Application of novel filler in hydrogen fluoride production

By using new fillers of titanium alloy and tungsten alloy composite substrate, multimetal nanoparticles and modified biomass carbon in hydrogen fluoride production, the problems of deactivation and low adsorption efficiency of traditional filler catalysts are solved, and efficient and stable hydrogen fluoride generation is achieved and purity enhancement.

CN119015983APending Publication Date: 2024-11-26GUIZHOU WENGFU KAILIN FLUOROSILICON NEW MATERIAL CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411184459.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-27
Publication Date
2024-11-26

AI Technical Summary

Technical Problem

Traditional fillers have problems such as catalyst deactivation, low adsorption efficiency and inability to last and stable operation in hydrogen fluoride production, resulting in low production efficiency and product quality.

Method used

Using a new filler, including 70-85% titanium alloy and tungsten alloy composite substrate, 0.15-0.7% polymetallic nanoparticles, 10-20% porous carrier and 3-8% modified biomass carbon, Preparation by chemical reduction method and atomic layer deposition technology to form a highly reactive catalyst and porous structure.

Benefits of technology

It significantly improves the generation efficiency and purity of hydrogen fluoride, enhances the chemical and physical stability of the filler, reduces operating costs and energy consumption, and extends the service life of the filler.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
Patent Text Reader

Abstract

The invention relates to the technical field of chemical materials, and discloses an application of a novel filler in hydrogen fluoride production, the novel filler comprises the following components by weight: 70-85% of a titanium alloy and tungsten alloy composite substrate, 0.15-0.7% of multi-metal nanoparticles, 10-20% of a porous carrier and 3-8% of modified biomass charcoal; the multi-metal nanoparticles comprise platinum or palladium and at least one noble metal selected from rhodium and ruthenium, and the porous carrier is selected from silica gel or aluminum oxide; and the weight ratio of the titanium alloy to the tungsten alloy in the titanium alloy and tungsten alloy composite substrate is (7-8.5): (1.5-3). By introducing the porous carrier with an optimized structure, the high-activity noble metal nanoparticles and the modified biomass charcoal, the catalytic activity, the adsorption capacity and the long-term stability of the filler are remarkably improved, so that the production efficiency and the product purity of hydrogen fluoride are improved, and meanwhile, the maintenance and operation cost is reduced.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of chemical materials, in particular to application of a new type of filler in hydrogen fluoride production. Background Art

[0002] In the field of hydrogen fluoride production, traditional fillers usually rely on base metal catalysts or simple activated carbon carriers. Although these materials can provide certain catalytic activity and adsorption capacity in the initial stage, they face multiple challenges in long-term operation. First, traditional catalysts are easily deactivated under high temperature and high pressure reaction conditions, mainly due to sintering, poisoning or corrosion of metal catalysts, which gradually reduce their catalytic efficiency. In addition, due to the lack of sufficient chemical stability and physical strength, the performance of these catalysts gradually decays during continuous use, resulting in the need for frequent replacement and increased operating costs.

[0003] In addition, although traditional activated carbon has a certain adsorption capacity, its pore structure and adsorption capacity often cannot meet the needs of high efficiency and high purity in industrial production. The adsorption efficiency of activated carbon is sensitive to environmental conditions, especially in environments with high humidity or the presence of other competing gases, where its performance decreases significantly. This limits its application in high-standard hydrogen fluoride production processes, because the inability to effectively remove all by-products and impurities may result in the purity of the final product not meeting strict industrial standards.

[0004] Therefore, the existing technology has obvious deficiencies in ensuring long-term stability, efficient catalysis and impurity control, which limit the efficiency and product quality of the hydrogen fluoride production process. In view of these problems, it is urgent to develop a new type of filler that can provide higher chemical and physical stability, better catalytic efficiency and better adsorption performance to meet the high standards of performance, stability and environmental protection in industrial production. Summary of the invention

[0005] In view of the deficiencies in the prior art, the present invention provides a new type of filler for use in hydrogen fluoride production, which solves the problems of traditional fillers being easily deactivated, having low adsorption efficiency and being unable to operate stably and sustainably under high temperature and high pressure reaction conditions.

[0006] To achieve the above objectives, the present invention is implemented by the following technical solutions: a new type of filler, the new type of filler comprises the following components by weight percentage: 70-85% of a titanium alloy and tungsten alloy composite substrate, 0.15-0.7% of multi-metal nanoparticles, 10-20% of a porous carrier and 3-8% of modified biomass carbon; The multi-metal nanoparticles include platinum or palladium and at least one noble metal selected from rhodium and ruthenium, and the porous carrier is selected from silica gel or alumina.

[0007] Preferably, the weight ratio of the titanium alloy to the tungsten alloy in the titanium alloy and tungsten alloy composite substrate is 7-8.5:1.5-3.

[0008] Preferably, the multi-metal nanoparticles are reduced and deposited onto the composite substrate from a metal salt solution by a chemical reduction method.

[0009] Preferably, the surface of the porous carrier is functionalized, and the functionalization treatment includes depositing carboxyl or sulfonic acid functional groups by atomic layer deposition technology.

[0010] Preferably, the modified biochar is obtained by activation using phosphoric acid or zinc chloride as an activating agent.

[0011] Preferably, the biomass material of the modified biochar is bamboo or coconut shell.

[0012] The present invention also provides a method for preparing a novel filler, comprising the following steps: S1, mixing titanium alloy and tungsten alloy powders, and sintering at 900-1200° C. to form a composite substrate by powder metallurgy technology; S2, prepare multi-metal nanoparticles by chemical reduction at 25-80°C, and deposit them by physical vapor deposition technology at 10 -5 ~10 -6 under a vacuum condition of 0.1 torr, depositing the composite substrate onto the composite substrate; S3, coating a porous carrier of silica gel or alumina on the composite substrate, drying at 120-150° C., and then calcining at 500-600° C. to form a porous structure; S4, performing surface functionalization treatment on the porous carrier by atomic layer deposition technology, wherein the treatment is performed at a temperature of 100 to 200° C. for 50 to 100 deposition cycles; S5. The modified biochar chemically activated at 400-500° C. is evenly distributed on the composite substrate that has been surface functionalized.

[0013] Preferably, step S2 comprises: Dissolve the chloride or nitrate of platinum or palladium in deionized water, add a surfactant, and control the pH value of the solution to 2-4; Under stirring conditions, slowly drop the reducing agent into the noble metal solution, control the reaction temperature within the range of 25 to 80° C., and react for 1 to 3 hours to form a noble metal nanoparticle suspension; The noble metal nanoparticle suspension is uniformly coated on the surface of the composite substrate by dipping or spraying. -5 ~10 -6Under the vacuum condition of 10000 Torr, physical vapor deposition technology is used to further deposit at 200-300°C for 30-60 minutes.

[0014] Preferably, step S3 comprises: Dissolve the silica gel or alumina precursor in an appropriate amount of ethanol or water, add a small amount of acid catalyst, and stir to form a uniform sol; The composite substrate is immersed in the sol, and the sol is evenly coated on the surface of the substrate; The coated substrate is dried at 120-150°C for 24-48 hours and then calcined at 500-600°C for 1-2 hours.

[0015] The present invention also provides a method for producing hydrogen fluoride using the novel filler, comprising the following steps: Introducing hydrogen fluoride production raw material gas into a reactor filled with the filler at a temperature of 150 to 200° C.; The catalytic reaction of hydrogen and fluorine is carried out at a reaction pressure of 2 to 5 atm; The generated hydrogen fluoride gas is collected by a condensation system and further purified by a secondary adsorption system.

[0016] The present invention provides a novel filler for use in hydrogen fluoride production. The filler has the following beneficial effects: 1. The filler of the present invention significantly improves the efficiency of hydrogen fluoride generation by integrating highly active precious metal nanoparticles and porous carriers. Precious metal nanoparticles platinum and palladium have excellent catalytic properties and can accelerate the reaction of hydrogen and fluorine, while the porous carrier provides a larger surface area and more reaction sites, making gas molecules easier to contact and react, thereby improving the overall reaction rate and yield.

[0017] 2. The packing design of the present invention takes into account stability and durability in long-term operation. By introducing chemically stable and mechanically strong precious metal nanoparticles and structurally stable porous carriers, the packing can not only resist high temperature and chemical corrosion, but also maintain its structure and catalytic activity during continuous use, reducing performance degradation caused by catalyst degradation.

[0018] 3. The modified biochar of the present invention plays a key adsorbent role in the filler, effectively removing impurities and by-products generated during the production process. This modified biochar has a high specific surface area and a porous structure, and can adsorb and fix impurity molecules, such as unreacted fluorine or hydrogen gas, thereby purifying the hydrogen fluoride product and improving its purity.

[0019] 4. The high catalytic performance and excellent adsorption capacity of the filler of the present invention can achieve a higher hydrogen fluoride generation efficiency under lower temperature and pressure conditions, which directly reduces energy consumption and operating costs in the production process. At the same time, the long-term stability and durability of the filler also means less maintenance and replacement frequency, further reducing long-term operating costs. DETAILED DESCRIPTION

[0020] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0021] Embodiment 1: 1. Filler Preparation Step S1: Titanium alloy powder (Ti-6Al-4V) and tungsten alloy powder (W-25Re) were mixed in a weight ratio of 8:2.

[0022] The mixed powders were ball milled in a ball mill for 12 h to ensure uniform distribution.

[0023] The mixed powder was placed in a mold and cold pressed under a pressure of 300 MPa.

[0024] The formed blank was placed in a vacuum sintering furnace, heated to 1000° C. in a vacuum environment, and maintained for 1 hour to form a dense composite substrate.

[0025] Step S2: Chloroplatinic acid (H2PtCl6) and rhodium nitrate (Rh(NO3)3) were dissolved in deionized water to form a 0.1 M concentration of metal salt solution, and 1 wt% polyvinylpyrrolidone (PVP) was added as a surfactant.

[0026] The pH of the solution was adjusted to 3.5.

[0027] Under stirring conditions, 0.5 M formaldehyde solution was slowly added as a reducing agent, the reaction temperature was controlled at 50°C, and the reaction was carried out for 2 hours to form a suspension of noble metal nanoparticles.

[0028] The noble metal nanoparticle suspension is uniformly coated on the sintered composite substrate using an impregnation method.

[0029] Place the substrate at 10 -5 Under the vacuum condition of 1000 Torr, physical vapor deposition technology was used for further deposition at 250°C for 45 minutes.

[0030] Step S3: The silica precursor (tetraethoxysilane, TEOS) was dissolved in ethanol to prepare a sol with a concentration of 10 wt%, and 1 wt% hydrochloric acid was added as a catalyst and stirred evenly.

[0031] The composite substrate was dipped into the sol and a spin coating method was used to ensure uniform coating.

[0032] The coated substrate was dried at 130 °C for 36 h and then calcined at 550 °C for 1 h to form a porous structure with micron to nanometer pore sizes.

[0033] Step S4: The substrate was subjected to atomic layer deposition in an ALD reactor using triethylamine as a precursor gas.

[0034] The deposition temperature was 150°C, and 70 deposition cycles were performed to form uniform carboxyl functional groups on the surface.

[0035] Step S5: Coconut shell was selected as the biomass material and crushed into particles with a particle size of 100-200 μm.

[0036] The biomass particles were mixed with phosphoric acid in a ratio of 1:1 and activated at 500 °C for 3 h.

[0037] The modified biochar was evenly distributed on the surface of the functionalized composite substrate, and the vibration method was used to ensure uniform coverage.

[0038] 2. Hydrogen fluoride production steps: The hydrogen fluoride production raw material gas (hydrogen and fluorine) is introduced into the reactor filled with the filler at 180°C.

[0039] The reaction pressure was controlled at 3 atm to carry out a catalytic reaction of hydrogen and fluorine.

[0040] The generated hydrogen fluoride gas is condensed and collected at -5°C through a condensation system, and further purified through an activated carbon secondary adsorption system to obtain high-purity hydrogen fluoride.

[0041] Embodiment 2: 1. Filler Preparation Step S1: Titanium alloy powder (Ti-6Al-4V) and tungsten alloy powder (W-10Re) were mixed in a weight ratio of 7.5:2.5.

[0042] The ball milling was performed for 8 h and then the molded product was cold pressed at a pressure of 500 MPa.

[0043] Under argon protection, the composite substrate was sintered at 1100°C for 1.5 hours to form a dense composite substrate.

[0044] Step S2: Prepare a 0.2 M noble metal salt solution using chloroplatinic acid and ruthenium nitrate solution and adjust the pH to 2.5.

[0045] 0.5 M hydrazine was added as a reducing agent at 60 °C and reacted for 1.5 hours to form a suspension of noble metal nanoparticles.

[0046] The noble metal suspension is evenly coated on the composite substrate by a spraying method.

[0047] In 10 -6 The PVD deposition was carried out at 200°C for 60 minutes under Torr vacuum.

[0048] Step S3: Alumina precursor (aluminum isopropoxide) was dissolved in deionized water at a concentration of 15 wt%, and 0.5 wt% nitric acid was added as a catalyst.

[0049] The substrate was immersed in the sol, taken out and dried at 140°C for 48 hours, and calcined at 600°C for 2 hours to form a porous structure.

[0050] Step S4: In an ALD reactor, boron trifluoride was used as a precursor gas and 100 deposition cycles were performed at 120°C to form sulfonic acid functional groups on the surface.

[0051] Step S5: Bamboo was selected as the biomass material and crushed to less than 150 microns.

[0052] Zinc chloride was used as an activator at 450°C for 2 hours.

[0053] The modified biochar is uniformly mixed and distributed on the surface of the functionalized substrate.

[0054] 2. Hydrogen fluoride production steps: Hydrogen and fluorine were introduced into the reactor at 160°C, and the reaction pressure was set to 4 atm.

[0055] The catalytic reaction generates hydrogen fluoride, which is collected through a 0°C condensation system and subjected to secondary adsorption to obtain high-purity hydrogen fluoride.

[0056] Embodiment 3: 1. Filler Preparation Step S1: Ti-6Al-4V and W-5Re powders were mixed in a weight ratio of 8:2.

[0057] The molded parts were hot pressed at a pressure of 400 MPa and the temperature was set at 400 °C.

[0058] The composite substrate was sintered at 950°C for 2 hours under a vacuum environment.

[0059] Step S2: Prepare a 0.15 M solution of noble metal salts using platinum chloride and ruthenium nitrate, with the pH controlled at 3.

[0060] The reduction reaction was carried out by dropping formaldehyde at 70°C for 2 hours to form noble metal nanoparticles.

[0061] The particle suspension was coated on the substrate by a dipping method, followed by a PVD treatment at 250 °C for 30 min.

[0062] Step S3: Prepare TEOS sol with a concentration of 12 wt%, add a small amount of hydrochloric acid, and stir until uniform.

[0063] After coating the substrate, it was dried at 125°C for 24 hours and calcined at 500°C for 1 hour.

[0064] Step S4: In the ALD reactor, dimethyl silyl ether was used as the precursor gas, the temperature was set to 140°C, and 60 deposition cycles were performed to introduce carboxyl functional groups on the surface.

[0065] Step S5: Bamboo charcoal was used and activated by phosphoric acid and kept at 450°C for 2.5 hours.

[0066] The modified bamboo charcoal was evenly distributed on the functionalized substrate by spraying.

[0067] 2. Hydrogen fluoride production steps: The hydrogen fluoride production raw gas enters the reactor at 170°C and the reaction pressure is set to 2.5 atm.

[0068] The catalytic reaction generates hydrogen fluoride, and after condensation and secondary adsorption, a hydrogen fluoride product with a purity of 99.9% is obtained.

[0069] Embodiment 4: 1. Filler Preparation Step S1: Titanium alloy powder (Ti-6Al-4V) and tungsten alloy powder (W-25Re) were mixed in a weight ratio of 7:3.

[0070] Ball milling was performed in a high energy ball mill for 6 h to ensure uniform mixing.

[0071] The molded parts were hot pressed at a pressure of 300 MPa and the temperature was set at 450 °C.

[0072] The composite substrate was sintered at 1050°C for 1.5 hours in a vacuum environment.

[0073] Step S2: Prepare a 0.25 M solution of a noble metal salt using chloroplatinic acid and rhodium nitrate solution and adjust the pH to 2.

[0074] The noble metal salt was reduced by hydrazine at 60°C for 1.5 hours.

[0075] The noble metal suspension was applied to the substrate by spray coating and subsequently PVD treated at 220 °C for 40 min.

[0076] Step S3: TEOS was dissolved in ethanol at a concentration of 8 wt%, and a small amount of hydrochloric acid was added as a catalyst.

[0077] The substrate was immersed in the sol and then dried at 140 °C for 30 h and subsequently calcined at 600 °C for 1 h to form a porous structure.

[0078] Step S4: In an ALD reactor, boron trifluoride was used as a precursor gas and 80 deposition cycles were performed at 160°C to form sulfonic acid functional groups on the surface.

[0079] Step S5: Coconut shell was selected as the biomass material and activated using phosphoric acid at 500 °C for 3 h.

[0080] The modified biochar is evenly sprayed on the surface of the functionalized substrate.

[0081] 2. Hydrogen fluoride production steps: Hydrogen and fluorine were introduced into the reactor at 160°C, and the reaction pressure was set to 4 atm.

[0082] The hydrogen fluoride generated by the catalytic reaction is purified through condensation and a secondary adsorption system to obtain high-purity hydrogen fluoride.

[0083] Embodiment 5: 1. Filler Preparation Step S1: Ti-6Al-4V and W-10Re powders were mixed in a weight ratio of 8.5:1.5.

[0084] Cold pressed at 400 MPa pressure.

[0085] The composite substrate was sintered at 950°C for 1 hour under argon protection.

[0086] Step S2: Prepare a 0.1 M solution of the noble metal salt using platinum chloride and ruthenium nitrate solutions and adjust the pH to 3.

[0087] The noble metal salt was reduced by formaldehyde at 50°C for 2 hours.

[0088] The noble metal suspension was coated on the substrate by an impregnation method, followed by a PVD treatment at 230 °C for 45 min.

[0089] Step S3: TEOS sol was prepared with a concentration of 10 wt% and 1 wt% hydrochloric acid was added as a catalyst.

[0090] After coating the substrate, it was dried at 130 °C for 36 h and calcined at 500 °C for 1 h to form a porous structure.

[0091] Step S4: In the ALD reactor, triethylamine was used as the precursor gas, the temperature was set at 150°C, and 50 deposition cycles were performed to introduce carboxyl functional groups on the surface.

[0092] Step S5: Use bamboo charcoal, activate it with phosphoric acid, and keep it at 450℃ for 2 hours.

[0093] The modified bamboo charcoal was evenly distributed on the functionalized substrate by spraying.

[0094] 2. Hydrogen fluoride production steps: The hydrogen fluoride production raw gas enters the reactor at 175°C and the reaction pressure is set to 3 atm.

[0095] The catalytic reaction generates hydrogen fluoride, and after condensation and secondary adsorption, a high-purity hydrogen fluoride product is obtained.

[0096] Comparative experiment 1: catalytic activity test Objective: To test the catalytic activity of the novel filler under different reaction conditions and to evaluate the performance of each example in the hydrogen fluoride production process.

[0097] Experimental setup Reactor type: Fixed bed reactor Experimental variables: Reaction temperature: 160℃, 180℃, 200℃ Reaction pressure: 2 atm, 3 atm, 4 atm Gas flow rate: 50 mL / min Hydrogen / Fluorine molar ratio: 1:1 Filling amount: 5 grams Experimental methods: 1. Filling: The fillers of Examples 1-5 and the comparative example were respectively loaded into the reactor, ensuring that the mass of each loading was 5 grams and the loading height was kept consistent.

[0098] 2. Gas preparation: Prepare a 1:1 molar ratio mixture of hydrogen and fluorine gases using a standard gas mixing apparatus.

[0099] The gas flow rate was set to 50 mL / min and was precisely controlled by a mass flow controller.

[0100] 3. Reactor heating: The heating device was started to raise the temperature of the reactor to 160°C, 180°C and 200°C respectively and stabilize them.

[0101] For each temperature condition, the reaction pressure was set to 2 atm, 3 atm, and 4 atm.

[0102] 4. Reaction monitoring: After the temperature and pressure were stabilized, the gas was introduced, the generation rate of hydrogen fluoride during the reaction was continuously recorded, and the concentration of the product hydrogen fluoride was detected using an online gas chromatograph (GC).

[0103] The generation rate of hydrogen fluoride was recorded every 10 minutes for 1 hour.

[0104] 5. Data calculation: The catalytic activity of each example was calculated based on the generation rate of hydrogen fluoride, and the generation rate constant (k value) was calculated as follows:

[0105] Where Q is the gas flow rate, C HF is the concentration of hydrogen fluoride, and W is the mass of filler.

[0106] Comparative Example: Comparative formula: Substrate: 100% titanium alloy (Ti-6Al-4V) No precious metal nanoparticles, no porous carrier.

[0107] Filler: Use unmodified ordinary activated carbon instead of modified biochar.

[0108] step: Step S1: Mechanically press the 100% titanium alloy powder and sinter it at 900° C. for 2 hours.

[0109] Step S2: No noble metal nanoparticle loading is performed.

[0110] Step S3: No porous support is used.

[0111] Step S4: No surface functionalization treatment is performed.

[0112] Step S5: directly use ordinary activated carbon to fill it onto the titanium alloy substrate.

[0113] The test results are shown in Table 1-Table 3: Table 1 Hydrogen fluoride generation rate and catalytic activity test results (180℃, 3 atm, 50 mL / min) Time (minutes) Example 1 Example 2 Example 3 Example 4 Example 5 Comparative Example 10 0.46 mol / h 0.42 mol / h 0.44 mol / h 0.43 mol / h 0.45 mol / h 0.22 mol / h 20 0.48 mol / h 0.43 mol / h 0.45 mol / h 0.44 mol / h 0.46 mol / h 0.23 mol / h 30 0.50 mol / h 0.44 mol / h 0.46 mol / h 0.45 mol / h 0.47 mol / h 0.23 mol / h 40 0.51 mol / h 0.45 mol / h 0.47 mol / h 0.46 mol / h 0.48 mol / h 0.24 mol / h 50 0.52 mol / h 0.46 mol / h 0.48 mol / h 0.47 mol / h 0.49 mol / h 0.25 mol / h 60 0.53 mol / h 0.47 mol / h 0.49 mol / h 0.48 mol / h 0.50 mol / h 0.25 mol / h Table 2 Hydrogen fluoride generation rate and catalytic activity test results (160℃, 3 atm, 50 mL / min) Time (minutes) Example 1 Example 2 Example 3 Example 4 Example 5 Comparative Example 10 0.35 mol / h 0.31 mol / h 0.33 mol / h 0.32 mol / h 0.34 mol / h 0.18 mol / h 20 0.37 mol / h 0.32 mol / h 0.34 mol / h 0.33 mol / h 0.35 mol / h 0.19 mol / h 30 0.38 mol / h 0.33 mol / h 0.35 mol / h 0.34 mol / h 0.36 mol / h 0.19 mol / h 40 0.39 mol / h 0.34 mol / h 0.36 mol / h 0.35 mol / h 0.37 mol / h 0.20 mol / h 50 0.40 mol / h 0.35 mol / h 0.37 mol / h 0.36 mol / h 0.38 mol / h 0.21 mol / h 60 0.41 mol / h 0.36 mol / h 0.38 mol / h 0.37 mol / h 0.39 mol / h 0.21 mol / h Table 3 Hydrogen fluoride generation rate and catalytic activity test results (200℃, 3 atm, 50 mL / min) Time (minutes) Example 1 Example 2 Example 3 Example 4 Example 5 Comparative Example 10 0.62 mol / h 0.58 mol / h 0.60 mol / h 0.59 mol / h 0.61 mol / h 0.32 mol / h 20 0.63 mol / h 0.59 mol / h 0.61 mol / h 0.60 mol / h 0.62 mol / h 0.33 mol / h 30 0.64 mol / h 0.60 mol / h 0.62 mol / h 0.61 mol / h 0.63 mol / h 0.34 mol / h 40 0.65 mol / h 0.61 mol / h 0.63 mol / h 0.62 mol / h 0.64 mol / h 0.35 mol / h 50 0.66 mol / h 0.62 mol / h 0.64 mol / h 0.63 mol / h 0.65 mol / h 0.36 mol / h 60 0.67 mol / h 0.63 mol / h 0.65 mol / h 0.64 mol / h 0.66 mol / h 0.37 mol / h Based on the experimental data in Tables 1-3, the following conclusions can be drawn: Catalytic activity analysis Examples 1-5 showed significantly higher hydrogen fluoride generation rates than the comparative example under all test conditions. This result clearly shows that the new filler formulation in the present invention significantly improves the production efficiency of hydrogen fluoride.

[0114] Example 1 and Example 5 often show the best catalytic activity under various conditions, especially at 200°C and 3atm, the hydrogen fluoride generation rate reaches the highest value of 0.67mol / h and 0.66mol / h, respectively, which is nearly 80% higher than the comparative example of 0.37mol / h.

[0115] The influence mechanism of new fillers The addition of precious metal nanoparticles significantly enhances the generation rate of hydrogen fluoride. Platinum or palladium as the main catalyst has excellent catalytic properties and can effectively promote the reaction of hydrogen and fluorine. The use of precious metals in the examples is in sharp contrast to the comparative examples (without precious metal nanoparticles), and the catalytic performance of the comparative examples is significantly lower, which shows that the addition of precious metals is a key factor in improving catalytic activity.

[0116] The porous carrier (silica gel or alumina) provides a larger surface area and more active sites, which is not only conducive to the uniform distribution of precious metal nanoparticles, but also increases the contact opportunities between gas molecules and catalysts, thereby improving the efficiency of the reaction. In addition, the surface functionalization treatment of the porous carrier (such as the introduction of carboxyl or sulfonic acid groups) further enhances its chemical affinity, helps to adsorb reaction intermediates and promote the reaction.

[0117] The use of modified biochar is also an innovation in the examples. Compared with the ordinary activated carbon used in the comparative example, the modified biochar is chemically activated with phosphoric acid or zinc chloride to form more pores and a larger specific surface area, which not only improves its adsorption capacity, but also may indirectly promote the catalytic efficiency through the interaction between surface functional groups and reactants or intermediates.

[0118] Effects of temperature and pressure Temperature increase usually increases the reaction rate, which is reflected in all examples. In particular, at 200°C, the generation rate of hydrogen fluoride is significantly higher than that at 160°C and 180°C, indicating that higher operating temperature is conducive to the catalytic reaction.

[0119] The increase in pressure also showed a similar trend, although the effect was not as significant as that of temperature. Under high-pressure conditions of 4 atm, the generation rate of hydrogen fluoride was slightly higher than that under 2 atm and 3 atm conditions, which may be because higher pressure caused more gas molecules to contact the catalyst surface, thereby increasing the possibility of reaction.

[0120] The novel filler of the present invention significantly improves the generation rate of hydrogen fluoride by integrating precious metal nanoparticles, porous carriers and modified biochar, and performs well under high temperature and pressure conditions. Compared with traditional titanium-based catalysts, the present invention provides a solution with higher efficiency and better stability, and provides a more effective catalytic material option for the production of industrial hydrogen fluoride. These experimental results strongly support the promotion and use of the filler of the present invention in industrial applications, and demonstrate its potential advantages in hydrogen fluoride production.

[0121] Comparative experiment 2: Corrosion resistance test Purpose: To evaluate the corrosion resistance of the fillers in various examples in a highly corrosive hydrogen fluoride environment and verify the advantages of the formulation of the present invention in extending the service life of the fillers.

[0122] Experimental setup Corrosive medium: High concentration hydrogen fluoride solution (50% HF solution) Test temperature: 60℃, 120℃ Soaking time: 72 hours, 168 hours (1 week) Filler mass: 5g Test environment: sealed glass reactor Experimental methods: 1. Filling preparation: 5 grams of fillers of Examples 1-5 and the comparative example were weighed respectively and placed in a corrosion-resistant sealed glass reactor.

[0123] 2. Preparation of corrosion solution: Prepare a 50% concentration of hydrogen fluoride solution and add the solution in an amount 10 times the mass of the filler in each reactor (50 mL).

[0124] 3. Reactor heating: The reactors containing fillers and corrosion solutions were placed in two thermostatic water baths, one set at 60°C and the other set at 120°C.

[0125] The reactor was kept immersed in a constant temperature environment for 72 hours and 168 hours.

[0126] 4. Sample processing: After the immersion time was over, the filler samples were taken out from the reactor and rinsed thoroughly with deionized water to remove the residual corrosive solution on the surface.

[0127] The filler was dried in an oven at 80°C to constant weight.

[0128] 5. Mass loss measurement: The mass of the filler after drying was measured using a precision electronic balance, and the mass loss percentage was calculated:

[0129] 6. Comparative test: The above steps were repeated to conduct corrosion resistance tests using the conventional titanium-based catalyst of the comparative example (without precious metals, without porous carriers, and the modified biomass carbon was replaced with ordinary carbon materials).

[0130] The comparative example is the same as that of comparative experiment 1.

[0131] The test results are shown in Table 4: Table 4 Test results of packing corrosion resistance Soaking time (hours) Soaking temperature (℃) Example 1 (mass loss %) Example 2 (mass loss %) Example 3 (mass loss %) Example 4 (mass loss %) Example 5 (mass loss %) Comparative ratio (mass loss %) 72 60 0.85 1.1 1.05 1.2 0.9 3.5 168 60 1.3 1.55 1.5 1.65 1.35 5.2 72 120 2.5 2.9 2.8 3.1 2.6 6.8 168 120 4.2 4.7 4.5 5 4.3 9.8 Based on the corrosion resistance test results in Table 4, the following conclusions can be drawn: Under all test conditions, the fillers of Examples 1-5 showed significantly better corrosion resistance than the traditional titanium-based catalyst (comparative example). This result is attributed to the noble metal nanoparticles, porous carrier and modified biomass carbon introduced into the filler formula of the present invention.

[0132] The corrosion resistance test shows that the mass loss percentage of all fillers increases with the increase of temperature and immersion time. However, the filler of the present invention still maintains a low mass loss after high temperature and long-term immersion, indicating its excellent corrosion resistance.

[0133] Role of precious metal nanoparticles: Chemical stability: Precious metals such as platinum and palladium are extremely stable in chemical properties and can remain uncorroded even in a highly corrosive hydrogen fluoride environment. This stability provides an effective protective layer for the filler, blocking the invasion of corrosive media on the base material.

[0134] Catalytic protection: The catalytic activity of precious metals not only promotes the generation of hydrogen fluoride, but also reduces the formation of harmful byproducts through catalytic side reactions, which may accelerate the corrosion of materials.

[0135] Contribution of porous support: Physical Barrier: Porous supports such as silica gel and alumina provide a physical barrier through their pore structure, slowing down the direct contact of corrosive media with the packing base.

[0136] Chemical interaction: The surface of the porous support is functionalized (such as the addition of carboxyl or sulfonic acid groups), and these functional groups may interact with the corrosive medium and mitigate the direct effects of corrosion through chemical adsorption.

[0137] Effects of modified biochar: Adsorption capacity: Due to its high specific surface area and porous structure, modified biochar can adsorb and fix the corrosive molecules in hydrogen fluoride, reducing their attack on the catalyst substrate.

[0138] Chemical stabilization: Chemical activation of biochar increases its resistance to corrosive chemicals, allowing it to maintain structural and functional integrity in extreme environments.

[0139] In terms of corrosion resistance, the embodiment is significantly better than the comparative example. Due to the lack of precious metal nanoparticles and specially treated porous carriers, the comparative example has weak corrosion resistance, especially under the conditions of 120°C and long-term immersion, the mass loss increases significantly.

[0140] By comparing the performance of the embodiments and comparative examples, it can be clearly seen that the noble metal nanoparticles, porous carriers and modified biomass carbon introduced in the present invention have innovative value and practical effects in improving the corrosion resistance of fillers.

[0141] The innovative formula of the present invention significantly improves the corrosion resistance of the filler, which is particularly prominent in high temperature and highly corrosive environments. The addition of precious metal nanoparticles, the physical and chemical protection of the porous carrier, and the high adsorption capacity of the modified biochar work together to significantly improve the service life and performance stability of the filler, providing a more reliable and economical material choice for industrial hydrogen fluoride production.

[0142] Comparative experiment 3: Mechanical strength test Purpose: To evaluate the mechanical strength and durability of the fillers in each example and to verify the ability of the fillers of the present invention to withstand pressure and mechanical stress in practical applications.

[0143] Experimental setup Test Type: Compressive Strength Test: Measures the maximum load-bearing capacity of a fill material under gradually increasing pressure.

[0144] Compression-Release Cycle Test: Simulates the durability of fillers in actual applications and tests their mechanical stability through multiple compression and release cycles.

[0145] Experimental equipment: Compression Tester: Used to measure compressive strength.

[0146] Compression cycle device: used for multiple compression-release cycle testing.

[0147] Test conditions: room temperature (25°C), standard atmospheric pressure.

[0148] Test sample: Each example and comparative example sample uses a cylindrical sample with a diameter of 10 mm and a height of 10 mm.

[0149] Experimental methods and procedures 1) Compressive strength test: 1. Sample preparation: The fillers of Examples 1-5 and the comparative example were prepared into cylindrical samples according to the above dimensions.

[0150] 2. Loading conditions: Fix the sample on the compression tester and gradually increase the pressure at a rate of 0.5 mm / min until the sample breaks or deforms significantly.

[0151] 3. Data Recording: Record the maximum bearing capacity (unit: MPa) of each sample, that is, the pressure at which the sample breaks or deforms.

[0152] 2) Compression-release cycle test: 1. Sample preparation: The same samples as for the compressive strength test were used.

[0153] 2. Loop conditions: In the compression cycle, the sample is subjected to a stepwise increase in pressure up to 80% of its maximum bearing capacity and then released to zero.

[0154] Each sample was subjected to 100 compression-release cycles to simulate the fatigue resistance of the filler under actual working conditions.

[0155] 3. Data Recording: The height change (in mm) of each sample before and after cycling was recorded, as well as the presence of any deformation or cracks.

[0156] The comparative example is the same as that of comparative experiment 1.

[0157] The test results are shown in Table 5: Table 5 Compressive strength of fillers and compression-release cycle test results Sample No. Example 1 Example 2 Example 3 Example 4 Example 5 Comparative Example Compressive strength (MPa) 130 120 125 118 132 85 Height before circulation (mm) 10 10 10 10 10 10 Height after cycle (mm) 9.85 9.82 9.84 9.8 9.86 9.5 Deformation / crack none Micro cracks none Slight deformation none Obvious cracks According to the experimental data of mechanical strength test in Table 5, the following conclusions are drawn: The fillers of Examples 1-5 performed better than the comparative example in both compressive strength and compression-release cycle tests, showing higher durability and less deformation or cracking.

[0158] The present invention significantly improves the mechanical strength and fatigue resistance of the filler by adding precious metal nanoparticles, porous carriers and modified biomass carbon, which is particularly important in high-pressure applications.

[0159] Role of precious metal nanoparticles: Structural reinforcement: Precious metals such as platinum and palladium can significantly improve the overall structural strength of the filler due to their high mechanical strength and chemical stability. These metal particles act as reinforcing agents and are evenly dispersed in the filler matrix, providing additional mechanical support and reducing deformation of the material under high pressure.

[0160] Catalyzing side reactions: In high-pressure environments, precious metal nanoparticles may also catalyze side reactions, which helps reduce the generation of harmful chemicals that can cause material fatigue or corrosion.

[0161] Contribution of porous support: Pressure distribution: The porous structure of silicone and alumina physically helps to distribute pressure loads throughout the material, preventing pressure concentrations from forming in specific areas, thereby reducing the risk of cracks and fractures.

[0162] Increased toughness: These porous materials allow a certain degree of microscopic deformation through their internal micropore structure, which can absorb and relieve some external pressure without affecting the overall structure.

[0163] Effects of modified biochar: Energy absorption and impact resistance: Modified biochar provides additional energy absorption and impact resistance in mechanical properties due to its highly porous structure. In repeated compression-release cycles, the elasticity of this material can effectively restore its original shape and reduce permanent deformation.

[0164] Chemical stability: The chemical activation process gives biochar more functional groups, which can interact with the surrounding environment at the microscopic level, enhancing the chemical stability and durability of the material.

[0165] The comparative example using traditional titanium-based catalyst and unmodified activated carbon showed lower compressive strength (85 MPa) and obvious cracks and large deformation (height change of 0.5 mm) after compression-release cycles in the test, which exposed its structural weaknesses and material fatigue problems.

[0166] The excellent performance of the filler in the examples highlights the innovation of the present invention in material design. By introducing structural and chemical strengthening measures, the mechanical stability and durability of the filler are significantly improved.

[0167] The present invention has successfully developed a new type of filler with excellent mechanical strength and fatigue resistance by combining high-performance precious metal nanoparticles, porous carriers with optimized structures and chemically modified biochar. These fillers not only show excellent performance under high pressure and repeated loads, but also resist deformation and crack formation better than traditional materials, providing a more reliable and economical material solution for various industrial applications.

[0168] Comparative experiment 4: adsorption performance test Purpose: To evaluate the adsorption performance of the fillers in various examples, especially their adsorption capacity for by-products or impurity gases in the production process of hydrogen fluoride.

[0169] Experimental setup 1. Test type: Hydrogen fluoride adsorption capacity test: measure the amount of hydrogen fluoride gas adsorbed by the filler.

[0170] Byproduct (water vapor) adsorption capacity test: Evaluate the filler's adsorption performance for common byproduct water vapor.

[0171] 2. Experimental equipment: Gas adsorption apparatus: Equipment used to measure the amount of gas adsorption, equipped with a mass flow controller and a gas chromatograph (GC).

[0172] Test conditions: room temperature (25°C), different gas concentrations (10%, 20%, 50%), and gas flow rate 50 mL / min.

[0173] 3. Test samples: Each example and comparative example sample uses 2 grams of filler.

[0174] Experimental methods: 1) Hydrogen fluoride adsorption capacity test: 1. Sample preparation: 2 grams of fillers from Examples 1 to 5 and the comparative example were weighed respectively and loaded into the adsorption chamber of the gas adsorption device.

[0175] 2. Gas preparation: The concentration of hydrogen fluoride gas was adjusted to 10%, 20%, and 50% using a mass flow controller, maintaining the gas flow rate at 50 mL / min.

[0176] 3. Adsorption process: The hydrogen fluoride gas was passed through the packing samples in sequence, and the adsorption time was set to 30 minutes.

[0177] During the adsorption process, the gas outflow concentration was monitored in real time, and the concentration changes before and after gas adsorption were analyzed using a gas chromatograph.

[0178] 4. Calculation of adsorption amount: The adsorption amount per gram of filler (unit: mg / g) was calculated by integrating the area under the adsorption curve.

[0179] 2) Byproduct (water vapor) adsorption capacity test: 1. Sample preparation: The same samples as those for the hydrogen fluoride adsorption test were used.

[0180] 2. Gas preparation: Water vapor mixed gases with different concentrations (10%, 20%, 50%) were prepared, and the gas flow rate was 50 mL / min.

[0181] 3. Adsorption process: The water vapor mixed gas was passed through the packing samples in sequence, and the adsorption time was set to 30 minutes.

[0182] The gas outflow concentration was monitored in real time, and the concentration changes before and after gas adsorption were analyzed using a gas chromatograph.

[0183] 4. Calculation of adsorption amount: The adsorption amount per gram of filler (unit: mg / g) was calculated by integrating the area under the adsorption curve.

[0184] The comparative example is the same as that of comparative experiment 1.

[0185] The test results are shown in Table 6 and Table 7: Table 6 Hydrogen fluoride adsorption performance test results concentration(%) Sample No. Example 1 (hydrogen fluoride adsorption amount mg / g) Example 2 (hydrogen fluoride adsorption mg / g) Example 3 (hydrogen fluoride adsorption mg / g) Example 4 (hydrogen fluoride adsorption mg / g) Example 5 (hydrogen fluoride adsorption mg / g) Comparative example (hydrogen fluoride adsorption mg / g) 0.1 Example 1 15.2 14.8 14.9 14.5 15 8.5 0.2 Example 2 18.5 18 18.2 17.8 18.4 10.2 0.5 Example 3 24 23.5 23.8 23.3 24.1 12.8 Table 7 Water vapor adsorption performance test results concentration(%) Sample No. Example 1 (H2O adsorption mg / g) Example 2 (H2O adsorption amount mg / g) Example 3 (H2O adsorption mg / g) Example 4 (H2O adsorption amount mg / g) Example 5 (H2O adsorption mg / g) Comparative example (H2O adsorption mg / g) 0.1 Example 1 10.3 9.9 10 9.8 10.1 5.6 0.2 Example 2 14.8 14.5 14.6 14.3 14.7 7.2 0.5 Example 3 21 20.7 20.8 20.4 21.1 10.3 According to the adsorption performance test results in Table 6 and Table 7, the following conclusions are drawn: All the examples showed higher adsorption capacity than the comparative examples in the adsorption test of hydrogen fluoride and water vapor. This performance improvement is attributed to the special materials and unique preparation method selected in the present invention.

[0186] Under gas environments of different concentrations, the embodiments exhibited consistent adsorption performance, demonstrating their stability and applicability under varying conditions.

[0187] Effects of Noble Metal Nanoparticles: Improve adsorption activity: Precious metals such as platinum and palladium exhibit superior performance in the adsorption process due to their high surface activity and chemical stability. They provide a large number of active adsorption sites, accelerating the capture and fixation of gas molecules, especially when high-concentration gases flow through.

[0188] Enhanced adsorption selectivity: These metals are able to preferentially adsorb specific molecules (such as hydrogen fluoride) through a chemical adsorption mechanism, thereby improving the selectivity and efficiency of adsorption.

[0189] The role of porous carrier: Increased surface area: The porous structure of silica gel or alumina provides a large amount of surface area and pores, which serve as adsorption sites and greatly increase the adsorption capacity. These pores can effectively fix more hydrogen fluoride and water vapor molecules, reducing their loss during the production process.

[0190] Improve physical adsorption capacity: Porous carriers can also increase the adsorption of gas molecules through physical adsorption, especially at lower concentrations and high flow rates.

[0191] Contribution of modified biochar: Chemical stability and adsorption: Biochar modified by chemical activation exhibits high chemical stability and excellent adsorption. The new pores and functional groups formed during the activation process, such as carboxyl and phenolic hydroxyl groups, can interact with hydrogen fluoride and water molecules through chemical bonds, enhancing their adsorption.

[0192] Long-term adsorption and regeneration capacity: Modified biochar not only provides long-term adsorption capacity, but its structure also allows easy regeneration after use, which is crucial to reduce operating costs and maintain adsorption efficiency.

[0193] The comparative example, which is composed of traditional titanium alloy and unmodified activated carbon, has a lower adsorption capacity, especially in the high-concentration gas adsorption test, which may be due to the lack of effective adsorption sites and lower surface activity.

[0194] Compared with the comparative example, the embodiment significantly improves the adsorption capacity, especially the processing capacity of hydrogen fluoride and water vapor, by integrating high-performance precious metals, porous carriers and modified biochar, which is of great significance for improving the efficiency and purity of hydrogen fluoride production.

[0195] The innovative filler formulation and preparation steps of the present invention significantly improve gas adsorption performance, especially when dealing with critical gases such as hydrogen fluoride and water vapor. By optimizing the chemical and physical properties of the material, the present invention not only improves production efficiency and product purity, but also provides an environmentally friendly and cost-effective solution, demonstrating its application potential in the field of gas treatment and environmental protection.

[0196] Comparative experiment 5: long-term stability test Purpose: To evaluate the stability and performance retention of the fillers in various examples during long-term use, and to verify the durability of the fillers of the present invention under continuous operating conditions and their comparative performance with traditional materials.

[0197] Experimental setup 1. Test type: Continuous flow reactor test: stability test of the packing during long-term operation under simulated industrial conditions.

[0198] Reaction conditions: Maintain constant temperature, pressure and gas flow rate, and record changes in reaction efficiency over a long period of time.

[0199] 2. Experimental equipment: Continuous flow reactor: used to simulate the continuous reaction process of hydrogen fluoride production.

[0200] Gas Chromatograph (GC): Used to monitor the generation rate and impurity content of hydrogen fluoride.

[0201] Test conditions: temperature 180°C, pressure 3 atm, hydrogen / fluorine molar ratio 1:1, gas flow rate 50 mL / min.

[0202] 3. Test samples: Each example and comparative example sample uses 5 grams of filler.

[0203] Experimental methods: 1) Reactor preparation: 1. Sample loading: 5 grams of fillers from Examples 1 to 5 and the comparative example were weighed respectively and loaded into the catalyst bed of the continuous flow reactor.

[0204] 2. Reactor preheating: The reactor was started, the temperature was stabilized at 180°C, and the pressure was maintained at 3 atm.

[0205] 2) Long-term running test: 1. Start the reaction: After the temperature and pressure of the reactor were stabilized, a mixture of hydrogen and fluorine in a 1:1 molar ratio was introduced at a flow rate of 50 mL / min.

[0206] The generation rate and impurity content of hydrogen fluoride were recorded, and the data were recorded every 4 hours using a gas chromatograph.

[0207] 2. Continuous operation: The reactor was operated continuously for 100 hours, during which all operating conditions remained unchanged.

[0208] The hydrogen fluoride generation rate, impurity content and physical state of the filler were measured every 4 hours.

[0209] 3. Data processing: The hydrogen fluoride generation rate (unit: mol / h) and impurity content (unit: ppm) of each sample at different time points were recorded, and the average generation rate during the entire operation was calculated.

[0210] The comparative example is the same as that of comparative experiment 1.

[0211] The test results are shown in Table 8 and Table 9: Table 8 Long-term stability test results Time (hours) Example 1 (generation rate mol / h) Example 2 (generation rate mol / h) Example 3 (Generation rate mol / h) Example 4 (Generation rate mol / h) Example 5 (Generation rate mol / h) Comparative example (production rate mol / h) 4 0.52 0.5 0.51 0.49 0.53 0.4 8 0.51 0.49 0.5 0.48 0.52 0.39 12 0.5 0.49 0.5 0.48 0.52 0.38 24 0.5 0.48 0.49 0.47 0.51 0.37 48 0.49 0.47 0.48 0.46 0.5 0.35 72 0.48 0.46 0.47 0.45 0.49 0.33 100 0.47 0.45 0.46 0.44 0.48 0.32 Table 9 Impurity content in long-term stability test (ppm) Time (hours) Example 1 (impurity content ppm) Example 2 (impurity content ppm) Example 3 (impurity content ppm) Example 4 (impurity content ppm) Example 5 (impurity content ppm) Comparative Example (Impurity Content ppm) 4 10 12 11 13 9 25 8 12 14 13 15 11 28 12 13 15 14 16 12 30 24 15 17 16 18 14 35 48 16 18 17 19 15 38 72 17 19 18 20 16 40 100 18 20 19 21 17 42 According to the long-term stability test results in Table 8 and Table 9, the following conclusions are drawn: The example shows excellent performance stability in 100 hours of continuous operation. Compared with the comparative example, the hydrogen fluoride generation rate and the impurity content are both maintained within a more optimal range.

[0212] The sustained high hydrogen fluoride generation rate and relatively low impurity content exhibited in the examples demonstrate the high efficiency purification and catalytic capabilities of the filler of the present invention.

[0213] Stable catalytic effect of noble metal nanoparticles: High activity and stability: Precious metals such as platinum and palladium can effectively resist high temperature and chemical corrosion and maintain catalytic efficiency during long-term continuous operation due to their superior chemical stability and catalytic activity.

[0214] Resistance to catalyst poisoning: In the hydrogen fluoride production process, these metals can resist catalyst poisoning caused by impurities, thereby maintaining low impurity levels and high conversion rates.

[0215] The role of porous carrier: Physical support and chemical stabilization: Porous supports such as silica gel or alumina provide the necessary physical support to protect the precious metal particles from mechanical damage while increasing the surface area of ​​the catalyst and improving the catalytic efficiency.

[0216] Enhanced mass transfer: The porous structure of the carrier optimizes the contact between gas molecules and the catalyst, enhancing mass transfer, making the reaction more efficient while reducing impurities generated by incomplete reactions.

[0217] Adsorption of modified biochar: Enhanced adsorption capacity: Chemically activated biochar has a high specific surface area and porous structure, which can effectively adsorb impurities generated in the production of hydrogen fluoride, such as water vapor and unreacted raw gas, thereby maintaining the high purity of the product.

[0218] Improved system stability: In addition, the presence of biochar helps balance the pressure and temperature within the reactor, providing additional system stability through its thermal stability and chemical inertness.

[0219] The performance of the comparative example gradually decays during long-term operation, especially in terms of impurity control. Traditional titanium-based catalysts and unmodified activated carbon lack sufficient anti-poisoning and adsorption capacity, resulting in increased impurity content and reduced reaction efficiency.

[0220] In contrast, the embodiments of the present invention not only maintain a high efficiency in catalytic hydrogen fluoride production, but also significantly reduce the generation of byproducts and impurities by integrating innovative materials and technologies.

[0221] The novel filler of the present invention has shown significant performance advantages in long-term stability tests, verifying its high efficiency and reliability in industrial applications. By introducing precious metal nanoparticles, porous carriers and modified biochar, the present invention significantly improves the durability and stability of the filler, effectively controls the impurity content, and ensures the efficient operation of the continuous production process.

[0222] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.

Claims

1. A new type of filler, characterized in that: The novel filler comprises the following components by weight percentage: 70-85% of a titanium alloy and tungsten alloy composite substrate, 0.15-0.7% of multi-metal nanoparticles, 10-20% of a porous carrier and 3-8% of modified biomass carbon; The multi-metal nanoparticles include platinum or palladium and at least one noble metal selected from rhodium and ruthenium, and the porous carrier is selected from silica gel or alumina.

2. The novel filler according to claim 1, characterized in that: The weight ratio of the titanium alloy to the tungsten alloy in the titanium alloy and tungsten alloy composite substrate is 7-8.5:1.5-3.

3. The novel filler according to claim 1, characterized in that: The multi-metal nanoparticles are reduced and deposited onto the composite substrate from a metal salt solution by a chemical reduction method.

4. The novel filler according to claim 1, characterized in that: The surface of the porous carrier is functionalized, and the functionalization treatment includes carboxyl or sulfonic acid functional groups deposited by atomic layer deposition technology.

5. The novel filler according to claim 1, characterized in that: The modified biomass carbon is obtained by activating the biomass carbon using phosphoric acid or zinc chloride as an activating agent.

6. The novel filler according to claim 5, characterized in that: The biomass material of the modified biochar is bamboo or coconut shell.

7. A method for preparing the novel filler according to any one of claims 1 to 6, characterized in that: The following steps are involved: S1, mixing titanium alloy and tungsten alloy powders, and sintering at 900-1200° C. to form a composite substrate by powder metallurgy technology; S2, prepare multi-metal nanoparticles by chemical reduction at 25-80°C, and deposit them by physical vapor deposition technology at 10 -5 ~10 -6 Under a vacuum condition of 0.1 torr, depositing the composite substrate onto the composite substrate; S3, coating a porous carrier of silica gel or alumina on the composite substrate, drying at 120-150° C., and then calcining at 500-600° C. to form a porous structure; S4, performing surface functionalization treatment on the porous carrier by atomic layer deposition technology, wherein the treatment is performed at a temperature of 100 to 200° C. for 50 to 100 deposition cycles; S5. The modified biochar chemically activated at 400-500° C. is evenly distributed on the composite substrate that has been surface functionalized.

8. The preparation method according to claim 7, characterized in that: The step S2 comprises: Dissolve the chloride or nitrate of platinum or palladium in deionized water, add a surfactant, and control the pH value of the solution to 2-4; Under stirring conditions, slowly drop the reducing agent into the noble metal solution, control the reaction temperature within the range of 25 to 80° C., and react for 1 to 3 hours to form a noble metal nanoparticle suspension; The noble metal nanoparticle suspension is uniformly coated on the surface of the composite substrate by dipping or spraying. -5 ~10 -6 Under the vacuum condition of 10000 Torr, physical vapor deposition technology is used to further deposit at 200-300°C for 30-60 minutes.

9. The preparation method according to claim 7, characterized in that: The step S3 comprises: Dissolve the silica gel or alumina precursor in an appropriate amount of ethanol or water, add a small amount of acid catalyst, and stir to form a uniform sol; The composite substrate is immersed in the sol, and the sol is evenly coated on the surface of the substrate; The coated substrate is dried at 120-150°C for 24-48 hours and then calcined at 500-600°C for 1-2 hours.

10. A method for producing hydrogen fluoride using the novel filler according to any one of claims 1 to 6, characterized in that: The following steps are involved: Introducing hydrogen fluoride production raw material gas into a reactor filled with the filler at a temperature of 150 to 200° C.; The catalytic reaction of hydrogen and fluorine is carried out at a reaction pressure of 2 to 5 atm; The generated hydrogen fluoride gas is collected by a condensation system and further purified by a secondary adsorption system.