Method for monitoring weakening of interface between substrate and layer and device for implementing such monitoring
By irradiating a monochromatic beam at a non-zero angle and measuring the intensity of the scattered beam, the problem of interface weakening monitoring in industrial rupture furnaces is solved, and the accurate monitoring of the interface and optimized rupture process is achieved, which is suitable for industrial microelectronics manufacturing.
Patent Information
- Application Number
- CN202380033664.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-02-14
- Filing Date
- 2023-02-14
- Publication Date
- 2024-11-22
AI Technical Summary
In the manufacturing of microelectronic and optoelectronic structures, it is difficult for the prior art to effectively monitor the weakening of the interface between the donor substrate and the layer to be transferred in an industrial rupture furnace, especially due to the limitations of the distance between the lens and sample by imaging requirements of infrared microscopes and the problem of infrared radiation interference.
A monochromatic beam is used to irradiate the substrate/layer components at a non-zero angle to measure the intensity of the scattered beam to determine the weakened state of the interface, and realize monitoring and control of the weakened interface, which is suitable for industrial rupture furnace environments.
This method allows accurate monitoring of the weakened state of the interface without the need for a powerful radiation source and close-range lens installation, optimizing the rupture process, suitable for industrial-scale microelectronic manufacturing.
Smart Images

Figure CN119013773A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the field of microelectronic and optoelectronic structure manufacturing, and in particular to the field of semiconductor layer transfer that can be used in such manufacturing.
[0002] The object of the invention is therefore more particularly a method for monitoring the weakening of an interface between a substrate and a layer, a method for weakening such an interface, a device capable of monitoring the weakening of the same interface and a system for rupturing an interface between a substrate and a layer. Background Art
[0003] In the manufacture of microelectronic and / or optoelectronic structures, Smart Cut is often used. TM The Smart Cut TM A method of this type comprises a step of implantation in a donor substrate to create a buried brittle interface defining the semiconductor layer to be transferred.
[0004] This transfer requires that the buried brittle interface between the donor substrate and the layer to be transferred be fractured after the donor substrate / layer assembly is bonded to the host substrate through the layer. This fracture is usually achieved by weakening annealing, thereby allowing the microcavities formed at the interface to grow and coalesce.
[0005] Figure 1 The roughness variation along the layer after the fracture is shown. This roughness variation is mainly due to the difference in crack size when the fracture occurs on the wafer scale. It can have various sources, in particular, non-uniformity of the implant or weakening annealing or stress variations in the stack.
[0006] It would thus be advantageous to be able to monitor the weakening of the interface between the donor substrate and the layer to be transferred during the weakening annealing. Currently, this monitoring can be achieved with infrared microscopy. Although this type of imaging allows obtaining images of the microcavities and thus quantifying the characteristics of their population and development, it is not really suitable for in situ measurements in a fracturing oven, especially when the latter is of industrial type.
[0007] This is because, for such imaging, the distance between the lens and the sample (i.e. the donor substrate / layer / host substrate assembly) has to be very small (a few millimeters at most), which makes its incorporation into an industrial fracturing furnace particularly complicated.
[0008] Furthermore, at this temperature, infrared radiation emitted by the plate and furnace may interfere with the infrared signal used for observation, so a very powerful light source is required to illuminate the wafer. Summary of the invention
[0009] The present invention aims to remedy the above-mentioned drawbacks and therefore has for its object to provide a method for monitoring weakening which is compatible with the limitations of fracturing furnaces (in particular industrial ones) and in particular does not require the installation of lenses at a close distance to the substrate / layer assembly whose interface has to be monitored and in particular does not require powerful radiation sources.
[0010] To this end, the invention relates to a method for monitoring the weakening of an interface between a layer and a substrate during a weakening annealing of said interface, the substrate / layer assembly having at least a first face and a second face, the method comprising the following steps:
[0011] - irradiating the first surface with a monochromatic light beam in a first direction,
[0012] - measuring the intensity of the light beam scattered by the substrate / layer assembly in at least one second direction, the second direction having a non-zero angle with the first direction,
[0013] - Determining the weakened state of the interface based on said strength.
[0014] The inventors have found that the intensity of light scattered at a given angle relative to the first direction is a characteristic of the size of the microcavity and the distance between the microcavities. Thus, by monitoring the change in this intensity during the weakening annealing, the weakening of the interface between the layer and the substrate can be monitored. This irradiation and this measurement can be implemented at a certain distance from the substrate / layer assembly, so the method has the advantage of being fully compatible with the constraints associated with the rupture furnace (especially industrial type). It should be noted in particular that the method according to the present invention makes it possible to implement this monitoring from outside the housing of the rupture furnace, because the light source and the sensor can be arranged at a certain distance from the substrate / layer assembly and are compatible with the use of an observation window.
[0015] It should be noted that the first direction corresponds to the incident direction of the monochromatic light beam, and the second direction corresponds to one or more observation directions for monitoring the rupture. Therefore, in this document, it is entirely possible to replace "incident direction" with "first direction" and "observation direction" with "second direction" without changing its teaching.
[0016] When measuring the intensity of the light beam, the intensity may be measured in a plurality of second directions, each second direction having a non-zero angle with the first direction, and preferably at least two of the second directions may have different angles relative to the first direction.
[0017] In this way, when the at least two directions have the same angle relative to the first direction, more accurate measurements can be obtained, and when the at least two directions have different angles relative to the first direction, at least two second directions of interest corresponding to the weakened state of interest can be focused on.
[0018] This possibility allows to measure the intensity in a second range of directions, as follows Figures 3 to 5 As discussed in .
[0019] A previous calibration step may be provided, carried out before the weakening annealing, comprising the following sub-steps:
[0020] - irradiating the first surface with a light beam in a first direction,
[0021] - measuring a reference intensity of the light beam scattered by the substrate / layer assembly in at least one second direction,
[0022] - wherein during the step of determining the weakened state, a sub-step of correcting the measured intensity based on a reference intensity is provided.
[0023] In this way, the scattering peaks associated with the cavities formed during the weakening of the interface can be easily identified, and the state of the weakening of the interface can be easily determined.
[0024] During illumination of the first surface with the light beam in the first direction, the light beam may move in at least two regions or sections of the first surface.
[0025] Thus, the uniformity of the weakening along the interface of the first face can be checked.
[0026] In a variant where the measurement is performed at two locations by moving the light beam, provision can be made to allow the measurement to be performed in at least two areas, for:
[0027] - irradiating the first surface in a first direction with both the light beam and the further light beam,
[0028] - measuring the intensity of the light beam scattered by the substrate / layer assembly and the other light beam at least in a second direction,
[0029] - determining a weakened state of the interface based on said strengths at said at least two regions.
[0030] The monochromatic light beam may have a wavelength comprised in the infrared wavelength range, preferably near infrared, said wavelength even more advantageously being between 1050 nm and 1550 nm.
[0031] Such wavelengths are particularly suitable when the substrate and / or THE layer are made of silicon, germanium or a silicon-germanium alloy.
[0032] It should be noted that the light beam may alternatively have a wavelength in the visible range.
[0033] This alternative is particularly applicable when the substrate and / or layers are made of large-gap semiconductors such as gallium nitride, aluminum nitride, alloys of both, or silicon carbide.
[0034] The invention also relates to a method for weakening an interface between a layer and a substrate, comprising a step of weakening annealing the substrate / layer assembly to weaken the interface, wherein during the annealing step the method according to the invention for monitoring the weakening is carried out.
[0035] This method benefits from the advantages associated with the monitoring allowed by the monitoring method according to the invention. With this method it is therefore easy to monitor the maturity of the cavities present at the interface and to take countermeasures where appropriate.
[0036] Therefore, the conditions of the weakening annealing can be adjusted accordingly, in particular to obtain the desired microcrack distribution. For example, the heating curve of the furnace can be modified in real time.
[0037] The weakening annealing step may be stopped when the weakened state of the interface measured by the weakening monitoring method reaches a given threshold, the weakened state preferably corresponding to a rupture of the interface, which is then detected by an intensity change in at least one second direction and / or a shift in the scattering peak.
[0038] In this way, the rupture can be optimized and the annealing can be stopped at the most appropriate moment.
[0039] It is particularly important to note that according to one possibility of the invention, the weakened state can be selected so that the rupture is performed outside the furnace where the weakening annealing is performed. In this way, the rupture can be performed outside the furnace if the weakening method so requires.
[0040] The annealing conditions used in the annealing step may be modified depending on the weakening state of the interface determined during implementation of the weakening monitoring method.
[0041] In this way, the weakening annealing, in particular the heating profile of the furnace, can be optimized according to the weakening state of the interface to obtain the desired distribution of microcracks at the interface.
[0042] The invention also relates to a device for monitoring the weakening of an interface, for monitoring the weakening of an interface between a layer and a substrate during a weakening annealing of said interface, the substrate / layer assembly having at least a first face and a second face, comprising:
[0043] - a light source capable of emitting a monochromatic light beam in a first direction towards the first face,
[0044] - an electromagnetic radiation detector capable of measuring the intensity of the light beam after scattering by the substrate / layer assembly, the electromagnetic radiation detector being arranged to measure the intensity of the light beam in a second direction having a non-zero angle with the first direction.
[0045] Such a device is suitable for carrying out the monitoring method according to the invention and therefore benefits from the associated advantages.
[0046] The electromagnetic radiation detector may be arranged to allow measuring the intensity of the light beam after scattering in a plurality of second directions, each second direction having a non-zero angle with the first direction, and preferably at least two of the second directions having different angles relative to the first direction.
[0047] In this way, more accurate measurements can be obtained when the at least two directions have the same angle relative to the first direction, and at least two second directions of interest corresponding to the weakened state of interest can be focused on when the at least two directions have different angles relative to the first direction.
[0048] It should be noted that such an arrangement of electromagnetic radiation detectors may be provided by using at least two electromagnetic radiation detection units, each electromagnetic radiation detection unit being arranged to detect the intensity of the light beam after being scattered in a respective second direction.
[0049] Thus, the detector may for example take the form of a matrix of such cells (or pixels) so as to allow measurements in a plurality of second directions.
[0050] It is worth noting that each of these units can be equipped with an optical element allowing to measure the intensity of the light beam after scattering in the corresponding second direction.
[0051] The weakening monitoring device may further include a processing unit configured to restore the intensity value of the light beam measured by the detector and determine the weakening state of the interface according to the intensity value of the light beam.
[0052] Such a processing unit is conducive to the use of the monitoring device according to the present invention, and the technicians who perform the weakening annealing can directly understand the weakening state of the interface.
[0053] The processing unit may also be configured to, when determining the weakened state of the interface, correct the measured intensity based on a reference intensity determined before the weakening annealing.
[0054] In this way, scattering peaks associated with cavities formed during the weakening of the interface can be easily identified.
[0055] The invention also relates to an annealing furnace 40 capable of carrying out weakening annealing to weaken the interface between a layer and a substrate, the annealing furnace comprising a weakening monitoring device according to the invention.
[0056] With the weakening monitoring device, the annealing furnace allows on-site weakening monitoring, which is very suitable for industrial type annealing furnaces.
[0057] The annealing furnace may comprise a first position for a substrate / layer assembly and at least one second position for a further substrate / layer assembly to allow a weakening annealing of the substrate / layer assembly and the further substrate / layer assembly to be performed simultaneously,
[0058] The second position is arranged such that the surface of the further substrate / layer assembly is illuminated by the light beam after the light beam has passed through the substrate / layer assembly,
[0059] And the electromagnetic radiation detector is also capable of measuring the intensity of the light beam after being scattered by the other substrate / layer assembly, and the electromagnetic radiation detector is arranged to measure the intensity of the light beam in another second direction having a non-zero angle with the first direction.
[0060] With such an annealing furnace, it is possible to carry out an interface weakening annealing on a plurality of substrate / layer assemblies, while simultaneously monitoring the weakening of at least two of said interfaces, or even all of said interfaces.
[0061] It should be noted that in such a configuration, the electromagnetic radiation detector may comprise at least two detection units, each detection unit being dedicated to a respective one of the first and second positions.
[0062] The annealing furnace may be configured such that, when performing a weakening anneal, annealing of the substrate / layer assembly is stopped when the weakening monitoring device determines that the weakened state of the measured interface reaches a given threshold value.
[0063] In this way, an optimized weakening annealing can be provided, since it is based on monitoring the weakening of the interface.
[0064] The annealing furnace may comprise a control unit configured to communicate with the processing unit of the weakening monitoring device and to adjust the conditions of the weakening annealing according to the weakening status provided by the weakening monitoring device. BRIEF DESCRIPTION OF THE DRAWINGS
[0065] The invention will be better understood by reading the description of exemplary embodiments given by way of indication only and not limitation, and with reference to the accompanying drawings, in which:
[0066] [ Figure 1 ] shows a roughness map performed on a semiconductor layer after rupture of the interface of the semiconductor layer with a donor substrate from which the semiconductor layer originates, wherein the light value corresponds to the maximum roughness;
[0067] [ Figure 2 ] shows a weakening furnace equipped with a weakening monitoring device according to the present invention;
[0068] [ Figure 3 ] graphically shows the variation of the intensity of the light beam scattered by the layer / substrate assembly as a function of the scattering angle, measured before and during the weakening annealing, respectively;
[0069] [ Figure 4 ] graphically shows the difference in intensity variation with scattering angle calculated by subtracting the intensity measured before the weakening annealing from the intensity measured during the weakening annealing;
[0070] [ Figure 5 ] graphically compares the intensity of the scattered light beam measured using the device of the present invention with the Fourier transform of the confocal microscope image implemented in the prior art.
[0071] Identical, similar or equivalent parts in the various figures have the same reference numerals to facilitate movement from one figure to another.
[0072] The various parts shown in the figures are not necessarily shown to uniform scale to make the figures clearer.
[0073] It has to be understood that the various possibilities (variants and embodiments) are not mutually exclusive and can be combined with one another. DETAILED DESCRIPTION
[0074] Figure 2 A weakening furnace 40 is shown, in which a weakening annealing of the interface 13 between the donor substrate 11 and the layer 12 is carried out, said weakening furnace 40 being equipped with a weakening monitoring device 30 according to the invention so as to enable the weakening of said interface 13 to be monitored.
[0075] It should be noted that in a normal configuration of the present invention, Figure 2 As shown, the elements of the weakening monitoring device 30 are arranged outside the housing 40A of the weakening furnace 40, and the housing 40A is equipped with a not shown observation window to allow weakening monitoring through the weakening monitoring device 30 according to the present invention. This normal configuration is by no means restrictive, and it is entirely conceivable that at least some elements of the weakening monitoring device 30 are at least partially arranged in the housing 40A of the weakening furnace 40 without departing from the scope of the present invention.
[0076] In the context of this exemplary embodiment, substrate (referred to as donor substrate) and layer to be transferred are substrate and layer of single crystal silicon Si respectively. Therefore, the wavelength, value and other measurements shown below and in the rest of this article are applicable to this material. Of course, according to this teaching, those skilled in the art can apply this teaching to other types of materials. Therefore, the present invention is also particularly applicable to the situation of the weakening of the interface between layer and substrate, and both the layer and substrate are made of germanium Ge, or made of silicon germanium Si-Ge alloy or silicon carbide SiC, or even made of silicon Si substrate and silicon carbide SiC layer.
[0077] Of course, if the invention relates to monitoring the weakening of the interface 13 between the substrate 11 and the layer 12 it supports, then in a conventional application of the invention, the weakening annealing is performed after the step of bonding the layer to the host substrate 14, the substrate 11 being the donor substrate used in the case of transferring the layer 12 to the host substrate 14. Therefore, if in the general case of the invention, the substrate 11 / layer 12 assembly 10 comprises the substrate 11 and the layer 12, then in a conventional application of the invention, the assembly 10 also comprises the host substrate, such as Figure 2 shown.
[0078] This weakening monitoring device 30 comprises:
[0079] a light source 31 capable of emitting a monochromatic light beam 25 in the direction of the first face 10A, the wavelength of said light beam 25 being chosen so that the layer 12 and the substrate 11 or 14 are substantially transparent for said wavelength,
[0080] The electromagnetic radiation detector 32 is able to measure the intensity of the light beam 25 after scattering by the substrate 11 / layer 12 assembly 10 , the electromagnetic radiation detector being arranged to measure said intensity of the light beam 25 in a second direction having a non-zero angle 2θ with the first direction 25A.
[0081] Of course, this second direction 25B in which the light beam 25 scattered by the substrate 11 / layer 12 assembly 10 is detected intersects the first direction 25A along which the light beam 25 is emitted, at the level of the scattering element at the origin of said scattering, i.e. at the level of the substrate 11 / layer 12 assembly 10 (or more precisely, the interface 13 between layer 11 and substrate 12).
[0082] In a normal scattering configuration, such as Figure 2 As shown, the second direction 25B can extend from the second face of the support while moving away from the latter. In a variant not shown, the scattering measured by the detector is backscattering and the second direction 25B can extend from the first face while moving away from the latter. This possibility is particularly advantageous in order to allow the observation of scattering with opaque host / receiving substrates or when the transmission angle is inaccessible.
[0083] It should therefore be noted that scattering of a light beam through the substrate 11 / layer 12 assembly 10 must be understood here and in the remainder of the text in terms of: scattering itself, i.e. scattering of the light beam from the interface 13 in the direction of the second face 10B, and backscattering, i.e. scattering of the light beam from the interface 13 in the direction of the first face 10B.
[0084] As described below, a processing unit 33 may also be provided which is able to control the light source and the electromagnetic radiation detector 32 in order to calibrate the weakened state of the interface 13 based on the intensity measured by the electromagnetic radiation detector 32 .
[0085] The light source 31 is a light source capable of providing / emitting a light beam 25, the wavelength of which is adapted to the transparency of the material of the substrate 11 and the layer 12. In the case of the present exemplary embodiment (i.e., the silicon layer and the substrate), the wavelength of the light beam may be an infrared wavelength, preferably a near-infrared wavelength. Thus, the wavelength of the light beam 25 may be between 1050 nm and 1550 nm, for example equal to 1.2 μm, 1.5 μm or 1.3 μm. To allow for such an arrangement, the light source may be a laser source, such as a semiconductor laser, a laser diode; or a light emitting diode. Preferably, the light source 31 may include a system for guiding the light beam 25, such as an optical fiber, advantageously including a collimation system (lenses, mirrors) to limit the size and divergence of the light beam after emission.
[0086] like Figure 2 As shown, the first direction 25A is preferably perpendicular to the first surface. Of course, other first directions 25A may be envisaged without departing from the scope of the present invention.
[0087] The electromagnetic radiation detector 32 is configured to receive electromagnetic radiation in a wavelength range including the wavelength of the light beam 25 emitted by the light source 31 and to provide a signal representative of the intensity of the received radiation. Thus, the electromagnetic radiation detector may comprise a photodetector, such as a photodiode or a plurality of photodiodes arranged in a matrix. Thus, for example, the electromagnetic radiation detector 32 may comprise a CMOS or CCD sensor, the spectral response of which is adapted to the source used. In this configuration, various photodiodes or pixels form a detection unit.
[0088] In addition to such a photodetector, the electromagnetic radiation detector 32 may also comprise a lens in order to focus the part of the light beam 25 scattered in the second direction 25B onto the photodetector.
[0089] According to a first possibility of the invention, the electromagnetic radiation detector can be arranged to receive the light beam portion scattered along a predetermined second direction 25B and selectively image the luminous segment. According to this possibility, the second direction is selected to correspond to a direction of interest, i.e. an angle of interest 2θ relative to the first direction 25A, corresponding to a predetermined weakening state of the interface 13.
[0090] It should be noted that, in the case where the electromagnetic radiation detector 32 comprises a plurality of detection units, the radiation detector may comprise a plurality of optical systems, each dedicated to one or a group of respective detection units. Said optical systems are each arranged to allow measuring the intensity of the light beam 25 scattered by the substrate 11 / layer 12 assembly 10 in the second direction 25B associated therewith.
[0091] According to this exemplary embodiment, the inventors have found that, in the context of this possibility, a second direction having an angle 2θ between 5° and 15°, preferably between 8° and 12° and substantially equal to 10°, corresponds to a weakened state of the interface 13 suitable for providing an optimized rupture. The inventors have indeed found that such an angle value of 10° of the second direction 25B with respect to the first direction 25A corresponds to a microcrack of 10 μm and a maturity of the weakening of the interface 13 suitable for its rupture.
[0092] According to a second possibility of the invention, the electromagnetic radiation detector and its optical elements can be arranged to receive a portion of the light beam scattered in a plurality of second directions 25B, 25B', each of which has a non-zero angle 2θ with the first direction. In this way, the weakened state of the interface can be accurately monitored. The plurality of second directions can correspond to an angle range of 2θ with the first direction, which corresponds to several weakened states of the interface 13 of interest (thus including, for example, 10° in the first possibility described above).
[0093] According to a third possibility of the invention, the electromagnetic radiation detector 32 may be arranged to be movable so as to allow measuring the intensity of the light beam after scattering in a plurality of second directions 25B, 25B', each second direction having a non-zero angle 2θ with the first direction. As in the second possibility disclosed above, the plurality of second directions may correspond to a range of angles 2θ with the first direction corresponding to several weakening states of the interface 13 of interest (thus including, for example, the 10° mentioned above in the context of the first possibility).
[0094] It should also be noted that, according to another possibility compatible with the three possibilities described above, the weakening monitoring device 30 can be configured to move the light beam 25 in at least two positions or regions of the first face 10A, and then for said at least two regions the detector is arranged to allow the measurement of the intensity of the light beam 25 scattered by the substrate 11 / layer 12 assembly 10 in at least one second direction 25B. This possibility allows the mapping of the weakening state of the interface 13 along the first face 10A. This movement of the light beam 25 can be achieved by a suitable configuration of the light source 31, which can be arranged to be movable, or include movable optical elements, such as optical fibers and / or lenses, to allow the movement of the light beam 25. Likewise, the electromagnetic radiation detector 31 is suitable for allowing the measurement of the intensity in at least one second direction 25B in all the measurement positions of the first face 10A, or by being movable to allow the measurement in each of these positions.
[0095] It should be noted that, in the present embodiment, although the weakening furnace 40 can accommodate a single substrate / layer assembly, it is fully contemplated that the weakening furnace 40 can be adapted to perform weakening annealing on greater than or equal to two assemblies.
[0096] According to this possibility, not shown, the weakening furnace 40 may include a first position for the substrate 11 / layer 12 assembly and one or more second positions for one or more other (another) substrate / layer assemblies, so as to allow weakening annealing of the substrate 11 / layer 12 assembly and the other substrate / layer assemblies at the same time.
[0097] According to this possibility, the second position or positions are arranged so that after the light beam passes through the substrate 11 / layer 12 assembly, the surface of the other substrate / layer assembly or the plurality of assemblies is illuminated by the light beam. In addition, the electromagnetic radiation detector 32 is capable of measuring the intensity of the light beam 25 after being scattered by the other substrate / layer assembly or the plurality of assemblies, and the electromagnetic radiation detector 32 is arranged to measure the intensity of the light beam 25 in another second direction having a non-zero angle 2θ with the first direction 25A. Such an arrangement can be obtained in particular by an electromagnetic radiation detector 32 comprising at least one corresponding unit for each position and a corresponding optical system dedicated to the unit.
[0098] Of course, in a variant, the weakness monitoring device 30 may include one or more other electromagnetic radiation detectors 32 in order to measure the intensity of the light beam 25 of one or more other substrate / layer assemblies.
[0099] The weakening monitoring device 30 may further include a processing unit 33 configured to restore the intensity value of the light beam measured by the detector and determine the weakening state of the interface according to the intensity value of the light beam.
[0100] The same processing unit can also be configured to correct the measured intensity during the determination of the weakened state of the interface based on a reference intensity determined before the weakening annealing. Likewise, according to a possibility implemented among the various possibilities described above, the processing unit is able to determine the weakened state of the interface 13 based on the intensity values measured in multiple second directions 25B, 25B' and at various positions of the first face 10A. To this end, when the light source 31 is configured to allow the light beam 25 to move, and / or when the electromagnetic radiation detector 32 is configured to measure the intensity in multiple second directions, the light source 31 and / or the electromagnetic radiation detector 32 are controlled according to the possibility or possibilities.
[0101] It is worth noting that according to one possibility of the present invention, the processing unit can be configured to supply the determined weakening state of the interface 13 to the weakening furnace 40. According to this possibility, when the weakening state of the interface 13 determined by the processing unit 33 reaches a given threshold, the weakening furnace 40 can be configured to stop the weakening annealing.
[0102] According to a variant of this possibility of the invention, the processing unit can also be configured to detect spontaneous rupture of the assembly at the end of the annealing. In practice, this matter is related to a sudden change in the intensity and position of the scattered intensity, which can be detected by the weakening monitoring device 30 according to the invention. Thus, according to this variant, a given threshold of the weakening state corresponds to a rupture of the interface 13, the rupture being detected by a sudden change in the intensity in at least one second direction 25B and / or a shift in the scattering peak. In the same way, the furnace can comprise a control unit configured to communicate with the processing unit of the weakening monitoring device and to adjust the weakening annealing conditions according to the weakening state provided by the weakening monitoring device.
[0103] According to this last possibility, the annealing conditions used during the annealing step can therefore be adjusted according to the weakening state of the interface 13 determined during the implementation of the weakening monitoring method. The weakening annealing, and in particular the heating curve of the furnace, can thus be optimized according to the weakening state of the interface in order to obtain the desired microcrack distribution at the interface. This is particularly advantageous when trying to obtain rupture outside the furnace.
[0104] The weakening monitoring device 30 according to the invention allows implementing a weakening monitoring method 30 comprising the following steps:
[0105] - illuminating the first face 10A in a first direction 25A with a monochromatic light beam 25, the wavelength of the light beam 25 being chosen such that the layer 12 and the substrate 13 are substantially transparent to this wavelength,
[0106] - measuring the intensity of the light beam 25 scattered by the substrate 11 / layer 12 assembly 10 in at least one second direction 25B having a non-zero angle 2θ with the first direction 25A,
[0107] - The weakening state of the interface 13 is determined from said strength.
[0108] Of course, the method is compatible with these various possibilities, in line with the possibilities described with respect to the weakening monitoring device 30. In particular, the method according to the invention may also include a previous calibration step implemented before the weakening annealing, the previous calibration step comprising the following sub-steps:
[0109] - irradiating the first face with a monochromatic light beam 25 in a first direction 25A,
[0110] - measuring a reference intensity of the light beam 25 scattered in at least one second direction 25B by the substrate 11 / layer 12 assembly 10. During the step of determining the weakening state, a sub-step of correcting the measured intensity according to the reference intensity is then provided.
[0111] If such a weakening monitoring device 30 and the corresponding method can be used in production for a step of monitoring the rupture of the interface 13 between the layer and the support, it can also be used in more specific cases, such as calibrating the weakening furnace 40 when installing or overhauling the furnace. In this case, the weakening monitoring device 30 is not necessarily incorporated in the weakening furnace 40 and can be removably mounted to implement the calibration step. Therefore, after implementing the calibration step, the weakening monitoring device 30 can be perfectly removed.
[0112] As indicated, in a normal configuration, the entire weakening monitoring device 30 can be mounted outside the housing 40A of the weakening furnace 40, said housing 40A being provided with a viewing window transparent to the incident light 25A and the scattered light 25B.
[0113] Examples of embodiments of the present invention
[0114] In order to illustrate the implementation principle of the monitoring method according to the invention and to provide an example of determining the weakening state of an interface, an example of measurements obtained by the inventors in this implementation context is described below.
[0115] Therefore, if Figure 3 As shown, in the implementation of the method, the inventors measured the variation of the intensity 102, 103 of the scattered light beam 25 as a function of the angle 2θ between the second direction 25B and the first direction 25A during the weakening annealing of a silicon layer 12 supported by a silicon substrate 11 of two different samples, the interface 13 between the silicon layer and the substrate having previously been implanted to form a microcavity at the interface 13. By comparison, the inventors show in the same figure the variation of the intensity 101 of the scattered light beam 25 obtained on the substrate 11 / layer 12 assembly 10 before the weakening annealing as a function of the angle θ between the second direction 25B and the first direction 25A, as described below with respect to Figure 4 As mentioned, this measurement can form a reference measurement.
[0116] It can thus be seen that the agglomeration of the microcavities and the increase in their size are due to this agglomeration and the significant increase in scattered light in the 2θ angle range from 1° to 12°. Therefore, as discovered by the inventors, the scattered light is a characteristic of the size and distribution of the cavities at the interface 13 (this characteristic can be formalized based on the Fraunhofer approximation).
[0117] In order to better explain this phenomenon, the inventors Figure 4 , the difference between the intensity of the light beam 102 measured during the weakening annealing and the intensity of the light beam 101 measured before the annealing is shown as a function of the angle 2θ between the second direction 25B and the first direction 25A. It can be seen that the intensity of the scattered light associated with the weakening annealing reaches a maximum at about 9°, i.e., the microcavity size is about 8 microns.
[0118] For comparison, the inventors used a confocal microscope to obtain an infrared image of the interface 13 characterized by the weakening monitoring device during the weakening annealing. The inventors Fourier transformed the image and radially averaged the image thus obtained.
[0119] Figure 5 The result of this Fourier transformation 111 is graphically compared with the variation of the intensity as a function of twice the angle between the second direction 25B and the first direction 25A. This comparison shows that both techniques allow similar results to be obtained and therefore allow both to characterize the weakening state of the interface 13. For this confocal imaging, the method of the invention has the advantage of not requiring the placement of a lens near the sample and is therefore fully capable of being equipped with large industrial weakening furnaces.
[0120] It should be noted that within the scope of the present invention, the surface weakening state determined using the method according to the present invention can be provided, for example, in the form of one of the following values:
[0121] the angle of the second direction 25B relative to the first direction, at which the increase in the scattered intensity relative to the reference intensity determined before the weakening annealing is greatest,
[0122] a value of the size of the microcavity estimated from the intensity of the light beam 25 scattered in a second direction or directions 25B, 25B',
[0123] - an intensity value of the light beam 25 scattered in a second reference direction 25B or in a plurality of reference directions 25B, 25B'.
Claims
1. A method for monitoring the weakening of an interface (13) between a layer (12) and a substrate (11) during a weakening annealing of the interface (13), the substrate (11) / layer (12) assembly having at least a first face and a second face (10A, 10B), the method comprising the following steps: - irradiating said first face (10A) in a first direction (25A) with a monochromatic light beam (25), the wavelength of said light beam (25) being chosen such that said layer (12) and said substrate (13) are substantially transparent to said wavelength, - measuring the intensity of a light beam (25) scattered by said substrate (11) / layer (12) assembly (10) in at least one second direction (25B), said second direction (25B) having a non-zero angle (2θ) with said first direction (25A), - Determining the weakened state of said interface (13) based on said strength.
2. The weakening monitoring method according to claim 1, wherein: During measurement of the intensity of the light beam (25), the intensity is measured in a plurality of second directions (25B, 25B'), each second direction having a non-zero angle with the first direction (25A), and wherein, preferably, at least two of the second directions (25B, 25B') have different angles with respect to the first direction (25).
3. The weakening monitoring method according to claim 1 or 2, wherein: A previous calibration step is provided which is carried out before the weakening annealing, the previous calibration step comprising the following sub-steps: - irradiating said first face with a light beam (25) in said first direction (25A), - measuring a reference intensity of a light beam (25) scattered by said substrate (11) / layer (12) assembly (10) in at least one of said second directions (25B), Therein, during the step of determining the weakened state, a sub-step of correcting the measured intensity based on the reference intensity is provided.
4. The weakening monitoring method according to any one of claims 1 to 3, wherein: During illumination of the first face (10A) with the light beam (25) in the first direction, the light beam (25) moves in at least two regions of the first face (10A).
5. The weakening monitoring method according to any one of claims 1 to 4, wherein: The monochromatic light beam (25) has a wavelength in the infrared wavelength range, preferably in the near infrared wavelength, even more advantageously between 1050 nm and 1550 nm.
6. A method for weakening an interface (13) between a layer (12) and a substrate (11), the method comprising the step of performing a weakening annealing on the substrate (11) / layer (12) assembly (10) to weaken the interface (13), wherein: During the annealing step, a weakening monitoring method according to any one of claims 1 to 6 is implemented.
7. The method for weakening an interface (13) according to claim 6, wherein: When the weakening state of the interface determined by the weakening monitoring method reaches a given threshold, the weakening annealing step is stopped, and the weakening state preferably corresponds to a rupture of the interface (13), and then the rupture is detected by an intensity change and / or a movement of a scattering peak in at least one of the second directions (25B).
8. The method for weakening an interface (13) according to claim 6 or 7, wherein: The annealing conditions used during the annealing step are modified according to the weakening state of the interface (13) determined during the implementation of the weakening monitoring method.
9. A device (30) for monitoring the weakening of an interface, to monitor the weakening of the interface (13) between a layer (12) and a substrate (11) during a weakening annealing of the interface (13), the substrate (11) / layer (12) assembly (10) having at least a first face and a second face (10A, 10B), the device comprising: - a light source (31) capable of emitting a monochromatic light beam (25) in a first direction towards said first face (10A), - an electromagnetic radiation detector (32) capable of measuring the intensity of the light beam (25) after scattering through the substrate (11) / layer (12) assembly (10), the electromagnetic radiation detector being arranged to measure the intensity of the light beam (25) in a second direction having a non-zero angle (2θ) with respect to the first direction (25A).
10. The weakening monitoring device (30) according to claim 9, wherein: The electromagnetic radiation detector is arranged to allow measurement of the intensity of the light beam (25) after scattering in a plurality of second directions (25B, 25B'), each second direction having a non-zero angle with the first direction (25A), and wherein, preferably, at least two of the second directions (25B, 25B') have different angles with respect to the first direction (25).
11. The weakening monitoring device (30) according to claim 9 or 10, further comprising a processing unit (33), which is configured to restore the intensity value of the light beam (25) measured by the detector (32) and determine the weakening state of the interface (13) based on the intensity value of the light beam (25).
12. The weakening monitoring device (30) according to claim 11, wherein: The processing unit (33) is further configured to correct the measured intensity according to a reference intensity determined before weakening annealing during determination of the weakened state of the interface.
13. An annealing furnace (40) capable of performing weakening annealing to weaken the interface between a layer and a substrate, the annealing furnace (40) comprising a weakening monitoring device according to any one of claims 9 to 12.
14. The annealing furnace (40) according to claim 13, comprising a first position for the substrate (11) / layer (12) assembly and at least one second position for a further substrate / layer assembly, so as to allow a weakening annealing of the substrate (11) / layer (12) assembly and the further substrate / layer assembly simultaneously, in, The second position is arranged such that the surface of the further substrate / layer assembly is illuminated by the light beam after the light beam has passed through the substrate (11) / layer (12) assembly, and The electromagnetic radiation detector (32) is also capable of measuring the intensity of the light beam (25) after being scattered by the other substrate / layer assembly, and the electromagnetic radiation detector (32) is arranged to measure the intensity of the light beam (25) in another second direction having a non-zero angle (2θ) with the first direction (25A).
15. The annealing furnace (40) according to claim 13 or 14 is configured so that when implementing weakening annealing, when the weakening monitoring device (30) determines that the weakened state of the measured interface (13) reaches a given threshold, the annealing of the substrate (11) / layer (12) assembly (10) is stopped.