphenylethane type solid epoxy resin, phenol benzopyrrolidone type solid epoxy resin can be cited.

[0039] Specific examples of (A-2) solid epoxy resins include "HP4032H" (naphthalene-type solid epoxy resin) manufactured by DIC Corporation; "HP-4700" and "HP-4710" (naphthalene-type tetrafunctional solid epoxy resin) manufactured by DIC Corporation; "N-690" (cresol novolac-type solid epoxy resin) manufactured by DIC Corporation; "N-695" (cresol novolac-type solid epoxy resin) manufactured by DIC Corporation; "HP-7200", "HP-7200HH", "HP-7200H", and "HP-7200L" (dicyclopentadiene-type solid epoxy resin) manufactured by DIC Corporation; and "HP-7200HH" and "HP-7200H" (dicyclopentadiene-type solid epoxy resin) manufactured by DIC Corporation. "EXA-7311", "EXA-7311-G3", "EXA-7311-G4", "EXA-7311-G4S", "HP6000" (naphthyl ether type solid epoxy resin) made by Nippon Kayaku Co., Ltd.; "EPPN-502H" (trisphenol type solid epoxy resin) made by Nippon Kayaku Co., Ltd.; "NC7000L" (naphthol novolac type solid epoxy resin) made by Nippon Kayaku Co., Ltd.; "NC3000H", "NC3000", "NC3000L", "NC3000FH", "NC3100" (biphenyl type solid epoxy resin) made by Nippon Kayaku Co., Ltd.; Nippon Steel Chemical Materials Co., Ltd. "ESN475V" (naphthol-type solid epoxy resin), "ESN4100V" (naphthalene-type solid epoxy resin) made by Nippon Steel Chemicals Co., Ltd.; "ESN485" (naphthol-type solid epoxy resin) made by Nippon Steel Chemicals Co., Ltd.; "ESN375" (dihydroxynaphthalene-type solid epoxy resin) made by Nippon Steel Chemicals Co., Ltd.; "YX4000H", "YX4000", "YX4000HK", "YL7890" (biphenyl-type solid epoxy resin) made by Mitsubishi Chemical Corporation; "YL6121" (biphenyl-type solid epoxy resin) made by Mitsubishi Chemical Corporation; "YX8800" (anthracene-type solid epoxy resin) made by Mitsubishi Chemical Corporation Resin); "YX7700" manufactured by Mitsubishi Chemical Corporation (phenol aralkyl type solid epoxy resin); "PG-100" and "CG-500" manufactured by Osaka Gas Chemical Co., Ltd.; "YL7760" manufactured by Mitsubishi Chemical Corporation (bisphenol AF type solid epoxy resin); "YL7800" manufactured by Mitsubishi Chemical Corporation (fluorene type solid epoxy resin); "jER1010" manufactured by Mitsubishi Chemical Corporation (bisphenol A type solid epoxy resin); "jER1031S" manufactured by Mitsubishi Chemical Corporation (tetraphenylethane type solid epoxy resin); "WHR991S" manufactured by Nippon Kayaku Co., Ltd. (phenol benzopyrrolidone type solid epoxy resin), etc.

[0040] The weight average molecular weight (Mw) of the (A-2) solid epoxy resin is preferably 100 to 5,000, more preferably 250 to 3,000, and even more preferably 400 to 1,500.

[0041] The epoxy equivalent of the solid epoxy resin (A-2) may be in the same range as the epoxy equivalent of the liquid epoxy resin (A-1).

[0042] As (A) epoxy resin, when (A-1) liquid epoxy resin and (A-2) solid epoxy resin are used in combination, their mass ratio ((A-1) liquid epoxy resin: (A-2) solid epoxy resin) is preferably 50:1 to 1:50, more preferably 30:1 to 1:30, and particularly preferably 10:1 to 1:10.

[0043] The (A) epoxy resin including the (A-1) liquid epoxy resin and the (A-2) solid epoxy resin preferably includes an epoxy resin having two or more epoxy groups in one molecule. The amount of the (A) epoxy resin having two or more epoxy groups in one molecule is preferably 50% by mass or more, more preferably 60% by mass or more, particularly preferably 70% by mass or more, and usually 100% by mass or less, relative to the total amount of the (A) epoxy resin (100% by mass).

[0044] The amount of the epoxy resin (A) in the resin composition is preferably 5% by mass or more, more preferably 10% by mass or more, and further preferably 15% by mass or more, relative to 100% by mass of the nonvolatile components in the resin composition, and is preferably 50% by mass or less, more preferably 40% by mass or less, and further preferably 30% by mass or less. When the amount of the epoxy resin (A) is within the above range, the fluidity and insulation reliability can be effectively improved, and the minimum melt viscosity and heat resistance can generally be made particularly good.

[0045] The amount of the epoxy resin (A) in the resin composition is preferably 10% by mass or more, more preferably 30% by mass or more, and even more preferably 50% by mass or more, relative to 100% by mass of the resin component in the resin composition, and is preferably 90% by mass or less, more preferably 80% by mass or less, and even more preferably 70% by mass or less. When the amount of the epoxy resin (A) is within the above range, the fluidity and insulation reliability can be effectively improved, and the minimum melt viscosity and heat resistance can generally be made particularly good.

[0046] [(B) Inorganic filler] The resin composition according to one embodiment of the present invention contains (B) an inorganic filler as the component (B). The (B) inorganic filler is usually contained in the resin composition in the form of particles.

[0047] (B) inorganic filler can be particles of inorganic compounds. As materials contained in (B) inorganic filler, for example, silica, aluminum oxide, glass, cordierite, silicon oxide, barium sulfate, barium carbonate, talc, clay, mica powder, zinc oxide, hydrotalcite, boehmite, aluminum hydroxide, magnesium hydroxide, calcium carbonate, magnesium carbonate, magnesium oxide, boron nitride, aluminum nitride, manganese nitride, aluminum borate, strontium carbonate, strontium titanate, calcium titanate, magnesium titanate, bismuth titanate, titanium oxide, zirconium oxide, barium titanate, barium zirconate, calcium zirconate, zirconium phosphate and zirconium tungstate phosphate, etc., can be cited. Among them, preferably silica, aluminum oxide, particularly preferably silica. As silica, for example, amorphous silica, fused silica, crystalline silica, synthetic silica, hollow silica, etc. can be cited. In addition, as silica, preferably spherical silica. (B) The inorganic filler may be used alone or in combination of two or more.

[0048] (B) The inorganic filler contains a specific range of amounts of (B-1) carbon-containing inorganic filler. (B-1) Carbon-containing inorganic filler means an inorganic filler containing a specific range of amounts of carbon. Therefore, (B-1) can be particles of an inorganic compound containing a specific range of amounts of carbon. The range of the carbon content of the (B-1) carbon-containing inorganic filler is usually 0.1% by mass or more, preferably 0.2% by mass or more, more preferably 0.3% by mass or more, particularly preferably 0.4% by mass or more, preferably 5% by mass or less, more preferably 3% by mass or less, and further preferably 1% by mass or less. The carbon content of the (B-1) carbon-containing inorganic filler does not include the amount of carbon atoms that the surface treatment agent may contain. Therefore, for example, the "carbon content" of the (B-1) carbon-containing inorganic filler that has been surface-treated by a surface treatment agent containing carbon atoms does not include the amount of carbon atoms of the above-mentioned surface treatment agent.

[0049] The carbon content of the inorganic filler can be measured by fluorescent X-ray analysis and solid NMR. For fluorescent X-ray analysis, for example, refer to "Center News" vol. 40 No. 1, 2021 (issued on July 5, 2021) of the Central Analysis Center of Kyushu University. However, as described above, the carbon content of the carbon-containing inorganic filler (B-1) does not include the amount of carbon atoms that the surface treatment agent may contain. Therefore, the carbon content of the carbon-containing inorganic filler (B-1) is preferably measured before surface treatment. For the surface-treated inorganic filler, for example, chemical treatment such as strong acid and strong alkali is performed to dissolve the surface treatment agent together with the outermost layer of the inorganic filler particles and then measure the amount of carbon atoms, thereby measuring the amount of carbon atoms.

[0050] (B-1) carbon-containing inorganic filler is usually a particle containing the above-mentioned inorganic compound as a main component. Therefore, the above-mentioned inorganic compound can be included in combination with carbon in (B-1) carbon-containing inorganic filler. In the above-mentioned inorganic compound, from the viewpoint of significantly exerting the effect of the present invention, silicon dioxide is preferably used. Therefore, as (B-1) carbon-containing inorganic filler, it is preferably silicon dioxide particles containing carbon in a specific range of amounts. The amount of silicon dioxide contained in the silicon dioxide particles is preferably 60% by mass or more, more preferably 70% by mass or more, further preferably 80% by mass or more, and particularly preferably 90% by mass or more. The amount of silicon dioxide can be measured by fluorescent X-ray analysis.

[0051] The manufacturing method of the above-mentioned (B-1) carbonaceous inorganic filler is not particularly limited. From the viewpoint of energy saving, cost saving and environmental protection, (B-1) carbonaceous inorganic filler is preferably manufactured from plant raw materials. For example, plants of Equisetaceae and Gramineae may have the property of absorbing and accumulating silicon components from the land. Therefore, by burning these plants, silicon dioxide can be manufactured as combustion ash (Japanese Patent Gazette No. 6389349). Hereinafter, silicon dioxide manufactured from plant raw materials in this way is sometimes referred to as "biomass silicon dioxide". Biomass silicon dioxide usually contains carbon, so it can be used as (B-1) carbonaceous inorganic filler. In addition, (B-1) carbonaceous inorganic filler can also use commercial products. Regarding the example of commercial products of (B-1) carbonaceous inorganic filler, as biomass silicon dioxide manufactured from rice husks, "Ethical Silica" manufactured by MIT can be cited.

[0052] (B-1) The carbon-containing inorganic filler may be used alone or in combination of two or more.

[0053] From the viewpoint of significantly obtaining the desired effect of the present invention, the average particle size of the carbon-containing inorganic filler (B-1) is preferably 0.01 μm or more, more preferably 0.1 μm or more, further preferably 0.5 μm or more, preferably 10 μm or less, more preferably 8 μm or less, further preferably 5 μm or less.

[0054] (B-1) The average particle size of inorganic fillers such as carbon-containing inorganic fillers can be measured by a laser diffraction / scattering method based on Mie scattering theory. Specifically, the particle size distribution of the inorganic filler can be made on a volume basis by a laser diffraction scattering particle size distribution measuring device, and the median particle size can be measured as the average particle size. The sample can be measured using a sample obtained by weighing 100 mg of inorganic filler and 10 g of methyl ethyl ketone into a vial and dispersing it by ultrasonic waves for 10 minutes. For the sample, a laser diffraction particle size distribution measuring device is used, and the light source wavelength is blue and red. The particle size distribution of the volume basis of the inorganic filler is measured in a flow cell manner, and the average particle size is calculated as the median particle size according to the obtained particle size distribution. As a laser diffraction particle size distribution measuring device, for example, "LA-960" made by Horiba, Ltd. can be cited.

[0055] From the viewpoint of significantly obtaining the desired effect of the present invention, the specific surface area of ​​the carbonaceous inorganic filler (B-1) is preferably 0.1 m 2 / g or more, more preferably 0.5m 2 / g or more, more preferably 1m 2 / g or more, particularly preferably 3m 2 / g or more, preferably 100m 2 / g or less, more preferably 70m 2 / g or less, more preferably 50m 2 / g or less, particularly preferably 40m 2 The specific surface area of ​​the inorganic filler can be measured by the BET method using a specific surface area measuring device (Macsorb HM-1210 manufactured by Mountec) by allowing nitrogen to adsorb on the surface of the sample and calculating the specific surface area using the BET multipoint method.

[0056] From the viewpoint of improving moisture resistance and dispersibility, the carbonaceous inorganic filler (B-1) is preferably treated with a surface treatment agent. As the surface treatment agent, for example, fluorine-containing silane coupling agents, aminosilane coupling agents, epoxysilane coupling agents, mercaptosilane coupling agents, silane coupling agents, alkoxysilanes, organosilazane compounds, titanate coupling agents, etc. can be cited. The surface treatment agent can be used alone or in any combination of two or more.

[0057] Commercially available products of the surface treatment agent include, for example, “KBM403” (3-glycidoxypropyltrimethoxysilane) manufactured by Shin-Etsu Chemical Co., Ltd., “KBM803” (3-mercaptopropyltrimethoxysilane) manufactured by Shin-Etsu Chemical Co., Ltd., “KBE903” (3-aminopropyltriethoxysilane) manufactured by Shin-Etsu Chemical Co., Ltd., “KBM573” (N-phenyl-3-aminopropyltrimethoxysilane) manufactured by Shin-Etsu Chemical Co., Ltd., “SZ-31” (hexamethyldisilazane) manufactured by Shin-Etsu Chemical Co., Ltd., “KBM103” (phenyltrimethoxysilane) manufactured by Shin-Etsu Chemical Co., Ltd., “KBM-4803” (long-chain epoxy-type silane coupling agent) manufactured by Shin-Etsu Chemical Co., Ltd., and “KBM-7103” (3,3,3-trifluoropropyltrimethoxysilane) manufactured by Shin-Etsu Chemical Co., Ltd.

[0058] From the viewpoint of improving the dispersibility of the carbonaceous inorganic filler (B-1), the degree of surface treatment by the surface treatment agent is preferably within a specific range. Specifically, 100% by mass of the carbonaceous inorganic filler (B-1) is preferably surface treated with a surface treatment agent of 0.2% to 5% by mass, more preferably with a surface treatment agent of 0.2% to 3% by mass, and further preferably with a surface treatment agent of 0.3% to 2% by mass.

[0059] The resin composition involved in one embodiment of the present invention contains (B-1) carbon-containing inorganic filler in an amount within a specific range. The range of the amount of (B-1) carbon-containing inorganic filler is generally 10% by mass or more, preferably 15% by mass or more, more preferably 20% by mass or more, preferably 90% by mass or less, more preferably 85% by mass or less, and further preferably 80% by mass or less, relative to 100% by mass of the non-volatile component in the resin composition. When the amount of (B-1) carbon-containing inorganic filler is within the above range, both fluidity and insulation reliability can be improved, and the minimum melt viscosity and heat resistance can generally be made good.

[0060] The amount of the carbon-containing inorganic filler (B-1) is preferably 20% by mass or more, more preferably 25% by mass, and further preferably 30% by mass or more, and usually 100% by mass or less, relative to the total amount of the inorganic filler (B) (100% by mass). When the amount of the carbon-containing inorganic filler (B-1) is within the above range, the fluidity and insulation reliability can be effectively improved, and the minimum melt viscosity and heat resistance can usually be particularly good.

[0061] The mass ratio of (B-1) carbon-containing inorganic filler to (A) epoxy resin ((B-1) carbon-containing inorganic filler / (A) epoxy resin) is preferably in the range of 0.5 or more, more preferably 1 or more, further preferably 1.2 or more, particularly preferably 1.5 or more, and preferably 10 or less, more preferably 8 or less, further preferably 6 or less. When the mass ratio ((B-1) carbon-containing inorganic filler / (A) epoxy resin) is within the above range, the fluidity and insulation reliability can be effectively improved, and the minimum melt viscosity and heat resistance can generally be made particularly good.

[0062] The mass ratio of (B-1) carbon-containing inorganic filler to (A-1) liquid epoxy resin ((B-1) carbon-containing inorganic filler / (A-1) liquid epoxy resin) is preferably in the range of 1 or more, more preferably 5 or more, further preferably 10 or more, and preferably 200 or less, more preferably 150 or less, further preferably 100 or less. When the mass ratio ((B-1) carbon-containing inorganic filler / (A-1) liquid epoxy resin) is within the above range, the fluidity and insulation reliability can be effectively improved, and the minimum melt viscosity and heat resistance can generally be made particularly good.

[0063] The mass ratio of the (B-1) carbon-containing inorganic filler to the "liquid epoxy resin having a viscosity of 1,000 mPa·s or less at 25°C" ((B-1) carbon-containing inorganic filler / "liquid epoxy resin having a viscosity of 1,000 mPa·s or less at 25°C") is preferably in the range of 1 or more, more preferably 5 or more, further preferably 10 or more, particularly preferably 20 or more, preferably 200 or less, more preferably 150 or less, further preferably 100 or less, and particularly preferably 70 or less. When the mass ratio ((B-1) carbon-containing inorganic filler / "liquid epoxy resin having a viscosity of 1,000 mPa·s or less at 25°C") is within the above range, the fluidity and insulation reliability can be effectively improved, and the minimum melt viscosity and heat resistance can generally be made particularly good.

[0064] In the resin composition involved in one embodiment of the present invention, (B-2) any inorganic filler can be combined with (B-1) carbon-containing inorganic filler. (B-2) Any inorganic filler means an inorganic filler other than (B-1) carbon-containing inorganic filler, and thus can mean an inorganic filler whose carbon content is not within the above range.

[0065] (B-2) Any inorganic filler may be particles of the above-mentioned inorganic compound. Among the inorganic compounds, silica and alumina are preferred, and silica is particularly preferred. As silica, for example, amorphous silica, fused silica, crystalline silica, synthetic silica, hollow silica, etc. may be cited. In addition, spherical silica is preferred as silica. (B-2) Any inorganic filler may be used alone or in combination of two or more.

[0066] As commercially available products of the optional inorganic filler (B-2), for example, there can be mentioned "SP60-05" and "SP507-05" manufactured by Nippon Steel Chemical Materials Co., Ltd.; "YC100C", "YA050C", "YA050C-MJE", "YA010C", "SC2500SQ", "SO-C4", "SO-C2", and "SO-C1" manufactured by Yaduma Co., Ltd.; "UFP-30", "DAW-03", and "FB-105FD" manufactured by Denka Co., Ltd.; "Silfil NSS-3N", "Silfil NSS-4N", and "Silfil NSS-5N" manufactured by Tokuyama Co., Ltd.; "MG-005" manufactured by Pacific Cement Co., Ltd., etc.

[0067] From the viewpoint of significantly obtaining the desired effect of the present invention, the average particle size of any inorganic filler (B-2) is preferably 0.01 μm or more, more preferably 0.05 μm or more, further preferably 0.1 μm or more, particularly preferably 0.2 μm or more, preferably 10 μm or less, more preferably 5 μm or less, further preferably 3 μm or less.

[0068] From the viewpoint of significantly obtaining the desired effect of the present invention, the specific surface area of ​​the optional inorganic filler (B-2) is preferably 0.1 m 2 / g or more, more preferably 0.5m 2 / g or more, more preferably 1m 2 / g or more, particularly preferably 3m 2 / g or more, preferably 100m 2 / g or less, more preferably 70m 2 / g or less, more preferably 50m 2 / g or less, particularly preferably 40m 2 / g or less.

[0069] From the viewpoint of improving moisture resistance and dispersibility, (B-2) any inorganic filler is preferably treated with a surface treatment agent. As examples of surface treatment agents for any inorganic filler (B-2), the same surface treatment agents as those for the surface treatment agents for the carbonaceous inorganic filler (B-1) can be cited. One surface treatment agent can be used alone, or two or more can be used in any combination. In addition, the range of the degree of surface treatment of any inorganic filler (B-2) using a surface treatment agent can be the same as the range of the degree of surface treatment of the carbonaceous inorganic filler (B-1) using a surface treatment agent.

[0070] The amount of the inorganic filler (B) in the resin composition is preferably 10% by mass or more, more preferably 20% by mass or more, further preferably 40% by mass or more, particularly preferably 50% by mass or more, preferably 90% by mass or less, more preferably 85% by mass or less, and particularly preferably 80% by mass or less, relative to 100% by mass of the non-volatile component of the resin composition. When the amount of the inorganic filler (B) is within the above range, the fluidity and insulation reliability can be effectively improved, and the minimum melt viscosity and heat resistance can generally be made particularly good.

[0071] [(C) Curing agent] In the resin composition involved in one embodiment of the present invention, (C) curing agent can be combined with (A) to (B) components and further include as an arbitrary component. Unless otherwise specified, the (C) curing agent as the (C) component does not include substances belonging to the above-mentioned (A) to (B) components. The (C) curing agent can have the function of reacting with the (A) epoxy resin to cure the resin composition. The (C) curing agent can be used alone or in combination of two or more.

[0072] Preferred examples of the (C) curing agent include active ester curing agents, cyanate curing agents, phenol curing agents, carbodiimide curing agents, acid anhydride curing agents, amine curing agents, benzoxazine curing agents, and thiol curing agents.

[0073] As active ester curing agent, generally preferably use phenolic esters, thiophenolic esters, N-hydroxylamine esters, esters of heterocyclic hydroxy compounds, etc., in 1 molecule, there are more than 2 compounds with high reactive ester groups. The active ester curing agent is preferably obtained by the condensation reaction of carboxylic acid compounds and / or thiocarboxylic acid compounds with hydroxy compounds and / or thiol compounds. Particularly from the viewpoint of improving heat resistance, preferably the active ester curing agent obtained by carboxylic acid compounds and hydroxy compounds, more preferably the active ester curing agent obtained by carboxylic acid compounds and phenolic compounds and / or naphthol compounds. As carboxylic acid compounds, for example benzoic acid, acetic acid, succinic acid, maleic acid, itaconic acid, phthalic acid, isophthalic acid, terephthalic acid, pyromellitic acid, etc. can be mentioned. Examples of the phenol compound or naphthol compound include hydroquinone, resorcinol, bisphenol A, bisphenol F, bisphenol S, phenolphthalein, methylated bisphenol A, methylated bisphenol F, methylated bisphenol S, phenol, o-cresol, m-cresol, p-cresol, catechol, α-naphthol, β-naphthol, 1,5-dihydroxynaphthalene, 1,6-dihydroxynaphthalene, 2,6-dihydroxynaphthalene, dihydroxybenzophenone, trihydroxybenzophenone, tetrahydroxybenzophenone, phloroglucinol, pyrogallol, dicyclopentadiene-type diphenol compounds, and novolac resins. Here, the "dicyclopentadiene-type diphenol compound" refers to a diphenol compound obtained by condensing two molecules of phenol with one molecule of dicyclopentadiene.

[0074] Specifically, as the active ester curing agent, preferably a dicyclopentadiene type active ester curing agent, a naphthalene type active ester curing agent containing a naphthalene structure, an active ester curing agent containing an acetylated product of a linear phenolic resin, and an active ester curing agent containing a benzoylated product of a linear phenolic resin, wherein at least one selected from the dicyclopentadiene type active ester curing agent and the naphthalene type active ester curing agent is more preferred. As the dicyclopentadiene type active ester curing agent, preferably an active ester curing agent containing a dicyclopentadiene type diphenol structure.

[0075] As for commercially available products of active ester curing agents, for example, as active ester curing agents containing a dicyclopentadiene-type diphenol structure, there are "EXB9451", "EXB9460", "EXB9460S", "EXB-8000L", "EXB-8000L-65M", "EXB-8000L-65TM", "HPC-8000L-65TM", "HPC-8000", "HPC-8000-65T", "HPC-8000H", "HPC-8000H-65TM" (manufactured by DIC Corporation); as active ester curing agents containing a naphthalene structure, there are "HP-B-8151-62T", "EXB-8100L-65T", "EXB-8150-60T", "EXB-81 Examples of the active ester curing agent include "EXB-50-62T", "EXB-9416-70BK", "HPC-8150-60T", "HPC-8150-62T", "EXB9416-70BK", and "EXB-8" (manufactured by DIC Corporation); as an active ester curing agent containing phosphorus, "EXB9401" (manufactured by DIC Corporation) can be cited; as an active ester curing agent that is an acetylated product of a linear phenolic resin, "DC808" (manufactured by Mitsubishi Chemical Corporation) can be cited; as an active ester curing agent that is a benzoylated product of a linear phenolic resin, "YLH1026", "YLH1030", and "YLH1048" (manufactured by Mitsubishi Chemical Corporation) can be cited; as an active ester curing agent containing a styryl group and a naphthalene structure, "PC1300-02-65MA" (manufactured by Air Water Corporation) and the like can be cited.

[0076] As the cyanate curing agent, a compound having one or more, preferably two or more, cyanate groups in one molecule can be used. Examples of the cyanate curing agent include difunctional cyanate curing agents such as bisphenol A dicyanate, polyphenol cyanate (oligo(3-methylene-1,5-phenylene cyanate)), 4,4'-methylenebis(2,6-dimethylphenylcyanate), 4,4'-ethylidene diphenyl dicyanate, hexafluorobisphenol A dicyanate, 2,2-bis(4-cyano)phenylpropane, 1,1-bis(4-cyanophenylmethane), bis(4-cyano-3,5-dimethylphenyl)methane, 1,3-bis(4-cyanophenyl-1-(methylethylidene))benzene, bis(4-cyanophenyl)sulfide and bis(4-cyanophenyl)ether; polyfunctional cyanate curing agents derived from phenol novolac resins and cresol novolac resins; and prepolymers obtained by triazinization of a portion of these cyanate curing agents. Specific examples of cyanate curing agents include "PT30" and "PT60" manufactured by Lonza Japan (both are linear phenolic resin type multifunctional cyanate curing agents), "BA230", "BA230S75" (prepolymers obtained by triazine-forming a trimer of part or all of bisphenol A dicyanate), etc.

[0077] As phenolic curing agents, compounds having one or more, preferably two or more, hydroxyl groups bonded to aromatic rings such as benzene rings and naphthalene rings in one molecule can be cited. From the viewpoint of heat resistance and water resistance, phenolic curing agents having a phenolic structure are preferred. In addition, from the viewpoint of close adhesion, nitrogen-containing phenolic curing agents are preferred, and phenolic curing agents containing a triazine skeleton are more preferred. Among them, from the viewpoint of highly satisfying heat resistance, water resistance and close adhesion, linear phenolic resin curing agents containing a triazine skeleton are preferred. Specific examples of phenolic curing agents include "MEH-7700", "MEH-7810", and "MEH-7851" manufactured by Meiwa Chemicals, "NHN", "CBN", and "GPH" manufactured by Nippon Kayaku Co., Ltd., "SN-170", "SN-180", "SN-190", "SN-475", "SN-485", "SN-495", "SN-375", and "SN-395" manufactured by Nippon Steel Chemicals Co., Ltd., and "LA-7052", "LA-7054", "LA-3018", "LA-3018-50P", "LA-1356", "TD2090", and "TD-2090-60M" manufactured by DIC Corporation.

[0078] As the carbodiimide curing agent, a compound having one or more, preferably two or more, carbodiimide groups in one molecule can be used. Specific examples of the carbodiimide curing agent include: aliphatic biscarbodiimides such as tetramethylene-bis(tert-butylcarbodiimide) and cyclohexanebis(methylene-tert-butylcarbodiimide); biscarbodiimides such as aromatic biscarbodiimides such as phenylene-bis(xylylcarbodiimide); aliphatic polycarbodiimides such as polyhexamethylenecarbodiimide, polytrimethylhexamethylenecarbodiimide, polycyclohexylenecarbodiimide, poly(methylenebiscyclohexylenecarbodiimide), poly(isophoronecarbodiimide); poly(phenylenecarbodiimide), poly Aromatic polycarbodiimides such as poly(naphthylene carbodiimide), poly(tolylene carbodiimide), poly(methyl diisopropyl phenylene carbodiimide), poly(triethyl phenylene carbodiimide), poly(diethyl phenylene carbodiimide), poly(triisopropyl phenylene carbodiimide), poly(diisopropyl phenylene carbodiimide), poly(xylylene carbodiimide), poly(tetramethyl xylylene carbodiimide), poly(methylene diphenylene carbodiimide), poly[methylene bis(methyl phenylene) carbodiimide], etc. Examples of commercially available carbodiimide resins include "CARBODILITE V-02B", "CARBODILITE V-03", "CARBODILITE V-04K", "CARBODILITE V-07" and "CARBODILITE V-09" manufactured by Nisshinbo Chemical Co., Ltd.; and "Stabaxol P", "Stabaxol P400" and "Hycasyl 510" manufactured by Rhein Chemie.

[0079] As an acid anhydride curing agent, a compound having one or more, preferably two or more, acid anhydride groups in one molecule can be used. Specific examples of the acid anhydride curing agent include phthalic anhydride, tetrahydrophthalic anhydride, hexahydrophthalic anhydride, methyltetrahydrophthalic anhydride, methylhexahydrophthalic anhydride, methylnadic anhydride, hydrogenated methylnadic anhydride, trialkyltetrahydrophthalic anhydride, dodecenylsuccinic anhydride, 5-(2,5-dioxotetrahydro-3-furanyl)-3-methyl-3-cyclohexene-1,2-dicarboxylic anhydride, trimellitic anhydride, pyromellitic anhydride, dicarboxylic anhydride, and the like. Polymer-type acid anhydrides such as benzophenone tetracarboxylic dianhydride, biphenyl tetracarboxylic dianhydride, naphthalene tetracarboxylic dianhydride, oxydiphthalic dianhydride, 3,3'-4,4'-diphenylsulfone tetracarboxylic dianhydride, 1,3,3a,4,5,9b-hexahydro-5-(tetrahydro-2,5-dioxo-3-furanyl)-naphtho[1,2-c]furan-1,3-dione, ethylene glycol bis(trimellitic anhydride), and styrene-maleic acid resin obtained by copolymerizing styrene with maleic acid. Commercially available products of anhydride curing agents include, for example, "HNA-100", "MH-700", "MTA-15", "DDSA", and "OSA" manufactured by Shin Nippon Chemical Co., Ltd.; "YH-306" and "YH-307" manufactured by Mitsubishi Chemical Corporation; "HN-2200" and "HN-5500" manufactured by Hitachi Chemical Co., Ltd.; and "EF-30", "EF-40", "EF-60", and "EF-80" manufactured by Cray Valley Co., Ltd.

[0080] As an amine curing agent, a compound having one or more, preferably two or more, amino groups in one molecule can be used. Examples of the amine curing agent include aliphatic amines, polyether amines, alicyclic amines, aromatic amines, and the like, among which aromatic amines are preferred. The amine curing agent is preferably a primary amine or a secondary amine, and a primary amine is more preferred. Specific examples of the amine curing agent include: 4,4'-methylenebis(2,6-dimethylaniline), 4,4'-diaminodiphenylmethane, 4,4'-diaminodiphenyl sulfone, 3,3'-diaminodiphenyl sulfone, metaphenylenediamine, metaphenylenediamine, diethyltoluenediamine, 4,4'-diaminodiphenyl ether, 3,3'-dimethyl-4,4'-diaminobiphenyl, 2,2'-dimethyl-4,4'-diaminobiphenyl, 3,3'-dihydroxybenzidine, 2,2-bis(3-amino-4-hydroxy phenyl)propane, 3,3-dimethyl-5,5-diethyl-4,4-diphenylmethanediamine, 2,2-bis(4-aminophenyl)propane, 2,2-bis(4-(4-aminophenoxy)phenyl)propane, 1,3-bis(3-aminophenoxy)benzene, 1,3-bis(4-aminophenoxy)benzene, 1,4-bis(4-aminophenoxy)benzene, 4,4'-bis(4-aminophenoxy)biphenyl, bis(4-(4-aminophenoxy)phenyl)sulfone, bis(4-(3-aminophenoxy)phenyl)sulfone, etc. Commercially available products of amine curing agents include, for example, "SEIKACURE-S" manufactured by Seika Corporation; "KAYABOND C-200S", "KAYABOND C-100", "KAYAHARD AA", "KAYAHARD AB", and "KAYAHARD AS" manufactured by Nippon Kayaku Co., Ltd.; "Epicure W" manufactured by Mitsubishi Chemical Corporation; and "DTDA" manufactured by Sumitomo Seika Chemicals Co., Ltd.

[0081] Specific examples of the benzoxazine-based curing agent include “JBZ-OP100D” and “ODA-BOZ” manufactured by JFE Chemical Co., Ltd.; “HFB2006M” manufactured by Showa High Molecular Co., Ltd.; and “Pd” and “Fa” manufactured by Shikoku Chemical Industry Co., Ltd.

[0082] Examples of the thiol-based curing agent include trimethylolpropane tris(3-mercaptopropionate), pentaerythritol tetrakis(3-mercaptobutyrate), and tris(3-mercaptopropyl)isocyanurate.

[0083] The active group equivalent of the curing agent (C) is preferably 50 g / eq. to 3000 g / eq., more preferably 100 g / eq. to 1000 g / eq., further preferably 100 g / eq. to 500 g / eq., particularly preferably 100 g / eq. to 350 g / eq. The active group equivalent indicates the mass of the resin per 1 equivalent of active groups.

[0084] When the number of epoxy groups of the epoxy resin (A) is set to 1, the number of active groups of the curing agent (C) is preferably 0.01 or more, more preferably 0.1 or more, further preferably 0.2 or more, preferably 10 or less, more preferably 5 or less, further preferably 1 or less. "The number of epoxy groups of the epoxy resin (A)" refers to the value obtained by adding up all the values ​​obtained by dividing the mass of the non-volatile components of the epoxy resin (A) present in the resin composition by the epoxy equivalent. In addition, "the number of active groups of the curing agent (C)" refers to the value obtained by adding up all the values ​​obtained by dividing the mass of the non-volatile components of the curing agent (C) present in the resin composition by the active group equivalent.

[0085] The amount of the (C) curing agent in the resin composition relative to 100% by mass of the non-volatile component of the resin composition may be 0% by mass or may be greater than 0% by mass, and is preferably 1% by mass or more, more preferably 2% by mass or more, further preferably 5% by mass or more, and is preferably 40% by mass or less, more preferably 30% by mass or less, and further preferably 20% by mass or less.

[0086] The amount of the (C) curing agent in the resin composition relative to 100% by mass of the resin component of the resin composition may be 0% by mass or may be greater than 0% by mass, and is preferably 5% by mass or more, more preferably 10% by mass or more, and further preferably 20% by mass or more, and is preferably 70% by mass or less, more preferably 60% by mass or less, and further preferably 50% by mass or less.

[0087] [(D) Curing accelerator] The resin composition according to one embodiment of the present invention may further include (D) a curing accelerator as an arbitrary component. Unless otherwise specified, the (D) curing accelerator as the (D) component does not include substances belonging to the above-mentioned (A) to (C) components. The (D) curing accelerator has a function as a curing catalyst that accelerates the curing of the (A) epoxy resin.

[0088] Examples of the curing accelerator (D) include phosphorus curing accelerators, urea curing accelerators, guanidine curing accelerators, imidazole curing accelerators, metal curing accelerators, and amine curing accelerators. Among them, imidazole curing accelerators are preferred. The curing accelerator (D) may be used alone or in combination of two or more.

[0089] Phosphorus curing accelerators include, for example, tetrabutylphosphonium bromide, tetrabutylphosphonium chloride, tetrabutylphosphonium acetate, tetrabutylphosphonium decanoate, tetrabutylphosphonium laurate, bis(tetrabutylphosphonium)pyromellitic acid salt, tetrabutylphosphonium hydrogen hexahydrophthalate, tetrabutylphosphonium 2,6-bis[(2-hydroxy-5-methylphenyl)methyl]-4-methylphenolate, di-tert-butyldimethylphosphonium tetraphenylborate and other aliphatic phosphonium salts; methyltriphenylphosphonium bromide, ethyltriphenylphosphonium bromide, propyltriphenylphosphonium bromide, butyltriphenylphosphonium bromide, benzyltriphenylphosphonium chloride, tetraphenylphosphonium bromide, para- Aromatic phosphonium salts such as tolyltriphenylphosphonium tetra-p-tolylborate, tetraphenylphosphonium tetraphenylborate, tetraphenylphosphonium tetra-p-tolylborate, triphenylethylphosphonium tetraphenylborate, tris(3-methylphenyl)ethylphosphonium tetraphenylborate, tris(2-methoxyphenyl)ethylphosphonium tetraphenylborate, (4-methylphenyl)triphenylphosphonium thiocyanate, tetraphenylphosphonium thiocyanate, butyltriphenylphosphonium thiocyanate, etc.; aromatic phosphine-borane complexes such as triphenylphosphine-triphenylborane, etc.; aromatic phosphine-quinone addition reactants such as triphenylphosphine-p-benzoquinone addition reactants, etc.; tributylphosphine, tri-tert-butylphosphine, trioctylphosphine aliphatic phosphines such as di-tert-butyl(2-butenyl)phosphine, di-tert-butyl(3-methyl-2-butenyl)phosphine, and tricyclohexylphosphine; dibutylphenylphosphine, di-tert-butylphenylphosphine, methyldiphenylphosphine, ethyldiphenylphosphine, butyldiphenylphosphine, diphenylcyclohexylphosphine, triphenylphosphine, tri-o-tolylphosphine, tri-m-tolylphosphine, tri-p-tolylphosphine, tri(4-ethylphenyl)phosphine, tri(4-propylphenyl)phosphine, tri(4-isopropylphenyl)phosphine, tri(4-butylphenyl)phosphine, tri(4-tert-butylphenyl)phosphine, tri(2,4-dimethylphenyl)phosphine, tri(2,5-dimethylphenyl)phosphine, tri( Aromatic phosphines such as tris(2,6-dimethylphenyl)phosphine, tris(3,5-dimethylphenyl)phosphine, tris(2,4,6-trimethylphenyl)phosphine, tris(2,6-dimethyl-4-ethoxyphenyl)phosphine, tris(2-methoxyphenyl)phosphine, tris(4-methoxyphenyl)phosphine, tris(4-ethoxyphenyl)phosphine, tris(4-tert-butoxyphenyl)phosphine, diphenyl-2-pyridylphosphine, 1,2-bis(diphenylphosphino)ethane, 1,3-bis(diphenylphosphino)propane, 1,4-bis(diphenylphosphino)butane, 1,2-bis(diphenylphosphino)acetylene, and 2,2'-bis(diphenylphosphino)diphenyl ether.

[0090] Examples of the urea curing accelerator include 1,1-dimethylurea; aliphatic dimethylureas such as 1,1,3-trimethylurea, 3-ethyl-1,1-dimethylurea, 3-cyclohexyl-1,1-dimethylurea, and 3-cyclooctyl-1,1-dimethylurea; 3-phenyl-1,1-dimethylurea, 3-(4-chlorophenyl)-1,1-dimethylurea, 3-(3,4-dichlorophenyl)-1,1-dimethylurea, 3-(3-chloro-4-methylphenyl)-1,1-dimethylurea, 3-(2-methylphenyl)-1,1-dimethylurea, 3-(4-methylphenyl)-1,1-dimethylurea, 3-(3,4-dimethylphenyl)-1, Aromatic dimethylureas such as 1-dimethylurea, 3-(4-isopropylphenyl)-1,1-dimethylurea, 3-(4-methoxyphenyl)-1,1-dimethylurea, 3-(4-nitrophenyl)-1,1-dimethylurea, 3-[4-(4-methoxyphenoxy)phenyl]-1,1-dimethylurea, 3-[4-(4-chlorophenoxy)phenyl]-1,1-dimethylurea, 3-[3-(trifluoromethyl)phenyl]-1,1-dimethylurea, N,N-(1,4-phenylene)bis(N',N'-dimethylurea), and N,N-(4-methyl-1,3-phenylene)bis(N',N'-dimethylurea) [toluenebisdimethylurea], and the like.

[0091] Examples of the guanidine curing accelerator include dicyandiamide, 1-methylguanidine, 1-ethylguanidine, 1-cyclohexylguanidine, 1-phenylguanidine, 1-(o-tolyl)guanidine, dimethylguanidine, diphenylguanidine, trimethylguanidine, tetramethylguanidine, pentamethylguanidine, 1,5,7-triazabicyclo[4.4.0]dec-5-ene, 7-methyl-1,5,7-triazabicyclo[4.4.0]dec-5-ene, 1-methylbiguanidine, 1-ethylbiguanidine, 1-n-butylbiguanidine, 1-n-octadecylbiguanidine, 1,1-dimethylbiguanidine, 1,1-diethylbiguanidine, 1-cyclohexylbiguanidine, 1-allylbiguanidine, 1-phenylbiguanidine, and 1-(o-tolyl)biguanidine.

[0092] Examples of the imidazole curing accelerator include 2-methylimidazole, 2-undecylimidazole, 2-heptadecylimidazole, 1,2-dimethylimidazole, 2-ethyl-4-methylimidazole, 1,2-dimethylimidazole, 2-ethyl-4-methylimidazole, 2-phenylimidazole, 2-phenyl-4-methylimidazole, 1-benzyl-2-methylimidazole, 1-benzyl-2-phenylimidazole, 1-cyanoethyl-2-methylimidazole, 1-cyanoethyl-2-undecylimidazole, 1-cyanoethyl-2-ethyl-4-methylimidazole, 1-cyanoethyl-2-phenylimidazole, 1-cyanoethyl-2-undecylimidazole, 1-cyanoethyl-2-ethyl-4-methylimidazole, 1-cyanoethyl-2-phenylimidazole, 1-cyanoethyl-2-undecylimidazole trimellitate, 1-cyanoethyl-2-phenylimidazole trimellitate, 2,4-diamino-6-[2'-methylimidazolyl-(1') imidazole compounds and adducts of imidazole compounds and epoxy resins such as 2,4-diamino-6-[2'-undecylimidazolyl-(1')]-ethyl-s-triazine, 2,4-diamino-6-[2'-ethyl-4'-methylimidazolyl-(1')]-ethyl-s-triazine, 2,4-diamino-6-[2'-methylimidazolyl-(1')]-ethyl-s-triazine, 2-phenylimidazole isocyanuric acid adduct, 2-phenyl-4,5-dihydroxymethylimidazole, 2-phenyl-4-methyl-5-hydroxymethylimidazole, 2,3-dihydro-1H-pyrrolo[1,2-a]benzimidazole, 1-dodecyl-2-methyl-3-benzylimidazolium chloride, 2-methylimidazoline, and 2-phenylimidazoline. Commercially available products of imidazole-based curing accelerators include, for example, "1B2PZ", "2E4MZ", "2MZA-PW", "2MZ-OK", "2MA-OK", "2MA-OK-PW", "2PHZ", "2PHZ-PW", "Cl1Z", "Cl1Z-CN", "Cl1Z-CNS", and "C11Z-A" manufactured by Shikoku Chemical Industries, Ltd.; and "P200-H50" manufactured by Mitsubishi Chemical Corporation.

[0093] As metal curing accelerators, organic metal complexes or organic metal salts of metals such as cobalt, copper, zinc, iron, nickel, manganese, and tin can be cited. Specific examples of organic metal complexes include organic cobalt complexes such as cobalt acetylacetonate (II), cobalt acetylacetonate (III), organic copper complexes such as copper acetylacetonate (II), organic zinc complexes such as zinc acetylacetonate (II), organic iron complexes such as iron acetylacetonate (III), organic nickel complexes such as nickel acetylacetonate (II), and organic manganese complexes such as manganese acetylacetonate (II). As organic metal salts, for example, zinc octoate, tin octoate, zinc naphthenate, cobalt naphthenate, tin stearate, zinc stearate, etc. can be cited.

[0094] Examples of the amine-based curing accelerator include trialkylamines such as triethylamine and tributylamine, 4-dimethylaminopyridine, benzyldimethylamine, 2,4,6-tris(dimethylaminomethyl)phenol, and 1,8-diazabicyclo(5,4,0)-undecene. A commercially available amine-based curing accelerator may be used, and examples thereof include "MY-25" manufactured by Ajinomoto Fine Technologies Co., Ltd.

[0095] The amount of the (D) curing accelerator in the resin composition relative to 100% by mass of the non-volatile component of the resin composition can be 0% by mass or greater than 0% by mass, and is preferably 0.01% by mass or more, more preferably 0.02% by mass or more, and further preferably 0.03% by mass or more, and is preferably 2% by mass or less, more preferably 1% by mass or less, and further preferably 0.5% by mass or less.

[0096] The amount of the (D) curing accelerator in the resin composition relative to 100% by mass of the resin component of the resin composition may be 0% by mass or may be greater than 0% by mass, and is preferably 0.01% by mass or more, more preferably 0.05% by mass or more, further preferably 0.1% by mass or more, preferably 5% by mass or less, more preferably 2% by mass or less, further preferably 1% by mass or less.

[0097] [(E) Thermoplastic resin] The resin composition according to one embodiment of the present invention may further contain (E) a thermoplastic resin as an optional component. Unless otherwise specified, the thermoplastic resin as the component (E) does not include those belonging to the above-mentioned components (A) to (D).

[0098] (E) Thermoplastic resins include, for example, phenoxy resins, polyimide resins, polyvinyl acetal resins, polyolefin resins, polybutadiene resins, polyamide-imide resins, polyetherimide resins, polysulfone resins, polyethersulfone resins, polyphenylene ether resins, polycarbonate resins, polyetheretherketone resins, polyester resins, etc. (E) Thermoplastic resins may be used alone or in combination of two or more.

[0099] Examples of the phenoxy resin include phenoxy resins having one or more skeletons selected from the group consisting of bisphenol A skeleton, bisphenol F skeleton, bisphenol S skeleton, bisphenol acetophenone skeleton, phenolic skeleton, biphenyl skeleton, fluorene skeleton, dicyclopentadiene skeleton, norbornene skeleton, naphthalene skeleton, anthracene skeleton, adamantane skeleton, terpene skeleton, and trimethylcyclohexane skeleton. The terminal of the phenoxy resin may be any functional group such as a phenolic hydroxyl group or an epoxy group. Specific examples of phenoxy resins include "1256" and "4250" manufactured by Mitsubishi Chemical Corporation (both are phenoxy resins containing a bisphenol A skeleton); "YX8100" manufactured by Mitsubishi Chemical Corporation (a phenoxy resin containing a bisphenol S skeleton); "YX6954" manufactured by Mitsubishi Chemical Corporation (a phenoxy resin containing a bisphenol acetophenone skeleton); "FX280" and "FX293" manufactured by Nippon Steel Chemical Materials Co., Ltd.; "YL7500BH30", "YX6954BH30", "YX7553", "YX7553BH30", "YL7769BH30", "YL6794", "YL7213", "YL7290", "YL7482" and "YL7891BH30" manufactured by Mitsubishi Chemical Corporation.

[0100] Specific examples of the polyimide resin include "SLK-6100" manufactured by Shin-Etsu Chemical Co., Ltd., and "RIKACOAT SN20" and "RIKACOAT PN20" manufactured by Shin Nippon Chemical Co., Ltd.

[0101] Examples of the polyvinyl acetal resin include polyvinyl formal resin and polyvinyl butyral resin, and polyvinyl butyral resin is preferred. Specific examples of the polyvinyl acetal resin include "Denka Butyral 4000-2", "Denka Butyral 5000-A", "Denka Butyral 6000-C", and "Denka Butyral 6000-EP" manufactured by Denki Kagaku Kogyo Co., Ltd.; and S-LEC BH series, BX series (e.g., BX-5Z), KS series (e.g., KS-1), BL series, and BM series manufactured by Sekisui Chemical Co., Ltd.

[0102] Examples of the polyolefin resin include ethylene copolymer resins such as low-density polyethylene, ultra-low-density polyethylene, high-density polyethylene, ethylene-vinyl acetate copolymers, ethylene-ethyl acrylate copolymers, and ethylene-methyl acrylate copolymers; and polyolefin polymers such as polypropylene and ethylene-propylene block copolymers.

[0103] Examples of the polybutadiene resin include a resin containing a hydrogenated polybutadiene skeleton, a polybutadiene resin containing a hydroxyl group, a polybutadiene resin containing a phenolic hydroxyl group, a polybutadiene resin containing a carboxyl group, a polybutadiene resin containing an acid anhydride group, a polybutadiene resin containing an epoxy group, a polybutadiene resin containing an isocyanate group, a polybutadiene resin containing a urethane group, and a polyphenylene ether-polybutadiene resin.

[0104] Specific examples of polyamideimide resins include "VYLOMAX HR11NN" and "VYLOMAX HR16NN" manufactured by Toyobo Co., Ltd. Specific examples of polyamideimide resins include modified polyamideimides such as "KS9100" and "KS9300" (polyamideimide containing a polysiloxane skeleton) manufactured by Hitachi Chemical Co., Ltd.

[0105] Specific examples of the polyethersulfone resin include "PES5003P" manufactured by Sumitomo Chemical Co., Ltd. and the like.

[0106] Specific examples of the polysulfone resin include polysulfone "P1700" and "P3500" manufactured by Solvay Performance Polymers.

[0107] Specific examples of polyphenylene ether resins include "NORYL SA90" manufactured by SABIC, etc. Specific examples of polyetherimide resins include "Ultem" manufactured by GE, etc.

[0108] As polycarbonate resins, for example, carbonate resins containing hydroxyl groups, carbonate resins containing phenolic hydroxyl groups, carbonate resins containing carboxyl groups, carbonate resins containing acid anhydride groups, carbonate resins containing isocyanate groups, carbonate resins containing urethane groups, etc. Specific examples of polycarbonate resins include "FPC0220" manufactured by Mitsubishi Gas Chemical Co., Ltd., "T6002", "T6001" (polycarbonate diol) manufactured by Asahi Kasei Chemicals Co., Ltd., "C-1090", "C-2090", "C-3090" (polycarbonate diol) manufactured by Kuraray Co., Ltd., etc. Specific examples of polyetheretherketone resins include "Sumiploy K" manufactured by Sumitomo Chemical Co., Ltd., etc.

[0109] Examples of the polyester resin include polyethylene terephthalate resin, polyethylene naphthalate resin, polybutylene terephthalate resin, polybutylene naphthalate resin, polytrimethylene terephthalate resin, polytrimethylene naphthalate resin, and polycyclohexane dimethyl terephthalate resin.

[0110] (E) The weight average molecular weight (Mw) of the thermoplastic resin is preferably greater than 5,000, more preferably 8,000 or more, further preferably 10,000 or more, particularly preferably 20,000 or more, and preferably 100,000 or less, more preferably 70,000 or less, further preferably 60,000 or less, particularly preferably 50,000 or less. The weight average molecular weight can be measured as a polystyrene-equivalent value by gel permeation chromatography (GPC).

[0111] The amount of the (E) thermoplastic resin in the resin composition relative to 100% by mass of the non-volatile component of the resin composition may be 0% by mass or may be greater than 0% by mass, and is preferably 0.01% by mass or more, more preferably 0.05% by mass or more, and further preferably 0.1% by mass or more, and is preferably 20% by mass or less, more preferably 10% by mass or less, and further preferably 5% by mass or less.

[0112] The amount of the (E) thermoplastic resin in the resin composition relative to 100% by mass of the resin component of the resin composition may be 0% by mass or may be greater than 0% by mass, and is preferably 0.01% by mass or more, more preferably 0.1% by mass or more, and further preferably 1% by mass or more, and is preferably 20% by mass or less, more preferably 10% by mass or less, and further preferably 5% by mass or less.

[0113] [(F) Radically polymerizable compound] The resin composition according to one embodiment of the present invention may further include (F) a radical polymerizable compound as an arbitrary component. The (F) radical polymerizable compound as the component (F) does not include compounds belonging to the above-mentioned components (A) to (E) unless otherwise specified. The (F) radical polymerizable compound may be used alone or in combination of two or more.

[0114] (F) The radical polymerizable compound may contain an ethylenically unsaturated bond. Therefore, the radical polymerizable compound (F) may have a radical polymerizable group containing an ethylenically unsaturated bond. Examples of the radical polymerizable group include unsaturated hydrocarbon groups such as vinyl, allyl, 1-propenyl, 3-cyclohexenyl, 3-cyclopentenyl, 2-vinylphenyl, 3-vinylphenyl, and 4-vinylphenyl; α,β-unsaturated carbonyl groups such as acryloyl, methacryloyl, and maleimide (2,5-dihydro-2,5-dioxo-1H-pyrrol-1-yl). The radical polymerizable compound (F) preferably has two or more radical polymerizable groups.

[0115] (F) As a radical polymerizable compound, a (meth)acrylic radical polymerizable compound, a styrene radical polymerizable compound, an allyl radical polymerizable compound, a maleimide radical polymerizable compound etc. are mentioned, for example.

[0116] The (meth)acrylic radical polymerizable compound is, for example, a compound having one or more, preferably two or more, acryloyl groups and / or methacryloyl groups. Examples of the (meth)acrylic radical polymerizable compound include aliphatic (meth)acrylate compounds of low molecular weight (molecular weight less than 1000) such as cyclohexane-1,4-dimethanol di(meth)acrylate, cyclohexane-1,3-dimethanol di(meth)acrylate, tricyclodecane dimethanol di(meth)acrylate, neopentyl glycol di(meth)acrylate, 1,4-butanediol di(meth)acrylate, 1,6-hexanediol di(meth)acrylate, 1,8-octanediol di(meth)acrylate, 1,9-nonanediol di(meth)acrylate, 1,10-decanediol di(meth)acrylate, trimethylolpropane tri(meth)acrylate, trimethylolethane tri(meth)acrylate, glycerol tri(meth)acrylate, and pentaerythritol tetra(meth)acrylate; and dioxanediol tri(meth)acrylate. low molecular weight (molecular weight) esters such as bisphenol A di(meth)acrylate, ... isocyanurate-containing (meth)acrylate compounds with a low molecular weight (molecular weight less than 1000) such as tris(3-hydroxypropyl)isocyanurate tri(meth)acrylate, tris(2-hydroxyethyl)isocyanurate tri(meth)acrylate, and ethoxylated isocyanurate tri(meth)acrylate; and high molecular weight (molecular weight 1000 or more) acrylate compounds such as (meth)acrylic acid-modified polyphenylene ether resin. Examples of commercially available (meth)acrylic radical polymerizable compounds include “A-DOG” (dioxanediol diacrylate) manufactured by Shin-Nakamura Chemical Co., Ltd., “DCP-A” (tricyclodecane dimethanol diacrylate) and “DCP” (tricyclodecane dimethanol dimethacrylate) manufactured by Kyoeisha Chemical Co., Ltd., “KAYARAD R-684” (tricyclodecane dimethanol diacrylate) and “KAYARAD R-604” (dioxanediol diacrylate) manufactured by Nippon Kayaku Co., Ltd., and “SA9000” and “SA9000-111” (methacrylic acid-modified polyphenylene ether) manufactured by SABIC Innovative Plastics.

[0117] The styrene-based free radical polymerizable compound may be, for example, a compound having one or more, preferably two or more, vinyl groups directly bonded to an aromatic carbon atom. Examples of the styrene-based free radical polymerizable compound include low molecular weight (molecular weight less than 1000) styrene-based compounds such as divinylbenzene, 2,4-divinyltoluene, 2,6-divinylnaphthalene, 1,4-divinylnaphthalene, 4,4'-divinylbiphenyl, 1,2-bis(4-vinylphenyl)ethane, 2,2-bis(4-vinylphenyl)propane, and bis(4-vinylphenyl)ether; and high molecular weight (molecular weight greater than 1000) styrene-based compounds such as vinylbenzyl-modified polyphenylene ether resins and styrene-divinylbenzene copolymers. Examples of commercially available styrene-based radical polymerizable compounds include “ODV-XET (X03)”, “ODV-XET (X04)”, and “ODV-XET (X05)” (styrene-divinylbenzene copolymers) manufactured by Nippon Steel Chemical Materials Co., Ltd. and “OPE-2St 1200” and “OPE-2St 2200” (vinyl benzyl-modified polyphenylene ether resins) manufactured by Mitsubishi Gas Chemical Co., Ltd.

[0118] Allyl radical polymerizable compounds are, for example, compounds having one or more, preferably two or more, allyl groups. Examples of allyl radical polymerizable compounds include aromatic carboxylic acid allyl ester compounds such as diallyl diphenate, triallyl trimellitate, diallyl phthalate, diallyl isophthalate, diallyl terephthalate, diallyl 2,6-naphthalene dicarboxylate, and diallyl 2,3-naphthalene dicarboxylate; 1,3,5-triallyl isocyanurate, 1,3-diallyl-5-glycidyl isocyanurate, and the like. Isocyanurate allyl ester compounds such as isocyanurate; 2,2-bis[3-allyl-4-(glycidyloxy)phenyl]propane and other aromatic allyl compounds containing epoxy groups; bis[3-allyl-4-(3,4-dihydro-2H-1,3-benzoxazin-3-yl)phenyl]methane and other aromatic allyl compounds containing benzoxazine; 1,3,5-triallyl ether benzene and other aromatic allyl compounds containing ethers; allyl silane compounds such as diallyldiphenylsilane, etc. Commercially available products of allyl-based free radical polymerizable compounds include, for example, "TAIC" (1,3,5-triallyl isocyanurate) manufactured by Nippon Chemical Industry Co., Ltd., Nisshoku TechnoFine "DAD" (diallyl biphenyldicarboxylate) manufactured by Wako Pure Chemical Industries, Ltd., "TRIAM-705" (triallyl trimellitate) manufactured by Wako Pure Chemical Industries, Ltd., "DAND" (diallyl 2,3-naphthoate) manufactured by Nippon Distillation Industries, Ltd., "ALP-d" (bis[3-allyl-4-(3,4-dihydro-2H-1,3-benzoxazin-3-yl)phenyl]methane) manufactured by Shikoku Chemical Industries, Ltd., "RE-810NM" (2,2-bis[3-allyl-4-(glycidyloxy)phenyl]propane) manufactured by Nippon Kayaku Co., Ltd., and "DA-MGIC" (1,3-diallyl-5-glycidyl isocyanurate) manufactured by Shikoku Chemical Industries, Ltd., etc.

[0119] The maleimide radical polymerizable compound is, for example, a compound having one or more, preferably two or more maleimide groups. The maleimide radical polymerizable compound may be an aliphatic maleimide compound having an aliphatic amine skeleton, or an aromatic maleimide compound having an aromatic amine skeleton. Commercially available products of maleimide-based free radical polymerizable compounds include, for example, "SLK-2600" manufactured by Shin-Etsu Chemical Co., Ltd., "BMI-1500", "BMI-1700", "BMI-3000J", "BMI-689", and "BMI-2500" (maleimide compounds containing a dimerized diamine structure) manufactured by Designer Molecules Co., Ltd., "BMI-6100" (aromatic maleimide compound) manufactured by Designer Molecules Co., Ltd., "MIR-5000-60T" and "MIR-3000-70MT" (biphenyl aralkyl type maleimide compounds) manufactured by Nippon Kayaku Co., Ltd., "BMI-70" and "BMI-80" manufactured by KI Chemicals Co., Ltd., and "BMI-2300" and "BMI-TMH" manufactured by Yamato Chemicals Co., Ltd. In addition, as the maleimide-based radical polymerizable compound, a maleimide resin (maleimide compound containing an indane ring skeleton) disclosed in Japan Invention Association Unexamined Technical Publication No. 2020-500211 can be used.

[0120] (F) The ethylenic unsaturated bond equivalent of the radical polymerizable compound is preferably 20 g / eq. to 3,000 g / eq., more preferably 50 g / eq. to 2,500 g / eq., further preferably 70 g / eq. to 2,000 g / eq., and particularly preferably 90 g / eq. to 1,500 g / eq. The ethylenic unsaturated bond equivalent refers to the mass of the radical polymerizable compound per 1 equivalent of ethylenic unsaturated bonds.

[0121] (F) The weight average molecular weight (Mw) of the radical polymerizable compound is preferably 40,000 or less, more preferably 10,000 or less, further preferably 5,000 or less, and particularly preferably 3,000 or less. The lower limit is not particularly limited, and may be, for example, 150 or more. The weight average molecular weight can be measured as a polystyrene-converted value by gel permeation chromatography (GPC).

[0122] The amount of the (F) free radical polymerizable compound in the resin composition relative to 100% by mass of the non-volatile component in the resin composition can be 0% by mass or greater than 0% by mass, and is preferably 0.01% by mass or more, more preferably 0.1% by mass or more, further preferably 0.5% by mass or more, preferably 10% by mass or less, more preferably 5% by mass or less, and further preferably 3% by mass or less.

[0123] The amount of the (F) free radical polymerizable compound in the resin composition relative to 100 mass % of the resin component in the resin composition can be 0 mass % or greater than 0 mass %, and is preferably 0.01 mass % or more, more preferably 0.1 mass % or more, and further preferably 1 mass % or more, and is preferably 20 mass % or less, more preferably 10 mass % or less, and further preferably 5 mass % or less.

[0124] [(G) Optional additives] The resin composition involved in one embodiment of the present invention may further contain (G) any additive as an arbitrary component. Examples of (G) any additive include: organic fillers such as rubber particles; organic metal compounds such as organic copper compounds, organic zinc compounds, and organic cobalt compounds; colorants such as phthalocyanine blue, phthalocyanine green, iodine green, and diazo yellow; polymerization inhibitors such as hydroquinone, catechol, pyrogallol, and phenothiazine; leveling agents such as silicone-based leveling agents and acrylic polymer-based leveling agents; thickeners such as bentonite and montmorillonite; defoamers such as silicone-based defoamers, acrylic defoamers, fluorine-based defoamers, and vinyl resin-based defoamers; ultraviolet absorbers such as benzotriazole-based ultraviolet absorbers; adhesion enhancers such as urea silane; triazole-based adhesion imparting agents, tetrazole-based adhesion imparting agents, and triazine-based adhesion imparting agents. Adhesion imparting agents such as phthalates, ...

[0125] [(H)Solvent] The resin composition involved in one embodiment of the present invention may be combined with non-volatile components such as the above-mentioned (A) to (G) components and further contain (H) solvent as an arbitrary volatile component. As the (H) solvent, an organic solvent is generally used. Examples of the organic solvent include: ketone solvents such as acetone, methyl ethyl ketone, methyl isobutyl ketone, and cyclohexanone; ester solvents such as methyl acetate, ethyl acetate, butyl acetate, isobutyl acetate, isoamyl acetate, methyl propionate, ethyl propionate, and γ-butyrolactone; ether solvents such as tetrahydropyran, tetrahydrofuran, 1,4-dioxane, diethyl ether, diisopropyl ether, dibutyl ether, diphenyl ether, and anisole; alcohol solvents such as methanol, ethanol, propanol, butanol, and ethylene glycol; 2-ethoxyethyl acetate, propylene glycol monomethyl ether acetate, diethylene glycol monoethyl ether acetate, carbitol acetate (ethyl Ether ester solvents such as diglycolacetate, γ-butyrolactone, and methyl methoxypropionate; ester alcohol solvents such as methyl lactate, ethyl lactate, and methyl 2-hydroxyisobutyrate; ether alcohol solvents such as 2-methoxypropanol, 2-methoxyethanol, 2-ethoxyethanol, propylene glycol monomethyl ether, and diethylene glycol monobutyl ether (butyl carbitol); amide solvents such as N,N-dimethylformamide, N,N-dimethylacetamide, and N-methyl-2-pyrrolidone; sulfoxide solvents such as dimethyl sulfoxide; nitrile solvents such as acetonitrile and propionitrile; aliphatic hydrocarbon solvents such as hexane, cyclopentane, cyclohexane, and methylcyclohexane; aromatic hydrocarbon solvents such as benzene, toluene, xylene, ethylbenzene, and trimethylbenzene. (H) Solvents may be used alone or in combination of two or more.

[0126] The amount of the (H) solvent is not particularly limited and may be, for example, 60% by mass or less, 40% by mass or less, 30% by mass or less, 20% by mass or less, 15% by mass or less, 10% by mass or less, etc., relative to 100% by mass of all components of the resin composition, or 0% by mass.

[0127] [Method for producing resin composition] The resin composition involved in one embodiment of the present invention can be manufactured by mixing the above-mentioned components, for example. The above-mentioned components can be mixed in part or in whole at the same time, or can be mixed in sequence. In the process of mixing each component, the temperature can be appropriately set, so heating and / or cooling can be performed temporarily or all the time. In addition, in the process of mixing each component, stirring or vibration can be performed.

[0128] [Characteristics of resin composition] The resin composition involved in one embodiment of the present invention may have high fluidity. The fluidity of the resin composition can be evaluated by undulation. The undulation represents the difference between the maximum and minimum values ​​of the surface height of the layer when forming a layer of the resin composition. Generally, the smaller the undulation, the higher the fluidity of the resin composition.

[0129] In one example, a conductor layer is formed in a comb-shaped pattern on a certain plane. The "pattern" of the conductor layer refers to the shape observed from the thickness direction of the conductor layer. At this time, the conductor layer is formed with a thickness of 35μm and L / S=160μm / 160μm. L / S represents the ratio (line width / line spacing) of the line width L (wiring width) of the conductor layer to the line spacing S (spacing width). On the plane where the conductor layer is formed, a layer is formed by a resin composition. Then, the resin composition layer is thermally cured to form an insulating layer. The height of the surface of the insulating layer (the surface on the opposite side of the conductor layer) is measured, and the difference between the highest height and the lowest height is measured as the undulation. Usually, the surface of the insulating layer is the highest in the part on the conductor layer, and the surface of the insulating layer is the lowest in the part other than the part on the conductor layer. When the undulation is measured as in this example, the undulation of the resin composition involved in one embodiment of the present invention is preferably 3.0μm or less, and more preferably 2.0μm or less. The specific method for measuring the undulation can adopt the method described in <Test Example 3: Determination of undulation> of the embodiment described later.

[0130] The resin composition involved in one embodiment of the present invention can generally have a low minimum melt viscosity. For example, when the minimum melt viscosity is measured by the method described in <Test Example 2: Determination of Minimum Melt Viscosity of Resin Composition> of the examples described later, the minimum melt viscosity of the resin composition involved in one embodiment of the present invention is preferably less than 4,000 poise, more preferably 3,500 poise or less, and further preferably 2,900 poise or less. From the viewpoint of smoothly forming a thicker insulating layer, the lower limit can be, for example, 500 poise or more, 700 poise or more, etc.

[0131] By curing the resin composition involved in one embodiment of the present invention, a cured product can be obtained. During the above-mentioned curing, heat is usually applied to the resin composition. Therefore, usually among the components contained in the resin composition, volatile components such as (H) solvents can be volatilized by the heat during curing, while non-volatile components such as (A) to (G) components will not volatilize due to the heat during curing. Therefore, the cured product of the resin composition can contain the non-volatile components of the resin composition or their reaction products.

[0132] According to the resin composition involved in one embodiment of the present invention, a cured product with high insulation reliability can be obtained. The insulation reliability of the cured product can be evaluated by the insulation resistance value of the cured product after a durability test of applying voltage in a high temperature and high humidity environment. In one example, the resin composition involved in one embodiment of the present invention is thermally cured at 190°C for 90 minutes to obtain a cured product, and the cured product is subjected to a durability test of applying a voltage of 3.3V for 100 hours in an environment of 130°C and 85% RH. When the durability test is carried out in this way, the insulation resistance value of the cured product measured using a comb-shaped electrode with a line width / line spacing of 15μm / 15μm is preferably 1.0×10 8 Ω or more, more preferably 1.0×10 9 The upper limit is as large as possible, for example, it can be 1.0×10 14 Ω or less. The specific evaluation method of the insulation reliability can be the method described in <Test Example 4: Evaluation of Insulation Reliability> of the Examples described later.

[0133] According to the resin composition involved in one embodiment of the present invention, a cured product with excellent heat resistance can usually be obtained. The heat resistance of the cured product can be represented by the glass transition temperature, for example. In one example, the glass transition temperature of the cured product obtained by heat curing the resin composition involved in one embodiment of the present invention under the curing conditions of 190°C and 90 minutes is preferably 130°C or more, more preferably 140°C or more, and further preferably 150°C or more. The higher the upper limit of the glass transition temperature, the better, for example, it can be below 200°C, below 190°C, below 180°C, etc. The glass transition temperature can be measured by thermomechanical analysis by tensile load method under the measuring conditions of load 1g and heating rate 5°C / min. The specific method for measuring the glass transition temperature can adopt the method described in <Test Example 1: Determination of glass transition temperature and linear thermal expansion coefficient of cured product> of the embodiment described later.

[0134] According to the resin composition involved in one embodiment of the present invention, a cured product with excellent reflow resistance can usually be obtained. Reflow resistance can be evaluated by forming a conductor layer on an insulating layer formed by curing the resin composition and performing a reflow resistance test including heating. In one example, a conductor layer is formed by plating on an insulating layer formed by thermally curing the resin composition involved in one embodiment of the present invention at 130°C for 30 minutes and at 170°C for 30 minutes to obtain two samples of 100mm×50mm. Then, these samples are subjected to a reflow resistance test 10 times in a reflow device that reproduces the solder reflow temperature of a peak temperature of 260°C (the reflow temperature curve is based on IPC / JEDEC J-STD-020C). At this time, the number of abnormal occurrence sites such as expansion is preferably 4 or less, and more preferably 0. The specific evaluation method of reflow resistance can adopt the method described in <Test Example 5: Evaluation of Reflow Resistance> of the embodiment described later.

[0135] According to the resin composition involved in one embodiment of the present invention, a cured product with a small linear thermal expansion coefficient can usually be obtained. In one example, the average linear thermal expansion coefficient of the cured product obtained by thermally curing the resin composition involved in one embodiment of the present invention under the curing conditions of 190°C and 90 minutes in the range of 25°C to 150°C is preferably 30 ppm or less, more preferably 25 ppm or less, and further preferably 23 ppm or less. The linear thermal expansion coefficient can be measured by thermomechanical analysis by a tensile load method under the measuring conditions of a load of 1g and a heating rate of 5°C / min. The specific method for measuring the linear thermal expansion coefficient can adopt the method described in <Test Example 1: Determination of glass transition temperature and linear thermal expansion coefficient of cured product> of the examples described later.

[0136] The cured product of the resin composition involved in one embodiment of the present invention can generally have excellent dielectric properties. For example, the relative dielectric constant of the cured product is preferably 5.0 or less, more preferably 4.0 or less, and further preferably 3.5 or less. There is no particular restriction on the lower limit of the relative dielectric constant, for example, it can be 1.5 or more, 2.0 or more, etc. In addition, for example, the dielectric loss tangent of the cured product is preferably 0.0200 or less, more preferably 0.0100 or less, further preferably 0.0050 or less, and particularly preferably 0.0030 or less. There is no particular restriction on the lower limit of the dielectric loss tangent, for example, it can be 0.0005 or more. The relative dielectric constant and dielectric loss tangent of the cured product can be obtained by heat curing the resin composition under curing conditions of 190°C and 90 minutes, and measured by the resonant cavity perturbation method under the conditions of measuring frequency 5.8GHz and measuring temperature 23°C. As a measuring device, for example, "HP8362B" manufactured by Agilent Technologies can be used.

[0137] [Application of resin composition] The resin composition involved in one embodiment of the present invention can be used as a resin composition for insulating purposes, and is particularly suitable for use as a resin composition for forming an insulating layer (resin composition for insulating layer formation). For example, the resin composition involved in this embodiment is suitable for use as a resin composition for forming an insulating layer of a semiconductor chip package (resin composition for insulating layer of a semiconductor chip package) and a resin composition for forming an insulating layer of a circuit substrate (including a printed wiring board) (resin composition for insulating layer of a circuit substrate). In particular, the resin composition is suitable for forming an interlayer insulating layer provided between a conductor layer and a conductor layer.

[0138] As semiconductor chip packages, for example, FC-CSP, MIS-BGA package, ETS-BGA package, fan-out type WLP (wafer level package), fan-in type WLP, fan-out type PLP (panel level package), and fan-in type PLP can be cited.

[0139] Furthermore, the resin composition can be used as an underfill material, for example, as a material for MUF (Molding Under Filling) used after connecting a semiconductor chip to a substrate.

[0140] Furthermore, the resin composition can be used in a wide range of applications using resin compositions, such as resin sheets, sheet-like laminated materials such as prepregs, solder resists, die bonding materials, semiconductor sealing materials, hole-filling resins, and component embedding resins.

[0141] [Sheet-like laminated material] The resin composition may be used by coating in a varnish state, but is preferably used in the form of a sheet-like laminated material containing the resin composition from an industrial point of view.

[0142] As the sheet-like laminated material, the following resin sheets and prepregs are preferred.

[0143] In one embodiment, the resin sheet comprises a support and a resin composition layer formed on the support. The resin composition layer is formed from the above-mentioned resin composition. Therefore, the resin composition layer usually contains the resin composition, and preferably contains only the resin composition.

[0144] From the viewpoint of thinning and the viewpoint that the resin composition can provide a cured product with excellent insulation even if it is thin, the thickness of the resin composition layer is preferably 50 μm or less, more preferably 40 μm or less. The lower limit of the thickness of the resin composition layer is not particularly limited, and can be 5 μm or more, 10 μm or more, etc.

[0145] Examples of the support include films made of plastic materials, metal foils, and release papers, and films made of plastic materials and metal foils are preferred.

[0146] When a film formed of a plastic material is used as a support, the plastic material includes polyesters such as polyethylene terephthalate (hereinafter sometimes referred to as "PET") and polyethylene naphthalate (hereinafter sometimes referred to as "PEN"), polycarbonate (hereinafter sometimes referred to as "PC"), acrylic polymers such as polymethyl methacrylate (PMMA), cyclic polyolefins, triacetyl cellulose (TAC), polyether sulfide (PES), polyether ketone, polyimide, etc. Among them, polyethylene terephthalate and polyethylene naphthalate are preferred, and inexpensive polyethylene terephthalate is particularly preferred.

[0147] When a metal foil is used as a support, examples of the metal foil include copper foil and aluminum foil. Copper foil is preferred. As the copper foil, a foil formed of a single metal of copper can be used, or a foil formed of an alloy of copper and other metals (such as tin, chromium, silver, magnesium, nickel, zirconium, silicon, titanium, etc.) can be used.

[0148] The support may be subjected to matte treatment, corona treatment, or antistatic treatment on the surface to be bonded to the resin composition layer.

[0149] As the support, a support with a release layer having a release layer on the surface bonded to the resin composition layer can be used. As a release agent used in the release layer of the support with a release layer, for example, one or more release agents selected from alkyd resins, polyolefin resins, polyurethane resins and silicone resins can be cited. The support with a release layer can use a commercial product, for example, it can be a PET film having a release layer with an alkyd resin-based release agent as a main component, i.e., "SK-1", "AL-5", "AL-7" manufactured by Lintec; "Lumirror T60" manufactured by Toray Industries; "Purex" manufactured by Teijin; "Unipeel" manufactured by Unitika, etc.

[0150] The thickness of the support is not particularly limited, but is preferably in the range of 5 μm to 75 μm, and more preferably in the range of 10 μm to 60 μm. When a support with a release layer is used, the thickness of the entire support with a release layer is preferably in the above range.

[0151] In one embodiment, the resin sheet may further include an arbitrary layer as required. As such an arbitrary layer, for example, a protective film based on a support provided on the surface of the resin composition layer that is not bonded to the support (i.e., the surface on the opposite side of the support) can be cited. The thickness of the protective film is not particularly limited, for example, 1 μm to 40 μm. By laminating the protective film, it is possible to suppress the attachment of garbage and damage to the surface of the resin composition layer.

[0152] The resin sheet can be produced, for example, by directly coating a liquid (varnish-like) resin composition on a support using a coating device such as a die coater, or by dissolving the resin composition in a solvent to prepare a liquid (varnish-like) resin composition and coating it on a support, followed by drying to form a resin composition layer.

[0153] Examples of the solvent include the same solvents as those described above as the (H) solvent as a component of the resin composition. The solvent may be used alone or in combination of two or more.

[0154] Drying can be carried out by drying methods such as heating and hot air blowing. The drying conditions are not particularly limited, and the drying is carried out in a manner such that the content of the organic solvent in the resin composition layer is generally 10% by mass or less, preferably 5% by mass or less. The drying conditions also vary depending on the boiling point of the solvent in the resin composition. For example, in the case of using a resin composition containing 30% to 60% by mass of a solvent, the resin composition layer can be formed by drying at 50° C. to 150° C. for 3 minutes to 10 minutes.

[0155] The resin sheet can be stored in a roll shape. When the resin sheet has a protective film, it can usually be used by peeling off the protective film.

[0156] In one embodiment, the prepreg is formed by impregnating a sheet-like fiber base material with the above-mentioned resin composition.

[0157] The sheet-like fiber substrate used for the prepreg can be, for example, glass cloth, aramid nonwoven fabric, liquid crystal polymer nonwoven fabric, etc. as materials commonly used as prepreg substrates. From the viewpoint of thinness, the thickness of the sheet-like fiber substrate is preferably 50 μm or less, more preferably 40 μm or less, more preferably 30 μm or less, and particularly preferably 20 μm or less. The lower limit of the thickness of the sheet-like fiber substrate is not particularly limited. It is usually 10 μm or more.

[0158] Prepregs can be produced by hot melt method, solvent method and the like.

[0159] The thickness of the prepreg may be in the same range as that of the resin composition layer in the above-mentioned resin sheet.

[0160] The sheet-like laminated material can be used, for example, to form an insulating layer in the manufacture of a semiconductor chip package (insulating resin sheet for semiconductor chip package). As applicable semiconductor chip packages, for example, fan-out WLP, fan-in WLP, fan-out PLP, fan-in PLP, etc. can be cited. In addition, the sheet-like laminated material can be used, for example, to form an insulating layer of a circuit substrate (insulating resin sheet for circuit substrate). Furthermore, the sheet-like laminated material can be used as a material for MUF used after connecting the semiconductor chip to the substrate. In particular, the sheet-like laminated material is suitable for forming an interlayer insulating layer.

[0161] [Circuit board] The circuit substrate involved in one embodiment of the present invention includes a cured product of a resin composition. Typically, the circuit substrate is provided with an insulating layer formed by a cured product of a resin composition. The insulating layer includes a cured product of the above-mentioned resin composition, preferably only includes a cured product of the above-mentioned resin composition. The circuit substrate can be manufactured, for example, by a manufacturing method comprising the following steps (I) and step (II). (I) A step of forming a resin composition layer on an inner layer substrate. (II) A step of curing the resin composition layer to form an insulating layer.

[0162] The "inner layer substrate" used in step (I) is a member of the base material that forms the circuit substrate, and examples thereof include glass epoxy substrates, metal substrates, polyester substrates, polyimide substrates, BT resin substrates, thermosetting polyphenylene ether substrates, and the like. In addition, the substrate may have a conductor layer on one or both sides thereof, and the conductor layer may be patterned. An inner layer substrate having a conductor layer (circuit) formed on one or both sides of the substrate is sometimes referred to as an "inner layer circuit substrate". In addition, when manufacturing a circuit substrate, an intermediate product on which an insulating layer and / or a conductor layer is to be further formed is also included in the above-mentioned "inner layer substrate". In the case where the circuit substrate is a circuit board with built-in components, an inner layer substrate with built-in components can be used.

[0163] In the case where the conductor layer possessed by the inner substrate is patterned, from the viewpoint of flexibly utilizing the advantages of excellent crack resistance, it is preferred that the minimum line width / line spacing of the conductor layer is relatively small. "Line width" represents the wiring width of the conductor layer, and "line spacing" represents the spacing width between the wirings. The range of the minimum line width / line spacing ratio is preferably less than 100 / 100μm (i.e., the spacing is less than 200μm), more preferably less than 50 / 50μm, further preferably less than 30 / 30μm, further preferably less than 20 / 20μm, and further preferably less than 10 / 10μm. The lower limit may be, for example, more than 0.5 / 0.5μm. The spacing may be uniform or uneven throughout the conductor layer. The minimum spacing of the conductor layer may be, for example, less than 100μm, less than 60μm, less than 40μm, less than 36μm, or less than 30μm.

[0164] The formation of the resin composition layer on the inner substrate can be carried out, for example, by laminating the inner substrate and the resin sheet. The lamination of the inner substrate and the resin sheet can be carried out, for example, by heating and pressing the resin sheet to the inner substrate from the support body side. As a component for heating and pressing the resin sheet to the inner substrate (hereinafter also referred to as "heating and pressing component"), for example, a heated metal plate (SUS end plate, etc.) or a metal roller (SUS roller) can be cited. It should be noted that it is preferred that the heating and pressing component is not directly pressed on the resin sheet, but is pressed via an elastic material such as heat-resistant rubber so that the resin sheet fully follows the surface unevenness of the inner substrate.

[0165] The lamination of the inner substrate and the resin sheet can be implemented by vacuum lamination. In the vacuum lamination method, the heating and pressing temperature is preferably 60°C to 160°C, more preferably in the range of 80°C to 140°C, the heating and pressing pressure is preferably 0.098MPa to 1.77MPa, more preferably in the range of 0.29MPa to 1.47MPa, and the heating and pressing time is preferably 20 seconds to 400 seconds, more preferably in the range of 30 seconds to 300 seconds. Lamination can be preferably implemented under reduced pressure conditions of a pressure of less than 26.7hPa.

[0166] Lamination can be performed by a commercially available vacuum laminator, such as a vacuum pressure laminator manufactured by Meiki Seisakusho Co., Ltd., a vacuum laminator manufactured by Nikko-Materials Co., Ltd., and a batch vacuum pressure laminator.

[0167] After lamination, the laminated resin sheet can be smoothed under normal pressure (atmospheric pressure), for example, by pressing the heating and pressing member from the support body side. The pressing conditions for the smoothing treatment can be the same conditions as the heating and pressing conditions for the above-mentioned lamination. The smoothing treatment can be performed using a commercially available laminator. It should be noted that the lamination and smoothing treatment can be performed continuously using the above-mentioned commercially available vacuum laminator.

[0168] The support may be removed between step (I) and step (II), or may be removed after step (II).

[0169] In step (II), the resin composition layer is cured to form an insulating layer formed by a cured product of the resin composition. The curing of the resin composition layer is usually carried out by thermal curing. The specific curing conditions of the resin composition layer may vary depending on the type of the resin composition. In one example, the curing temperature is preferably 120°C to 240°C, more preferably 150°C to 220°C, and further preferably 170°C to 210°C. The curing time is preferably 5 minutes to 120 minutes, more preferably 10 minutes to 100 minutes, and further preferably 15 minutes to 100 minutes.

[0170] The method for manufacturing a circuit board preferably includes preheating the resin composition layer at a temperature lower than the curing temperature before thermal curing of the resin composition layer. For example, before thermal curing the resin composition layer, the resin composition layer may be preheated at a temperature of 50°C to 150°C, preferably 60°C to 140°C, and more preferably 70°C to 130°C for usually 5 minutes or more, preferably 5 minutes to 150 minutes, more preferably 15 minutes to 120 minutes, and further preferably 15 minutes to 100 minutes.

[0171] When manufacturing a circuit substrate, the step of (III) opening holes in the insulating layer, the step of (IV) roughening the insulating layer, and the step of (V) forming a conductor layer can be further implemented. These steps (III) to (V) can be implemented according to various methods known to those skilled in the art used in the manufacture of the circuit substrate. It should be noted that when the support body is removed after step (II), the removal of the support body can be implemented between step (II) and step (III), between step (III) and step (IV), or between step (IV) and step (V). In addition, as needed, the formation of the insulating layer and the conductor layer of steps (I) to (V) can be repeatedly implemented to manufacture a circuit substrate with a multilayer structure such as a multilayer printed wiring board.

[0172] In other embodiments, the circuit board can be manufactured using the above-mentioned prepreg. The manufacturing method is basically the same as that in the case of using a resin sheet.

[0173] Step (III) is a step of opening holes in the insulating layer, thereby forming holes such as through holes and vias in the insulating layer. Step (III) can be implemented using, for example, a drill, laser, plasma, etc., depending on the composition of the resin composition used in forming the insulating layer. The size and shape of the hole can be appropriately determined according to the design of the circuit board.

[0174] Step (IV) is a step of roughening the insulating layer. Usually, in step (IV), contamination is also removed. Therefore, the aforementioned roughening treatment is sometimes referred to as "decontamination treatment". The order and conditions of the roughening treatment are not particularly limited, and the known order and conditions commonly used when forming the insulating layer of the circuit substrate can be adopted. For example, the insulating layer can be roughened by swelling treatment using a swelling solution, roughening treatment using an oxidizing agent, and neutralization treatment using a neutralizing solution in sequence.

[0175] As the swelling liquid used in the roughening treatment, for example, an alkaline solution, a surfactant solution, etc. can be cited, preferably an alkaline solution. As the alkaline solution, a sodium hydroxide solution and a potassium hydroxide solution are more preferred. As commercially available swelling liquids, for example, "Swelling Dip Securiganth P" and "Swelling Dip Securiganth SBU" manufactured by Atotech Japan Co., Ltd. can be cited. The swelling treatment using the swelling liquid can be carried out, for example, by immersing the insulating layer in a swelling liquid at 30°C to 90°C for 1 minute to 20 minutes. From the viewpoint of suppressing the swelling of the resin of the insulating layer to an appropriate level, it is preferred to immerse the insulating layer in a swelling liquid at 40°C to 80°C for 5 minutes to 15 minutes.

[0176] As the oxidant used in the roughening treatment, an alkaline permanganate solution in which potassium permanganate or sodium permanganate is dissolved in an aqueous solution of sodium hydroxide can be cited. The roughening treatment using an oxidant such as an alkaline permanganate solution is preferably performed by immersing the insulating layer in an oxidant solution heated to 60° C. to 100° C. for 10 to 30 minutes. In addition, the concentration of permanganate in the alkaline permanganate solution is preferably 5% to 10% by mass. As commercially available oxidants, alkaline permanganate solutions such as "Concentrate Compact CP" and "Dosing Solution Securiganth P" manufactured by Atotech Japan Co., Ltd. can be cited.

[0177] As the neutralizing solution used in the roughening treatment, an acidic aqueous solution is preferred. As a commercially available product, for example, "Reduction Solution Securiganth P" manufactured by Atotech Japan Co., Ltd. can be cited. The treatment with the neutralizing solution can be carried out by immersing the treated surface subjected to the roughening treatment using the oxidant in the neutralizing solution at 30°C to 80°C for 5 minutes to 30 minutes. In view of operability, etc., it is preferred to immerse the object subjected to the roughening treatment using the oxidant in the neutralizing solution at 40°C to 70°C for 5 minutes to 20 minutes.

[0178] Step (V) is a step of forming a conductor layer, and a conductor layer is formed on the insulating layer. The conductor material used in the conductor layer is not particularly limited. In a preferred embodiment, the conductor layer comprises one or more metals selected from gold, platinum, palladium, silver, copper, aluminum, cobalt, chromium, zinc, nickel, titanium, tungsten, iron, tin and indium. The conductor layer may be a single metal layer or an alloy layer. As the alloy layer, for example, a layer formed by an alloy of two or more metals selected from the above metals (e.g., nickel-chromium alloy, copper-nickel alloy and copper-titanium alloy) may be cited. Among them, from the viewpoints of versatility, cost, ease of pattern formation, etc. of the formation of the conductor layer, preferably a single metal layer of chromium, nickel, titanium, aluminum, zinc, gold, palladium, silver or copper, or an alloy layer of nickel-chromium alloy, copper-nickel alloy, or copper-titanium alloy, more preferably a single metal layer of chromium, nickel, titanium, aluminum, zinc, gold, palladium, silver or copper, or an alloy layer of nickel-chromium alloy, and even more preferably a single metal layer of copper.

[0179] The conductor layer may be a single-layer structure, or a multilayer structure in which two or more single metal layers or alloy layers formed of different types of metals or alloys are stacked. When the conductor layer is a multilayer structure, the layer in contact with the insulating layer is preferably a single metal layer of chromium, zinc or titanium, or an alloy layer of a nickel-chromium alloy.

[0180] The thickness of the conductor layer depends on the desired design of the circuit board, but is generally 3 μm to 35 μm, preferably 5 μm to 30 μm.

[0181] In one embodiment, the conductor layer can be formed by plating. For example, the surface of the insulating layer can be plated by a conventionally known technique such as a semi-additive method or a full-additive method to form a conductor layer having a desired wiring pattern. From the viewpoint of simplicity of manufacture, a semi-additive method is preferred. An example of forming a conductor layer by a semi-additive method is shown below.

[0182] First, a plating seed layer is formed on the surface of the insulating layer by electroless plating. Next, a mask pattern is formed on the formed plating seed layer to expose a portion of the plating seed layer corresponding to the desired wiring pattern. After a metal layer is formed on the exposed plating seed layer by electrolytic plating, the mask pattern is removed. Then, the unnecessary plating seed layer is removed by etching or the like, and a conductor layer having a desired wiring pattern can be formed.

[0183] In other embodiments, the conductor layer can be formed using a metal foil. When a metal foil is used to form a conductor layer, it is preferred to implement step (V) between step (I) and step (II). For example, after step (I), the support is removed and a metal foil is laminated on the surface of the exposed resin composition layer. The lamination of the resin composition layer and the metal foil can be implemented by a vacuum lamination method. The lamination conditions can be the same as those described for step (I). Next, step (II) is implemented to form an insulating layer. Then, using the metal foil on the insulating layer, a conductor layer with a desired wiring pattern can be formed by previously known techniques such as a subtractive method and a modified semi-additive method.

[0184] The metal foil can be produced by a known method such as electrolysis or rolling. Commercially available metal foils include HLP foil and JXUT-III foil manufactured by JX Nippon Mining & Metals Co., Ltd., 3EC-III foil and TP-III foil manufactured by Mitsui Mining & Co., Ltd.

[0185] [Semiconductor chip packaging] The semiconductor chip package involved in one embodiment of the present invention includes a cured product of a resin composition. Typically, the semiconductor chip package includes an insulating layer formed by a cured product of a resin composition. The insulating layer includes a cured product of the above-mentioned resin composition, preferably only includes a cured product of the above-mentioned resin composition. As the semiconductor chip package, for example, the following semiconductor chip package can be cited.

[0186] The semiconductor chip package according to the first example includes the above-mentioned circuit substrate and a semiconductor chip mounted on the circuit substrate. The semiconductor chip package can be manufactured by bonding the semiconductor chip to the circuit substrate.

[0187] The bonding conditions between the circuit substrate and the semiconductor chip may be any conditions that can connect the terminal electrodes of the semiconductor chip to the circuit wiring of the circuit substrate by conductor. For example, the conditions used in flip chip mounting of the semiconductor chip may be used. In addition, for example, the semiconductor chip and the circuit substrate may be bonded via an insulating adhesive.

[0188] As an example of a joining method, a method of crimping a semiconductor chip to a circuit substrate can be cited. As crimping conditions, the crimping temperature is usually in the range of 120°C to 240°C (preferably in the range of 130°C to 200°C, more preferably in the range of 140°C to 180°C), and the crimping time is usually in the range of 1 second to 60 seconds (preferably in the range of 5 seconds to 30 seconds).

[0189] Another example of the bonding method is to bond the semiconductor chip to the circuit board by reflowing. The reflow conditions can be set to a range of 120°C to 300°C.

[0190] After the semiconductor chip is bonded to the circuit board, the semiconductor chip may be filled with a mold underfill material. As the mold underfill material, the above-mentioned resin composition may be used.

[0191] The semiconductor chip package according to the second example includes a semiconductor chip and an insulating layer formed of a cured product of a resin composition. Examples of the semiconductor chip package according to the second example include a fan-out WLP and a fan-out PLP.

[0192] Figure 1 FIG. 1 is a cross-sectional view schematically showing a fan-out type WLP as an example of a semiconductor chip package according to an embodiment of the present invention. Figure 1 As shown, a semiconductor chip package 100 as a fan-out WLP comprises: a semiconductor chip 110; a sealing layer 120 formed in a manner covering the periphery of the semiconductor chip 110; a rewiring forming layer 130 as an insulating layer arranged on a surface on the opposite side of the sealing layer 120 of the semiconductor chip 110; a rewiring layer 140 as a conductive layer; a solder resist layer 150; and a bump 160.

[0193] Such a method for manufacturing a semiconductor chip package includes: (i) a step of laminating a temporary fixing film on a substrate, (ii) a step of temporarily fixing the semiconductor chip on the temporary fixing film, (iii) forming a sealing layer on the semiconductor chip, (iv) a step of peeling the substrate and the temporary fixing film from the semiconductor chip, (v) forming a rewiring formation layer on the surface of the semiconductor chip from which the substrate and the temporary fixing film have been peeled off, (vi) a step of forming a rewiring layer as a conductor layer on the rewiring formation layer, and (vii) a step of forming a solder resist layer on the rewiring layer. In addition, the above-mentioned method for manufacturing the semiconductor chip package may also include: (viii) A step of cutting a plurality of semiconductor chip packages into individual semiconductor chip packages to separate them into pieces.

[0194] (Process (i)) Step (i) is a step of laminating the temporary fixing film on the substrate. The lamination conditions of the substrate and the temporary fixing film may be the same as the lamination conditions of the inner layer substrate and the resin sheet in the method for producing the circuit board.

[0195] As the substrate, for example, there can be mentioned: silicon wafers; glass wafers; glass substrates; metal substrates such as copper, titanium, stainless steel, cold-rolled steel sheets (SPCC); substrates such as FR-4 substrates in which glass fibers are impregnated with epoxy resin and subjected to heat curing treatment; substrates formed from bismaleimide triazine resins such as BT resin; etc.

[0196] Any material that can be peeled from the semiconductor chip and can temporarily fix the semiconductor chip can be used as the temporary fixing film. Examples of commercially available products include "REVALPHA" manufactured by Nitto Denko Corporation.

[0197] (Step (ii)) Step (ii) is a step of temporarily fixing the semiconductor chip on the temporary fixing film. The temporary fixing of the semiconductor chip can be performed using, for example, a flip chip bonder, a die bonder, or the like. The layout and number of configurations of the semiconductor chip can be appropriately set according to the shape and size of the temporary fixing film, the number of production of the target semiconductor chip package, etc. For example, the semiconductor chips can be arranged in a matrix of multiple rows and columns for temporary fixing.

[0198] (Process (iii)) Step (iii) is a step of forming a sealing layer on a semiconductor chip. The sealing layer can be formed, for example, using a photosensitive resin composition or a thermosetting resin composition. The sealing layer can also be formed using a cured product of the resin composition involved in the above-mentioned embodiment. The sealing layer can usually be formed by a method comprising a step of forming a resin composition layer on a semiconductor chip and a step of curing the resin composition layer to form a sealing layer.

[0199] (Process (iv)) Step (iv) is a step of peeling off the substrate and the temporary fixing film from the semiconductor chip. It is desirable that the peeling method adopts an appropriate method adapted to the material of the temporary fixing film. As the peeling method, for example, a method of peeling off by heating, foaming or expanding the temporary fixing film can be cited. In addition, as the peeling method, for example, a method of peeling off by irradiating the temporary fixing film with ultraviolet rays through the substrate to reduce the adhesive force of the temporary fixing film can be cited.

[0200] When the substrate and the temporary fixing film are peeled off from the semiconductor chip as described above, the surface of the sealing layer is exposed. The method for manufacturing a semiconductor chip package may include a step of grinding the exposed surface of the sealing layer. By grinding, the smoothness of the surface of the sealing layer can be improved.

[0201] (Process (v)) Step (v) is a step of forming a rewiring forming layer as an insulating layer on the surface of the semiconductor chip from which the substrate and the temporary fixing film are peeled off. Usually, the rewiring forming layer is formed on the semiconductor chip and the sealing layer. The rewiring forming layer can be formed using a cured product of the resin composition involved in the above-mentioned embodiment. The rewiring forming layer can usually be formed using a method including a step of forming a resin composition layer on a semiconductor chip and a step of curing the resin composition layer to form a rewiring forming layer. The formation of the resin composition layer on the semiconductor chip can be carried out, for example, by the same method as the method for forming the resin composition layer on the inner substrate described in the above-mentioned method for manufacturing the circuit substrate, except that a semiconductor chip is used instead of the inner substrate.

[0202] After forming a resin composition layer on the semiconductor chip, the resin composition layer is cured to obtain a rewiring forming layer as an insulating layer of a cured product containing a resin composition. The curing conditions of the resin composition layer can adopt the same conditions as the curing conditions of the resin composition layer in the manufacturing method of the circuit substrate. In the case of thermally curing the resin composition layer, a preheating treatment of heating at a temperature lower than the curing temperature can be applied to the resin composition layer before the thermal curing. The processing conditions of the preheating treatment can adopt the same conditions as the preheating treatment in the manufacturing method of the circuit substrate. Usually, after forming the rewiring forming layer, in order to connect the semiconductor chip to the rewiring layer, a hole is formed in the rewiring forming layer.

[0203] (Step (vi)) Step (vi) is a step of forming a rewiring layer as a conductor layer on the rewiring forming layer. The method of forming the rewiring layer on the rewiring forming layer may be the same as the method of forming the conductor layer on the insulating layer in the method of manufacturing the circuit substrate. In addition, steps (v) and (vi) may be repeated to alternately overlap (stack) the rewiring layer and the rewiring forming layer.

[0204] (Process (vii)) Step (vii) is a step of forming a solder resist layer on the rewiring layer. The material of the solder resist layer can use any material with insulation. Among them, from the perspective of the ease of manufacturing of semiconductor chip packaging, photosensitive resin compositions and thermosetting resin compositions are preferred. The solder resist layer can be formed using a cured product of the resin composition involved in the above-mentioned embodiment.

[0205] In step (vii), bump processing for forming bumps may be performed as necessary. The bump processing may be performed using methods such as solder balls and solder plating. In addition, the formation of through holes in the bump processing may be performed in the same manner as in step (v).

[0206] (Process (viii)) The method for manufacturing a semiconductor chip package may include step (viii) in addition to steps (i) to (vii). Step (viii) is a step of cutting a plurality of semiconductor chip packages into individual semiconductor chip packages for singulation. The method for cutting a semiconductor chip package into individual semiconductor chip packages is not particularly limited.

[0207] [Semiconductor devices] The semiconductor device has the above-mentioned circuit substrate or semiconductor chip package. Examples of the semiconductor device include various semiconductor devices that can be used in electrical products (e.g., computers, mobile phones, smart phones, tablet devices, wearable devices, digital cameras, medical equipment, and televisions) and transportation vehicles (e.g., motorcycles, cars, trains, ships, and airplanes). Example

[0208] The present invention is specifically described below with reference to the following embodiments. However, the present invention is not limited to the following embodiments. In the following description, "parts" and "%" indicating quantities refer to "parts by mass" and "% by mass" respectively, unless otherwise expressly stated. The temperature conditions and pressure conditions when the temperature and pressure are not particularly specified are room temperature (25°C) and atmospheric pressure (1atm). In the following description, the so-called "L / S" refers to the line width (wiring width) / line spacing (spacing width) ratio of the conductor pattern, unless otherwise stated.

[0209] <Example 1> 70 parts of methyl ethyl ketone (MEK) were added to 25 parts of biphenyl type solid epoxy resin ("NC3000L" manufactured by Nippon Kayaku Co., Ltd., epoxy equivalent of about 269 g / eq.), 15 parts of naphthalene type solid epoxy resin ("ESN475V" manufactured by Nippon Kayaku Co., Ltd., epoxy equivalent of about 332 g / eq.), and 5 parts of trimethylolpropane type liquid epoxy resin ("ED-505" manufactured by ADEKA Co., Ltd., epoxy equivalent of about 150 g / eq., 150 mPa·s), and heated and dissolved while stirring to obtain a solution. The solution was cooled to room temperature to prepare a dissolved composition of epoxy resin.

[0210] In this dissolved composition, 5 parts of a phenolic curing agent containing a triazine skeleton ("LA-3018-50P" manufactured by DIC Corporation, a 2-methoxypropanol solution with an active group equivalent of about 151 g / eq. and a non-volatile content of 50%), 26 parts of an active ester compound ("HPC-8000-65T" manufactured by DIC Corporation, a toluene solution with an active ester group equivalent of about 223 g / eq. and a non-volatile content of 65%), 8 parts of a phenoxy resin ("YX7553BH30" manufactured by Mitsubishi Chemical Corporation, a 1:1 solution of MEK and cyclohexanone with a non-volatile content of 30% by mass), and biomass silica ("Ethical Silica" manufactured by MIT Corporation) surface-treated with a silane coupling agent ("KBM-573" manufactured by Shin-Etsu Chemical Co., Ltd.) were mixed. Silica", average particle size 3.7μm, carbon content 0.6% by mass) 180 parts, amine curing accelerator (4-dimethylaminopyridine (DMAP), MEK solution with 5% by mass of non-volatile components) 4 parts are uniformly dispersed in a high-speed rotary mixer to prepare a resin varnish.

[0211] As a support, a polyethylene terephthalate film ("AL5" manufactured by Lintec Corporation, thickness 38 μm) subjected to a demolding treatment was prepared. A resin varnish was evenly applied to the demolding surface (the surface subjected to the demolding treatment) of the support so that the thickness of the resin composition layer was 40 μm, and dried at 80° C. to 120° C. (average 100° C.) for 5 minutes to produce a resin sheet having a support and a resin composition layer.

[0212] <Example 2> In Example 1, the amount of the phenolic curing agent containing a triazine skeleton ("LA-3018-50P" manufactured by DIC Corporation, an active group equivalent of about 151 g / eq., a 2-methoxypropanol solution with a non-volatile content of 50%) was changed from 5 parts to 12 parts. In addition, 26 parts of the active ester compound ("HPC-8000-65T" manufactured by DIC Corporation, an active ester group equivalent of about 223 g / eq., a toluene solution with a non-volatile content of 65%) were changed to 12 parts of a naphthol-type curing agent ("SN-485" manufactured by Nippon Steel Chemical Materials Co., Ltd., a hydroxyl group equivalent of about 205 g / eq.). Except for the above matters, the resin varnish and the resin sheet were manufactured by the same method as in Example 1.

[0213] <Example 3> In Example 1, a resin varnish and a resin sheet were prepared in the same manner as in Example 1, except that 5 parts of a carbodiimide curing agent ("V-03" manufactured by Nisshinbo Chemical Co., Ltd., an active group equivalent of about 216 g / eq., a toluene solution with a non-volatile content of 50%) were added to the resin composition.

[0214] <Example 4> In Example 1, 5 parts of a phenolic curing agent containing a triazine skeleton ("LA-3018-50P" manufactured by DIC Corporation, an active group equivalent of about 151 g / eq., a 2-methoxypropanol solution having a non-volatile content of 50%) were not used. In addition, the amount of an active ester compound ("HPC-8000-65T" manufactured by DIC Corporation, an active ester group equivalent of about 223 g / eq., a toluene solution having a non-volatile content of 65%) was changed from 26 parts to 20 parts. Furthermore, 15 parts of a prepolymer of bisphenol A diisocyanate ("BA230S75" manufactured by Lonza Japan Corporation, a cyanate equivalent of about 232 g / eq., a MEK solution having a non-volatile content of 75% by mass) and 1 part of a 1% by mass MEK solution of cobalt (III) acetylacetonate (manufactured by Tokyo Chemical Industry Co., Ltd.) were added to the resin composition. In addition, the amount of biomass silica ("Ethical Silica" manufactured by MIT, average particle size 3.7 μm, carbon content 0.6 mass%) surface-treated with a silane coupling agent ("KBM-573" manufactured by Shin-Etsu Chemical Co., Ltd.) was changed from 180 parts to 150 parts. Except for the above matters, the resin varnish and the resin sheet were manufactured in the same manner as in Example 1.

[0215] <Example 5> In Example 1, 5 parts of a trimethylolpropane type liquid epoxy resin ("ED-505" manufactured by ADEKA, epoxy equivalent of about 150 g / eq., 150 mPa·s) were replaced with 5 parts of a neopentyl glycol type liquid epoxy resin ("ED-523T" manufactured by ADEKA, epoxy equivalent of about 140 g / eq., 15 mPa·s). In addition, the amount of biomass silica ("Ethical Silica" manufactured by MIT, average particle size 3.7 μm, carbon content 0.6 mass%) surface-treated with a silane coupling agent ("KBM-573" manufactured by Shin-Etsu Chemical Co., Ltd.) was changed from 180 parts to 60 parts. Furthermore, 5 parts of vinyl benzyl-modified polyphenylene ether ("OPE-2St 2200" manufactured by Mitsubishi Gas Chemical Co., Ltd., a toluene solution with a non-volatile content of 65%) and 120 parts of spherical silica ("SO-C2" manufactured by Yaduma Co., Ltd., with an average particle size of 0.5 μm, a carbon content of 0%, and a biomass ratio of 0%) surface-treated with a silane coupling agent ("KBM-573" manufactured by Shin-Etsu Chemical Co., Ltd.) were added to the resin composition. Except for the above matters, a resin varnish and a resin sheet were prepared in the same manner as in Example 1.

[0216] <Example 6> 70 parts of methyl ethyl ketone were added to 10 parts of a biphenyl type epoxy resin ("NC3000L" manufactured by Nippon Kayaku Co., Ltd., epoxy equivalent of about 269 g / eq.), 5 parts of a bisphenol type liquid epoxy resin ("ZX1059" manufactured by Nippon Steel Chemical Materials Co., Ltd., a 1:1 mixture of bisphenol A type and bisphenol F type, epoxy equivalent of about 169 g / eq., 2600 mPa·s), 20 parts of a naphthyl ether type solid epoxy resin ("HP-6000" manufactured by DIC Corporation, epoxy equivalent of about 250 g / eq.), 5 parts of a dicyclopentadiene type solid epoxy resin ("HP7200HH" manufactured by DIC Corporation, epoxy equivalent of about 283 g / eq.), and 5 parts of a trimethylolpropane type liquid epoxy resin ("ED-505" manufactured by ADEKA Corporation, epoxy equivalent of about 150 g / eq., 150 mPa·s), and the mixture was dissolved by heating while stirring to obtain a solution. The solution was cooled to room temperature to prepare a dissolved composition of the epoxy resin.

[0217] In this dissolved composition, 5 parts of a phenolic curing agent containing a triazine skeleton (a 2-methoxypropanol solution of "LA-3018-50P" manufactured by DIC Corporation, an active group equivalent of about 151 g / eq., and a non-volatile content of 50%), 24 parts of an active ester compound (a methyl isobutyl ketone solution of "EXB9416-70BK" manufactured by DIC Corporation, an active ester group equivalent of about 330 g / eq., and a non-volatile content of 70%), and 1,2-diphenylaralkylphenol novolac-type maleic acid were mixed. 3 parts of imide ("MIR-3000-70MT" manufactured by Nippon Kayaku Co., Ltd., a mixed solution of MEK / toluene with a nonvolatile content of 70%), 8 parts of phenoxy resin ("YX7553BH30" manufactured by Mitsubishi Chemical Corporation, a 1:1 solution of MEK and cyclohexanone with a nonvolatile content of 30% by mass), 180 parts of biomass silica ("Ethical Silica" manufactured by MIT, an average particle size of 3.7 μm, a carbon content of 0.6% by mass) surface-treated with a silane coupling agent ("KBM-573" manufactured by Shin-Etsu Chemical Co., Ltd.), and 4 parts of an imidazole-based curing accelerator ("1B2PZ" manufactured by Shikoku Chemical Co., Ltd., 1-benzyl-2-phenylimidazole, a MEK solution with a nonvolatile content of 10% by mass) were uniformly dispersed using a high-speed rotary mixer to prepare a resin varnish.

[0218] As a support, a polyethylene terephthalate film ("AL5" manufactured by Lintec Corporation, thickness 38 μm) subjected to a demolding treatment was prepared. A resin varnish was evenly applied to the demolding surface (the surface subjected to the demolding treatment) of the support so that the thickness of the resin composition layer was 40 μm, and dried at 80° C. to 120° C. (average 100° C.) for 5 minutes to produce a resin sheet having a support and a resin composition layer.

[0219] <Example 7> In Example 1, a resin varnish and a resin sheet are prepared in the same manner as in Example 1, except that 5 parts of a trimethylolpropane liquid epoxy resin ("ED-505" manufactured by ADEKA Corporation, with an epoxy equivalent of approximately 150 g / eq., 150 mPa·s) are replaced with 5 parts of a bisphenol A liquid epoxy resin ("828EL" manufactured by Mitsubishi Chemical Corporation, with an epoxy equivalent of approximately 180 g / eq., 13,000 mPa·s).

[0220] <Example 8> In Example 1, the amount of trimethylolpropane type liquid epoxy resin ("ED-505" manufactured by ADEKA, epoxy equivalent of about 150 g / eq., 150 mPa·s) was changed from 5 parts to 2 parts. In addition, 3 parts of bimethylolphenol type solid epoxy resin (epoxy equivalent of 190 g / eq., "YX4000HK" manufactured by Mitsubishi Chemical Corporation) were added to the resin composition. Except for the above matters, the resin varnish and the resin sheet were manufactured by the same method as in Example 1.

[0221] <Comparative Example 1> In Example 1, 5 parts of trimethylolpropane type liquid epoxy resin ("ED-505" manufactured by ADEKA, epoxy equivalent of about 150 g / eq., 150 mPa·s) were not used. In addition, the amount of naphthalene type solid epoxy resin ("ESN475V" manufactured by Nippon Kayaku Co., Ltd., epoxy equivalent of about 332 g / eq.) was changed from 15 parts to 20 parts. Except for the above matters, the resin varnish and the resin sheet were manufactured by the same method as in Example 1.

[0222] <Comparative Example 2> In Example 1, a resin varnish and a resin sheet were prepared in the same manner as in Example 1, except that 180 parts of biomass silica ("Ethical Silica" manufactured by MIT, average particle size 3.7 μm, carbon content 0.6 mass%) surface-treated with a silane coupling agent ("KBM-573" manufactured by Shin-Etsu Chemical Co., Ltd.) was replaced with 180 parts of spherical silica ("SO-C2" manufactured by Yaduma Co., Ltd., average particle size 0.5 μm, biomass ratio 0%) surface-treated with a silane coupling agent ("KBM-573" manufactured by Shin-Etsu Chemical Co., Ltd.).

[0223] <Comparative Example 3> In Comparative Example 2, a resin varnish and a resin sheet were produced in the same manner as in Comparative Example 2 except that 5 parts of an ion scavenger ("IXEPLAS-A3" manufactured by Toagosei Co., Ltd., a mixture of hydrotalcite and zirconium phosphate) was added to the resin composition.

[0224] <Comparative Example 4> In Comparative Example 2, the amount of biphenyl type solid epoxy resin ("NC3000L" manufactured by Nippon Kayaku Co., Ltd., epoxy equivalent of about 269 g / eq.) was changed from 25 parts to 20 parts. In addition, 5 parts of black pigment dispersion ("NV-7-201" manufactured by Nippon Pigment Co., Ltd., liquid bisphenol F type epoxy resin containing carbon black, carbon black content 25%) were added to the resin composition. Except for the above matters, the resin varnish and resin sheet were manufactured by the same method as Comparative Example 2.

[0225] <Measurement of Viscosity of Epoxy Resin> The viscosity of the liquid epoxy resin was measured using an E-type viscometer (using a conical rotor of 1°34′×R24, “RE-25U” manufactured by Toki Sangyo) at 25° C. and 20 rpm.

[0226] <Test Example 1: Measurement of Glass Transition Temperature and Linear Thermal Expansion Coefficient of Cured Material> (1) Preparation of cured product for evaluation: A PET film (“501010” manufactured by Lintec, 50 μm thick, 240 mm square) having a treated surface subjected to a release treatment and an untreated surface subjected to no release treatment was prepared. A glass cloth-based epoxy resin double-sided copper-clad laminate (“R5715ES” manufactured by Panasonic, 0.7 mm thick, 255 mm square) was stacked on the untreated surface of the PET film, and the four sides were fixed with a polyimide adhesive tape (10 mm wide).

[0227] The resin varnish prepared in the examples and comparative examples was applied on the treated surface of the PET film using a die coater so that the thickness of the resin composition layer after drying was 40 μm, and dried at 80°C to 120°C (average 100°C) for 10 minutes to obtain a resin sheet. Next, the resin composition layer was thermally cured under curing conditions of 90 minutes after being placed in an oven at 190°C. After thermal curing, the polyimide adhesive tape was peeled off, the glass cloth substrate epoxy resin double-sided copper-clad laminate was removed, and the PET film was further peeled off to obtain a sheet-like cured product. The obtained cured product is referred to as a "cured product for evaluation".

[0228] (2) Determination of glass transition temperature and linear thermal expansion coefficient: The cured product for evaluation was cut to obtain a test piece with a width of about 5 mm and a length of about 15 mm. For the test piece, a thermomechanical analysis was performed using a thermomechanical analysis device ("Thermo Plus TMA8310" manufactured by Rigaku Corporation) using a tensile load method. In detail, after the test piece was installed in the above-mentioned thermomechanical analysis device, two measurements were performed continuously under the measurement conditions of a load of 1 g and a heating rate of 5°C / min. Then, in the second measurement, the glass transition temperature Tg (°C) and the average linear thermal expansion coefficient CTE (ppm / °C) in the range of 25°C to 150°C were calculated.

[0229] <Test Example 2: Measurement of Minimum Melt Viscosity of Resin Composition> The melt viscosity of the resin composition contained in the resin composition layer of the resin sheet manufactured in the examples and comparative examples was measured using a dynamic viscoelasticity measuring device ("Rheosol-G3000" manufactured by UBM). The measurement was performed on a 1 g sample collected from the resin composition layer using a parallel plate with a diameter of 18 mm. The measurement conditions were set to a starting temperature of 60°C to 200°C, a heating rate of 5°C / min, a measurement temperature interval of 2.5°C, and a vibration of 1 Hz / deg. The minimum melt viscosity was determined based on the measured value of the melt viscosity obtained.

[0230] <Test Example 3: Measurement of undulation> The resin sheets prepared in the examples and comparative examples were laminated on a conductor layer (thickness 35 μm, L / S=160 μm / 160 μm) formed in a comb-shaped pattern using a batch vacuum press laminator (MVLP-500 manufactured by Meiki Co., Ltd.). The lamination was performed by reducing the pressure for 30 seconds to a pressure of 13 hPa or less, and then pressing at 100° C. and a pressure of 0.74 MPa for 30 seconds. After lamination, the PET film serving as the support was peeled off, and the resin composition was cured under curing conditions of 100° C. for 30 minutes and then 180° C. for 30 minutes to form an insulating layer.

[0231] The difference between the surface height of the portion of the insulating layer on the conductor layer and the surface height of the portion of the insulating layer other than the portion is determined as the undulation Rt of the insulating layer. The undulation Rt of the insulating layer is measured using a non-contact surface roughness meter (WYKO NT3300 manufactured by Veeco Precision Instruments) in VSI mode and a 10x lens with a measurement range of 1.2 mm × 0.91 mm as the maximum peak-to-valley value. The case where the undulation Rt is less than 2.0 μm is evaluated as "0", the case where the undulation Rt is 2.0 μm to 3.0 μm is evaluated as "△", and the case where the undulation Rt is greater than 3.0 μm is evaluated as "×".

[0232] <Test Example 4: Evaluation of insulation reliability> Prepare a polyimide film having a comb-shaped electrode (L / S=15μm / 15μm) formed on the surface by a copper circuit. Use a batch vacuum pressure laminator ("MVLP-500" manufactured by Mingji Co., Ltd.) to laminate the resin sheets manufactured in the examples and comparative examples on the polyimide film in such a way that the resin composition layer of the resin sheet is in contact with the surface of the copper circuit. Lamination is performed by reducing the pressure for 30 seconds to make the air pressure below 13hPa, and then pressing at 100°C and a pressure of 0.74MPa for 30 seconds. After peeling off the PET film as a support, the resin composition layer is thermally cured at 190°C for 90 minutes to obtain a sample laminate for insulation reliability evaluation.

[0233] The sample laminate was placed in a highly accelerated life tester ("PM422" manufactured by Kusumoto Chemicals Co., Ltd.) and subjected to a voltage of 3.3 V at 130°C and 85% RH for 100 hours. The insulation resistance of the sample laminate was then measured. The insulation resistance value was 1.0×10 9 The case with a value of Ω or above was evaluated as “○”, and the insulation resistance value was set to 1.0×10 8 Ω or more and less than 1.0×10 9 Ω is evaluated as "△", and the insulation resistance value is less than 1.0×10 8 The case of Ω was evaluated as "×".

[0234] <Test Example 5: Evaluation of Reflow Resistance> (1) Base treatment: Preparation of inner substrate: A glass cloth substrate epoxy resin double-sided copper-clad laminate with copper foil on the surface was prepared (copper foil thickness 18 μm, substrate thickness 0.8 mm, Panasonic "R1515A"). The copper foil on the surface of the inner substrate was etched with a copper etching amount of 1 μm using a microetchant (MEC "CZ8101") to perform a roughening treatment. Then, it was dried at 190°C for 30 minutes to prepare a base-treated inner substrate.

[0235] (2) Lamination and curing of resin sheets: Using a batch vacuum pressure laminator (Nikko-materials 2-stage stacking laminator "CVP700"), the resin sheets manufactured in the embodiments and comparative examples are laminated on both sides of the base treated inner layer substrate in such a way that the resin composition layer is bonded to the above-mentioned base treated inner layer substrate. The lamination is implemented by reducing the pressure for 30 seconds so that the air pressure is below 13hPa, and then pressing at a temperature of 100°C and a pressure of 0.74MPa for 30 seconds. Then, under atmospheric pressure, the laminated resin sheet is hot pressed for 60 seconds at 100°C and a pressure of 0.5MPa to smooth it. Furthermore, it is placed in an oven at 130°C and heated for 30 minutes, and then transferred to an oven at 170°C and heated for 30 minutes to thermally cure the resin composition layer to obtain an intermediate substrate having a layer structure of a support body / insulating layer / base treated inner layer substrate / insulating layer / support body.

[0236] (3) Conductor formation based on plating: The support body was peeled off from the intermediate substrate. Then, the intermediate substrate was immersed in a swelling solution (Swelling Dip Securigant P manufactured by Atotech Japan) at 60°C for 10 minutes. Next, the intermediate substrate was immersed in a roughening solution (Concentrate Compact P manufactured by Atotech Japan; an aqueous solution containing 60 g / L KMnO4 and 40 g / L NaOH) at 80°C for 20 minutes. Furthermore, the intermediate substrate was immersed in a neutralizing solution (Reductionsolution Securigant P manufactured by Atotech Japan) at 40°C for 5 minutes.

[0237] Next, the intermediate substrate was immersed in an electroless plating solution containing PdCl2 at 40°C for 5 minutes, and then immersed in an electroless copper plating solution at 25°C for 20 minutes. After an annealing treatment of heating at 150°C for 30 minutes, the intermediate substrate was further electrolytically plated with copper sulfate to form a conductor layer with a thickness of 30 μm. Next, an annealing treatment was performed at 190°C for 60 minutes to obtain a substrate for evaluating reflow resistance.

[0238] (4) Evaluation of reflow resistance: The substrate for evaluating the reflow resistance was cut into small pieces of 100 mm × 50 mm, and passed through a reflow device ("HAS-6116" manufactured by Antom Co., Ltd., Japan) that reproduced the peak temperature of 260°C solder reflow temperature 10 times (the reflow temperature curve was in accordance with IPC / JEDEC J-STD-020C). Two small pieces were evaluated, and by visual observation, the case with more than 5 abnormalities such as expansion was judged as "×", the case with 1 to 4 abnormalities was judged as "△", and the case with no abnormalities in all small pieces was evaluated as "○".

[0239] [result] The results of the above-mentioned Examples and Comparative Examples are shown in the following tables.

[0240] [Table 1] [Table 1. Results of Examples 1 to 6]

[0241] [Table 2] [Table 2. Results of Examples 7 to 8 and Comparative Examples 1 to 4] Explanation of symbols

[0242] 100 Semiconductor chip packaging 110 Semiconductor Chip 120 Sealing layer 130 Rewiring formation layer 140 Rewiring Layer 150 Solder Mask 160 Bumps.

Claims

1. A resin composition comprising (A) an epoxy resin and (B) an inorganic filler, wherein: (A) the epoxy resin comprises (A-1) a liquid epoxy resin, (B) the inorganic filler includes (B-1) a carbon-containing inorganic filler having a carbon content of 0.1 mass % or more, The amount of (A-1) the liquid epoxy resin is 0.5% by mass or more relative to 100% by mass of the nonvolatile components of the resin composition. The amount of the carbon-containing inorganic filler (B-1) is 10% by mass or more relative to 100% by mass of the nonvolatile components of the resin composition.

2. The resin composition according to claim 1, wherein The composition further comprises (C) a curing agent.

3. The resin composition according to claim 1, wherein The amount of the carbon-containing inorganic filler (B-1) is 20% by mass or more relative to 100% by mass of the total amount of the inorganic filler (B).

4. The resin composition according to claim 1, wherein (B-1) The carbon-containing inorganic filler is silica particles having a carbon content of 0.2 mass % or more.

5. The resin composition according to claim 1, wherein (B-1) The carbon content of the carbon-containing inorganic filler is 5 mass % or less.

6. The resin composition according to claim 1, wherein (A-1) The liquid epoxy resin has a weight average molecular weight of 1,000 or less.

7. The resin composition according to claim 1, wherein (A-1) The liquid epoxy resin is a non-aromatic epoxy resin.

8. The resin composition according to claim 1, wherein (A-1) The liquid epoxy resin has a viscosity of 15,000 mPa·s or less at 25°C.

9. The resin composition according to claim 1, wherein (D) a curing accelerator is included.

10. The resin composition according to claim 1, wherein (E) A thermoplastic resin is included.

11. The resin composition according to claim 1, wherein Has a minimum melt viscosity of less than 4,000 poise.

12. The resin composition according to claim 1, wherein The resin composition was thermally cured at 190°C for 90 minutes to obtain a cured product. When a voltage of 3.3 V was applied to the cured product at 130°C and 85% RH for 100 hours, the insulation resistance of the cured product measured using a comb-shaped electrode with a line width / line spacing of 15 μm / 15 μm was 1.0×10 8 Ω or more.

13. The resin composition according to claim 1, which is used for forming an insulating layer.

14. A cured product of the resin composition according to any one of claims 1 to 13.

15. A sheet-like laminated material, wherein: A resin composition comprising the resin composition according to any one of claims 1 to 13.

16. A resin sheet, wherein: The invention comprises a support and a resin composition layer formed on the support, wherein the resin composition layer comprises the resin composition according to any one of claims 1 to 13.

17. A circuit substrate, wherein: A cured product comprising the resin composition according to any one of claims 1 to 13.

18. A semiconductor chip package, wherein: A cured product comprising the resin composition according to any one of claims 1 to 13.

19. A semiconductor device, wherein: A circuit board according to claim 17 is provided.

20. A semiconductor device, wherein: A semiconductor chip package according to claim 18.