Silicon-containing heat-conducting paste

By using 30-200 μm of main circular silicon particles in the thermally conductive silicone composition, the problems of high density, high combustion and low filling level in the prior art are solved, and the effects of low density, high thermal conductivity and safe processing are achieved. .

CN119013369APending Publication Date: 2024-11-22WACKER CHEMIE AG
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202280094734.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2022-07-11
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

While improving thermal conductivity, the existing thermal silicone compositions have problems such as high density, expensive cost, high combustion, large viscosity, low filling level and dust explosion risk, and small-grain silicon powder is difficult to process and safely handle.

Method used

Using non-crosslinkable thermally conductive silicone compositions, containing 30-200μm main circular silicon particles, combined with specific particle size distribution and shape characteristics, reduces flammability, and prepares silicon particles by melting to reduce viscosity and density. Increase the filling level.

Benefits of technology

The silicone composition with low density, low cost and high thermal conductivity is achieved, reducing the risk of combustion and dust explosion, and improving processing safety and filling effect.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119013369A_ABST
    Figure CN119013369A_ABST
Patent Text Reader

Abstract

The invention relates to a non-crosslinkable thermally conductive silicone composition (Y) comprising-5-50% by volume of at least one non-crosslinkable silicone composition (S), and-50-95% by volume of at least one thermally conductive filler (Z) having a thermal conductivity of at least 5 W / mK, with the proviso that the non-crosslinkable thermally conductive silicone composition (Y) has a thermal conductivity of at least 0.6 W / mK, and at least 20 vol% of the metallic silicon particles present as the thermally conductive filler (Z) fulfill the following features: a) their median diameter x50 is in the range of 30-200 [mu] m; b) they are mainly circular and are characterized by a width / length ratio (aspect ratio w / l) of at least 0.76; c) their distribution range SPAN ((x90-x10) / x50) of at least 0.28.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to thermally conductive silicone compositions, and their preparation and use. Background Art

[0002] Thermally conductive silicone compositions are widely used for thermal management in the automotive and electronics industries. Examples of important manifestations include thermally conductive adhesives, thermally conductive pads, gap fillers, potting compounds and pastes. A thermally conductive paste is a paste that improves the heat transfer between two objects, such as the cooling surface / housing of an integrated circuit and a heat sink. The assembly area of ​​heat sinks and components always contains more or less uneven depths and deviations from planarity. Thermal pastes fill such unevennesses and thus enable better heat transfer to the cooling housing or heat sink.

[0003] The prior art includes different thermally conductive fillers that are added to increase the thermal conductivity of silicone compositions. However, these have serious disadvantages. Ceramic fillers (such as aluminum oxide) have a very high density and therefore increase the weight of the component very significantly. In addition, they are relatively expensive. Metal fillers (such as aluminum powder or silver powder) are conductive, which is unacceptable for many applications. In addition, many metals and alloys are relatively expensive.

[0004] Many other fillers with high thermal conductivity (eg, carbon nanotubes, boron nitride, and aluminum nitride) may also be used only to a limited extent due to their relatively high cost, or in small quantities, or in specific applications.

[0005] The prior art includes various thermally conductive silicone compositions containing silicon particles as thermally conductive fillers. These are relatively light and inexpensive. Furthermore, silicon, as a semiconductor, has extremely low electrical conductivity. However, silicon particles according to the prior art are not suitable for use in electric vehicles and electronic components:

[0006] The Si particles used in the prior art are usually obtained via a grinding process. The disadvantage is that such particles have a high surface area and bind a very large amount of polymer. This increases the viscosity of the silicone composition very significantly. Only mixtures with relatively low filling levels and low thermal conductivity can be produced. In the case of higher filling levels, the composition becomes very hard and can no longer be processed by conventional methods (e.g. dispensers). It has also been found that silicone compositions containing ground silicon particles have relatively high flammability.

[0007] The use of silicon particles smaller than 30 μm is disadvantageous since such small particles have a relatively low minimum ignition energy and therefore present a dust explosion hazard and require complex and expensive safety precautions in industrial processing.

[0008] JP2019131669A2 teaches the use of metal Si particles with a size of 0.1-200 μm and an electrically insulating coating as a thermally conductive filler for an organic resin that does not contain siloxane. The particles can be produced via thermal decomposition or melting or grinding methods, or obtained by polishing or grinding methods. The particles are provided with an electrically insulating coating in a separate method step. In an embodiment, JP2019131669A2 discloses an organic resin containing up to 65% by volume of ground Si particles, the ground Si particles having an average particle size of 32 μm and having a thermal conductivity of up to 7 W / mK. The disadvantage is the use of abrasive particles with relatively high combustibility. The disclosed sulfide product is non-elastic and is therefore not suitable for use as a gap filler in a lithium-ion battery.

[0009] US2016122611 teaches an electrically and thermally conductive silicone elastomer composition containing a thermally conductive filler of less than 30 μm, more preferably 2-8 μm, in combination with carbon black. The thermally conductive filler can be silicon powder. Disclosed in the embodiments is a composition containing up to 60% by weight of ground Si particles with an average particle size of 5 μm or up to 46% by weight of ground Si particles with an average particle size of 40 μm. The thermal conductivity of the composition is at most 1.0 W / mK. The disadvantage is the use of abrasive particles, which have relatively high flammability and allow compositions with only relatively low filling levels and low thermal conductivity.

[0010] US2007135555 teaches a heat-crosslinked thermally conductive silicone composition containing spherical metal Si particles prepared via a melting process, or ground metal Si particles, each metal Si particle having an average particle size of up to 100 μm, more preferably 2-25 μm. Disclosed in the embodiments is a composition containing up to 71% by weight of ground Si particles with an average particle size of 12 μm or up to 71% by weight of spherical Si particles with an average particle size of 5 μm, each particle being combined with an oxidic filler (e.g., Fe2O3 or Al2O3). The thermal conductivity of the composition is up to 1.2 W / mK. The disadvantage is the use of very small Si particles, which are relatively highly flammable and allow compositions with only relatively low filling levels and low thermal conductivity.

[0011] US2007117920 teaches a heat-crosslinked thermally conductive silicone composition containing spherical or ground metal Si particles with an average particle size of 2 to 100 μm, more preferably 2 to 25 μm. Disclosed in the examples are compositions containing up to 67% by weight of ground Si particles with an average particle size of 5-12 μm as the sole filler or in combination with Al2O3. The viscosity of the mixture is in the range of 30 000 to 260 000 mPa·s at a thermal conductivity of up to 1.0 W / mK. The disadvantage is the use of very small Si particles, which are relatively highly flammable and allow compositions with only relatively high viscosities, low filling levels and low thermal conductivity.

[0012] US2001051673 teaches a heat-crosslinked thermally conductive silicone elastomer composition composed of a Fe-Si alloy containing magnetic silicon, the composition comprising flake particles with an average particle size of 0.1 to 350 μm or round particles with an average particle size of 0.1 to 50 μm, preferably 0.5 to 20 μm, preferably flake. Disclosed in the examples is a composition containing 30% by volume of spherical Fe-Si particles combined with 40% by volume of Al2O3 particles, the spherical Fe-Si particles consisting of 97% by weight of Fe and 3% by weight of Si, with an average particle size of 8 μm. The thermal conductivity is 4.0 W / mK. The disadvantage is the use of very small Fe-Si particles with a very high iron content. As a result, the particles are conductive, have a relatively high density and are relatively highly combustible. Another disadvantage is the use of a large amount of Al2O3, which means that the density of the composition is very high.

[0013] US4292223 teaches a cross-linkable thermally conductive silicone elastomer composition containing metal particles (e.g. silicon, preferably an alloy) with an average particle size of 40 to 300 μm. The particles can be spherical or irregularly shaped, with an aspect ratio of up to 8 (corresponding to an aspect ratio (w / l) of not less than 0.125 according to ISO 9276-6). This leads to a very broad definition of possible particle forms, since the particles can be spherical, corresponding to an aspect ratio of 1, or rod-shaped, where the length can be 8 times greater than the width. Disclosed is a composition containing 28% by weight of ground Si particles with an average particle size of 44 μm, without disclosing the w / l ratio. A disadvantage is the use of relatively highly flammable abrasive particles. In addition, the abrasive particles have a relatively high surface area, so that the composition containing the abrasive particles has a relatively high viscosity and is difficult to process. The cross-linked material has low flexibility and is brittle.

[0014] US2006228542 describes a thermally conductive elastomer comprising two thermally conductive fillers of different sizes. The elastomer may in particular be silicone. The first thermally conductive filler is formed of an electrically insulating and thermally conductive ceramic. As one of several examples of suitable ceramic materials, "silicone" is mistakenly listed instead of "silicon dioxide". However, it is fully clear to a person skilled in the art when reading the disclosure that silicon dioxide ceramics are actually referred to, since silicon metal is not a ceramic, but fused silica ceramics (i.e., SiO2 ceramics) are very well known. The first thermally conductive filler further has a unimodal distribution and an average particle size of at least 20 μm. It is disclosed that the first filler particles are spherical or spherical and may also be hollow. It has a preferred average particle size of 30 to 95 μm with a standard deviation of 15 to 40 μm. This is an extremely non-precise definition of the possible distribution range, so the particles may have a very narrow or very wide distribution.

[0015] This is exemplified by the observation that a 40 μm standard deviation about a 30 μm mean particle size corresponds to a very broad particle size distribution, whereas a 15 μm standard deviation about a 95 μm mean particle size corresponds to a very narrow particle size distribution. There is no teaching in US2006228542 about the effect of the standard deviation of the filler particle size distribution on elastomer properties. Summary of the invention

[0016] It was therefore an object of the present invention to provide a non-crosslinkable thermally conductive silicone composition which does not exhibit the above-mentioned disadvantages of the prior art and which combines the properties of low density, low cost and high thermal conductivity.

[0017] This object is achieved by the non-crosslinkable thermally conductive silicone composition (Y) according to the invention, which contains relatively large Si particles with a predominantly rounded surface shape and an average particle size of 30 to 200 μm and at the same time has a particularly large or broad particle distribution range. Completely unexpectedly, it was found in experiments that these non-crosslinkable thermally conductive silicone compositions (Y) according to the invention have a significantly reduced flammability.

[0018] In the context of the present invention, Si particles of "predominantly round" form are understood to mean those having a spherical to ellipsoidal shape with a smooth surface. They may also be referred to as potato-shaped. Figure 1 The inventive, predominantly rounded shape of these Si particles is shown by way of example. The non-inventive Si particle shape is shown by Figure 2 Shown as "sputtered" particles, by Figure 3 shown as "nodular" particles and by Figure 4Shown as "angular" and "sharp" particles. Thus, the metal Si particles of the present invention are not sputtered, nodular, or angular or sharp. But they can contain such particles to an impurity level without destroying their inventive effect.

[0019] according to Figures 1 to 4 The characteristics of the Si particles are additionally shown in the table below.

[0020] picture X50(mm) w / l SPHT 1 98 0.84 0.87 The present invention 2 38 0.68 0.70 Not the present invention 3 73 0.67 0.72 Not the present invention 4 37 0.67 0.76 Not the present invention

[0021] The present invention provides a non-crosslinkable thermally conductive silicone composition (Y), comprising

[0022] - 5 to 50% by volume of a non-crosslinkable silicone composition (S), and

[0023] - 50 to 95% by volume of at least one thermally conductive filler (Z) having a thermal conductivity of at least 5 W / mK, with the proviso that

[0024] The non-crosslinkable thermally conductive silicone composition (Y) has a thermal conductivity of at least 0.6 W / mK, and

[0025] At least 20% by volume of metallic silicon particles present as thermally conductive filler (Z) meet the following characteristics:

[0026] a) their median diameter x50 is in the range of 30-200 μm;

[0027] b) they are predominantly circular and characterized by a width / length ratio (aspect ratio w / l) of at least 0.76;

[0028] c) their distribution range SPAN ((x90-x10) / x50) is at least 0.28.

[0029] In the context of the present invention, the terms "heat-conducting" and "thermally conductive" are equivalent.

[0030] A thermally conductive filler (Z) in the context of the present invention is understood to mean any filler having a thermal conductivity of at least 5 W / mK.

[0031] Thermally conductive silicone compositions (Y) in the context of the present invention are understood to mean those silicone compositions which clearly exceed the thermal conductivity of polydimethylsiloxanes without fillers and additives (typically about 0.2 W / mK), characterized in that they have a thermal conductivity of at least 0.6 W / mK.

[0032] In the context of the present invention, all parameters describing the particle size (parameter: median diameter x50) or the particle size distribution (parameter: standard deviation σ and distribution range SPAN) or the particle shape (parameter: aspect ratio w / l and sphericity SPHT) are based on volume-based distribution. The mentioned indices can be determined, for example, by means of dynamic image analysis according to ISO 13322-2 and ISO 9276-6, for example using a Camsizer X2 from Retsch Technology.

[0033] Those skilled in the art know that standard deviation is not standardized and is a viable feature for evaluating the particle size distribution of different samples only when the mean particle size of the compared samples is approximately the same. Therefore, to describe the relative width of the particle size distribution in the context of the present invention, the particle size distribution range weighted by the median particle size x50 is used, and the dimensionless distribution range SPAN is defined as:

[0034] SPAN = (x90-x10) / x50.

[0035] The aspect ratio is used as an indicator to describe the shape of a particle. Early prior art often described the aspect ratio in terms of the ratio of length to width (l / w). This leads to values ​​not less than 1. In more recent literature, for example according to ISO 9276-6, the aspect ratio is calculated from the reciprocal ratio of width to length (w / l). This leads to values ​​not exceeding 1. The two indices can be converted into each other by forming the reciprocal. In the context of the present invention, the aspect ratio is defined as the ratio of the width of a particle to its length (w / l). The width of a particle is given by x c最小 (the minimum chord among all the maximum chords measured in the particle projection) is given by, and the particle length is given by x Fe最大 (the longest Feret diameter among all Feret diameters measured in the particle) is given. More detailed information can be found, for example, in "Operating Instructions / Manual Particle Size Analysis System ”, Retsch Technology GmbH, 42781 Haan; Doc. No. CAMSIZER V0115. This yields the following formula for the aspect ratio:

[0036] w / l=x c最小 / x Fe最大

[0037] The sphericity SPHT is calculated from the projected area A of the analyzed particle relative to the area of ​​a circle with the same circumference P of the projected particle according to the following formula (more detailed information can be found in, for example, "Operating Instructions / Manual Particle Size Analysis System ”, Retsch Technology GmbH, 42781 Haan; Doc. No. CAMSIZER V0115:

[0038] SPHT=4πA / P 2

[0039] According to ISO 9276-6, the index SPHT corresponds to the square of the roundness C.

[0040] In order not to create too many pages in the description of the present invention, only preferred embodiments of individual features are described in detail below.

[0041] However, an expert reader will clearly understand this manner of disclosure such that any combination of different preference levels is therefore also clearly disclosed and clearly intended.

[0042] Non-crosslinkable silicone composition (S)

[0043] The non-crosslinkable silicone composition (S) comprises:

[0044] An organopolysiloxane (T) having the following properties or a mixture of at least two organopolysiloxanes (T) having the following properties:

[0045] - They are linear, branched or cyclic, preferably linear

[0046] - terminated at both ends or terminated with Si-OH alone or terminated with alkoxy-silyl alone, preferably terminated at both ends,

[0047] -Si bonding side and terminal group R 1 R is independently a substituted or unsubstituted C1-C18 hydrocarbon group, preferably a C1-C10 monovalent hydrocarbon group. 1Examples include straight chain, branched and cyclic alkyl, alkenyl, aryl, aralkyl and haloalkyl. Suitable pure alkyl groups include methyl, ethyl, propyl, hexyl and octyl. Suitable branched alkyl groups include isopropyl, isobutyl, tert-butyl and 2-ethylhexyl. Suitable cyclic alkyl groups include cyclopentyl and cyclohexyl. Suitable alkenyl groups are vinyl and allyl. Suitable aryl groups include phenyl and tolyl. Suitable aralkyl groups include 2-phenylethyl and 2-methyl-2-phenylethyl. Suitable haloalkyl groups include 3,3,3-trifluoropropyl, 2-(nonafluorobutyl)ethyl and 2-(heptadecafluorooctyl)ethyl. Preferred R 1 It is methyl or phenyl.

[0048] Processes for preparing terminal-capped organopolysiloxanes have long been known to those skilled in the art and proceed, for example, from dichloromethylsilane in the presence of water to give linear terminal-capped polymethylpolysiloxanes.

[0049] These organopolysiloxanes (T) have a dynamic viscosity of between 35 and 1 000 000 mPas, preferably between 50 and 100 000 mPas, at 25° C. They have long been known in the prior art and are generally referred to as silicone oils.

[0050] In order to adjust the stability of the non-crosslinkable silicone composition (S) under load or the rheology, so-called rheology additives (E) (=structure formers) can be added. These are known to the person skilled in the art from the prior art.

[0051] Suitable rheological additives (E) are solid finely divided inorganic fillers. Suitable examples are reinforcing and non-reinforcing fillers, such as metal oxides or furnace black and acetylene black.

[0052] Suitable reinforcing fillers (E) (ie, having at least 50 m 2 Examples of fillers having a BET surface area of ​​greater than 50 m / g are fillers having a BET surface area of ​​greater than 50 m / g. 2 / g BET surface area of ​​fumed silica, precipitated silica or mixed silica-aluminum oxide. The fillers mentioned may have been hydrophobized, for example by treatment with organosilanes, -silazanes or -siloxanes, or by etherification of hydroxyl groups to alkoxy groups. As a result of the surface treatment, this silica has a carbon content of at least 0.01% by weight and at most 20% by weight, preferably between 0.1% by weight and 10% by weight, more preferably between 0.5% by weight and 6% by weight.

[0053] Suitable non-reinforcing fillers (E) (ie, having a diameter of less than 50 m 2Examples of fillers with a BET surface area of ​​20 m / g are powders of quartz, cristobalite, diatomaceous earth, calcium silicate, zirconium silicate, montmorillonite (such as bentonite), zeolites including molecular sieves (such as sodium aluminum silicate), metal oxides (such as aluminum oxide or zinc oxide or mixed oxides thereof), metal hydroxides (such as aluminum hydroxide), barium sulfate, calcium carbonate, gypsum, silicon nitride, silicon carbide, boron nitride, glass powder, carbon powder and polymer powder, as well as hollow glass and plastic beads. The BET surface area of ​​non-reinforcing fillers is preferably less than 20 m 2 / g.

[0054] Also suitable as rheological additives (E) are crosslinked hydrosilylation reaction products obtainable by reaction of:

[0055] - at least one alkenyl-terminated polydiorganosiloxane having a degree of polymerization of at least 300, and

[0056] - at least one organohydrogensiloxane crosslinking agent having an average of 2 or more SiH groups per molecule,

[0057] The ratio of the alkenyl-terminated polydiorganosiloxane to the organohydrogensiloxane is adjusted so that the molar ratio of SiH groups to alkenyl groups is in the range of 0.5 to 2.0.

[0058] The crosslinking of rheological additives (E) of this type is known to the person skilled in the art from the prior art and can be carried out before addition to the abovementioned non-crosslinkable silicone composition (S), or the structure formers are crosslinked in situ in the abovementioned non-crosslinkable silicone composition (S).

[0059] Also suitable as rheological additives (E) are non-particulate organic rheological additives, or those based on organic polymers. These are commercially available. BASF sells such rheological additives under the following trade names: and Other suitable rheological additives are available from CRODA as Atlox Rheostrux TM 100 (a polyester block copolymer) or Atlox Rheostrux TM 200 (a polyamide) is sold under the trade name PTFE.

[0060] One type of rheological additive (E) may be used, or a mixture of at least two rheological additives.

[0061] If rheological additives (E) are present, they are preferably present in an amount of 1 to 9% by weight, preferably 2 to 8% by weight, based on the total mass of the silicone composition (S).

[0062] The non-crosslinkable silicone composition (S) according to the invention may contain alkyltrialkoxysilanes (F) as further additives to reduce their viscosity. If they are present, they are preferably present in an amount of 0.1-8% by weight, preferably 0.2-6% by weight, based on the total mass of the silicone composition (S), wherein the alkyl group may be a saturated or unsaturated, linear or branched alkyl group having 2-20, preferably 8-18 carbon atoms, and the alkoxy group may have 1-5 carbon atoms. Examples of alkoxy groups include methoxy, ethoxy, propoxy and butoxy, particularly preferably methoxy and ethoxy. Particularly preferred for (F) are n-octyltrimethoxysilane, n-dodecyltrimethoxysilane, n-hexadecyltrimethoxysilane and n-octadecyltrimethoxysilane.

[0063] The non-crosslinkable silicone composition (S) according to the present invention may optionally contain other components (G). These optional additives are resinous polyorganosiloxanes, fungicides, fragrances, corrosion inhibitors, oxidation inhibitors, light stabilizers, flame retardants and compositions for influencing electrical properties, dispersing aids, solvents, pigments, dyes, organic polymers, heat stabilizers, etc.

[0064] Thermally conductive filler (Z)

[0065] The non-crosslinkable thermally conductive silicone composition (Y) according to the invention contains at least one thermally conductive filler (Z) having a thermal conductivity of at least 5 W / mK, provided that the non-crosslinkable thermally conductive silicone composition (Y) according to the invention contains at least 20% by volume of metal silicon particles as thermally conductive filler (Z), which metal silicon particles must still at least meet the further specific features a) to c) and, in a preferred embodiment, also d), the total amount of thermally conductive filler (Z) being at least 50% by volume.

[0066] a) The median diameter x50 of the metallic silicon particles (Z) according to the present invention is in the range of 30-200 μm, preferably in the range of 40-180 μm, more preferably in the range of 50-160 μm.

[0067] b) The metallic silicon particles (Z) according to the invention are predominantly round and are preferably produced by a melt process. The predominantly round shape of the particles according to the invention is characterized by a width / length ratio (aspect ratio w / l) of at least 0.76, preferably at least 0.77, more preferably at least 0.78, in particular at least 0.79.

[0068] The silicon particles (Z) according to the invention preferably have a sphericity value SPHT of at least 0.75, preferably at least 0.76, more preferably at least 0.78 and particularly preferably at least 0.79.

[0069] In a particularly preferred embodiment, the silicon particles (Z) according to the invention have an aspect ratio of at least 0.76 and at the same time a sphericity value SPHT of at least 0.75, preferably at least 0.76, more preferably at least 0.78 and particularly preferably at least 0.79.

[0070] c) The distribution range of particle size (SPAN) is defined as SPAN=(x90-x10) / x50. The SPAN of the metal silicon particles (Z) according to the present invention is at least 0.28, preferably at least 0.30, more preferably at least 0.35, and particularly preferably at least 0.38. In a preferred embodiment, SPAN is between 0.40 and 2.5, preferably between 0.41 and 2.2, and in particular between 0.5 and 2.0.

[0071] It is unimportant here whether a single fraction of silicon particles (Z) with a SPAN within the scope of the invention is used, or whether two or more fractions of silicon particles are mixed and thus the particle size distribution range according to the invention of feature c) of the silicon particles (Z) according to the invention is achieved. If two or more fractions of silicon particles are mixed, this can precede mixing with one or more components of the composition according to the invention, or the silicon particle fractions can also be mixed separately from one another with one or more components of the composition according to the invention. The order of addition here is immaterial.

[0072] Preferably, no more than four fractions of silicon particles are mixed to achieve the distribution range according to the present invention, preferably, no more than three fractions of silicon particles are mixed to achieve the distribution range according to the present invention, more preferably, no more than two fractions of silicon particles according to the present invention are used to achieve the distribution range according to the present invention, and particularly preferably, only a single silicon powder according to the present invention is used.

[0073] d) In a preferred embodiment, the silicon particles (Z) according to the invention contain not more than 1.5% by weight, preferably not more than 1% by weight, more preferably not more than 0.5% by weight, of silicon particles smaller than 2 μm, based in each case on the total amount of silicon particles (Z). Particularly preferred silicon particles (Z) are substantially free of particle fractions smaller than 2 μm. "Substantially free" means that the presence of such particles is tolerable within the scope of "impurities" in the particles (Z) according to the invention and does not affect their inventive effect.

[0074] The silicon particles (Z) according to the invention preferably contain less than 20% by weight, more preferably less than 15% by weight, particularly preferably less than 10% by weight, of a particle fraction having a diameter of not more than 20 μm, based in each case on the total amount of silicon particles.

[0075] The inventive silicon particles (Z) contain preferably less than 15% by weight, more preferably less than 10% by weight, particularly preferably less than 5% by weight, of a particle fraction having a diameter of not more than 10 μm, based in each case on the total amount of silicon particles.

[0076] In a particularly preferred embodiment, no silicon particles having an average diameter of not more than 10 μm are intentionally added. Preferably, no silicon particles not larger than 15 μm are added. Particularly preferably, no silicon particles having an average diameter of not more than 20 μm are intentionally added.

[0077] A disadvantage of very fine silicon particles or ground silicon particles is also that such particles have a relatively large surface area and bind very large amounts of polymer. This increases the viscosity of the silicone composition very significantly, so that only mixtures with relatively low filler levels and therefore low thermal conductivity can be produced. In the case of higher filler levels, the composition becomes very hard and can no longer be handled by conventional methods (e.g. dispensers). It has also been found that silicone compositions containing ground silicon particles are relatively highly flammable.

[0078] Metallic silicon has a number of very advantageous properties for use as a thermally conductive filler (Z). For example, the exceptionally high thermal conductivity of the silicon particles (Z) increases the thermal conductivity of the thermally conductive silicone composition (Y) produced therefrom. The low density of the silicon particles (Z) reduces the weight of the composition and the parts produced therefrom and contributes to cost savings. Low electrical conductivity enables the production of electrically insulating parts and improves resistance to electrical breakdown. The low Mohs hardness of the silicon particles (Z) reduces wear during processing. It will be clear to those skilled in the art that the advantages mentioned are completely or partially lost as the purity of the silicon decreases. The purity of the silicon particles (Z) according to the present invention and therefore the silicon content is at least 80%, preferably at least 90%, more preferably at least 95%.

[0079] It is also clear to the skilled person that metallic silicon particles are combustible under certain conditions and that dust presents an explosion risk. It is also known to the skilled person that as the particle size decreases, the risk of dust formation, flammability and explosion risk associated with metal powders increase significantly. For this reason, very small silicon particles below 30 μm are not suitable for many applications. Due to the low minimum ignition energy, such particles are dangerous to handle and require complex and expensive safety precautions in industrial processing. It has also been found that compositions containing very small silicon particles below 30 μm are relatively highly flammable.

[0080] Larger silicon particles with an average particle size in excess of 30 μm have a relatively high minimum ignition energy and are therefore safer and easier to process in industrial processes. However, compositions containing non-inventive ground angular silicon particles larger than 30 μm were found to be relatively highly flammable.

[0081] Silicon particles having an average particle size exceeding 200 μm are not suitable for use in many thermally conductive silicone composition applications because such large silicon particles are often unsuitable for fine gaps that must be filled, for example, with gap fillers. In addition, such large silicon particles have been found to exhibit relatively high flammability.

[0082] The use of spherical fillers to improve the flow and processability of filled polymers is well known in the prior art. However, there are only a few prior art documents for the use of spherical silicon particles in thermally conductive silicone compositions. The compositions disclosed contain only very small spherical silicon particles with an average particle size of less than 25 μm, the disadvantages of which have been described.

[0083] It has been found that, completely unexpectedly, the non-crosslinkable thermally conductive silicone compositions (Y) according to the invention are thermally conductive and at the same time have low flammability when they contain the required minimum amount of metallic silicon particles according to the invention which simultaneously meet features a) to c).

[0084] The non-crosslinkable silicone composition (Y) according to the invention contains at least 20% by volume, preferably at least 25% by volume, more preferably at least 30% by volume, and particularly preferably at least 35% by volume of such metal silicon particles (Z). If the silicone composition (Y) contains a smaller amount of metal silicon particles (Z), the desired advantageous effects of metal silicon, such as low density and high thermal conductivity, are no longer sufficiently provided.

[0085] The prior art includes various methods for producing finely divided metal particles with a rounded shape. The silicon particles (Z) according to the present invention are preferably produced from a molten state, as a result of which they have a relatively smooth surface and are substantially free of cracks, sharp edges and sharp corners. In this way, they are different from conventional abrasive particles that have been converted into a final form, for example, by means of crushing, grinding or milling. Here, it is unimportant whether these particles are cold crushed (e.g., by grinding) in a first method step and then converted into a molten form by heating to a temperature above the melting point (e.g., by heat treatment in a hot zone, for example, by means of plasma), or whether a silicon melt is first produced and then crushed (e.g., by atomization). The silicon particles according to the present invention are preferably converted into a solid form according to the present invention by spraying or atomizing a silicon melt, followed by cooling.

[0086] Suitable methods for producing the silicon particles (Z) according to the invention are known to the person skilled in the art and are described, for example, in Chapter 2.2 of "Pulvermetallurgie: Technologien and Werkstoffe [Powder Metallurgy: Technologies and Materials], Schatt, Werner, Wieters, Klaus-Peter, Kieback, Bernd, p. 5-48, ISBN 978-3-540-681112-0, E-Book: https: / / doi.org / 10.1007 / 978-3-540-68112-0_2". Preferred methods for producing the silicon particles (Z) according to the invention are inert gas atomization (also called gas atomization), pressurized water atomization (also called liquid atomization or water atomization method) or melt spinning (also called centrifugal atomization or rotary atomization).

[0087] The method described allows the production of metallic silicon particles in a very different particle size range, in particular in an average particle size range from a few micrometers to a few millimeters. It is also possible to produce metallic silicon particles in very different particle forms (e.g. "sputtered", i.e. very irregularly, ellipsoidally or spherically) and in a very variable particle size distribution range. Completely unexpectedly, it has been found that the advantageous properties according to the invention, in particular the relatively low flammability, are exhibited only by those silicon particles which are predominantly round and which simultaneously meet features a) to c) of the invention.

[0088] The method for producing the metallic silicon particles (Z) according to the invention should preferably be carried out in such a way that the particles are obtained in their predominantly round form according to the invention and therefore satisfy features a) to c) and are substantially free of sputtered, nodular, angular or sharp particles. The solidified particles can be separated by size in subsequent method steps by standard methods (e.g. by means of sieving classification or by means of sieving). In these methods, agglomerates and bonded particles can be separated, but substantially no particles are destroyed. "Predominantly round" and "substantially free" mean that the presence of such particles is tolerable within the range of impurities in the particles (Z) according to the invention and does not destroy their inventive effect.

[0089] In addition to these metal silicon particles (Z), the non-crosslinkable silicone composition (Y) according to the present invention may contain additional thermally conductive fillers (Z) having a thermal conductivity greater than 5 W / mK. Examples of such additional thermally conductive fillers (Z) are magnesium oxide, metal aluminum powder, metal silver powder, zinc oxide, boron nitride, silicon carbide, aluminum nitride, aluminum hydroxide, aluminum oxide, graphite, etc. Preferred additional fillers are aluminum powder, magnesium oxide, aluminum hydroxide, zinc oxide and aluminum oxide. Particularly preferred fillers are aluminum hydroxide and aluminum oxide, of which aluminum hydroxide is particularly preferred. The shape of the additional filler is substantially unrestricted. The particles may have, for example, a spherical, elliptical, needle-shaped, tubular, flaky, fibrous or irregular shape. They preferably have a spherical, ellipsoidal or irregular shape. The average diameter of the additional thermally conductive filler (Z) is preferably in the range of 0.01-200 μm, preferably in the range of 0.1-150 μm, more preferably in the range of 0.2-120 μm, especially in the range of 0.4-80 μm.

[0090] Fillers with very high density are disadvantageous for use in, for example, aircraft and electric vehicles, since they increase the weight of the component very significantly. The additional thermally conductive filler (Z) preferably has a density of not more than 6.0 g / cm 3 , preferably not more than 4.5g / cm 3 , more preferably not more than 3.0g / cm 3 density.

[0091] The non-crosslinkable silicone composition (Y) of the present invention preferably contains not more than 24% by weight, preferably not more than 20% by weight, more preferably not more than 16% by weight, and particularly preferably not more than 12% by weight of polyols having a molecular weight of more than 5.0 g / cm 3 In a particularly preferred embodiment, the non-crosslinkable silicone composition (Y) according to the invention does not contain any thermally conductive filler (Z) having a density of more than 5.0 g / cm 3 An additional thermally conductive filler (Z) of density.

[0092] Preferably, the non-crosslinkable silicone composition (Y) of the present invention contains not more than 60% by weight, preferably not more than 45% by weight, more preferably not more than 30% by weight, and particularly preferably not more than 20% by weight of polyols having a molecular weight of more than 3.0 g / cm 3 An additional thermally conductive filler (Z) of density.

[0093] In many applications, the electrical conductivity of the thermally conductive composition is undesirable since this could lead to short circuits, for example. The composition (Y) according to the invention preferably comprises only thermally conductive compositions having a specific electrical resistivity of at least 1 Ω·mm 2 / m of thermal conductive filler (Z).

[0094] The preferred non-crosslinkable thermally conductive silicone composition (Y) according to the invention contains the metal silicon particles according to the invention as the thermally conductive filler (Z) in the form of the only thermally conductive filler (Z) or in combination with up to three further thermally conductive fillers (Z). Impurities of up to 5% are not considered as further fillers (Z).

[0095] If the preferred composition according to the invention contains the metal silicon particles (Z) according to the invention in the form of the only thermally conductive filler (Z) having a thermal conductivity of more than 5 W / mK, a rheology modifier or thickener is preferably added to prevent sedimentation of the filler. Suitable rheology modifiers are known to those skilled in the art, preferably fumed silica.

[0096] The total amount of thermally conductive filler (Z) in the non-crosslinkable thermally conductive silicone composition (Y) according to the present invention is 50-95% by volume, preferably 60-90% by volume, more preferably 65-88% by volume. If the silicone composition (Y) contains a smaller amount of thermally conductive filler (Z), the thermal conductivity will be insufficient; if the silicone composition (Y) contains a larger amount of thermally conductive filler (Z), the composition (Y) will be difficult to process because it will have a high viscosity or even be brittle.

[0097] The non-crosslinkable thermally conductive silicone composition (Y) according to the invention has a thermal conductivity of at least 0.6 W / mK, preferably at least 0.8 W / mK, more preferably at least 1.2 W / mK, in particular at least 1.5 W / mK.

[0098] The viscosity of the non-crosslinkable thermally conductive silicone composition (Y) according to the present invention can be varied within a very wide range and matched to the requirements of the application. The viscosity of the non-crosslinkable thermally conductive silicone composition (Y) according to the present invention is preferably adjusted by standard methods in the art via the content of the thermally conductive filler (Z) and / or the composition of the silicone composition (Z). These are known to those skilled in the art. The viscosity is preferably adjusted via the selection and combination of components (T) and (Z) and the optional addition of (E) and / or (F).

[0099] In each case at a shear rate of D = 10 s -1 The dynamic viscosity of the non-crosslinkable thermally conductive silicone composition (Y) according to the present invention at 25° C. is preferably in the range of 100-1 000 000 mPa·s, preferably in the range of 1000-750 000 mPa·s, more preferably in the range of 2000-500 000 mPa·s, in particular not more than 250 000 mPa·s.

[0100] The density of the non-crosslinkable thermally conductive silicone composition (Y) according to the present invention is less than 4.5 g / cm 3 , preferably less than 4.0g / cm 3, more preferably less than 3.5g / cm 3 , especially less than 3.3g / cm 3 .

[0101] The present invention further provides a process for producing the non-crosslinkable thermally conductive silicone composition (Y) according to the invention by mixing the components.

[0102] The components can be mixed by conventional continuous and batch prior art methods. Suitable mixing equipment is any known equipment. Examples of these are single-shaft or double-shaft continuous mixers, double-roll mills, Ross mixers, Hobart mixers, dental mixers, planetary mixers, kneaders and Henschel mixers or similar mixers. Preferably, they are mixed in a planetary mixer, kneader or continuous mixer. The non-crosslinkable silicone composition (Y) can optionally be heated during mixing, preferably in a temperature range of 15-140° C., preferably in a range of 15-60° C. The procedure for producing the preferred non-crosslinkable silicone composition (Y) is also known to those skilled in the art. In principle, the components can be added in any order. For example, component e) and optional g) can be premixed and then mixed with component a) and / or b). The mixture can also be optionally heated here. Preferably, at least a portion of a) and alkoxysilane g) are mixed and then mixed in the thermally conductive filler (Z). Production is preferably carried out without active heating.

[0103] The non-crosslinkable silicone composition (Y) according to the invention has very good processing properties with regard to flowability, gap-filling properties and layer thickness control and can be applied precisely.

[0104] The present invention further provides a non-crosslinkable thermally conductive silicone composition (Y) as a heat dissipation paste for dissipating heat from a heat generator in an electronic device. The non-crosslinkable thermally conductive silicone composition (Y) is applied to a heat generator or a heat sink, or is coated with it. Heat generators are encountered in electronic devices and electronic devices of power supplies, such as power transistors, power modules, transistors, thermocouples and temperature sensors; heat generating electronic components, such as components of integrated circuits such as CPUs and batteries. Suitable heat sinks include heat dissipation components, such as heat distributors, heat sinks and cooling sheet layers. If the non-crosslinkable thermally conductive silicone composition (Y) is introduced between the heat generator and the heat sink, heat can be effectively directed from the heat generator to the heat sink. This achieves an effective cooling effect on the heat generator.

[0105] Test Method

[0106] Measurement of thermal conductivity λ

[0107] Thermal conductivity was measured according to ASTM D5470-12 using a TIM tester (Steinbeis Transferzentrum in der Elektronik,Lindenstr.13 / 1,72141 Germany). This determines the thermal resistance of the sample between two test cylinders with the aid of a constant heat flow. The layer thickness of the sample is used to calculate the effective thermal conductivity.

[0108] For the measurement, the sample is applied with the aid of a stencil and the measuring cylinder is narrowed manually to a thickness of 1.9-2.0 mm, then excess material is removed. The thermal conductivity is measured at a constant gap of 1.8-1.6-1.4-1.2-1.0 mm. The evaluation is carried out with the aid of a comprehensive report of the material position. After a reasonableness test (linear determination coefficient> 0.998), the thermal conductivity λ is reported as an effective thermal conductivity in W / (m*K).

[0109] Measurement of dynamic viscosity

[0110] The dynamic viscosity was measured with an Anton Paar MCR 302 rheometer according to DIN EN ISO 3219:1994 and DIN 53019 using a flow curve with the following parameters: Measurement type: T / D; Temperature: 25.0°C; Measuring element: PP25; Measuring gap: 0.50 mm; Shear rate: 0.1-10 s -1 ; Time: 120 sec; Measurements: 30. Viscosity reported in Pa·s is at shear rate D = 10 s -1 The interpolated value below.

[0111] Density measurement

[0112] The density of the uncrosslinked thermally conductive silicone composition is determined according to ISO 1183, and the density of the crosslinked thermally conductive silicone composition is determined according to ISO 1184.

[0113] Particle size and shape analysis

[0114] The particle size (median diameter x50), particle size distribution (parameters: standard deviation σ and distribution range SPAN) and particle shape (parameters: aspect ratio w / l and sphericity SPHT) were analyzed using a Camsizer X2 from Retsch Technology (measuring principle: dynamic image analysis) according to ISO 13322-2 and ISO 9276-6 (analytical method: dry test of powders and granules; measuring range: 0.8 μm-30 mm; compressed air dispersion with "X-Jet"; dispersion pressure = 0.3 bar). The evaluation is volume-based and is determined by x cmin Model.

[0115] The following examples illustrate the basic feasibility of the invention without limiting it to what is disclosed therein.

[0116] In the following examples, unless otherwise stated, all figures for parts and percentages are based on weight. Unless otherwise stated, the following examples are carried out at ambient atmospheric pressure (i.e., about 1000 hPa) and room temperature (i.e., about 20° C.), or at a temperature established in conjunction with the reactants at room temperature without additional heating or cooling. DETAILED DESCRIPTION

[0117] Example

[0118] Overview of the silicon powders and silicon powder mixtures used according to the invention and not according to the invention

[0119] Table 1 summarizes the properties of the silicon powders according to the invention and not according to the invention used in the examples.

[0120] Inventive Examples 1 to 3 used inventive silicon powder which was obtained by means of inert gas atomization and was therefore predominantly round and additionally had a relatively broad particle size distribution according to the invention.

[0121] Non-inventive comparative examples V1-V2 used non-inventive silicon powder which was obtained by means of inert gas atomization and was therefore predominantly round, but had a relatively narrow, non-inventive particle size distribution and did not satisfy feature c) of the invention.

[0122] Non-inventive comparative examples V3 to V5 use non-inventive silicon powders which have a relatively broad particle size distribution but were obtained by means of a grinding process and are therefore essentially angular, have sharp edges and do not satisfy feature b) of the invention. Comparative example V5 has a content of silicon particles smaller than 2 μm of 3.8% by weight and therefore additionally does not satisfy feature d).

[0123] Example 4: Production of Silicon Powder Mixture 4 (Present Invention)

[0124] 100 g of a non-inventive silicon powder having an x50 of 68.6 μm, a SPAN of 0.20, a w / l of 0.85 and a SPHT of 0.84, 200 g of a non-inventive silicon powder from comparative example V2, 400 g of a non-inventive silicon powder having an x50 of 105.4 μm, a SPAN of 0.24, a w / l of 0.83 and a SPHT of 0.92, 200 g of a non-inventive silicon powder having an x50 of 133.8 μm, a SPAN of 0.25, a w / l of 0.82 and a SPHT of 0.94, and 100 g of a non-inventive silicon powder having an x50 of 162.1 μm, a SPAN of 0.22, a w / l of 0.82 and a SPHT of 0.94 were stirred with a commercial RW28 laboratory stirrer system ( The obtained silicon powder mixture has an x50 of 107.8 μm, a SPAN of 0.75, a w / l of 0.83 and a SPHT of 0.91 and satisfies the features a) to c) and even d) of the present invention.

[0125] abbreviation

[0126] Ex. Example

[0127] V Comparative ratio

[0128] PS particle shape

[0129] r Main round

[0130] e has corners

[0131] n Nodular

[0132] I. The present invention

[0133] NI Not Invention

[0134] nd Not determined

[0135] Table 1: Overview of the silica powders used

[0136]

[0137]

[0138] *Within the measurement accuracy, the content of silicon particles < 2 μm is 0.0 wt. %.

[0139] **The content of silicon particles <2 μm is 3.8% by weight.

[0140] General Method 1 (GM1) for the Production of Non-Crosslinkable, Thermally Conductive, Silicone Powder-Containing Silicone Compositions (Examples 5 to 8 of the Invention and Examples V6 to V12 Not of the Invention)

[0141] Step 1: Preparation of a non-crosslinkable, thermally conductive silicone composition containing silicon powder

[0142] 40.8 g of trimethylsiloxy-terminated polydimethylsiloxane having a viscosity of 1000 mPa·s and 5.18 g of trimethylsiloxy-terminated polydimethylsiloxane having a viscosity of 200 mPa·s and a content of Si-bonded hydrogen of 0.18 wt. % were homogenized by means of a SpeedMixer DAC 400 FVZ (Hauschild & Co KG, Waterkamp 1, 59075 Hamm, Germany) at 2350 rpm for 25 seconds.

[0143] Thereafter, silicon powder was added in each case in a ratio according to Table 2 or according to Table 3 and mixed for 25 seconds at 2350 rpm by means of a SpeedMixer. The silicone composition containing silicon particles was stirred with a spatula to mix in silicon powder residues from the edge of the container. This was followed by homogenization by SpeedMixer at 2350 rpm for another 25 seconds and cooling to room temperature.

[0144] A paste-like mass was obtained.

[0145] Example 9 Combustibility Test

[0146] The flammability of the non-crosslinkable silicone composition according to the invention according to Example 5 and the non-inventive silicone compositions according to Comparative Examples V6 to V8 were tested in a simplified test based on UL 94 HB.

[0147] The non-crosslinkable silicone composition of the present invention according to Example 5 and the non-inventive silicone composition according to Comparative Examples V6 to V8 are applied to an aluminum plate of 150 mm length, 10 mm width and 2 mm thickness in a layer of 2 mm thickness. The plate is fixed in a vertical position along the long side on the right side so that the aluminum backing faces backward and the sample coated with a scraper faces forward. The burner is adjusted to produce a blue flame of 325 mm length. The flame points to the front of the sample in a horizontal position at right angles to the test piece so that the tip of the blue flame points to the front of the test piece 20 mm from the left end of the test piece. After contact for 30 seconds, the flame is removed.

[0148] Flammability test and evaluation: During the flame application, observe the appearance of the flame and possible dripping of the burning sample material. Record the afterflame time (total afterburning and afterglow time) of the test piece. The sample should show a weak flame appearance during the flame application and should not emit burning drops. After the flame is removed, the sample should be extinguished immediately and show an afterburning or glow of less than 1 second. The test is carried out on 3 different test pieces, and the average value of the afterflame time is determined. The results are shown in Table 2.

[0149] In the non-inventive comparative experiment V7, which contained 62.5% by volume of non-inventive silicon particles according to comparative example V5, which more particularly did not meet feature b)), a very viscous silicone composition was formed which could not be applied and tested in a homogeneous layer.

[0150] Table 2: Composition and flammability of silicone compositions containing silicon powder

[0151]

[0152] In the test of flammability, it was found that Comparative Examples V6 and V8 containing non-inventive silicon powders according to Comparative Examples V1 or V5 which did not satisfy one or more of the characteristics a) to d) showed relatively unfavorable combustion properties.

[0153] Completely unexpectedly, it was found that the inventive silicon powder from Example 1 which simultaneously meets features a) to c) and even d) exhibits the inventive advantage of reduced flammability.

[0154] Example 10 Combustibility Test

[0155] The flammability of the inventive non-crosslinkable silicone compositions according to Examples 6 to 8 and the non-inventive silicone compositions according to Comparative Examples V9 to V12 was tested in a simplified test based on UL 94 HB. In contrast to Example 9, the plates were fixed in a horizontal position with the aluminum backing facing downwards and the knife-coated specimen facing upwards.

[0156] In the case of non-inventive comparative experiment V10, which contained 62.5% by volume of non-inventive silicon particles according to comparative example V3, which more particularly did not meet feature b)), the result was a very viscous silicone composition which could not be applied and tested in a homogeneous layer.

[0157] Flammability test and evaluation: During the flame application, observe the appearance of the flame and possible dripping of the burning sample material. Record the afterflame time (total afterburning and afterglow time) of the test piece. The sample should show a weak flame appearance during the flame application and should not emit burning drops. After the flame is removed, the sample should be extinguished immediately and show an afterburning or glow of less than 1 second. The test is carried out on 3 different test pieces and the average value of the afterflame time is determined. The results are shown in Table 3.

[0158] Table 3: Composition and flammability of silicone compositions containing silicon powder

[0159]

[0160]

[0161] It was found that the inventive non-crosslinkable silicone compositions according to Examples 6 to 8, which comprise the inventive silicon powders from Examples 2 to 4 which simultaneously satisfy features a) to c) and even d), exhibit the inventive advantage of reduced flammability.

[0162] Furthermore, in Example 8 of the invention, it was found, completely unexpectedly, that the mixing of a plurality of non-inventive silicon powders can produce the inventive silicon powder mixture according to Example 4 with the advantageous properties according to the invention of low flammability, provided that the resulting mixture satisfies features a) to c) and even d).

[0163] Example 11 Production of a non-crosslinkable thermally conductive silicone composition containing an in-situ mixture of silicon powder (present invention)

[0164] According to the general method GM1, the non-crosslinkable thermally conductive silicone composition of the present invention is produced by adding as silicon powder 18.4 g of a non-inventive silicon powder having an x50 of 68.6 μm, a SPAN of 0.20, a w / l of 0.85 and a SPHT of 0.84, 36.8 g of a non-inventive silicon powder from comparative example V2, 73.6 g of a non-inventive silicon powder having an x50 of 105.4 μm, a SPAN of 0.24, a w / l of 0.83 and a SPHT of 0.92, 36.8 g of a non-inventive silicon powder having an x50 of 133.8 μm, a SPAN of 0.25, a w / l of 0.82 and a SPHT of 0.94, and 18.4 g of a non-inventive silicon powder having an x50 of 162.1 μm, a SPAN of 0.22, a w / l of 0.82 and a SPHT of 0.94, respectively, and mixing them in situ to form the silicon powder mixture of the present invention.

[0165] The result was a non-crosslinkable silicone composition according to the invention having a content of 62.5% by weight of silicon particles according to the invention. The thermal conductivity was 1.9 W / mK and the density was 1.82 g / cm 3The paste-like substance according to the invention has good processability, high thermal conductivity and low density and is very suitable for use in electronic components.

[0166] The flammability test according to Example 10 gave a weak flame appearance, an afterflame time of less than 1 second and no burning debris.

Claims

1. A non-crosslinkable thermally conductive silicone composition (Y), comprising - 5 to 50% by volume of at least one non-crosslinkable silicone composition (S), and - 50 to 95% by volume of at least one thermally conductive filler (Z) having a thermal conductivity of at least 5 W / mK, with the proviso that The non-crosslinkable thermally conductive silicone composition (Y) has a thermal conductivity of at least 0.6 W / mK, and At least 20% by volume of metallic silicon particles present as thermally conductive filler (Z) meet the following characteristics: a) their median diameter x50 is in the range of 30-200 μm; b) they are predominantly circular and characterized by a width / length ratio (aspect ratio w / l) of at least 0.76; c) their distribution range SPAN ((x90-x10) / x50) is at least 0.

28.

2. The non-crosslinkable silicone composition (Y) according to claim 1, It is characterized in that The non-crosslinkable silicone composition (S) contains an organopolysiloxane (T) having the following properties: - they are linear, branched or cyclic, - terminated at both ends or terminated with Si-OH alone or terminated with alkoxy-silyl alone, -Si bonding side and terminal group R 1 are independently substituted or unsubstituted C1-C18 hydrocarbon groups.

3. The non-crosslinkable silicone composition (Y) according to claim 2, It is characterized in that The non-crosslinkable silicone composition (S) furthermore contains rheological additives (E) which serve to adjust its stability under load.

4. The non-crosslinkable silicone composition (Y) according to any one of claims 1 to 3, It is characterized in that It contains at least 25% by volume of metallic silicon particles as thermally conductive filler (Z).

5. The non-crosslinkable silicone composition (Y) according to any one of claims 1 to 4, It is characterized in that Besides the metallic silicon particles (Z), it comprises only one to three further thermally conductive fillers (Z).

6. The non-crosslinkable silicone composition (Y) according to any one of claims 1 to 5, It is characterized in that In addition to the metallic silicon particles (Z), it also contains not more than 24% by weight of a material having a density greater than 5.0 g / cm 3 of additional thermally conductive filler (Z).

7. The non-crosslinkable silicone composition (Y) according to any one of claims 1 to 6, It is characterized in that In addition to the metallic silicon particles (Z), it also contains not more than 60% by weight of a material having a density greater than 3.0 g / cm 3 of additional thermally conductive filler (Z).

8. The non-crosslinkable silicone composition (Y) according to any one of claims 1 to 7, It is characterized in that The metallic silicon particles (Z) have a sphericity value SPHT of at least 0.

75.

9. The non-crosslinkable silicone composition (Y) according to any one of claims 1 to 8, It is characterized in that The median diameter x50 of the metal silicon particles is in the range of 40-180 μm.

10. The non-crosslinkable silicone composition (Y) according to any one of claims 1 to 9, It is characterized in that The metallic silicon particles (Z) satisfy the following additional characteristics: d) They contain not more than 1.5% by weight of silicon particles smaller than 2 μm.

11. A process for producing the non-crosslinkable silicone composition (Y) of the invention according to any one of claims 1 to 9 by mixing the individual components. 12 . Use of the non-crosslinkable silicone composition (Y) according to claim 1 as a heat dissipation paste for dissipating heat from heat generators in electronic devices.

Citation Information

Patent Citations

  • Electromagnetic wave absorbing, heat conductive silicone rubber compositions

    US20010051673A1

  • Thermal interface material having spheroidal particulate filler

    US20060228542A1

  • Highly heat conductive silicone rubber composition

    US20070117920A1

  • Heat fixing roll and fixing belt

    US20070135555A1

  • Silicone rubber composition for thermally conductive silicone-rubber development member, and thermally conductive silicone-rubber development member

    US20160122611A1