Photosensitive resin composition, resin film having pattern, method for producing resin film having pattern, and semiconductor circuit board

By using a photosensitive resin composition with specific structural units and photopolymerization initiator on a semiconductor circuit substrate, a patterned resin film with high elongation and high pressure cooker test resistance is solved, the insulating film warping in temperature changes and pressure cooker tests is formed. The problem of deformation and insufficient resistance improves the reliability and performance of the circuit substrate.

CN119013625APending Publication Date: 2024-11-22JICC 02 LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202380033518.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-06-14
Filing Date
2023-04-10
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

The insulating film of the existing semiconductor circuit substrate is prone to warping and deforming when temperature changes, and it is difficult to maintain high reliability in the use environment of information terminal machines, especially in pressure cooker testing, which cannot meet elongation and resistance requirements.

Method used

A photosensitive resin composition containing a polymer with a specific structural unit and a photopolymerization initiator is used to form a patterned resin film through exposure and development techniques to improve the elongation of the resin film and the resistance to pressure cooker test.

Benefits of technology

The resin film with high elongation and high pressure cooker test resistance is achieved, and is suitable for the insulating film of semiconductor circuit substrates, improving the reliability and performance of the circuit substrate.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119013625A_ABST
    Figure CN119013625A_ABST
Patent Text Reader

Abstract

One embodiment of the present invention relates to a photosensitive resin composition, a resin film having a pattern, a method for producing a resin film having a pattern, and a semiconductor circuit board, the photosensitive resin composition containing: (A) a polymer; the polyimide polymer is at least one type selected from the group consisting of polyimides and polyimide precursors, contains a structural unit (a) having a structural unit derived from an acid anhydride represented by formula (1) and a structural unit (b) derived from a diamine, and has a maleimide group or the like at the terminal of the polymer. (B) a photopolymerization initiator; and (D) a solvent. (In formula (1), L represents a single bond or the like, R1-R3 represent a hydrogen atom or the like, or represent an alkylene group in which R1 and R2 (or R3) in the same ring are bonded to each other, n1-n2 represent an integer of 0-3, and Y1 represents a structure represented by formula (Y1) (-Ar1-) or the like. > # imgabs0 #
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] One embodiment of the present invention relates to a photosensitive resin composition, a resin film having a pattern, a method for producing a resin film having a pattern, and a semiconductor circuit board. Background Art

[0002] Various photosensitive resin compositions have been proposed as materials for forming surface protective films and interlayer insulating films used in semiconductor circuit boards among electronic components. For example, a photosensitive resin composition containing a resin having a phenolic hydroxyl group as an alkali-soluble resin has been studied (Patent Documents 1 and 2).

[0003] Prior art literature

[0004] Patent Literature

[0005] Patent Document 1: Japanese Patent Application Publication No. 2014-186300

[0006] Patent Document 2: Japanese Patent Application Publication No. 2013-210606 Summary of the invention

[0007] Problems to be solved by the invention

[0008] In order to increase the density or performance of semiconductor circuit substrates, packaging technology using silicon interposers and fan-out packaging technology using molded substrates have been proposed. However, in such substrate materials and insulating films, due to the difference in their thermal linear expansion coefficients, warping and deformation are sometimes easily caused by temperature changes in the manufacturing process of the semiconductor circuit substrate or the use environment of the information terminal device. In the case where the elongation of the insulating film is small, there is a problem that the insulating film cannot withstand the warping and deformation and is damaged. In addition, it is required to maintain high reliability of elongation in environmental load tests (for example, pressure cooker test (PCT) test) that assume the use environment of the information terminal device.

[0009] Furthermore, the insulating film used in the semiconductor circuit substrate is used between the electrode pads or wirings with fine pitches. Therefore, in the composition for forming the resin film such as the insulating film with pattern (hereinafter also referred to as "patterned resin film"), it is necessary to have photolithography properties that can be patterned by exposure and development.

[0010] The present invention is an invention for solving the above-mentioned problems, and its purpose is to: provide a photosensitive resin composition that can form a resin film with excellent elongation and high PCT resistance and excellent photolithography; provide a patterned resin film with excellent elongation and high PCT resistance and a method for manufacturing the same; and provide a semiconductor circuit substrate including a patterned resin film with excellent elongation and high PCT resistance.

[0011] Technical means of solving problems

[0012] The present inventors have conducted intensive research to solve the above problems. As a result, they have found that the above problems can be solved by a photosensitive resin composition containing a polymer having a specific structural unit and a specific photopolymerization initiator, thereby completing the present invention. The following is an example of the present invention. [1]

[0014] A photosensitive resin composition comprising:

[0015] (A) a polymer, which is at least one selected from the group consisting of polyimide and a polyimide precursor;

[0016] (B) a photopolymerization initiator; and

[0017] (D)solvent,

[0018] The polymer (A) comprises a structural unit (a) derived from an acid anhydride and a structural unit (b) derived from a diamine,

[0019] The structural unit (a) includes a structural unit (a1) derived from an acid anhydride represented by the following formula (1):

[0020] The polymer (A) has a group represented by the following formula (eg1) or formula (eg2), or a maleimide group, at at least one of a side chain terminal and a main chain terminal.

[0021] [Chemistry 1]

[0022]

[0023] [In the above formula (1),

[0024] L independently represents a single bond, an ester bond, or an amide bond,

[0025] R 1 , R 2 and R 3 Each independently represents a hydrogen atom, an alkyl group having 1 to 6 carbon atoms, or represents R 1 With R 2 or R 1 With R 3an alkylene group having 1 to 4 carbon atoms bonded to each other,

[0026] n 1 and n 2 Each independently represents an integer from 0 to 3 (wherein, within the same ring, n 1 With n 2 is an integer greater than 1),

[0027] Y 1 represents a structure represented by the following formula (Y1) or formula (Y2);

[0028] *-Ar 1 -*…(Y1)

[0029] *-Ar 2 -Y 2 -Ar 2 -*…(Y2)

[0030] In the above formula (Y1) and formula (Y2), * represents a bond with respect to L in the above formula (1),

[0031] Ar 1 and Ar 2 Each independently represents a group formed by removing two hydrogen atoms from an unsubstituted aromatic ring or an aromatic ring substituted with an alkyl or alkoxy group having 1 to 6 carbon atoms,

[0032] Y in the formula (Y2) 2 is a single bond, an oxygen atom, a sulfur atom, at least one group selected from the group consisting of a sulfonyl group, a carbonyl group, a methylene group, a dimethylmethylene group, and a bis(trifluoromethyl)methylene group]

[0033] [Chemistry 2]

[0034]

[0035] [In the above formula (eg1) and formula (eg2),

[0036] L eg1 and L eg2 Each independently represents an alkanediyl group having 1 to 5 carbon atoms, an aromatic hydrocarbon group having 6 to 10 carbon atoms, or a group in which two or more groups selected from these are linked via a single bond, -O-, -S-, -SO2-, -NH-, -NH-C(O)-, -C(O)-, or -C(O)O-,

[0037] R eg1 and R eg2 each independently represents a vinyl group or a (meth)acryloyl group,

[0038] *Indicates the bonding site with the polymer chain〕 [2]

[0040] The photosensitive resin composition according to [1] further contains (C) a photopolymerizable compound. [3]

[0042] The photosensitive resin composition according to [1] or [2], wherein the polymer (A) has a group represented by the formula (eg1) or (eg2) or a maleimide group at at least one of the main chain terminals. [4]

[0044] The photosensitive resin composition according to any one of [1] to [3], wherein the polymer (A) is a linear polymer having no branched structure. [5]

[0046] The photosensitive resin composition according to any one of [1] to [4], wherein the polymer (A) has a group represented by the following formula (eg1-1) to (eg1-3), formula (eg2-1), or formula (eg3-1) at at least one of the main chain terminals.

[0047] [Chemistry 3]

[0048]

[0049] (In the formula,

[0050] L eg1 , R eg1 , L eg2 , and R eg2 The same symbols as in the formula (eg1) and the formula (eg2) have the same meanings,

[0051] R eg3 R independently represents a hydrogen atom, an alkyl group having 1 to 5 carbon atoms, eg3 Can bond to each other to form a ring,

[0052] *Indicates the bonding site with the polymer chain) [6]

[0054] A method for producing a resin film having a pattern, comprising: a step (1) of forming a coating film of the photosensitive resin composition according to any one of [1] to [5] on a substrate; a step (2) of selectively exposing the coating film; and a step (3) of developing the exposed coating film using a developer containing an organic solvent. [7]

[0056] A resin film having a pattern is obtained by curing the photosensitive resin composition according to any one of [1] to [5]. [8]

[0058] A semiconductor circuit substrate includes the resin film having a pattern according to [7].

[0059] Effects of the Invention

[0060] According to one embodiment of the present invention, there can be provided a photosensitive resin composition capable of forming a resin film having excellent elongation and high PCT resistance and having excellent photolithography properties, and further a patterned resin film having excellent elongation and high PCT resistance and a method for manufacturing the same, and a semiconductor circuit substrate comprising a patterned resin film having excellent elongation and high PCT resistance. DETAILED DESCRIPTION

[0061] Hereinafter, the present invention will be described in detail including preferred embodiments thereof.

[0062] [Photosensitive resin composition]

[0063] The photosensitive resin composition of one embodiment of the present invention (hereinafter, also simply referred to as “the present composition”) contains:

[0064] (A) a polymer, which is at least one selected from the group consisting of polyimide and a polyimide precursor (hereinafter also referred to as “polymer (A)”);

[0065] (B) a photopolymerization initiator; and

[0066] (D) Solvent.

[0067] <Polymer (A)>

[0068] The polymer (A) contained in the present composition is a polymer (resin) selected from at least one of the groups consisting of polyimide and polyimide precursor, and contains a structural unit (a) derived from an acid anhydride and a structural unit (b) derived from a diamine, and has a specific group at least one of the side chain end and the main chain end. In particular, when the main chain end has the specific group, the molecular weight of the resin accompanying the cross-linking reaction increases, and an increase in elongation can be expected. Due to the presence of such a structure, the polymer (A) contained in the present composition can have both high i-ray transmittance and high elongation.

[0069] (Structural unit (a))

[0070] The structural unit (a) includes a structural unit (a1) derived from an acid anhydride represented by the following formula (1). It is believed that the acid anhydride group having an alicyclic structure in the structural unit (a1) contributes to the improvement of i-ray transmittance, solvent solubility, and PCT resistance, and the aromatic group contributes to the improvement of elongation. By including the structural unit (a1) in the polymer (A), the present composition has both high i-ray transmittance and high elongation. The structural unit (a1) may include one or more than two.

[0071] [Chemistry 4]

[0072]

[0073] In the formula (1), Y 1 It represents a structure represented by the following formula (Y1) or formula (Y2), and preferably a structure represented by the following formula (Y1). In the following formula, * represents a bond with respect to L in the above formula (1).

[0074] *-Ar 1 -*…(Y1)

[0075] *-Ar 2 -Y 2 -Ar 2 -*…(Y2)

[0076] In the formula (Y1) and the formula (Y2), Ar 1 and Ar 2 Each independently represents a group formed by removing two hydrogen atoms on an unsubstituted aromatic ring or an aromatic ring substituted with an alkyl or alkoxy group having 1 to 6 carbon atoms.

[0077] Examples of the aromatic ring include aromatic hydrocarbon compounds such as a benzene ring and a naphthalene ring, and heteroaromatic compounds such as a furan ring and a pyrrole ring. An aromatic hydrocarbon compound having 6 to 10 carbon atoms such as a benzene ring and a naphthalene ring is preferred.

[0078] Examples of the alkyl group having 1 to 6 carbon atoms include methyl, ethyl, n-propyl, isopropyl, n-butyl, n-pentyl, and n-hexyl. Examples of the alkoxy group having 1 to 6 carbon atoms include methoxy and ethoxy. Among these, alkyl groups having 1 or 2 carbon atoms, such as methyl and ethyl, or alkoxy groups having 1 or 2 carbon atoms, such as methoxy and ethoxy, are preferred.

[0079] In the formula (Y2), Y 2 It is a single bond, an oxygen atom, a sulfur atom, or at least one group selected from the group consisting of a sulfonyl group, a carbonyl group, a methylene group, a dimethylmethylene group, and a bis(trifluoromethyl)methylene group.

[0080] In the formula (1), L independently represents a single bond, an ester bond, or an amide bond, wherein the ester bond includes any bond represented by -OC(O)- or -C(O)-O-, and the amide bond includes any bond represented by -NH-C(O)- or -C(O)-NH-.

[0081] In the formula (1), R 1 , R 2 and R 3 Each independently represents a hydrogen atom, an alkyl group having 1 to 6 carbon atoms, or represents R 1 With R 2 or R 1 With R 3 An alkylene group having 1 to 4 carbon atoms formed by bonding to each other. Examples of the alkyl group having 1 to 6 carbon atoms include the same groups as those mentioned above, and a methyl group and an ethyl group are preferred.

[0082] In the formula (1), n 1 and n 2 Each independently represents an integer from 0 to 3, and is preferably 0 or 1. 1 With n 2 At least one of is an integer greater than 1.

[0083] The acid anhydride represented by the formula (1) is preferably 1 ~R 3 All hydrogen atoms, or one R in the same ring 1 With an R 2 , or an R 1 With an R 3 Specific preferred examples of the acid anhydride represented by the formula (1) include acid anhydrides represented by the following formulas (1-1) to (1-3), and more preferred examples include acid anhydrides represented by the following formulas (1-1) or (1-2).

[0084] [Chemistry 5]

[0085]

[0086] The structural unit (a) may include a structural unit (a2) derived from an acid anhydride other than the acid anhydride represented by the formula (1) within a range not impairing the effects of the present invention. The structural unit (a2) may include one or more types.

[0087] As the acid anhydride other than the acid anhydride represented by the above formula (1) (hereinafter also referred to as “other acid anhydride”), an acid anhydride represented by the following formula (2) is preferred.

[0088] [Chemistry 6]

[0089]

[0090] In the above formula (2), X can be, for example, a group represented by the following formula: In the following formula, * represents a bond to the carbon atom to which X in the above formula (2) is bonded.

[0091] [Chemistry 7]

[0092]

[0093] [Chemistry 8]

[0094]

[0095] The hydrogen atom (omitted in the formula) in the group represented by the above formula may be substituted by an alkyl group or alkoxy group having 1 to 6 carbon atoms, or a group in which the hydrogen atom in the alkyl group or alkoxy group is substituted by a halogen atom (for example, trifluoromethyl group).

[0096] When the polymer (A) contains the structural unit (a2), the molar ratio of the structural unit (a1) to the structural unit (a2) (structural unit (a1) / structural unit (a2)) is preferably 99 / 1 to 50 / 50, and more preferably 95 / 5 to 60 / 40. The content ratio of each structural unit can be calculated by 13 C-NMR ( 13 C-Nuclear Magnetic Resonance, 13 C-NMR). If the molar ratio of the structural unit (a1) to the structural unit (a2) is within the above range, the above effect brought about by using the structural unit (a1) can be easily obtained. In addition, a polymer in which the molar ratio of each monomer in the monomer mixture (anhydride, diamine described later, and any other monomer component except the terminal modifier described later) is within the above range can also be said to be a polymer in which the molar ratio of the structural unit derived from the monomer is within the above range.

[0097] (Structural unit (b))

[0098] The structural unit (b) is not particularly limited as long as it is a structural unit derived from a diamine, and may include either a structural unit derived from a diamine having a hydroxyl group or a structural unit derived from a diamine not having a hydroxyl group. The structural unit (b) may include one or more types.

[0099] Examples of the diamine having a hydroxyl group include diamines represented by the following formula (3).

[0100] [Chemistry 9]

[0101] H2N-Z 1 -NH2...(3)

[0102] In the formula (3), Z 1 represents a divalent group having a hydroxyl group, and specific examples thereof include the divalent groups having a hydroxyl group shown below. In the following formula, * represents Z in the formula (3) 1 The bond to the nitrogen atom.

[0103] [Chemistry 10]

[0104]

[0105] Examples of the diamine not having a hydroxyl group include p-phenylenediamine, m-phenylenediamine, 4,4'-diaminodiphenylmethane, 4,4'-diaminodiphenylethane, 4,4'-diaminodiphenyl sulfide, 4,4'-diaminodiphenyl sulfone, 3,3'-dimethyl-4,4'-diaminobiphenyl, 4,4'-diaminobenzanilide, 4,4'-diaminodiphenyl ether, 1,5-diaminonaphthalene, 2,2'-dimethyl-4,4'-diaminobiphenyl, 5-amino-1-(4'-aminophenyl)-1,3,3-trimethylindane, 6-amino-1-(4'-aminophenyl)-1,3,3-trimethylindane, 3,4'-diaminodiphenyl ether, 3,3'-diaminodiphenyl ether, and 2,2'-dimethyl-4,4'-diaminobiphenyl. diaminobenzophenone, 3,4'-diaminobenzophenone, 4,4'-diaminobenzophenone, 1,3-bis(4-aminophenoxy)propane, 1,4-bis(4-aminophenoxy)butane, 1,5-bis(4-aminophenoxy)pentane, 1,6-bis(4-aminophenoxy)hexane, 2,2-bis[4-(4-aminophenoxy)phenyl]propane, 2,2-bis[4-(4-aminophenoxy)phenyl]hexafluoropropane, 2,2-bis(4-aminophenyl)hexafluoropropane, bis[4-(4-aminophenoxy)phenyl]sulfone, 1,4-bis(4-aminophenoxy)benzene, 1,3-bis(4-aminophenoxy)benzene, 1,3-bis(3-aminophenoxy)benzene, 9,9-bis(4-aminophenyl)-10-hydroanthracene, 2,7-diaminofluorene, 9,9-bis(4-aminophenyl)fluorene, 4,4'-methylene-bis(2-chloroaniline), 2,2',5,5'-tetrachloro-4,4'-diaminobiphenyl, 2,2'-dichloro-4,4'-diamino-5,5'-dimethoxybiphenyl, 3,3'-dimethoxy-4,4'-diaminobiphenyl, 1,4,4'-(p-phenyleneisopropylidene)dianiline, 4,4'-(m-phenyleneisopropylidene)dianiline, 2,2'-bis[4-(4-amino-2-trifluoromethylphenoxy)phenyl]hexafluoropropane, 4,4'-bis(4-aminophenoxy)biphenyl, 4,4'-diamino Aromatic diamines such as 2,2'-bis(trifluoromethyl)biphenyl, 4,4'-bis[(4-amino-2-trifluoromethyl)phenoxy]-octafluorobiphenyl; m-phenylenediamine, p-phenylenediamine, 1,3-propylenediamine, tetramethylenediamine, pentamethylenediamine, hexamethylenediamine, heptamethylenediamine, octamethylenediamine, nonamethylenediamine, decamethylenediamine, dodecamethylenediamine, 4,4'-diaminoheptamethylenediamine, 1,4-diaminocyclohexane, 1,3-bis(aminomethyl)cyclohexane, 1,4-bis(aminomethyl)cyclohexane, isophoronediamine, tetrahydrodicyclopentadienyldiamine, hexahydro-4,7-methanodihydroindenyl dimethylenediamine, tricyclo[6.2.1.02,7]-undecyl dimethyl diamine, 4,4'-methylenebis(cyclohexylamine) and other aliphatic or alicyclic diamines; 1,3-bis(3-aminopropyl)tetramethyldisiloxane and other siloxane-containing diamines; polyether diamines; polyoxyalkylene diamines. .

[0106] The molar ratio of the structural unit (a) to the structural unit (b) in the polymer (A) (structural unit (a) / structural unit (b)) is preferably 60 / 40 to 40 / 60, more preferably 55 / 45 to 45 / 55. The content ratio of each structural unit can be determined by 13 Furthermore, a polymer in which the molar ratio of each monomer in the monomer mixture is within the above range can also be referred to as a polymer in which the molar ratio of the structural unit derived from each monomer is within the above range.

[0107] (Terminal structure)

[0108] The polymer (A) has a side chain terminal and a main chain terminal (hereinafter also collectively referred to as "polymer terminal"

[0109] ) has a group represented by the following formula (eg1) or formula (eg2) or a maleimide group in at least one of the main chain terminals, preferably has a group represented by the following formula (eg1) or formula (eg2) or a maleimide group in at least one of the main chain terminals, and more preferably has a group represented by the following formula (eg1) or formula (eg2) or a maleimide group at both ends of the main chain terminals. When polymer (A) has the above-mentioned group at the main chain terminal, the molecular weight of the resin accompanying the cross-linking reaction increases, and an increase in elongation can be expected.

[0110] [Chemistry 11]

[0111] *-L eg1 -R eg1 ...(eg1)

[0112]

[0113] In the formula, L eg1 and L eg2 represents an alkanediyl group having 1 to 5 carbon atoms, an aromatic hydrocarbon group having 6 to 10 carbon atoms, or a group in which two or more groups selected from these groups are linked via a single bond, -O-, -S-, -SO2-, -NH-, -NH-C(O)-, -C(O)-, or -C(O)O-, and R eg1 and R eg2In the above formula, * represents a bonding site with a polymer chain, but there are cases where the group represented by the above formula or a maleimide group is introduced into the terminal of the polymer chain using a terminal modifier described later, and there are cases where the structure (atomic group) derived from the monomer providing each structural unit is included.

[0114] Examples of the alkanediyl group having 1 to 5 carbon atoms include methylene, ethanediyl, propanediyl, etc. Examples of the aromatic hydrocarbon group having 6 to 10 carbon atoms include groups derived from the aromatic hydrocarbon compounds having 6 to 10 carbon atoms.

[0115] As a preferred method for introducing the group represented by the formula (eg1) or (eg2) or the maleimide group into the polymer terminal, the group represented by the following formula (eg1-1) to (eg1-3), formula (eg2-1), or formula (eg3-1) can be cited. That is, the polymer (A) preferably has a group represented by the following formula (eg1-1) to (eg1-3), formula (eg2-1), or formula (eg3-1) at its polymer terminal. The groups represented by the following formulas (eg1-1) to (eg1-3) and (eg2-1) are those in which the atoms that are not specified in the groups represented by the formulas (eg1) and (eg2) and are bonded to the polymer chain are further specified one by one.

[0116] [Chemistry 12]

[0117]

[0118] In the formula, L eg1 , R eg1 , L eg2 , and R eg2 has the same meaning as in the above formula (eg1) and formula (eg2), R eg3 R independently represents a hydrogen atom, an alkyl group having 1 to 5 carbon atoms, eg3 In the above formula, * represents a bonding site with a polymer chain, but there is not only a case where the group represented by the above formula is introduced into the terminal of the polymer chain using a terminal modifier described later, but also a case where the structure derived from the monomer providing each structural unit is included.

[0119] In order to introduce such terminal structure into polymer (A), it is preferred to use a terminal modifier. As for the terminal modifier, for example, as a terminal modifier providing the group represented by the formula (eg1), 4-chloromethylstyrene, 2-hydroxyethyl methacrylate, 2-isocyanatoethyl methacrylate, glycidyl methacrylate, 3-isopropenylcumyl isocyanate, etc. can be listed; as a terminal modifier providing the group represented by the formula (eg2), a combination of two or more modifiers such as 4-aminostyrene, 3-aminostyrene, tyramine / 4-chloromethylstyrene can be listed (for example, after modification with tyramine, modification with 4-chloromethylstyrene); as a terminal modifier providing a maleimide group, maleic anhydride, citraconic anhydride, etc. can be listed.

[0120] When a terminal modifier is used, it can be added in excess of the absolute value of the difference between the molar amount of the structural unit (a) and the molar amount of the structural unit (b), that is, the absolute value of the difference between the molar amount of the monomer providing the structural unit (a) and the molar amount of the monomer providing the structural unit (b), and the unreacted terminal modifier can be removed by purification after the reaction is completed. Therefore, the amount of the terminal modifier added is not particularly limited as long as it is in excess of the absolute value of the difference between the molar amount of the structural unit (a) and the molar amount of the structural unit (b).

[0121] (Characteristics of polymer (A))

[0122] Regarding the polymer (A), the polystyrene-equivalent weight average molecular weight (hereinafter also referred to as "Mw") measured by gel permeation chromatography (GPC) is preferably about 2,000 to 100,000. When the polymer (A) is used in a photosensitive resin composition, it is more preferably about 2,000 to 50,000, and further preferably about 3,000 to 30,000. When the polymer (A) is used in a photosensitive resin composition, if Mw is less than 2,000, there is a tendency that sufficient mechanical properties as an insulating film cannot be obtained. On the other hand, if Mw exceeds 100,000, there is a tendency that the unexposed portion of the photosensitive resin composition obtained using the polymer (A) lacks solubility in a solvent or a developer.

[0123] The polymer (A) may be used alone or in combination of two or more.

[0124] The lower limit of the content of the polymer (A) in 100% by mass of the solid content of the present composition is usually 20% by mass, preferably 40% by mass, and more preferably 60% by mass; the upper limit is usually 99% by mass, preferably 95% by mass. In addition, the solid content refers to all components that may be contained in the present composition except the solvent (D) described later.

[0125] The polymer (A) has at least one structure selected from the group consisting of polyimide and polyimide precursor. The polyimide precursor includes polyamic acid and polyamic acid ester. The structure of the polymer (A) can be 1 H-NMR etc. to confirm.

[0126] In terms of being able to form a patterned resin film with excellent elongation using the present composition, it is preferred that the polymer (A) is a linear polymer without a branched structure. In order to make the polymer (A) a linear polymer, for example, it is preferred that monomers having trifunctional or higher amino groups or acid anhydride groups are not used, but only monomers having difunctional polymerizable groups such as diamines and acid dianhydrides are used. Although described later, since the polymer (A) is synthesized by reacting anhydrides and amines so as to have a polyimide or a polyimide precursor in a repeating unit, for example, sometimes the amine used has three or more amino groups, resulting in a polymer having a branched structure.

[0127] (Method for producing polymer (A))

[0128] Polymer (A) can be obtained, for example, by the following method: using anhydrides, diamines (for example, diamines with phenolic hydroxyl groups) represented by the formula (1), and anhydrides and diamines other than the above as needed, and terminal modifiers, react in a polymerization solvent to synthesize polyamic acid, and then carry out imidization reaction to synthesize polyimide. The terminal modifier can be reacted before the synthesis of polyamic acid, during the synthesis of polyamic acid, or after the imidization reaction according to the introduction site (main chain end or side chain end). At this time, the polyamic acid synthesized midway can be used as a polymer (A) having the polyimide precursor structure. In addition, polyamic acid esters obtained by esterifying polyamic acid according to an existing method can also be used as a polymer (A) having the polyimide precursor structure.

[0129] At this time, the synthesis sequence of the polyamic acid for obtaining the polyimide can be applied to the following two methods, or can be synthesized by any method. That is, the following methods: (i) a method of dissolving an acid anhydride in a polymerization solvent and then reacting a diamine; (ii) a method of dissolving a diamine in a polymerization solvent and then reacting an acid anhydride.

[0130] As the polymerization solvent, a solvent that can dissolve the raw materials and products during the synthesis of the polymer (A) is selected. As the polymerization solvent, it is preferred to use at least one selected from the group consisting of N-methyl-2-pyrrolidone, 1,3-dimethyl-2-imidazolidinone, and γ-butyrolactone. These compounds can be used alone as the polymerization solvent, or two or more can be mixed and used.

[0131] In addition to the polymerization solvent, other solvents may be used in combination as needed. Examples of other solvents include: diethylene glycol dialkyl ethers such as diethylene glycol dimethyl ether and diethylene glycol diethyl ether; ethylene glycol monoalkyl ether acetates such as ethylene glycol monomethyl ether acetate; diethylene glycol monoalkyl ether acetates such as diethylene glycol monomethyl ether acetate; propylene glycol monoalkyl ether acetates such as propylene glycol monomethyl ether acetate; ketones such as methyl ethyl ketone and cyclohexanone; alcohols such as methanol, ethanol, and propanol; ether solvents such as diethylene glycol dimethyl ether and triethylene glycol dimethyl ether; and aromatic hydrocarbons such as toluene and xylene.

[0132] The imidization reaction for obtaining the polymer (A) having a polyimide structure can be applied to existing methods such as thermal imidization reaction and chemical imidization reaction. In the case of synthesizing the polymer (A) by thermal imidization reaction, it is preferably carried out by heating the synthetic solution of polyamic acid at 120° C. to 210° C. for 1 to 16 hours. In addition, the reaction can be carried out while removing water in the system using an azeotropic solvent such as toluene or xylene as needed.

[0133] <Photopolymerization initiator (B)>

[0134] The present composition contains a photopolymerization initiator (B). The photopolymerization initiator (B) is a compound that generates active species that promote the crosslinking reaction between the photopolymerizable compounds (C) described below, the crosslinking reaction between the polymer terminal groups in the polymer (A), and the crosslinking reaction between the terminal groups and the photopolymerizable compound (C) by exposure to radiation such as visible light, ultraviolet light, far ultraviolet light, electron beams, and X-rays. The photopolymerization initiator (B) may be used alone or in combination of two or more.

[0135] It is considered that the exposure treatment of the coating film formed from the present composition promotes the above-mentioned various crosslinking reactions, and a crosslinked structure is formed in the exposed portion, thereby reducing the solubility in the developer.

[0136] As the photopolymerization initiator (B), preferably a photosensitive radical polymerization initiator that generates radicals by light irradiation, for example, oxime compounds, organic halogenated compounds, oxydiazole compounds, carbonyl compounds, ketal compounds, benzoin compounds, acridine compounds, organic peroxide compounds, azo compounds, coumarin compounds, azide compounds, metallocene compounds, hexaarylbiimidazole compounds, organic boronic acid compounds, disulfonic acid compounds, onium salt compounds, acylphosphine (oxide) compounds. Among these, oxime compounds, especially photoradical polymerization initiators having an oxime ester structure, are preferred in terms of sensitivity.

[0137] Although the photoradical polymerization initiator having an oxime ester structure may have geometrical isomers due to the double bond of oxime, these are not distinguished and all of them are included in the photopolymerization initiator (B).

[0138] Examples of the photoradical polymerization initiator having an oxime ester structure include photoradical polymerization initiators described in International Publication No. 2010 / 146883, Japanese Patent Application Laid-Open No. 2011-132215, Japanese National Publication No. 2008-506749, Japanese National Publication No. 2009-519904, and Japanese National Publication No. 2009-519991.

[0139] Specific examples of the photoradical polymerization initiator having an oxime ester structure include N-benzoyloxy-1-(4-phenylthiophenyl)butane-1-one-2-imine, N-ethoxycarbonyloxy-1-phenylpropane-1-one-2-imine, N-benzoyloxy-1-(4-phenylthiophenyl)octane-1-one-2-imine, N-acetoxy-1-[9-ethyl-6-(2-methylbenzoyl) -9H-carbazole-3-yl]ethane-1-imine, and N-acetoxy-1-[9-ethyl-6-{2-methyl-4-(3,3-dimethyl-2,4-dioxolanylmethyloxy)benzoyl}-9H-carbazole-3-yl]ethane-1-imine, ethyl ketone, 1-[9-ethyl-6-(2-methylbenzoyl)-9H-carbazole-3-yl]-, 1-(O-acetyl oxime), etc.

[0140] Relative to 100 parts by mass of the polymer (A) in the present composition, the lower limit of the content of the photopolymerization initiator (B) is usually 0.01 parts by mass, preferably 0.1 parts by mass, and more preferably 0.5 parts by mass; the upper limit is usually 30 parts by mass, preferably 20 parts by mass, and more preferably 10 parts by mass. If the content of the photopolymerization initiator (B) is above the lower limit, the curing of the exposure portion becomes sufficient, and the heat resistance of the patterned resin film is easily improved. If the content of the photopolymerization initiator (B) is below the upper limit, the transparency relative to the light used in the exposure will not be reduced, and a patterned resin film with high resolution is easily obtained.

[0141] <Photopolymerizable compound (C)>

[0142] For the purpose of hardening the patterned resin film, the present composition preferably further contains a photopolymerizable compound (C). The photopolymerizable compound (C) is a crosslinking component (hardening component) that reacts with a vinyl group, a (meth)acryloyl group, or a maleimide group at the polymer terminal in the polymer (A), and the photopolymerizable compounds (C) may also react with each other. One type of photopolymerizable compound (C) may be used, or two or more types may be used in combination.

[0143] Examples of the photopolymerizable compound (C) include a crosslinking agent having at least two (meth)acrylic groups, a crosslinking agent having at least two maleimide groups, a crosslinking agent having at least two styrene groups, and a crosslinking agent having at least two thiol groups. Among these, a crosslinking agent having at least two maleimide groups and a crosslinking agent having at least two styrene groups are preferred.

[0144] The crosslinking agent having at least two maleimide groups is a compound having two or more, preferably three or more maleimide groups in the molecule, and the upper limit of the number of maleimide groups is preferably 10, more preferably 4. The maleimide group is a group that directly acts on the polymer terminal during photocrosslinking or thermal crosslinking, and the cured film formed from the present composition can further exert the effect of improving the elongation or reliability.

[0145] Specific examples of the crosslinking agent having at least two maleimide groups include: N,N'-ethylenebismaleimide, N,N'-hexamethylenebismaleimide, N,N'-(2,2,4-trimethylhexane)bismaleimide, N,N'-p-phenylenebismaleimide, N,N'-m-phenylenebismaleimide, N,N'-4-methyl-1,3-phenylenebismaleimide, N,N'-2 ,4-tolylene bismaleimide, N,N'-2,6-tolylene bismaleimide, N,N'-p-xylylene bismaleimide, N,N'-m-xylylene bismaleimide, N,N'-(1,3-dimethylenecyclohexane) bismaleimide, N,N'-(1,4-dimethylenecyclohexane) bismaleimide, N,N'-(4,4'-biphenylene) bismaleimide, N,N' -(4,4'-diphenylmethane)bismaleimide, N,N'-(3,3'-dimethyl-5,5'-diethyl-4,4'-diphenylmethane)bismaleimide, N,N'-(4,4'-dicyclohexylmethane)bismaleimide, N,N'-(4,4'-diphenyloxy)bismaleimide, N,N'-(4,4'-diphenylsulfone)bismaleimide, bisphenol A diphenyl ether bismaleimide , bis[4-(4-maleimidophenoxy)phenyl]methane, 2,2-bis[4-(4-maleimidophenoxy)phenyl]propane, bis[4-(4-maleimidophenoxy)phenyl]octane, bis[4-(4-maleimidophenoxy)phenyl]decane, bis[4-(4-maleimidophenoxy)phenyl]cyclohexane, bis[4-(4-maleimidophenoxy)phenyl]-tricyclo-[5.2.1.0 2.6 ]Decane.

[0146] As a cross-linking agent having at least two maleimide groups, commercial products can also be used. Commercial products of cross-linking agents having at least two maleimide groups include, for example, "BMI-2000", "BMI-2300", "BMI-TMH", "BMI-1000", "BMI-3000", "BMI-4000", "BMI-5100", and "BMI-7000" manufactured by Yamato Chemical Industries, Ltd.; "MIR-3000" and "MIR-5000" manufactured by Nippon Kayaku Co., Ltd.; "SLK-3000", "SLK-6895", "SLK-1500", "SLK-2500", and "SLK-6100" manufactured by Shin-Etsu Chemical Co., Ltd.

[0147] In addition, bismaleimide compounds in which both ends of polyoxyalkylene diamine are sealed with maleic anhydride can also be used. For example, bismaleimide compounds in which both ends of polyoxyethylene diamine are sealed with maleic anhydride, bismaleimide compounds in which both ends of polyoxypropylene diamine are sealed with maleic anhydride, and bismaleimide compounds in which both ends of polyoxybutylene diamine are sealed with maleic anhydride.

[0148] The crosslinking agent having at least two styryl groups is a compound having two or more, preferably three or more, styryl groups in the molecule, and the upper limit of the number of styryl groups is preferably 10, more preferably 4. The styryl group is a group that directly acts on the polymer terminal during photocrosslinking or thermal crosslinking, and the cured film formed from the present composition can further exert the effect of improving the elongation or reliability.

[0149] Specific examples of the cross-linking agent having at least two styryl groups include divinylbenzene and a compound represented by the following formula.

[0150] [Chemistry 13]

[0151]

[0152] At least one hydrogen atom in the benzene ring in the above-mentioned exemplary compounds may be independently substituted with an alkyl group having 1 to 10 carbon atoms. Examples of the alkyl group include a methyl group, an ethyl group, and a propyl group.

[0153] The cross-linking agent having at least two styryl groups may be used alone or in combination of two or more. In addition, the cross-linking agent having at least two styryl groups may be used in combination with a cross-linking agent having at least two maleimide groups. By using both in combination, the residual film rate (ratio of the patterned film appropriately remaining) after development is sometimes increased.

[0154] When the present composition contains a photopolymerizable compound (C), the lower limit of the content of the photopolymerizable compound (C) is usually 0.1 parts by mass, preferably 1 part by mass, and more preferably 2 parts by mass, relative to 100 parts by mass of the polymer (A) in the present composition; the upper limit is usually 40 parts by mass, preferably 30 parts by mass, and more preferably 20 parts by mass. If the content of the photopolymerizable compound (C) is above the lower limit or below the upper limit, there is a tendency to form a patterned resin film having excellent resolution, heat resistance, and elongation.

[0155] <Solvent(D)>

[0156] The present composition contains a solvent (D). By using a solvent (D), the handleability of the present composition can be improved, or the viscosity or storage stability can be adjusted.

[0157] The solvent (D) is not particularly limited as long as it is an organic solvent that can dissolve or disperse the components such as the polymer (A), the compound (B) and the crosslinking agent (C). Examples of the solvent (D) include ketone solvents, alcohol solvents, ether solvents, ester solvents, amide solvents, hydrocarbon solvents, and lactone solvents. The solvent (D) preferably contains at least one selected from the group consisting of ketone solvents, amide solvents, and lactone solvents because of its excellent solubility.

[0158] Examples of the ketone solvent include cyclic ketone solvents such as cyclohexanone, examples of the amide solvent include cyclic amide solvents such as N-methyl-2-pyrrolidone (NMP) and dimethylimidazolidinone (DMI), and examples of the lactone solvent include cyclic lactone solvents such as γ-butyrolactone (GBL).

[0159] The solvent (D) may be used alone or in combination of two or more.

[0160] The content of the solvent (D) in the present composition is an amount such that the solid content concentration in the composition is usually 10% by mass to 50% by mass.

[0161] <Additives (E)>

[0162] In addition to the above-mentioned components, the present composition may also contain additives (E) within the range that does not impair the purpose and characteristics of the present invention. Examples of the additives (E) include polymers other than the polymer (A), surfactants, low molecular weight phenol compounds, silane coupling agents, rust inhibitors, adhesion aids, crosslinked microparticles, leveling agents, sensitizers, inorganic fillers, and quenchers.

[0163] (Surfactant)

[0164] The present composition may contain a surfactant from the viewpoint of improving coating properties, defoaming properties, leveling properties, etc. The surfactant is not particularly limited, and existing nonionic surfactants, fluorine-based surfactants, and silicone-based surfactants can be used.

[0165] Examples of commercially available surfactants include BM-1000 and BM-1100 (BM Chemicals, Inc. Chemie), Megafac F142D, Megafac F172, Megafac F173, Megafac F183 (manufactured by Dainippon Ink & Chemicals Co., Ltd.), Fluorad FC-135, Fluorad FC-170C, Fluorad FC-430, Fluorad FC-431 (manufactured by Sumitomo 3M Co., Ltd.), Surflon S-112, Surflon S-113, Surflon S-131, Surflon S-141, Surflon S-145 (manufactured by Asahi Glass Co., Ltd.), SH-28PA, SH-19 Fluorine-based surfactants marketed under the names of 0, SH-193, SZ-6032, SF-8428 (manufactured by Toray Silicones Co., Ltd.), NBX-15 (manufactured by NEOS Co., Ltd.); silicone-based surfactants marketed under the names of KL-245, KL-270 (manufactured by Kyoeisha Chemical Co., Ltd.), SH28PA (manufactured by Toray Dow Corning Co., Ltd.); nonionic surfactants marketed under the names of nonion S-6, nonion 0-4, Pronon 201, Pronon 204 (manufactured by NOF Corp.), Emulgen A-60, Emulgen A-90, Emulgen A-500 (manufactured by Kao Corp.), KL-600 (manufactured by Kyoeisha Chemical Co., Ltd.), etc.

[0166] The surfactant may be used alone or in combination of two or more. The surfactant is preferably used in an amount of 5 parts by mass or less, more preferably in an amount of 0.01 to 2 parts by mass, based on 100 parts by mass of the polymer (A).

[0167] (Adhesive agent)

[0168] From the viewpoint of improving the adhesion to various substrates, the present composition may also contain a close contact auxiliary agent. The close contact auxiliary agent is not particularly limited, and examples thereof include functional silane coupling agents such as silane coupling agents having reactive functional groups such as carboxyl groups, methacryloyl groups, vinyl groups, isocyanate groups, epoxy groups, and amino groups.

[0169] The adhesion aid may be used alone or in combination of two or more. The adhesion aid is preferably used in an amount of 20 parts by mass or less, more preferably in a range of 0.5 to 10 parts by mass, based on 100 parts by mass of the polymer (A).

[0170] <Method for producing photosensitive resin composition>

[0171] The present composition can be produced by uniformly mixing the components constituting the present composition using a conventional method. In addition, after uniformly mixing the components, the obtained mixture can be filtered through a filter or the like to remove foreign matter.

[0172] [Resin film having a pattern]

[0173] The resin film with a pattern (patterned resin film) of one embodiment of the present invention is formed by curing the present composition. Specifically, it is obtained by the manufacturing method described below, and the patterned resin film can be preferably used as an insulating film (for example: surface protection film, interlayer insulating film, planarization film) possessed by a semiconductor circuit substrate.

[0174] [Method for producing a resin film having a pattern]

[0175] The patterned resin film can be manufactured by the following method, which comprises: a step (1) of forming a coating film of the present composition on a substrate; a step (2) of selectively exposing the coating film; and a step (3) of developing the exposed coating film using a developer containing an organic solvent.

[0176] <Process (1)>

[0177] In step (1), the present composition is usually applied to a substrate so that the thickness of the patterned resin film finally obtained is, for example, 0.1 μm to 100 μm. The substrate coated with the composition is heated using an oven or a hot plate, usually at 50° C. to 140° C. for 10 seconds to 360 seconds. In this way, a coating film containing the present composition is formed on the substrate.

[0178] Examples of the substrate include silicon wafers, compound semiconductor wafers, wafers with metal thin films, glass substrates, quartz substrates, ceramic substrates, aluminum substrates, and substrates having semiconductor chips on the surfaces of these substrates. Examples of the coating method include dipping, spraying, bar coating, roll coating, spin coating, curtain coating, gravure printing, screen coating, and inkjet.

[0179] <Process (2)>

[0180] In step (2), the coating film is selectively exposed using, for example, a contact aligner, a stepper, or a scanner. Specifically, the term "selectively" refers to exposure via a photomask having a predetermined mask pattern.

[0181] As exposure light, ultraviolet rays, visible light, etc. can be cited, and light with a wavelength of 200nm to 500nm is usually used (for example, i-ray (365nm)). The irradiation amount based on exposure varies depending on the type of each component in the composition, the mixing ratio, the thickness of the coating film, etc., and is usually 100mJ / cm 2 ~1500mJ / cm 2 .

[0182] In addition, in order to allow the crosslinking reaction to proceed sufficiently, it is preferred to perform a heat treatment after exposure (post-exposure baking). The conditions for the post-exposure heat treatment vary depending on the content of each component in the composition and the thickness of the coating film, and are usually performed at 70°C to 250°C, preferably 80°C to 200°C for about 1 minute to 60 minutes.

[0183] <Step (3)>

[0184] In step (3), the exposed coating film is developed with a developer containing an organic solvent to dissolve and remove the non-exposed portion, thereby forming a desired patterned resin film on the substrate. Examples of the developing method include a shower developing method, a spray developing method, an immersion developing method, and a liquid coating developing method. The developing conditions are generally 20° C. to 40° C. for about 1 minute to 10 minutes. In addition, after the resin film is developed with a developer containing an organic solvent, the resin film can be washed with water or an organic solvent and dried.

[0185] The developer contains one or more organic solvents. Examples of the developer include organic solvents such as ketone solvents, alcohol solvents, ether solvents, ester solvents, amide solvents, and hydrocarbon solvents; or liquids containing the organic solvents. Among these, at least one selected from ketone solvents, ester solvents, and amide solvents is preferred. Examples of components other than organic solvents in the developer include water, silicone oil, and surfactants.

[0186] The content of the organic solvent in the developer is preferably 80% by mass or more, more preferably 90% by mass or more, further preferably 95% by mass or more, particularly preferably 99% by mass or more.

[0187] The shape of the pattern in the patterned resin film is not particularly limited as long as it has a concavo-convex structure, and examples thereof include a line and space pattern, a dot pattern, a hole pattern, and a lattice pattern.

[0188] <Step (4)>

[0189] In order to fully demonstrate the characteristics as an insulating film, the method for manufacturing a patterned resin film according to one embodiment of the present invention may, after step (3), optionally include a step (4) of fully curing the patterned resin film by heat treatment (post-baking). The curing conditions are not particularly limited, and may be, for example, heated at a temperature of 100° C. to 350° C. for about 30 minutes to 10 hours depending on the use of the patterned resin film.

[0190] [Semiconductor circuit substrate]

[0191] By using the present composition, a semiconductor circuit substrate including the patterned resin film can be manufactured. The semiconductor circuit substrate has a patterned resin film formed from the present composition, preferably a patterned insulating film such as a surface protection film, an interlayer insulating film, and a planarizing film, and is therefore useful as a circuit substrate with high reliability.

[0192] Example

[0193] Hereinafter, the present invention will be described in more detail based on Examples, but the present invention is not limited to these Examples. In the following Examples and the like, "parts" are used to mean "parts by mass" unless otherwise specified.

[0194] <Polymer Synthesis>

[0195] The weight average molecular weight (Mw) of the polymers obtained in the following synthesis examples was measured by gel permeation chromatography (GPC) under the following conditions.

[0196] Column: Product name "TSKgel α-M" (manufactured by Tosoh Corporation)

[0197] Solvent: N-methyl-2-pyrrolidone (NMP)

[0198] Temperature: 40℃

[0199] ·Detection method: Refractive index method

[0200] ·Standard material: polystyrene

[0201] ·GPC device: Device name: "HLC-8320-GPC" (manufactured by Tosoh Co., Ltd.)

[0202] [Synthesis Example 1] Synthesis of polymer (A1)

[0203] In a four-necked flask, 162.23 mmol of BzDAxx (manufactured by ENEOS Co., Ltd., the following formula (a1-1)) as an acid anhydride, 175.39 mmol of 2,2-bis[4-(4-aminophenoxy)phenyl]propane as a diamine, and N-methyl-2-pyrrolidone (NMP) as a polymerization solvent (2.0 g relative to the total amount of 1 mmol of the acid anhydride and the diamine). After nitrogen substitution in the flask, the contents of the flask were heated at 40°C for 4 hours, and then heated at 180°C for 4 hours. After the contents of the flask were cooled to room temperature, 420.94 mmol of 4-(chloromethyl)styrene as a terminal modifier and 420.94 mmol of potassium carbonate as an alkali metal compound were added, and the contents of the flask were heated at 40°C for 4 hours. After the contents of the flask were cooled to room temperature, the precipitated solid components were separated by filtration, methanol was added to the filtrate, the precipitated solid components were washed with methanol, and the solid components were dried to obtain a polymer (A1). 13 The obtained polymer (A1) was analyzed by C-NMR and the like, and it was confirmed that it was a polymer having a structure represented by the following formula (A1). 1 The obtained polymer (A1) was analyzed by H-NMR and the like, and the imidization rate was found to be 100%. The weight average molecular weight (Mw) of the polymer (A1) was 18,000.

[0204] [Chemistry 14]

[0205]

[0206] [Synthesis Example 2] Synthesis of polymer (A2)

[0207] In a four-necked flask, 162.23 mmol of BzDAxx as an acid anhydride, 175.39 mmol of 2,2-bis[4-(4-aminophenoxy)phenyl]propane as a diamine, and NMP as a polymerization solvent (2.0 g relative to 1 mmol of the total amount of acid dianhydride and diamine). After nitrogen substitution in the flask, the contents of the flask were heated at 40°C for 4 hours, and then heated at 180°C for 4 hours. After the contents of the flask were cooled to room temperature, 280.62 mmol of maleic anhydride as a terminal modifier was added, and the contents of the flask were heated at 40°C for 2 hours. After the contents of the flask were cooled to room temperature, 1052.34 mmol of acetic anhydride and 70.1 mmol of sodium acetate were added, and the contents of the flask were heated at 80°C for 4 hours. After the contents of the flask were cooled to room temperature, the precipitated solid components were separated by filtration, methanol was added to the filtrate, the precipitated solid components were washed with methanol, and the solid components were dried to obtain a polymer (A2).13 The obtained polymer (A2) was analyzed by C-NMR and the like, and it was confirmed that it was a polymer having a structure represented by the following formula (A2). 1 The obtained polymer (A2) was analyzed by H-NMR and the like, and the imidization rate was found to be 100%. The weight average molecular weight (Mw) of the polymer (A2) was 19,000.

[0208] [Chemistry 15]

[0209]

[0210] [Synthesis Example 3] Synthesis of polymer (A3)

[0211] In a four-necked flask, 173.04 mmol of BzDAxx as an acid anhydride, 346.07 mmol of 2-hydroxyethyl methacrylate as a terminal modifier, 346.07 mmol of pyridine as a base, and NMP as a polymerization solvent (2.0 g relative to 1 mmol of the total amount of acid dianhydride and diamine). After nitrogen substitution in the flask, the contents of the flask were heated at 40°C for 4 hours. After the contents of the flask were cooled to room temperature, 181.69 mmol of 2,2-bis[4-(4-aminophenoxy)phenyl]propane as a diamine was added, and then 346.07 mmol of dicyclohexyl carbodiimide (DCC) was added under ice cooling, and the contents of the flask were stirred at room temperature for 4 hours. The precipitated solid components were separated by filtration, methanol was added to the filtrate, the precipitated solid components were washed with methanol, and the solid components were dried to obtain a polymer (A3). 13 The obtained polymer (A3) was analyzed by C-NMR and the like, and it was confirmed that it was a polymer having a structure represented by the following formula (A3). The weight average molecular weight (Mw) of the polymer (A3) was 19,000.

[0212] [Chemistry 16]

[0213]

[0214] [Synthesis Example 4] Synthesis of polymer (A4)

[0215] In Synthesis Example 1, the same operation as in Synthesis Example 1 was performed except that the acid anhydride used was 162.23 mmol of BzDAxx, the diamine was 173.64 mmol of 2,2-bis[4-(4-aminophenoxy)phenyl]propane, and 1.75 mmol of 1,3-bis(3-aminopropyl)tetramethyldisiloxane, and the terminal modifier was 420.94 mmol of 4-(chloromethyl)styrene, to obtain a polymer (A4). 13 The obtained polymer (A4) was analyzed by C-NMR and the like, and it was confirmed that it was a polymer (A4) represented by the following formula (A4). 1 The obtained polymer (A4) was analyzed by H-NMR and the like, and the imidization rate was found to be 100%. The weight average molecular weight (Mw) of the polymer (A4) was 19,000.

[0216] [Chemistry 17]

[0217]

[0218] [Synthesis Example 5] Synthesis of polymer (A5)

[0219] In Synthesis Example 1, the same operation as in Synthesis Example 1 was performed except that the acid anhydride used was 113.56 mmol of BzDAxx and 48.67 mmol of 4,4'-(4,4'-isopropylidene diphenyloxy)bis(phthalic anhydride), the diamine was 175.39 mmol of 2,2-bis[4-(4-aminophenoxy)phenyl]propane, and the terminal modifier was 420.94 mmol of 4-(chloromethyl)styrene, to obtain a polymer (A5). 13 The obtained polymer (A5) was analyzed by C-NMR and the like, and it was confirmed that it was a polymer (A5) represented by the following formula (A5). 1 The obtained polymer (A5) was analyzed by H-NMR and the like, and the imidization rate was found to be 100%. The weight average molecular weight (Mw) of the polymer (A5) was 20,000.

[0220] [Chemistry 18]

[0221]

[0222] [Synthesis Example 6] Synthesis of polymer (A6)

[0223] In Synthesis Example 1, except that the acid anhydride used was 162.23 mmol of PPHT (manufactured by Nippon Seika Co., Ltd., formula (a1-2) below), the same operation as in Synthesis Example 1 was carried out to obtain a polymer (A6). 13The obtained polymer (A6) was analyzed by C-NMR and the like, and the result showed that it was a polymer (A6) represented by the following formula (A6). 1 The obtained polymer (A6) was analyzed by H-NMR and the like, and the imidization rate was found to be 100%. The weight average molecular weight (Mw) of the polymer (A6) was 17,000.

[0224] [Chemistry 19]

[0225]

[0226] [Comparative Synthesis Example 1] Synthesis of Polymer (RA1)

[0227] In a four-necked flask, 162.23 mmol of 1,2,4,5-cyclohexanetetracarboxylic dianhydride as an acid anhydride, 175.39 mmol of 2,2-bis[4-(4-aminophenoxy)phenyl]propane as a diamine, and NMP as a polymerization solvent (2.0 g per 1 mmol of the total amount of the acid anhydride and the diamine) were placed. After the atmosphere in the flask was replaced with nitrogen, the contents of the flask were heated at 40°C for 4 hours and then at 180°C for 4 hours.

[0228] After the contents of the flask were cooled to room temperature, 420.94 mmol of 4-(chloromethyl)styrene as a terminal modifier and 420.94 mmol of potassium carbonate as an alkali metal compound were added, and the contents of the flask were heated at 40°C for 4 hours. After the contents of the flask were cooled to room temperature, the precipitated solid components were filtered and separated, methanol was added to the filtrate, the precipitated solid components were washed with methanol, and the solid components were dried to obtain a polymer (RA1). 13 The obtained polymer (RA1) was analyzed by C-NMR and the like, and it was confirmed that it was a polymer having a structure represented by the following formula (RA1). 1 The obtained polymer (RA1) was analyzed by H-NMR and the like, and the imidization rate was found to be 100%. The weight average molecular weight (Mw) of the polymer (RA1) was 17,000.

[0229] [Chemistry 20]

[0230]

[0231] [Comparative Synthesis Example 2] Synthesis of Polymer (RA2)

[0232] In a four-necked flask, 162.23 mmol of 4,4'-(4,4'-isopropylidene diphenyloxy)bis(phthalic anhydride) as an acid anhydride, 175.39 mmol of 2,2-bis[4-(4-aminophenoxy)phenyl]propane as a diamine, and NMP as a polymerization solvent (2.0 g relative to 1 mmol of the total amount of the acid dianhydride and the diamine). After nitrogen substitution in the flask, the contents of the flask were heated at 40°C for 4 hours, and then heated at 180°C for 4 hours. After the contents of the flask were cooled to room temperature, 280.62 mmol of maleic anhydride as a terminal modifier was added, and the contents of the flask were heated at 40°C for 2 hours. After the contents of the flask were cooled to room temperature, 1052.34 mmol of acetic anhydride and 70.1 mmol of sodium acetate were added, and the contents of the flask were heated at 80°C for 4 hours. After the contents of the flask were cooled to room temperature, the precipitated solid components were separated by filtration, methanol was added to the filtrate, the precipitated solid components were washed with methanol, and the solid components were dried to obtain a polymer (RA2). 13 The obtained polymer (RA2) was analyzed by C-NMR and the like, and the results showed that it was a polymer having a structure represented by the following formula (RA2). 1 The obtained polymer (RA2) was analyzed by H-NMR and the like, and the imidization rate was found to be 100%. The weight average molecular weight (Mw) of the polymer (RA2) was 20,000.

[0233] [Chemistry 21]

[0234]

[0235] [Comparative Synthesis Example 3] Synthesis of Polymer (RA3)

[0236] In a four-necked flask, 162.23 mmol of BzDAxx as an acid anhydride, 175.39 mmol of 4-[(4-aminophenyl)oxy]-1,3-phenylenediamine as a diamine, and NMP as a polymerization solvent (2.0 g relative to 1 mmol of the total amount of the acid anhydride and the amine). After nitrogen substitution in the flask, the contents of the flask were heated at 40° C. for 4 hours and then at 180° C. for 4 hours. As a result, the contents of the flask became gel-like. The gel-like polymer was designated as polymer (RA3), and the weight average molecular weight (Mw) and imidization rate of polymer (RA3) were not measured.

[0237] <Synthesis of photopolymerizable compounds>

[0238] [Synthesis Example 6] Synthesis of polyfunctional styryl compound (C2)

[0239] In a four-necked flask, 157.69 mmol of bisphenol A as a phenol compound, 946.17 mmol of 4-(chloromethyl)styrene as a halogen compound, 946.17 mmol of potassium carbonate as an alkali metal compound, and N-methyl-2-pyrrolidone as a synthetic solvent (0.5 g relative to 1 mmol of the total amount of the halogen compound and the phenol compound) were placed. After nitrogen substitution in the flask, the contents of the flask were heated at 80°C for 4 hours. After the contents of the flask were cooled to room temperature, the precipitated solid components were separated by filtration. Methanol was added to the filtrate, and the precipitated solid components were dried to obtain a multifunctional styrene-based compound (C2) (following formula). By 13 C-NMR analysis confirmed the structure represented by the following formula.

[0240] [Chemistry 22]

[0241]

[0242] The types and amounts of monomers used in Synthesis Examples 1 to 6 and Comparative Synthesis Examples 1 to 3, and various physical properties of the obtained polymers are shown in Table 1 below.

[0243] [Table 1]

[0244] Table 1

[0245]

[0246] The details of the acid anhydride, diamine, and terminal modifier used in Table 1 are shown below.

[0247] ·Acid anhydride

[0248] (a1-1): BzDAxx (manufactured by ENEOS)

[0249] (a2-1): PPHT (manufactured by Nippon Seika Co., Ltd.)

[0250] (a2-1): 1,2,4,5-cyclohexanetetracarboxylic dianhydride

[0251] (a2-2): 4,4'-(4,4'-isopropylidene diphenoxy)bis(phthalic anhydride)

[0252] ·Diamine

[0253] (b-1): 2,2-bis[4-(4-aminophenoxy)phenyl]propane

[0254] (b-2): 1,3-bis(3-aminopropyl)tetramethyldisiloxane

[0255] Other diamines

[0256] (b'-1): 4-[(4-aminophenyl)oxy]-1,3-phenylenediamine

[0257] Terminal modifier

[0258] (c1): 4-(Chloromethyl)styrene

[0259] (c2): Maleic anhydride

[0260] (c3): 2-hydroxyethyl methacrylate (HEMA)

[0261] <Production of photosensitive resin composition>

[0262] [Examples 1 to 9 and Comparative Examples 1 to 3]

[0263] The polymer, photopolymerization initiator, photopolymerizable compound, and additive shown in Table 2 were uniformly mixed in the amounts shown in Table 2 using the solvents shown in Table 2 to obtain the solid content concentrations shown in Table 2, and the photosensitive resin compositions of Examples 1 to 9 and Comparative Examples 1 to 3 were prepared at the curing temperatures and curing times shown in Table 2. The obtained photosensitive resin compositions were evaluated as follows. The results are shown in Table 2.

[0264] Analytical

[0265] The radiation-sensitive composition was spin-coated on a 6-inch silicon wafer, and then heated at 110°C for 5 minutes using a hot plate to form a coating film (film thickness: 10 μm). Then, an alignment machine (manufactured by Suss Microtec, model "MA-150") was used to align the wafer with a 50×50 μm gap. 2 The exposure dose of the square photomask at a wavelength of 365 nm is 500 mJ / cm 2 The coating film was exposed to ultraviolet light from a high-pressure mercury lamp in a manner. Then, it was heated at 150°C for 3 minutes using a hot plate, and then, immersion development was performed at 23°C for 3 minutes using a developer (cyclopentanone). The developed coating film was heated in an oven under a nitrogen environment under the heating conditions (curing temperature, curing time) shown in Table 2 to produce a resin film with a pattern. The produced resin film with a pattern was observed using an electron microscope and evaluated according to the following criteria.

[0266] ○: A pattern can be formed.

[0267] ×: A pattern cannot be formed.

[0268] Tensile elongation

[0269] The photosensitive resin composition was applied onto a substrate with a release material, and then heated in an oven at 110° C. for 5 minutes to prepare a coating film. Then, an alignment machine (manufactured by Suss Microtec Co., Ltd., model “MA-150”) was used to expose the film at a wavelength of 365 nm at an exposure dose of 500 mJ / cm 2 The entire surface of the coating film was irradiated with ultraviolet rays from a high pressure mercury lamp in a manner of . Then, the coating film was heated at 150° C. for 3 minutes using a hot plate, and then heated in an oven under a nitrogen atmosphere under the heating conditions (curing temperature, curing time) shown in Table 2.

[0270] The substrate with a release material is peeled off by post-baking and heating the coating to obtain a resin film with a thickness of 15 μm. The obtained resin film is cut into strips of 5 cm in length and 0.5 cm in width to make tensile test pieces. The tensile breaking elongation (%) of the long strip resin film is measured using a tensile compression testing machine (product name "AGS-500NX", manufactured by Shimadzu Corporation (Co., Ltd.)). The measurement conditions are: chuck distance = 2.5 cm, tensile speed = 5 mm / min, and measurement temperature = 23°C. The average value of the 5 measured values ​​is set as "elongation (composition)" and evaluated according to the following criteria.

[0271] ◎: Elongation is 50% or more

[0272] ○: Elongation is 20% or more and less than 50%

[0273] ×: Elongation is less than 20% or cannot be measured

[0274] "PCT Patience"

[0275] The prepared tensile test piece was subjected to three reflows (maximum temperature 260°C) in the atmosphere and then exposed to an environment of 130°C / 85%RH / 96hr. The tensile elongation of the test piece after exposure was measured in the same manner as in "Elongation (composition)", and the maintenance rate of the tensile elongation relative to the tensile elongation before exposure was evaluated according to the following criteria.

[0276] ○: Maintenance rate is 50% or more

[0277] ×: Maintenance rate is less than 50% or cannot be measured

[0278]

[0279] Details of the photopolymerization initiator (B), the photopolymerizable compound (C), the additive (E), and the solvent (D) used in Table 2 are shown below.

[0280] Photopolymerization initiator (B)

[0281] (B1): Irgacure OXE02 (ethyl ketone, 1-[9-ethyl-6-(2-methylbenzoyl)-9H-carbazol-3-yl]-, 1-(O-acetyl oxime), manufactured by BASF)

[0282] ·Photopolymerizable compound (C)

[0283] (C1): BMI-2300 (a polyfunctional maleimide compound represented by the following formula (C1), manufactured by Yamato Chemical Industries, Ltd.)

[0284] (C2): The multifunctional styryl compound synthesized in Synthesis Example 6

[0285] Additives (E)

[0286] (E1): NBX-15 (fluorine-based surfactant, manufactured by NEOS Co., Ltd.)

[0287] (E2): KBM-503 (a compound represented by the following formula (E2), manufactured by Shin-Etsu Chemical Co., Ltd.)

[0288] ·Solvent(D)

[0289] (D1): Cyclohexanone

[0290] [Chemistry 23]

[0291]

Claims

1. A photosensitive resin composition comprising: (A) a polymer, which is at least one selected from the group consisting of polyimide and a polyimide precursor; (B) a photopolymerization initiator; and (D)solvent, The polymer (A) comprises a structural unit (a) derived from an acid anhydride and a structural unit (b) derived from a diamine, The structural unit (a) includes a structural unit (a1) derived from an acid anhydride represented by the following formula (1): The polymer (A) has a group represented by the following formula (eg1) or formula (eg2), or a maleimide group, at at least one of a side chain terminal and a main chain terminal. [Chemistry 1] [In the above formula (1), L independently represents a single bond, an ester bond, or an amide bond, R 1 , R 2 and R 3 Each independently represents a hydrogen atom, an alkyl group having 1 to 6 carbon atoms, or represents R 1 With R 2 or R 1 With R 3 an alkylene group having 1 to 4 carbon atoms bonded to each other, n 1 and n 2 Each independently represents an integer from 0 to 3 (wherein, In the same ring, n 1 With n 2 At least one of is an integer greater than 1. ), Y 1 represents a structure represented by the following formula (Y1) or formula (Y2); *-Ar 1 -*…(Y1) *-On 2 -Y 2 -On 2 -*…(Y2) In the above formula (Y1) and formula (Y2), * represents a bond with respect to L in the above formula (1), Ar 1 and Ar 2 Each independently represents a group formed by removing two hydrogen atoms from an unsubstituted aromatic ring or an aromatic ring substituted with an alkyl or alkoxy group having 1 to 6 carbon atoms, Y in the formula (Y2) 2 is a single bond, an oxygen atom, a sulfur atom, or at least one group selected from the group consisting of a sulfonyl group, a carbonyl group, a methylene group, a dimethylmethylene group, and a bis(trifluoromethyl)methylene group. [Chemistry 2] *-Leg1—Reg1 ( e g1 ) [In the above formula (eg1) and formula (eg2), Leg 1 Leg 2 Each independently represents an alkanediyl group having 1 to 5 carbon atoms, an aromatic hydrocarbon group having 6 to 10 carbon atoms, or a group in which two or more groups selected from these are linked via a single bond, -O-, -S-, -SO2-, -NH-, -NH-C(O)-, -C(O)-, or -C(O)O-, Reg 1 and Reg 2 each independently represents a vinyl group or a (meth)acryloyl group, *Indicates the bonding site with the polymer chain. 〕 2 . The photosensitive resin composition according to claim 1 , further comprising (C) a photopolymerizable compound. 3 . The photosensitive resin composition according to claim 1 , wherein the polymer (A) has a group represented by the formula (eg1) or (eg2) or a maleimide group at at least one of the main chain terminals. The photosensitive resin composition according to claim 3 , wherein the polymer (A) is a linear polymer having no branched structure.

5. The photosensitive resin composition according to claim 4, wherein the polymer (A) has a group represented by the following formula (eg1-1) to formula (eg1-3), formula (eg2-1), or formula (eg3-1) at at least one of the main chain terminals, [Chemistry 3] (In the formula, Leg 1 , Reg 1 、Leg 2 , and Reg 2 The same symbols as in the formula (eg1) and the formula (eg2) have the same meanings, Reg 3 independently represent a hydrogen atom, an alkyl group having 1 to 5 carbon atoms, Reg 3 Can bond to each other to form a ring, *Indicates the bonding site with the polymer chain. ) 6. A method for producing a resin film having a pattern, comprising: a step (1) of forming a coating film of the photosensitive resin composition as described in any one of claims 1 to 5 on a substrate; a step (2) of selectively exposing the coating film; and a step (3) of developing the exposed coating film using a developer containing an organic solvent. 7 . A resin film having a pattern, which is obtained by curing the photosensitive resin composition according to claim 1 .

8. A semiconductor circuit substrate comprising the resin film having a pattern according to claim 7.