Textile fabric children mask and preparation method thereof
By adopting a three-layer textile fabric design, the problem of poor moisture permeability and breathability of children's masks is solved, and the moisture permeability of the inner layer of the mask is improved and the wear comfort is achieved, meeting the filtering performance and hygiene requirements of children's masks.
Patent Information
- Application Number
- CN202310585896.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-05-23
- Publication Date
- 2024-11-26
AI Technical Summary
Existing children's masks have poor moisture permeability and breathability, which causes exhaled water vapor to condense in the inner layer of the mask, causing skin discomfort and is not suitable for long-term use.
Design of a three-layer structural mask consisting of textile fabric A, hydrogen-adjusting polypropylene meltblown fabric and textile fabric B, textile fabric A is used as the outer layer, hydrogen-adjusting polypropylene meltblown fabric is used as the intermediate layer, and textile fabric B is used as the inner layer. The layer, through specific lamination arrangement and process processing, improves the one-way guide wettability and breathability of the mask.
It has achieved improved moisture permeability of the inner layer of the mask, prevented water vapor from condensing, enhanced wear comfort, and met the filtering performance indicators of children's masks, and has no odor, which is suitable for medical and health purposes.
Smart Images

Figure CN119014624A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of polypropylene materials, and in particular to a children's mask made of textile fabrics and a preparation method thereof. Background Art
[0002] With the rapid growth of my country's national economy and the continuous acceleration of urbanization, the problem of air pollution has aroused widespread concern in the whole society.
[0003] At present, most children's masks on the market can only block the spread of large particles such as droplets, pollen, and microorganisms in daily environments. They are not ideal in blocking pollutants such as PM2.5 and are not suitable for young children. At the same time, although the N95 series of protective masks have good blocking effects, they have poor breathability and are not suitable for long-term use by young children.
[0004] CN114714707A discloses a breathable and highly elastic mask fabric and a preparation method thereof. Modified graphene oxide is introduced when preparing the upper and lower layers of non-woven fabrics. The calcium ions interact with the amino graphene oxide sheets to improve the elasticity of the non-woven fabrics. Tannic acid is used to cross-link the modified graphene oxide to improve the heat resistance of the non-woven fabrics.
[0005] However, when using anti-stick non-woven materials, the water vapor exhaled by the human body often condenses on the inner layer of the mask, and long-term use may cause problems such as skin discomfort in children.
[0006] Therefore, it is necessary to provide a children's mask that can improve the moisture permeability of the inner layer of the mask and the air permeability of the outer layer of the mask while meeting the filtering performance indicators. Summary of the invention
[0007] The purpose of the invention is to overcome the defects of the prior art children's mask that has poor moisture permeability, poor air permeability and is not suitable for long-term use.
[0008] In order to achieve the above-mentioned object, the first aspect of the present invention provides a textile fabric children's mask, the textile fabric children's mask comprising a mask body, a nose bridge strip, and mask ropes fixed on both sides of the mask body, the mask body comprising an outer layer, an inner layer, and an intermediate layer arranged between the outer layer and the inner layer;
[0009] The material forming the outer layer is a textile fabric A, the air permeability of the textile fabric A is 1500-1800 mm / s, and the water contact angle is 120-130°;
[0010] The material forming the inner layer is a textile fabric B, the wetting time of the textile fabric B is 2-3s, and the maximum wetting radius is 20-30mm;
[0011] The textile fabric A and the textile fabric B both contain polyester, and the mass content of polyester in the textile fabric A is higher than the mass content of polyester in the textile fabric B;
[0012] The material forming the intermediate layer is hydrogen-adjusted polypropylene melt-blown cloth, and the hydrogen-adjusted polypropylene melt-blown cloth is prepared by sequentially subjecting hydrogen-adjusted polypropylene and electret masterbatch to melt blending, melt-blowing spinning, and cooling and solidification treatment;
[0013] The melt-blowing spinning treatment conditions at least meet the following requirements: screw speed of 2-6 rpm, spinneret temperature of 200-220° C., hot air temperature of 220-240° C., hot air blower frequency of 20-30 Hz, receiving distance of 16-22 cm, and electret voltage of 0-60 kV.
[0014] The second aspect of the present invention provides a method for preparing the textile fabric children's mask according to the first aspect, the method comprising:
[0015] (1) stacking the textile fabric A, the hydrogen-adjusted polypropylene meltblown fabric, and the textile fabric B in order from outside to inside to obtain a mask body;
[0016] (2) A nose bridge strip is sewn on the upper side of the mask body, and the mask rope is fixed on the left and right sides of the mask body.
[0017] The present invention synergistically compounds specific types of textile fabrics A and textile fabrics B with a hydrogen-adjusted polypropylene melt-blown cloth in a specific ratio to form a mask body. The textile fabric children's mask prepared by the mask body has excellent unidirectional moisture conductivity, waterproofness and air permeability, and is also odorless and comfortable to wear.
[0018] The textile fabric children's mask provided by the present invention has a reasonable structural design and is comfortable to wear. Its outer layer has the characteristics of being water-repellent and breathable, and its inner layer has the characteristics of being unidirectional moisture conduction and non-irritating to the skin. While meeting the filtering performance indicators, the moisture permeability of the inner layer of the mask is improved, so that the exhaled water vapor does not condense on the inner layer of the mask, and secondly, the comfort of contact with the skin is improved.
[0019] The middle layer of the textile fabric children's mask provided by the present invention adopts hydrogen-adjusted polypropylene melt-blown cloth, which is different from the polypropylene melt-blown cloth commonly prepared by the degradation method in industry. The melt-blown cloth of the children's mask is made by using hydrogen-adjusted polypropylene as the raw material for melt-blown spinning. The volatile organic matter content of the product is lower than that of the product of the chemical degradation method, and it is more hygienic and environmentally friendly, and is more suitable for medical and sanitary products such as masks.
[0020] The process optimization of meltblown spinning treatment involved in the present invention realizes the characteristics of high efficiency and low resistance of meltblown cloth for children's masks, meets the relevant filtration performance requirements of children's sanitary masks in the "GB / T 38880-2020 Technical Specifications for Children's Masks", and does not have an unpleasant odor when used to make masks, solving the problem of strong odor caused by the use of polypropylene obtained by ordinary degradation method to make meltblown cloth for existing children's masks. BRIEF DESCRIPTION OF THE DRAWINGS
[0021] Figure 1 is a schematic diagram of the surface water contact angle of the textile fabric A1 in Example 1;
[0022] Figure 2a is a scanning electron microscope spectrum of the textile fabric A1 in Example 1;
[0023] Figure 2b is a scanning electron microscope spectrum of the textile fabric A1 in Example 1;
[0024] Figure 2c is a scanning electron microscope spectrum of the textile fabric A1 in Example 1;
[0025] Figure 2d is a scanning electron microscope spectrum of the textile fabric A1 in Example 1;
[0026] Figure 3a is a scanning electron microscope spectrum of the textile fabric B1 in Example 1;
[0027] Figure 3b is a scanning electron microscope spectrum of the textile fabric B1 in Example 1;
[0028] Figure 3c is a scanning electron microscope spectrum of the textile fabric B1 in Example 1;
[0029] Figure 3d is a scanning electron microscope spectrum of the textile fabric B1 in Example 1;
[0030] Figure 4 is a scanning electron microscope spectrum of the hydrogen-adjusted polypropylene melt-blown fabric C1 in Example 1;
[0031] Figure 5a is a scanning electron microscope spectrum of the cross-sectional structure of the textile fabric B1 in Example 1;
[0032] Figure 5b This is a scanning electron microscope spectrum of the cross-sectional structure of the textile fabric B1 in Example 1. DETAILED DESCRIPTION
[0033] The endpoints and any values of the ranges disclosed in this article are not limited to the precise ranges or values, and these ranges or values should be understood to include values close to these ranges or values. For numerical ranges, the endpoint values of each range, the endpoint values of each range and the individual point values, and the individual point values can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed in this article.
[0034] In the present invention, unless otherwise specified, the room temperature or normal temperature refers to 25±2°C.
[0035] In the present invention, unless otherwise specified, the hot air temperature refers to the temperature of air after being heated in the melt-blowing spinning process.
[0036] In the present invention, unless otherwise stated, the receiving distance is the horizontal distance from the mesh curtain receiver to the outlet of the spinneret.
[0037] As mentioned above, the first aspect of the present invention provides a textile fabric children's mask, which includes a mask body, a nose bridge strip, and mask ropes fixed to both sides of the mask body, wherein the mask body includes an outer layer, an inner layer, and an intermediate layer arranged between the outer layer and the inner layer;
[0038] The material forming the outer layer is a textile fabric A, the air permeability of the textile fabric A is 1500-1800 mm / s, and the water contact angle is 120-130°;
[0039] The material forming the inner layer is a textile fabric B, the wetting time of the textile fabric B is 2-3s, and the maximum wetting radius is 20-30mm;
[0040] The textile fabric A and the textile fabric B both contain polyester, and the mass content of polyester in the textile fabric A is higher than the mass content of polyester in the textile fabric B;
[0041] The material forming the intermediate layer is hydrogen-adjusted polypropylene melt-blown cloth, and the hydrogen-adjusted polypropylene melt-blown cloth is prepared by sequentially subjecting hydrogen-adjusted polypropylene and electret masterbatch to melt blending, melt-blowing spinning, and cooling and solidification treatment;
[0042] The melt-blowing spinning treatment conditions at least meet the following requirements: screw speed of 2-6 rpm, spinneret temperature of 200-220° C., hot air temperature of 220-240° C., hot air blower frequency of 20-30 Hz, receiving distance of 16-22 cm, and electret voltage of 0-60 kV.
[0043] The textile fabrics described in the present invention refer to knitted fabrics or woven fabrics, excluding non-woven fabrics. Woven fabrics refer to fabrics formed by interweaving warp yarns and weft yarns perpendicular to each other according to a certain pattern; knitted fabrics refer to fabrics formed by knitting needles to form coils of yarns, which are then longitudinally strung and transversely connected.
[0044] According to a particularly preferred embodiment, the hydrogen-adjusted polypropylene meltblown fabric is prepared by a method comprising the following steps:
[0045] S1: melt-blending the hydrogen-modulated polypropylene and the electret masterbatch at a speed of 60-100 rpm to obtain a melt-blended material, and filtering the melt-blended material to obtain a hydrogen-modulated polypropylene melt;
[0046] S2: subjecting the hydrogen-conditioned polypropylene melt to melt-blown spinning to obtain hydrogen-conditioned melt-blown fabric fibers;
[0047] S3: Cooling and solidifying the hydrogen-adjusted meltblown fabric fibers in a mesh curtain receiving device to obtain the hydrogen-adjusted polypropylene meltblown fabric.
[0048] Preferably, in step S1, the conditions of the melt blending treatment at least meet the following conditions: temperature of 200-260°C, time of 0.2-1h, and pressure of 3-5MPa.
[0049] The present invention has no special requirements on the equipment and process used for the filtration treatment, and any commercial filtration technology can be used. The present invention will not describe in detail the specific preparation methods of the various compounds of the present invention, and those skilled in the art should not understand this as a limitation of the present invention.
[0050] Preferably, in step S2, the conditions of the melt-blown spinning treatment at least meet the following requirements: the screw speed is 4-6rpm, the spinneret temperature is 210-220°C, the hot air temperature is 230-240°C, the hot air blower frequency is 25-30Hz, the receiving distance is 16-20cm, and the electret voltage is 30-60kV. The inventors of the present invention found in their research that when the spinneret temperature of the melt-blown spinning treatment is higher than 220°C, the melt flow is unstable, resulting in the paralleling of the wires, which makes the wire diameter thicker, and the obtained hydrogen-adjusted polypropylene melt-blown cloth has uneven wire diameter and reduced filtration efficiency. Therefore, the present invention preferably has a spinneret temperature of 210-220°C for the melt-blown spinning treatment. In addition, the screw speed of the melt-blown spinning treatment directly affects the extrusion amount of the material, and thus affects the mechanical properties and filtration properties of the hydrogen-adjusted melt-blown cloth fibers. The inventors of the present invention found in their research that controlling the screw speed of the melt-blown spinning treatment in the range of 4-6rpm can obtain a hydrogen-adjusted polypropylene melt-blown cloth with better mechanical properties and filtration properties.
[0051] The present invention has no particular limitation on the specific models of the instruments and equipment used for the meltblowing spinning process. As long as the condition parameters specified in the present invention can be achieved, those skilled in the art can choose the instruments and equipment known in the art. The present invention will not go into details here, and those skilled in the art should not understand it as a limitation of the present invention.
[0052] Preferably, in step S2, the average diameter of the hydrogen-adjusted meltblown fabric fibers is 1-7 μm.
[0053] Preferably, in step S3, the cooling and curing treatment conditions at least meet the following conditions: temperature of 20-30°C and time of 0.2-0.5h.
[0054] The present invention has no special requirements for the net curtain receiving device, and any commercial net curtain receiving device can be used. The present invention will not describe in detail the specific preparation methods of the various compounds of the present invention, and those skilled in the art should not understand this as a limitation of the present invention; illustratively, the net curtain receiving device used in the present invention is a net curtain receiver.
[0055] Preferably, the content of polyester in the textile fabric A is 5-50wt% higher than that in the textile fabric B. More preferably, the content of polyester in the textile fabric A is 5-30wt% higher than that in the textile fabric B. The inventors found in their research that making the mass content of polyester in the textile fabric A higher than that in the textile fabric B can make the fabric have stronger light resistance and sun fastness.
[0056] According to a preferred specific implementation, based on the total mass of the textile fabric A, the textile fabric A contains 80-100wt% of polyester and 0-20wt% of spandex.
[0057] According to a preferred specific implementation, based on the total mass of the textile fabric B, the textile fabric B contains 50-75wt% of polyester, 0-30wt% of polypropylene, and 10-30wt% of spandex.
[0058] According to a particularly preferred embodiment, based on the total mass of the textile fabric B, the textile fabric B contains 70-75wt% of polyester and 25-30wt% of spandex.
[0059] Preferably, the water absorption rate of the textile fabric B is 20-30% / s, and the diffusion speed is 4-6.5 mm / s.
[0060] It should be noted that the present invention has no special requirements for the method for obtaining the textile fabric A and the textile fabric B. They can be obtained through commercial purchase or prepared in combination with methods known in the art. The present invention will not be elaborated here, and those skilled in the art should not understand it as a limitation of the present invention.
[0061] Preferably, in the hydrogen-adjusted polypropylene meltblown fabric, the mass ratio of the hydrogen-adjusted polypropylene to the electret masterbatch is 15-30:1. More preferably, in the hydrogen-adjusted polypropylene meltblown fabric, the mass ratio of the hydrogen-adjusted polypropylene to the electret masterbatch is 19-25:1. The inventors found in their research that adding electret masterbatch to the hydrogen-adjusted polypropylene meltblown fabric and limiting the mass ratio of the two under the aforementioned more preferred conditions can effectively increase the density and depth of the charge capture energy well in the meltblown non-woven fabric, thereby improving the comprehensive filtration efficiency and thermal attenuation resistance of the meltblown non-woven fabric.
[0062] Preferably, the hydrogen-adjusted polypropylene has a melt flow rate of 1500-1600 g / 10 min at 230° C. and 0.3 MPa, a total volatile organic compound content of 10-90 μg / g, a weight average molecular weight of 63,000-67,000, a number average molecular weight of 18,000-22,000, and a molecular weight distribution of 3.0-3.5.
[0063] The calculation formula of the molecular weight distribution in the present invention is: molecular weight distribution = weight average molecular weight / number average molecular weight.
[0064] In the present invention, the total volatile organic compounds include aromatic hydrocarbons (benzene, toluene, xylene), ketones, aldehydes, amines, halogenated hydrocarbons, unsaturated hydrocarbons, etc.
[0065] Preferably, in the hydrogen-adjusted polypropylene, based on the total number of molecules in the hydrogen-adjusted polypropylene, the number of molecules with a weight average molecular weight of 0-10,000 accounts for 9.5-12.5%, the number of molecules with a weight average molecular weight of 10,000-50,000 accounts for 39.5-43.5%, the number of molecules with a weight average molecular weight of 50,000-100,000 accounts for 26.1-30.1%, the number of molecules with a weight average molecular weight of 100,000-500,000 accounts for 17.5-21.5%, and the number of molecules with a weight average molecular weight of 500,000-1,000,000 accounts for 0.01-0.05%.
[0066] Preferably, the hydrogen-adjusted polypropylene has a melting temperature of 145.5-155.5°C, a crystallization temperature of 100.5-115.5°C, a melting enthalpy of 115-130 kJ / kg, and a crystallization enthalpy of 110-115 kJ / kg.
[0067] Particularly preferably, the hydrogen-regulated polypropylene is a hydrogen-regulated polypropylene of model MJ1H15 purchased from Beijing Yanshan Petrochemical Co., Ltd. The inventors found in their research that the use of hydrogen-regulated polypropylene in this preferred case is more conducive to the cooling and shaping of the yarns during the melt-blown spinning process, maintains the uniformity of the yarn diameter, and reduces the proportion of parallel yarns.
[0068] As mentioned above, the second aspect of the present invention provides a method for preparing the textile fabric children's mask described in the first aspect, the method comprising:
[0069] (1) stacking the textile fabric A, the hydrogen-adjusted polypropylene meltblown fabric, and the textile fabric B in order from outside to inside to obtain a mask body;
[0070] (2) A nose bridge strip is sewn on the upper side of the mask body, and the mask rope is fixed on the left and right sides of the mask body.
[0071] Preferably, in step (1), the textile fabric A is subjected to a water-repellent treatment before the lamination is performed.
[0072] The present invention has no special requirements on the equipment and specific process used for the water repellent treatment, and any water repellent treatment technology known in the art can be used. For example, the present invention provides a preferred specific embodiment of the water repellent treatment, including:
[0073] Y1: soaking the textile fabric A in a 10-30wt% perfluoro acrylic copolymer solution for 30-60 minutes, drying it, and curing it in an oven at 100-120°C for 1-2 hours to obtain a textile fabric I; and
[0074] Dissolving polydimethylsiloxane in heptane to obtain a polydimethylsiloxane solution with a concentration of 15-20 wt %, and subjecting the silicon dioxide nanoparticles and the polydimethylsiloxane solution to ultrasonic treatment to obtain a mixed solution;
[0075] Y2: coating the mixed solution on the textile fabric I, and crosslinking the coated textile fabric for 20-30 hours at a temperature of 20-40° C. and a relative humidity of 60-70% to obtain a water-repellent treated textile fabric.
[0076] Preferably, in step Y1, the drying treatment conditions at least meet the following conditions: temperature is 100-110° C., and time is 10-20 s.
[0077] Preferably, in step Y1, the conditions of the ultrasonic treatment at least meet the following requirements: time of 15-30s, frequency of 20-30kHz, power of 700-800W.
[0078] The present invention has no special requirements for the specific process equipment and specific process methods used to prepare the textile fabric children's mask. Those skilled in the art can carry out the preparation in combination with the equipment and process methods known in the art. The present invention will not be repeated here, and those skilled in the art should not understand it as a limitation of the present invention.
[0079] The present invention will be described in detail below by way of examples. In the following examples, unless otherwise specified, all the raw materials used are commercially available products.
[0080] In the following examples, the textile fabric children's mask was prepared in accordance with the provisions of the national standard GB / T 38880-2020.
[0081] In the following examples, the main properties of the used textile fabrics A and B are shown in Table 1 and Table 2 respectively.
[0082] In the following examples, the air permeability is measured according to the GB / T5453-1997 method using a YG813 fully automatic air permeability tester (purchased from Quanzhou Meibang Instrument Co., Ltd.).
[0083] In the following examples, the water contact angle was measured according to ISO / TS 14778:2021 method using a dynamic / static water contact angle meter SL200B (purchased from Conoco Industries, Inc., USA).
[0084] In the following examples, the wetting time, water absorption rate, diffusion rate, and maximum wetting radius were measured according to the AATCC TM 195 method using an M290 fabric moisture management instrument (SILAC Atlas (Shenzhen) Co., Ltd.).
[0085] Outer material: 100wt% polyester, white fabric 20074696, purchased from Dongguan Chaoying Textile Co., Ltd., named textile fabric A1.
[0086] Outer material: 80wt% polyester, 20% spandex, black fabric D-P32064S, purchased from Guangdong Derun Textile Co., Ltd., named textile fabric A2.
[0087] Inner layer material: 72wt% polyester and 28wt% spandex, white lining material WB200490D1, purchased from Dongguan Chaoying Textile Co., Ltd., named textile fabric B1.
[0088] Inner layer material: 53wt% polyester and 47wt% polypropylene, grey lining U00088SD, purchased from Quanzhou Haitian Materials Technology Co., Ltd., named textile fabric B2.
[0089] Hydrogen-adjusted polypropylene: MJ1H15, purchased from Beijing Yanshan Petrochemical Co., Ltd.; the melt flow rate at 230°C and 0.3MPa is 1570g / 10min, the total volatile organic compound content is 50μg / g, the weight average molecular weight is 65,000, the number average molecular weight is 20,000, and the molecular weight distribution is 3.3; based on the total number of molecules in hydrogen-adjusted polypropylene, the number of molecules with a weight average molecular weight of 0-10,000 accounts for 10.9%, and the weight average molecular weight is 20,000. The number of molecules with a weight average molecular weight of 10,000-50,000 accounts for 41.39%, the number of molecules with a weight average molecular weight of 50,000-100,000 accounts for 28.13%, the number of molecules with a weight average molecular weight of 100,000-500,000 accounts for 19.55%, and the number of molecules with a weight average molecular weight of 500,000-1,000,000 accounts for 0.03%; the melting temperature is 150.5°C, the crystallization temperature is 107.7°C, the melting enthalpy is 124.1 kJ / kg, and the crystallization enthalpy is 113.3 kJ / kg.
[0090] Polypropylene meltblown material: model PP-91500, purchased from Kingfa Technology Co., Ltd.
[0091] Spunbond nonwoven fabric: purchased from Quanzhou Smartin Import and Export Trading Co., Ltd.
[0092] Electret masterbatch: model JZ-1500, purchased from Guangxi Dongqin Chemical Co., Ltd.
[0093] In the following examples, the amount of hydrogen-adjusted polypropylene used is 2.5 kg.
[0094] Table 1
[0095] Textile fabrics Air permeability (mm / s) Water contact angle (°) Textile fabric A1 1706.17 124.5 Textile fabric A2 457.25 63.5
[0096] Table 2
[0097]
[0098]
[0099] Preparation Example 1
[0100] This preparation example provides a method for preparing a hydrogen-adjusted polypropylene melt-blown cloth, the method comprising:
[0101] S1: melt blending hydrogen-modulated polypropylene and electret masterbatch in a mass ratio of 24:1 in a screw extruder at a speed of 70 rpm at 230°C and 5 MPa for 0.2 h, and then filtering the obtained molten blended material to obtain a hydrogen-modulated polypropylene melt;
[0102] S2: melt-blowing the hydrogen-adjusted polypropylene melt under the conditions of a screw speed of 6 rpm, a spinneret temperature of 220° C., a hot air temperature of 240° C., a hot air blower frequency of 30 Hz, a receiving distance of 16 cm, and an electret voltage of 60 kV to obtain hydrogen-adjusted melt-blown fabric fibers;
[0103] S3: Cooling and curing the hydrogen-conditioned meltblown fabric fibers in a mesh curtain receiver at 20° C. for 0.2 h to obtain a hydrogen-conditioned polypropylene meltblown fabric C1.
[0104] Preparation Example 2
[0105] S1: melt blending hydrogen-modulated polypropylene and electret masterbatch in a mass ratio of 20:1 in a screw extruder at a speed of 70 rpm at 230°C and 5 MPa for 0.2 h, and then filtering the obtained molten blended material to obtain a hydrogen-modulated polypropylene melt;
[0106] S2: melt-blowing the hydrogen-adjusted polypropylene melt under the conditions of a screw speed of 6 rpm, a spinneret temperature of 220° C., a hot air temperature of 240° C., a hot air blower frequency of 30 Hz, a receiving distance of 16 cm, and an electret voltage of 60 kV to obtain hydrogen-adjusted melt-blown fabric fibers;
[0107] S3: Cooling and curing the hydrogen-conditioned meltblown fabric fibers in a mesh curtain receiver at 20° C. for 0.2 h to obtain a hydrogen-conditioned polypropylene meltblown fabric C2.
[0108] Preparation Example 3
[0109] This preparation example was carried out using a process similar to that of Preparation Example 1, except that in step S2, the screw speed of the melt-blown spinning process was adjusted from 6 rpm to 3 rpm;
[0110] The rest is the same as in Preparation Example 1, and hydrogen-adjusted polypropylene meltblown cloth C3 is prepared.
[0111] Preparation Example 4
[0112] This preparation example was carried out using a process similar to that of Preparation Example 1, except that in step S2, the temperature of the spinneret for melt-blowing treatment was adjusted from 220°C to 200°C;
[0113] The rest is the same as in Preparation Example 1, and hydrogen-adjusted polypropylene melt-blown cloth C4 is prepared.
[0114] Comparative Preparation Example 1
[0115] This comparative preparation example was carried out using a process similar to that of Preparation Example 1, except that in step S2, the screw speed of the melt-blown spinning process was adjusted from 6 rpm to 8 rpm;
[0116] The rest is the same as in Preparation Example 1, and hydrogen-adjusted polypropylene melt-blown cloth DC1 is prepared.
[0117] Comparative Preparation Example 2
[0118] This comparative preparation example was carried out using a process similar to that of Preparation Example 1, except that in step S2, the spinneret temperature of the melt-blown spinning treatment was adjusted from 220°C to 240°C;
[0119] The rest is the same as in Preparation Example 1, and hydrogen-adjusted polypropylene melt-blown cloth DC2 is prepared.
[0120] Example 1
[0121] This embodiment provides a method for preparing a children's mask made of textile fabric, the method comprising:
[0122] (1) Soaking a cleaned 20 cm×20 cm textile fabric A1 in 1000 mL of a 15 wt % perfluoroacrylic copolymer solution for 30 min, drying the dried textile fabric at 105° C. for 10 s, and curing the dried textile fabric in an oven at 120° C. for 1 h to obtain a textile fabric I; and dissolving polydimethylsiloxane in heptane to obtain a 15 wt % polydimethylsiloxane solution, and ultrasonically treating the silicon dioxide nanoparticles and the polydimethylsiloxane solution at a frequency of 20 kHz and a power of 750 W for 15 s to obtain a mixed solution;
[0123] (2) coating the mixed solution on the textile fabric I, and crosslinking the coated textile fabric for 24 hours at a temperature of 25° C. and a relative humidity of 65%, to obtain a water-repellent treated textile fabric A1;
[0124] (3) stacking the water-repellent treated textile fabric A1, hydrogen-adjusted polypropylene meltblown fabric C1, and textile fabric B1 in order from outside to inside to obtain a mask body;
[0125] (4) A nose bridge strip is sewn on the upper side of the mask body, and mask ropes are fixed on the left and right sides of the mask body to obtain a textile fabric children's mask.
[0126] Example 2
[0127] A textile fabric children's mask is prepared in a manner similar to that of Example 1, except that in step (3), the hydrogen-adjusted polypropylene meltblown cloth C1 is replaced with an equal mass of hydrogen-adjusted polypropylene meltblown cloth C2.
[0128] The remaining steps are the same as those in Example 1 to obtain a children's mask made of textile fabric.
[0129] Example 3
[0130] A textile fabric children's mask is prepared in a manner similar to that of Example 1, except that in step (3), the hydrogen-adjusted polypropylene meltblown cloth C1 is replaced with an equal mass of hydrogen-adjusted polypropylene meltblown cloth C3.
[0131] The remaining steps are the same as those in Example 1 to obtain a children's mask made of textile fabric.
[0132] Example 4
[0133] A textile fabric children's mask is prepared in a manner similar to that of Example 1, except that in step (3), the hydrogen-adjusted polypropylene meltblown cloth C1 is replaced with an equal mass of hydrogen-adjusted polypropylene meltblown cloth C4.
[0134] The remaining steps are the same as those in Example 1 to obtain a children's mask made of textile fabric.
[0135] Comparative Example 1
[0136] A children's mask made of textile fabric is prepared in a manner similar to that of Example 1, except that in step (1), the textile fabric A1 is replaced with a spunbonded nonwoven fabric of equal mass.
[0137] The remaining steps are the same as those in Example 1 to obtain a children's mask made of textile fabric.
[0138] Comparative Example 2
[0139] A children's mask made of textile fabric is prepared in a manner similar to that of Example 1, except that in step (3), the textile fabric B1 is replaced with a spunbonded nonwoven fabric of equal mass.
[0140] The remaining steps are the same as those in Example 1 to obtain a children's mask made of textile fabric.
[0141] Comparative Example 3
[0142] A textile fabric children's mask was prepared in a manner similar to that of Example 1, except that in step (3), the hydrogen-adjusted polypropylene meltblown cloth C1 was replaced with a polypropylene meltblown material of model PP-91500 of equal mass.
[0143] The remaining steps are the same as those in Example 1 to obtain a children's mask made of textile fabric.
[0144] Comparative Example 4
[0145] A textile fabric children's mask is prepared in a manner similar to that of Example 1, except that in step (3), the hydrogen-adjusted polypropylene meltblown cloth C1 is replaced with an equal mass of hydrogen-adjusted polypropylene meltblown cloth DC1.
[0146] The remaining steps are the same as those in Example 1 to obtain a children's mask made of textile fabric.
[0147] Comparative Example 5
[0148] A textile fabric children's mask is prepared according to a method similar to Example 1, except that in step (3), the hydrogen-adjusted polypropylene melt-blown cloth C1 is replaced with an equal mass of hydrogen-adjusted polypropylene melt-blown cloth DC2.
[0149] The remaining steps are the same as those in Example 1 to obtain a children's mask made of textile fabric.
[0150] Comparative Example 6
[0151] A textile fabric children's mask is prepared in a manner similar to that of Example 1, except that in step (1), textile fabric A1 is replaced with textile fabric A2 of equal mass.
[0152] The remaining steps are the same as those in Example 1 to obtain a children's mask made of textile fabric.
[0153] Comparative Example 7
[0154] A textile fabric children's mask is prepared in a manner similar to that of Example 1, except that in step (3), the textile fabric B1 is replaced with a textile fabric B2 of equal mass.
[0155] The remaining steps are the same as those in Example 1 to obtain a children's mask made of textile fabric.
[0156] Test Example 1
[0157] Under the condition of an air flow rate of 32 L / min, the counting scanning air filter material detector TSI 3160 produced by TSI of the United States was used. In accordance with the provisions of the national standard GB / T 38880-2020, the materials prepared in the preparation example, embodiment and comparative example were respectively tested for particulate matter filtration efficiency and filtration resistance. The specific test results are shown in Table 3.
[0158] Table 3
[0159]
[0160]
[0161] It can be seen from the above results that the textile fabric children's mask prepared by the method provided by the present invention has high particle filtration efficiency, can effectively block the spread of pollutants, and meets the relevant technical indicators in the Technical Specifications for Children's Masks (GB / T 38880-2020).
[0162] At the same time, the textile fabric children's mask prepared by the method provided by the present invention has good waterproof performance and air permeability, so that the exhaled water vapor does not condense on the inner layer of the mask, and is comfortable to wear and has no odor.
[0163] The present invention illustratively provides a schematic diagram of the surface water contact angle of the textile fabric A1 in Example 1, a scanning electron microscope spectrum of the textile fabric A1, a scanning electron microscope spectrum of the textile fabric B1, a scanning electron microscope spectrum of the hydrogen-modulated polypropylene meltblown cloth C1 at different temperatures, and a scanning electron microscope spectrum of the cross-sectional structure of the textile fabric B1.
[0164] Figure 1 Schematic diagram of the surface water contact angle of the textile fabric A1 in Example 1. It can be seen from the figure that the water contact angle of the textile fabric A1 is 124.5°, which shows hydrophobicity.
[0165] Figure 2a is a scanning electron microscope spectrum of the textile fabric A1 in Example 1. Figure 2a In the scanning electron microscope, the acceleration voltage is 8 kV and the magnification is 500 times.
[0166] Figure 2b is a scanning electron microscope spectrum of the textile fabric A1 in Example 1. Figure 2b In the scanning electron microscope, the acceleration voltage is 8 kV and the magnification is 200 times.
[0167] Figure 2c is a scanning electron microscope spectrum of the textile fabric A1 in Example 1. Figure 2c In the scanning electron microscope, the acceleration voltage is 8 kV and the magnification is 500 times.
[0168] Figure 2d is a scanning electron microscope spectrum of the textile fabric A1 in Example 1. Figure 2d In the scanning electron microscope, the acceleration voltage is 8 kV and the magnification is 500 times.
[0169] Combination Figure 2a , Figure 2b , Figure 2c and Figure 2d It can be seen that the fiber surface is smooth and the thickness is uniform, and the weaving is neatly arranged.
[0170] Figure 3a is a scanning electron microscope spectrum of the textile fabric B1 in Example 1. Figure 3a In the scanning electron microscope, the accelerating voltage is 8 kV and the magnification is 100 times.
[0171] Figure 3b is a scanning electron microscope spectrum of the textile fabric B1 in Example 1. Figure 3b In the scanning electron microscope, the acceleration voltage is 8 kV and the magnification is 200 times.
[0172] Figure 3cis a scanning electron microscope spectrum of the textile fabric B1 in Example 1. Figure 3c In the scanning electron microscope, the acceleration voltage is 8 kV and the magnification is 500 times.
[0173] Figure 3d is a scanning electron microscope spectrum of the textile fabric B1 in Example 1. Figure 3d In the scanning electron microscope, the acceleration voltage is 8 kV and the magnification is 500 times.
[0174] Combination Figure 3a , Figure 3b , Figure 3c and Figure 3d It can be seen that the fiber surface is smooth and uniform in thickness, the weaving is neatly arranged, and the gaps between the fibers are conducive to increasing air permeability and effectively reducing breathing resistance.
[0175] Figure 4 This is a scanning electron microscope spectrum of the hydrogen-adjusted polypropylene meltblown fabric C1 in Example 1. Figure 4 In the scanning electron microscope, the acceleration voltage is 5kV, the working distance is 10mm, and the magnification is 500 times. The average diameter of the hydrogen-adjusted polypropylene meltblown fabric at position ① in the figure is 4.76μm, the average diameter of the hydrogen-adjusted polypropylene meltblown fabric at position ② is 6.45μm, and the average diameter of the hydrogen-adjusted polypropylene meltblown fabric at position ③ is 2.09μm.
[0176] from Figure 4 It can be seen that the hydrogen-adjusted polypropylene melt-blown cloth prepared by the method provided by the present invention has uniform wire diameter and no obvious wire paralleling phenomenon.
[0177] Figure 5a is a scanning electron microscope spectrum of the cross-sectional structure of the textile fabric B1 in Example 1. Figure 5a In the scanning electron microscope, the acceleration voltage is 8 kV and the magnification is 1000 times.
[0178] Figure 5b is a scanning electron microscope spectrum of the cross-sectional structure of the textile fabric B1 in Example 1. Figure 5b In the scanning electron microscope, the acceleration voltage is 8 kV and the magnification is 2000 times.
[0179] Combination Figure 5a and Figure 5b It can be seen that the cross-section of the textile fabric is a common circular cross-section, and the fibers are arranged closely.
[0180] The preferred embodiments of the present invention are described in detail above, but the present invention is not limited thereto. Within the technical concept of the present invention, the technical solution of the present invention can be subjected to a variety of simple modifications, including the combination of various technical features in any other suitable manner, and these simple modifications and combinations should also be regarded as the contents disclosed by the present invention and belong to the protection scope of the present invention.
Claims
1. A children's mask made of textile fabric, characterized in that: The textile fabric children's mask comprises a mask body, a nose bridge strip, and mask ropes fixed to both sides of the mask body, wherein the mask body comprises an outer layer, an inner layer, and an intermediate layer arranged between the outer layer and the inner layer; The material forming the outer layer is a textile fabric A, the air permeability of the textile fabric A is 1500-1800 mm / s, and the water contact angle is 120-130°; The material forming the inner layer is a textile fabric B, the wetting time of the textile fabric B is 2-3s, and the maximum wetting radius is 20-30mm; The textile fabric A and the textile fabric B both contain polyester, and the mass content of polyester in the textile fabric A is higher than the mass content of polyester in the textile fabric B; The material forming the intermediate layer is hydrogen-adjusted polypropylene melt-blown cloth, and the hydrogen-adjusted polypropylene melt-blown cloth is prepared by sequentially subjecting hydrogen-adjusted polypropylene and electret masterbatch to melt blending, melt-blowing spinning, and cooling and solidification treatment; The melt-blowing spinning treatment conditions at least meet the following requirements: screw speed of 2-6 rpm, spinneret temperature of 200-220° C., hot air temperature of 220-240° C., hot air blower frequency of 20-30 Hz, receiving distance of 16-22 cm, and electret voltage of 0-60 kV.
2. The textile fabric children's mask according to claim 1, wherein: The content of polyester in the textile fabric A is higher than that in the textile fabric B by 5-50wt%.
3. The textile fabric children's mask according to claim 1 or 2, wherein: Based on the total mass of the textile fabric A, the textile fabric A contains 80-100wt% of polyester and 0-20wt% of spandex.
4. The textile fabric children's mask according to any one of claims 1 to 3, wherein: Based on the total mass of the textile fabric B, the textile fabric B contains 50-75wt% of polyester, 0-30wt% of polypropylene, and 10-30wt% of spandex.
5. The textile fabric children's mask according to any one of claims 1 to 4, wherein: In the hydrogen-adjusted polypropylene melt-blown fabric, the mass ratio of the hydrogen-adjusted polypropylene to the electret masterbatch is 15-30:
1.
6. The textile fabric children's mask according to any one of claims 1 to 5, wherein: The hydrogen-adjusted polypropylene has a melt flow rate of 1500-1600 g / 10 min at 230° C. and 0.3 MPa, a total volatile organic compound content of 10-90 μg / g, a weight average molecular weight of 63,000-67,000, a number average molecular weight of 18,000-22,000, and a molecular weight distribution of 3.0-3.
5.
7. The textile fabric children's mask according to any one of claims 1 to 6, wherein: In the hydrogen-adjusted polypropylene, based on the total number of molecules in the hydrogen-adjusted polypropylene, the number of molecules with a weight average molecular weight of 0-10,000 accounts for 9.5-12.5%, the number of molecules with a weight average molecular weight of 10,000-50,000 accounts for 39.5-43.5%, the number of molecules with a weight average molecular weight of 50,000-100,000 accounts for 26.1-30.1%, the number of molecules with a weight average molecular weight of 100,000-500,000 accounts for 17.5-21.5%, and the number of molecules with a weight average molecular weight of 500,000-1,000,000 accounts for 0.01-0.05%.
8. The textile fabric children's mask according to any one of claims 1 to 7, wherein: The hydrogen-adjusted polypropylene has a melting temperature of 145.5-155.5° C., a crystallization temperature of 100.5-115.5° C., a melting enthalpy of 115-130 kJ / kg, and a crystallization enthalpy of 110-115 kJ / kg.
9. The textile fabric children's mask according to any one of claims 1 to 8, wherein: The melt blending treatment conditions at least meet the following requirements: temperature of 200-260° C., time of 0.2-1 h, and pressure of 3-5 MPa.
10. The textile fabric children's mask according to any one of claims 1 to 9, wherein: The cooling and curing treatment conditions at least meet the following requirements: temperature of 20-30° C. and time of 0.2-0.5 h.
11. A method for preparing the textile fabric children's mask according to claims 1-10, characterized in that: The method includes: (1) stacking the textile fabric A, the hydrogen-adjusted polypropylene meltblown fabric, and the textile fabric B in order from outside to inside to obtain a mask body; (2) A nose bridge strip is sewn on the upper side of the mask body, and the mask rope is fixed on the left and right sides of the mask body.